A hierarchical porous transport electrode with electrode-flow field synergistic defoaming, its preparation method, and a water electrolysis cell.
By setting electrode microchannels and superhydrophobic micro/nano structures on porous metal electrodes, the problem of bubble retention under high current density was solved, enabling directional bubble discharge and synergistic electrolyte transport, thus improving the operational stability and voltage performance of the water electrolysis cell.
Patent Information
- Application Number
- CN202611370483.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Under high current density, during the anion exchange membrane water electrolysis process, bubbles are retained inside the porous metal electrode, in the flow field rib region, and at the electrode-flow field interface, leading to increased electrolysis cell voltage and decreased operational stability.
Electrode microchannels are set on the side of the porous metal electrode facing the anode flow field, and superhydrophobic micro/nano structures are constructed on the porous framework and the surface of the electrode microchannels to form directional bubble removal channels. The self-pumping effect of bubbles is realized by using the interface curvature and capillary pressure difference, which promotes the bubbles to enter the electrode microchannel laterally from the original pores and be discharged into the anode flow field channel.
It effectively solved the problem of bubble retention, improved the wetting ability of the electrolyte and the desorption efficiency of bubbles, reduced the voltage of the electrolytic cell, and enhanced operational stability.
Smart Images

Figure CN123108600A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical water splitting and multiphase transport technology, specifically relating to an electrode-flow field synergistic defoaming hierarchical porous transport electrode for anion exchange membrane water electrolysis, its preparation method, and a water electrolysis cell. Background Technology
[0002] Anion exchange membrane water electrolysis achieves water splitting through the hydrogen evolution reaction at the cathode and the oxygen evolution reaction at the anode. Under high current density operating conditions, the large amount of oxygen generated at the anode needs to leave the catalytic reaction interface in a timely manner and be discharged through the porous electrode and the flow field. If bubbles remain continuously inside the porous electrode, at the electrode-flow field interface, or in the region under the flow field ribs, they will shield the reactive sites, hinder electrolyte transport, and increase bubble-related mass transfer losses, thereby leading to increased cell voltage and decreased operational stability.
[0003] Sintered porous metals possess good mechanical strength, electrical conductivity, and fluid permeability, making them suitable as porous metal electrodes on the anode side of anion exchange membranes used in water electrolysis. However, the pores formed during sintering are typically random, tortuous, and interconnected, requiring bubbles to migrate along these winding channels. When the porous metal electrode is blocked by flow field ribs, bubbles under the ribs cannot directly enter the flow field channels along the thickness direction, and tend to coalesce inside the porous electrode or at the electrode-flow field interface, forming large gas retention areas.
[0004] Existing technologies typically improve gas-liquid transport by adjusting the porosity, pore size, thickness, or surface wettability of porous materials. For example, Chinese patent application CN113731771A discloses a gradient porous transport layer that improves gas-liquid transport through interlayer porosity differences, but its structure mainly relies on multilayer material assembly and does not solve the problem of the lack of direct exhaust paths in the flow field rib region. Chinese patent application CN121373806B discloses a hydrophilic / hydrophobic gradient bilayer porous transport layer that promotes gas-liquid separation through wettability differences, but it does not form directional bubble removal channels directly corresponding to the flow field channels. Chinese patent application CN121528969A discloses a self-driven porous transport layer based on wettability gradients, which can drive bubble migration using surface energy differences, but its driving force mainly comes from the wettability gradient and does not simultaneously solve the problems of lateral bubble breakthrough paths under the flow field ribs and electrode-flow field contact.
[0005] Furthermore, while surface micro / nanostructure manipulation alone can reduce bubble adhesion and promote bubble desorption, the desorbed bubbles may still be constrained by the random pores and flow field ribs inside the porous metal electrode; and processing channels only in the porous electrode may disrupt the contact between the electrode and the flow field ribs, affecting mechanical support and electronic conduction.
[0006] Therefore, the retention of air bubbles inside porous metal electrodes, in the flow field rib region, and at the electrode-flow field interface during water electrolysis remains a problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the problem of bubble retention inside the porous anode, under the flow field ribs, and at the electrode-flow field interface during high current density water electrolysis, this invention provides a graded porous transport electrode with synergistic bubble removal by the electrode and flow field, its preparation method, and a water electrolysis cell.
[0008] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a hierarchical porous transport electrode for electrode-flow field synergistic defoaming, comprising a porous metal electrode, wherein an electrode microchannel is provided on one side of the porous metal electrode, the electrode microchannel corresponding to the anodic flow field channel provided on the anodic flow field plate in the water electrolysis cell; the porous skeleton surface of the porous metal electrode and the electrode microchannel surface have superhydrophobic micro / nano structures.
[0009] Preferably, the electrode microchannels are arranged in a serpentine pattern.
[0010] Preferably, the width of the electrode microchannel is 400~600 μm.
[0011] Preferably, the porous metal electrode is a sintered 316L stainless steel porous metal electrode.
[0012] Secondly, the present invention provides a method for preparing the aforementioned electrode-flow field synergistic defoaming hierarchical porous transport electrode, comprising: (1) Laser processing is performed on one side of the porous metal electrode to form an electrode microchannel, thus obtaining a laser-etched electrode; (2) The laser etching electrode is immersed in an aqueous solution of oxalic acid for chemical etching to obtain a hierarchical porous transport electrode.
[0013] Preferably, the temperature of the chemical etching is 60~80 ℃.
[0014] Preferably, the chemical etching time is 80-100 min.
[0015] Preferably, the oxalic acid aqueous solution contains 15% oxalic acid by mass.
[0016] Thirdly, the present invention provides a water electrolysis cell, comprising: an anode flow field plate and a hierarchical porous transport electrode for electrode-flow field coordinated defoaming disposed opposite to the anode flow field plate; an anode flow field channel is provided on one side of the anode flow field plate, and the electrode microchannels in the hierarchical porous transport electrode are aligned with the anode flow field channel along the flow path direction.
[0017] Preferably, in the water electrolysis cell, the width of the electrode microchannel is smaller than the width of the anode flow field channel.
[0018] Compared with the prior art, the present invention has the following beneficial effects: This invention provides an electrode microchannel corresponding to the anode flow field channel on the side of a porous metal electrode facing the anode flow field, and forms a superhydrophobic micro / nanostructure on the porous framework surface of the porous metal electrode and the surface of the electrode microchannel. The superhydrophobic micro / nanostructure improves electrolyte wetting ability and forms a low-bubble adhesion interface underwater, facilitating bubble detachment from the electrode surface with minimal adhesion. The electrode microchannel corresponding to the anode flow field channel provides a nearby lateral bubble removal outlet in the flow field rib region, shortening the migration distance of bubbles in the randomly tortuous pores and reducing bubble retention inside the porous metal electrode and at the electrode-flow field interface. When bubbles enter the more open electrode microchannel from the confined pores, their interface curvature and local capillary pressure change. The porous structure (original pores of the porous metal electrode) and the electrode microchannel... The scale transition between the channel and the anode flow field creates a capillary pressure difference that facilitates the directional migration of bubbles, generating a passive bubble self-pumping effect without the need for external driving components. This promotes the entry of bubbles from the porous structure into the electrode microchannel and further into the anode flow field channel, forming a continuous bubble removal path of "porous structure - electrode microchannel - anode flow field channel." This allows bubbles to sequentially complete interface desorption, lateral breakthrough from the original pores into the electrode microchannel, aggregation within the electrode microchannel, and discharge into the anode flow field channel, overcoming the problem of bubble retention inside the porous metal electrode, under the flow field ribs, and at the electrode-flow field interface. Simultaneously, the superhydrophobic micro / nanostructure promotes the wetting and replenishment of electrolyte into the porous framework, complementing the gas phase discharge path formed by the electrode microchannel to achieve coordinated transport of gas phase discharge and liquid phase replenishment.
[0019] Furthermore, the present invention uses a serpentine arrangement of electrode microchannels to create a continuous correspondence between the electrode microchannels and the serpentine anode flow field channel in the flow path direction, which is beneficial for bubbles to gather in the electrode microchannels and then smoothly discharge into the anode flow field channel along the serpentine path.
[0020] Furthermore, by employing a sintered 316L stainless steel porous metal electrode, the present invention enables the electrode to possess both excellent mechanical strength, conductivity, and corrosion resistance, thus meeting the stringent operating environment requirements of the anode side of anion exchange membrane water electrolysis.
[0021] The preparation method of this invention forms electrode microchannels by laser processing on one side of a porous metal electrode, followed by chemical etching with oxalic acid aqueous solution, so that the porous framework and the surface of the electrode microchannels form a superhydrophobic micro / nano structure, which improves the electrolyte wetting ability and forms a low bubble adhesion interface underwater, which is conducive to the rapid detachment of bubbles from the electrode surface in a small state. At the same time, the combination of laser processing to form directional channels and oxalic acid etching to form surface structures achieves the synergistic effect of "directional bubble removal channels" and "low adhesion interface".
[0022] The water electrolysis cell of this invention includes an anode flow field plate and a graded porous transport electrode arranged opposite to the anode flow field plate. The electrode microchannel and the anode flow field channel are aligned along the flow path direction, so that the bubbles inside the graded porous transport electrode can enter the electrode microchannel laterally from the original pores, and then enter the anode flow field channel from the electrode microchannel. This realizes a continuous bubble removal path from the inside of the porous metal electrode to the flow field channel, and overcomes the problem of bubbles being trapped inside the porous metal electrode, in the flow field rib area, and at the electrode-flow field interface.
[0023] Furthermore, the width of the electrode microchannel of the present invention is smaller than the width of the anode flow field channel, so that the unprocessed electrode ridges retained between adjacent electrode microchannels are in direct contact with the anode flow field ribs, thus maintaining electrode compression, mechanical support and electronic conduction while introducing the defoaming channel.
[0024] This invention involves creating electrode microchannels corresponding to the upper anode flow field channel on the side of a continuously sintered porous metal electrode facing the anode flow field, and forming superhydrophobic micro / nano structures on the porous framework and the surface of the electrode microchannels. This allows bubbles to sequentially complete interfacial desorption, lateral breakthrough from the original pores into the electrode microchannels, converge within the electrode microchannels, and discharge into the upper anode flow field channel. Simultaneously, the unprocessed electrode ridges retained between adjacent electrode microchannels contact the anode flow field ribs to maintain mechanical support, assembly clamping, and electronic conduction. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a schematic diagram of the partial coordination structure of the anion exchange membrane water electrolysis cell and electrode microchannel-anodine flow field channel of the present invention.
[0027] Figure 2 This is a schematic diagram of the local fit structure of the original electrode-anode flow field channel in Comparative Example 1.
[0028] Figure 3 This is a schematic diagram of the gas-liquid transport and bubble self-pumping mechanism in Example 1, showing the gas phase path of the bubbles entering the electrode microchannel laterally from the porous structure and further being discharged into the anode flow field channel, as well as the liquid phase path of the electrolyte replenishing the interior of the porous framework.
[0029] Figure 4 This is a schematic diagram of the fabrication process of the hierarchical porous transport electrode in Example 1.
[0030] Figure 5 This is a scanning electron microscope image of the electrode microchannel obtained by laser processing in Example 1.
[0031] Figure 6 This is a scanning electron microscope image of the porous framework and micron-sized pores of the hierarchical porous transport electrode in Example 1.
[0032] Figure 7 This is a high-magnification scanning electron microscope image of the surface of the original electrode skeleton in Comparative Example 1.
[0033] Figure 8 This is a high-magnification scanning electron microscope image of the micro / nanostructures on the electrode skeleton surface after oxalic acid treatment in Example 1.
[0034] Figure 9 The image shows the underwater bubble contact angle test result on the original electrode surface in Comparative Example 1.
[0035] Figure 10 This is a test diagram of the underwater bubble contact angle on the surface of the graded porous transmission electrode in Example 1.
[0036] Figure 11 The polarization curves of the full electrolytic cell corresponding to the hierarchical porous transport electrodes with different electrode microchannel widths obtained in Examples 2, 1, and 3 are shown.
[0037] Figure 12 The full electrolytic cell polarization curves are for the hierarchical porous transport electrodes obtained by etching at different temperatures in Examples 4 and 1.
[0038] Figure 13 The full electrolytic cell polarization curves are for the original electrode of Comparative Example 1, the laser-processed electrode of Comparative Example 2, the oxalic acid-etched electrode of Comparative Example 3, and the hierarchical porous transport electrode of Example 1.
[0039] Figure 14 This is a visualization of in-situ bubbles in the flow field corresponding to the original electrode in Comparative Example 1.
[0040] Figure 15 This is a visualization of in-situ bubbles in the flow field corresponding to the graded porous transport electrode in Example 1.
[0041] in, Figure 1 and Figure 2 The following are explanations of the reference numerals in the attached figures: 1 is cathode carbon paper, 2 is cathode catalyst layer, 3 is anion exchange membrane, 4 is anode side sealing gasket, 5 is hierarchical porous transport electrode, 6 is anode flow field plate, 7 is anode flow field channel, 8 is anode flow field rib, 9 is unprocessed electrode ridge, and 10 is electrode microchannel. Detailed Implementation
[0042] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0043] It should be noted that the process equipment or apparatus not specifically mentioned in the following embodiments are all conventional equipment or apparatus in the art.
[0044] It should be noted that the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products, or apparatuses. Furthermore, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not intended to limit the order of the method steps or define the scope of the invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.
[0045] Existing water electrolysis cells use sintered porous metal electrodes as anodes. However, the pores of these electrodes are random, tortuous, and interconnected. Bubbles need to migrate along these winding channels. When the electrode is blocked by the anode flow field ribs, the bubbles under the ribs cannot directly enter the anode flow field channel along the thickness direction. Instead, they tend to coalesce inside the porous metal electrode or at the electrode-flow field interface, forming large gas retention areas. Existing solutions, by simply adjusting the porosity, pore size, or surface wettability of the porous material, cannot fundamentally solve the problem of the lack of direct exhaust paths in the region under the flow field ribs.
[0046] To address the aforementioned problems in the prior art, this invention provides an electrode microchannel corresponding to the anode flow field channel on the side of the porous metal electrode facing the anode flow field, and constructs a superhydrophobic micro / nano structure on the porous framework of the porous metal electrode and the surface of the electrode microchannel. This allows bubbles to sequentially complete interface desorption, lateral breakthrough from the original pores into the electrode microchannel, aggregation within the electrode microchannel, and discharge into the anode flow field channel. This effectively solves the problem of bubble retention inside the porous metal electrode, in the flow field rib region, and at the electrode-flow field interface during water electrolysis at high current densities.
[0047] Specifically, the graded porous transport electrode for electrode-flow field synergistic defoaming according to the present invention includes a porous metal electrode, wherein an electrode microchannel is formed on one side of the porous metal electrode, and the electrode microchannel corresponds to the anolyte flow field channel formed on the anolyte flow field plate in the water electrolysis cell; the porous skeleton surface of the porous metal electrode and the electrode microchannel surface have superhydrophobic micro / nano structures.
[0048] Among them, the porous metal electrode is a porous body with a three-dimensional interconnected pore structure formed by sintering metal powder. Its pores are random, curved and interconnected.
[0049] The electrode microchannel is a groove structure formed by laser processing on the side surface of a porous metal electrode facing the anode flow field. The electrode microchannel has a continuously extending groove shape on the electrode surface.
[0050] The superhydrophobic micro / nanostructure is a microstructure formed by oxalic acid etching on the porous framework surface of a porous metal electrode and the walls of the electrode microchannels. This structure maintains the original micron-level porosity of the porous framework at the micron scale, while simultaneously forming undulating, uneven surface textures at the nanoscale. The superhydrophobic micro / nanostructure exhibits excellent electrolyte wetting ability, displaying a large bubble contact angle (preferably greater than 150°) underwater, which helps reduce the effective contact area between bubbles and the electrode surface and reduces bubble adhesion.
[0051] The hierarchical porous transport electrode of this invention establishes electrode microchannels corresponding to the anolyte flow field channel within a porous metal electrode, and constructs a superhydrophobic micro / nanostructure with low bubble adhesion on the porous framework and the surface of the electrode microchannels. This allows bubbles to sequentially complete interface desorption, lateral breakthrough from the original pores into the electrode microchannels, aggregation within the electrode microchannels, and discharge into the anolyte flow field channel. This constructs a continuous bubble removal path of "original pores of the porous metal electrode – electrode microchannels – anolyte flow field channel," enabling bubbles under the flow field ribs to laterally enter the electrode microchannels and further discharge into the anolyte flow field channel. Simultaneously, the passive bubble self-pumping effect is generated by utilizing the interface curvature and capillary pressure difference between channels of different scales, which, combined with the electrolyte replenishment promoted by the superhydrophobic micro / nanostructure, achieves coordinated transport of gas phase discharge and liquid phase replenishment. This effectively solves the problem of bubble retention inside the porous metal electrode, in the flow field rib region, and at the electrode-flow field interface during water electrolysis at high current densities.
[0052] In some embodiments of the present invention, the electrode microchannels are arranged in a serpentine pattern. A serpentine pattern means that the electrode microchannels extend on the electrode surface in a continuous, zigzagging or meandering manner, forming a path shape similar to a snake crawling, so that the extension path shape of the electrode microchannels matches the serpentine path shape of the anode flow field channel. After the water electrolysis cell is assembled, the electrode microchannels and the anode flow field channel are aligned along the flow path direction; that is, the position of the electrode microchannels on the electrode surface and the position of the anode flow field channel on the anode flow field plate are aligned in the electrode-flow field plate overlapping direction, allowing bubbles inside the porous metal electrode to enter laterally from the original pores into the electrode microchannels, and then from the electrode microchannels into the anode flow field channel.
[0053] In some embodiments of the present invention, the width of the electrode microchannel is 400-600 μm, for example, 400 μm, 450 μm, 500 μm, 550 μm, or 600 μm. Controlling the width of the electrode microchannel within this range, and making it smaller than the width of the anode flow field channel (the anode flow field channel width is 1500 μm), ensures effective contact between the unprocessed electrode ridge and the anode flow field rib to maintain mechanical support and electronic conduction, while providing sufficient lateral space for bubble breakthrough and discharge. Experimental results show that, under the same test conditions, the water electrolysis cell voltage is lowest when the electrode microchannel width is 600 μm; therefore, a width of 600 μm is more preferable for the electrode microchannel.
[0054] The porous metal electrode can be made of stainless steel, nickel-based alloys, titanium-based alloys, or other metal materials with good electrical conductivity and corrosion resistance, preferably sintered 316L stainless steel porous metal electrodes. 316L stainless steel refers to austenitic stainless steel containing molybdenum, with a carbon content of less than 0.03%, exhibiting excellent corrosion resistance. By sintering 316L stainless steel powder, a porous body with a three-dimensional interconnected pore structure can be formed. Using sintered 316L stainless steel porous metal electrodes gives the electrode both good mechanical strength, electrical conductivity, and corrosion resistance, meeting the harsh operating environment requirements of the anode side of anion exchange membrane water electrolysis.
[0055] This invention provides a method for preparing the hierarchical porous transport electrode with electrode-flow field synergistic debubbling, comprising the following steps: (1) Laser processing is performed on one side of the porous metal electrode to form an electrode microchannel, thus obtaining a laser-etched electrode; (2) The laser etching electrode is immersed in an aqueous solution of oxalic acid for chemical etching to obtain a hierarchical porous transport electrode.
[0056] In the above preparation method, the laser processing in step (1) refers to scanning and irradiating the surface of the porous metal electrode with a laser beam, using the high energy density of the laser to melt or vaporize the material on the electrode surface, thereby forming a groove structure on the electrode surface. The laser processing can use pulsed lasers such as nanosecond lasers, picosecond lasers, or femtosecond lasers, with femtosecond lasers being preferred to avoid excessive heat-affected zones that could damage the porous structure. The chemical etching in step (2) utilizes the chemical corrosion effect of oxalic acid on the surface of the porous metal electrode to form a superhydrophobic micro / nanostructure on the porous framework and electrode microchannel surface. The laser processing forms directional bubble removal channels, and then the oxalic acid etching constructs a low-bubble adhesion interface on the surface. The two work together to achieve the combination of directional bubble removal channels and low-bubble adhesion interface.
[0057] In some embodiments of the present invention, the chemical etching temperature is 60-80 °C, for example, 60 °C, 65 °C, 70 °C, 75 °C, or 80 °C. Controlling the chemical etching temperature within this range is beneficial for the oxalic acid to fully react with the surface of the porous metal electrode framework, forming a uniform micro / nano structure while maintaining the integrity of the overall framework structure. Experimental data show that the water electrolysis cell voltage corresponding to the hierarchical porous transport electrode obtained by treatment at 80 °C is lower; therefore, the preferred chemical etching temperature is 80 °C.
[0058] In some embodiments of the present invention, the chemical etching time is 80-100 min, for example, 80 min, 90 min, 100 min, etc. Controlling the chemical etching time ensures sufficient formation of the micro / nanostructure while avoiding the adverse effects of over-etching on the electrode framework strength and conductivity.
[0059] In some embodiments of the present invention, the mass fraction of the oxalic acid aqueous solution (i.e., the percentage of oxalic acid in the oxalic acid aqueous solution) is preferably 15%. Controlling the mass fraction of the oxalic acid aqueous solution to 15% ensures a moderate etching reaction rate, which is beneficial for forming a uniform and structurally stable micro / nano morphology on the skeleton surface.
[0060] like Figure 1 As shown, the present invention also provides a water electrolysis cell, comprising: an anode flow field plate 6 and a hierarchical porous transport electrode 5 disposed opposite to the anode flow field plate 6; an anode flow field channel 7 is provided on one side of the anode flow field plate 6, and the electrode microchannel 10 in the hierarchical porous transport electrode 5 is aligned with the anode flow field channel 7 along the flow path direction.
[0061] In addition, the water electrolysis cell also includes cathode carbon paper 1, cathode catalyst layer 2, anion exchange membrane 3, and anode side sealing gasket 4. These components are assembled according to the conventional electrolysis cell assembly method.
[0062] In this water electrolysis cell, the anode flow field plate 6 is a plate with a flow guiding structure. An anode flow field channel 7 is formed on the side facing the hierarchical porous transport electrode 5. The anode flow field channel 7 is a channel for the flow of the anolyte and the generated gas. The electrode microchannel 10 is aligned with the anode flow field channel 7 along the flow path, so that the bubbles inside the hierarchical porous transport electrode 5 can enter the electrode microchannel 10 laterally from the original pores, and then enter the anode flow field channel 7 from the electrode microchannel 10, realizing a continuous bubble removal path from the inside of the porous metal electrode to the flow field channel.
[0063] In some embodiments of the present invention, the width of the electrode microchannel 10 is smaller than the width of the anode flow field channel 7. By setting the width of the electrode microchannel 10 to be smaller than the width of the anode flow field channel 7, the unprocessed electrode ridges 9 retained between adjacent electrode microchannels 10 are in direct contact with the anode flow field ribs 8, thus maintaining electrode compression, mechanical support, and electronic conduction while introducing a degassing channel. The open area of the electrode microchannel 10 then constitutes a preferred degassing path.
[0064] Example 1 A sintered 316L stainless steel porous metal electrode was used as the initial electrode and ultrasonically cleaned sequentially with ethanol and deionized water at room temperature for 30 min. After cleaning, the initial electrode was placed in an oven and dried at 80 °C for 12 h. Subsequently, laser processing was performed on the side of the porous metal electrode facing the anode flow field plate using a femtosecond fiber laser (wavelength 1030 nm, pulse duration 290 fs). The laser processing parameters were set as follows: scanning speed 500 mm / s. -1The repetition frequency was 200 kHz, and the average power was 10 W. This formed a continuous serpentine electrode microchannel with a depth of approximately 600 μm and a width of 600 μm, resulting in a laser-etched electrode. The laser-etched electrode was then immersed in a 15% (w / w) oxalic acid aqueous solution and treated at 80 °C for 90 min. After treatment, it was cleaned and dried to obtain a hierarchical porous transport electrode. The preparation process is as follows: Figure 4 As shown.
[0065] The obtained hierarchical porous transport electrode was assembled on the anode side of an anion exchange membrane water electrolysis cell, aligning the electrode microchannels with the anode flow field channels on the anode flow field plate along the flow path. The unprocessed electrode ridges retained between adjacent electrode microchannels on the hierarchical porous transport electrode contact the anode flow field ribs on the anode flow field plate. The open regions of the electrode microchannels are connected to the anode flow field channels, forming a continuous degassing path from the porous structure of the hierarchical porous transport electrode through the electrode microchannels into the anode flow field channels. Its structure and transport mechanism are as follows: Figure 1 and Figure 3 As shown.
[0066] Example 2 The hierarchical porous transport electrode was prepared according to the method of Example 1, except that the width of the electrode microchannel was 400 μm, while the other laser processing, oxalic acid treatment and assembly conditions were the same as in Example 1.
[0067] Example 3 The hierarchical porous transport electrode was prepared according to the method of Example 1, except that the electrode microchannel width was 800 μm, while the other laser processing, oxalic acid treatment and assembly conditions were the same as in Example 1.
[0068] Example 4 The hierarchical porous transport electrode was prepared according to the method of Example 1, with the only difference being that the oxalic acid treatment temperature was 60 °C. The oxalic acid mass fraction was 15%, the treatment time was 90 min, and all other processing and assembly conditions were the same as in Example 1.
[0069] Comparative Example 1 A water electrolysis cell equipped with anion exchange membrane using sintered 316L stainless steel porous metal electrodes that have not undergone laser processing or oxalic acid treatment. Figure 2 The remaining assembly conditions are the same as in Example 1.
[0070] Comparative Example 2 The same sintered 316L stainless steel porous metal electrode as in Example 1 was used, and a continuous serpentine electrode microchannel with a width of 600 μm was fabricated, but without oxalic acid treatment. During assembly, the electrode microchannel was aligned with the anode flow field channel along the flow path direction, and the remaining conditions were the same as in Example 1.
[0071] Comparative Example 3 Using the same sintered 316L stainless steel porous metal electrode as in Example 1, without laser processing, it was directly immersed in a 15% oxalic acid aqueous solution and treated at 80 °C for 90 min, followed by cleaning and drying. The remaining assembly conditions were the same as in Example 1.
[0072] I. Surface morphology and hydrophilicity / hydrophobicity verification 1. After cleaning and drying, the electrode to be tested was fixed on the sample stage of a scanning electron microscope (SEM). The overall structure, microchannel morphology, porous framework, and surface microstructure of the electrode were observed using a SEM (TESCAN MIRA LMS). The imaging acceleration voltage was 15 kV. Low-magnification observation was used to characterize the continuity of the electrode microchannels and the overall morphology of the porous framework, while high-magnification observation was used to compare the changes in the micro / nanostructure of the framework surface before and after oxalic acid treatment.
[0073] Figure 5 and Figure 6 The results showed that the hierarchical porous transport electrode obtained in Example 1 formed a continuous electrode microchannel on its surface and retained the sintered porous framework and its micron-sized pores. Figure 7 and Figure 8 The results showed that, compared with the surface of the sintered 316L stainless steel porous metal electrode (original electrode) of Comparative Example 1, the skeleton surface of Example 1 after oxalic acid treatment formed obvious nanoscale undulation structure.
[0074] 2. The underwater bubble contact angle of the electrode surface was measured at room temperature using a contact angle meter (KINO SL200 series). During the test, the electrode test surface was fixed horizontally and completely immersed in deionized water. A 5 μL air bubble was formed below the electrode using an injection needle, allowing the bubble to contact the electrode surface. After the bubble profile stabilized, an image was acquired, and the apparent underwater bubble contact angle was obtained by fitting the profile near the bubble-water-solid three-phase contact line. The same bubble volume and imaging conditions were used for different electrodes.
[0075] like Figure 9 and Figure 10 As shown, the underwater bubble contact angle on the surface of the original electrode in Comparative Example 1 is approximately 139°, while the underwater bubble contact angle on the surface of the hierarchical porous transport electrode in Example 1 is approximately 151°. This result indicates that the electrode surface treated with oxalic acid exhibits reduced affinity for underwater bubbles and stronger underwater gas-repellency.
[0076] II. Electrochemical Performance Testing Each electrode to be tested was cut into 2.0 cm × 2.0 cm pieces and ultrasonically cleaned for 30 min each in ethanol and deionized water. Before testing, the electrodes to be tested were immersed in 1.0 mol L... -1The sample was soaked in KOH solution for 1 hour. The electrode under test was used as the anode, and Pt / C catalyst coated with carbon paper was used as the cathode. These were then assembled with an anion exchange membrane to form an anion exchange membrane water electrolyzer. Nickel serpentine flow field plates were used as the anode flow field plates, and graphite serpentine flow field plates were used as the cathode flow field plates, both sealed with polytetrafluoroethylene gaskets. The electrolyzer was secured with four bolts, each with an assembly torque of 4.0 N·m.
[0077] Electrochemical tests were performed at 80 °C using 1.0 mol L⁻¹. -1 KOH was used as the anolyte circulating electrolyte, and the solution was pumped at a rate of 5 mL / min using a peristaltic pump. -1 The electrolyte was continuously supplied with liquid, and the cathode operated in a dry cathode mode with no liquid supply. Polarization tests of the entire electrolytic cell were conducted using an Autolab PGSTAT302N electrochemical workstation equipped with a high-current extension module. During the tests, the current density was increased from 0.01 A / cm². -2 Gradually increase to 5.0 A cm -2 A constant current was maintained for 300 s at each current density, and the average voltage over the last 10 s was taken as the steady-state voltage at that current density. All embodiments and comparative examples used the same membrane electrode assembly, assembly pressure, electrolyte concentration, temperature, flow rate, and test procedures.
[0078] 1. The hierarchical porous transport electrodes of Examples 2, 1, and 3 were subjected to full electrolytic cell polarization tests to compare the electrochemical performance when the electrode microchannel width was 400 μm, 600 μm, and 800 μm, respectively.
[0079] like Figure 11 As shown, in the range of 0.01~5.0 A cm -2 Within the current density range, the voltage corresponding to the electrode microchannel width of 600 μm in Example 1 is lower than the voltages corresponding to 400 μm in Example 2 and 800 μm in Example 3, respectively. Therefore, among the three electrode microchannel widths tested, 600 μm is the preferred width, and the electrode microchannel is aligned with the 1500 μm wide anode flow field channel during the electrolytic cell assembly process.
[0080] 2. Full electrolytic cell polarization tests were conducted on the hierarchical porous transport electrodes of Example 4 and Example 1 to compare the effects of different oxalic acid treatment temperatures on electrochemical performance. The oxalic acid aqueous solutions used in Example 4 and Example 1 contained 15% oxalic acid by mass, and the treatment time was 90 min for both. The only difference was the treatment temperature, which was 60 ℃ and 80 ℃, respectively.
[0081] like Figure 12 As shown, in the range of 0.01~5.0 A cm -2Within the current density range, the voltage corresponding to the hierarchical porous transport electrode obtained in Example 1 at 80 °C is lower than that of the hierarchical porous transport electrode obtained in Example 4 at 60 °C. Therefore, of the two processing temperatures tested, 80 °C is the preferred processing temperature.
[0082] 3. Perform full electrolytic cell polarization tests on the electrodes of Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1, and compare the performance of the original electrode, the laser-processed electrode, the oxalic acid-treated electrode and the hierarchical porous transport electrode, respectively.
[0083] like Figure 13 As shown, in the range of 0.01~5.0 A cm -2 Within the current density range, the electrolytic cell voltage corresponding to the hierarchical porous transport electrode in Example 1 is lower than the electrolytic cell voltage corresponding to each comparative example, indicating that the electrode microchannel formed by laser and the superhydrophobic micro / nanostructure formed by oxalic acid treatment can synergistically improve the performance of the entire electrolytic cell.
[0084] III. Verification of Bubble Ejection Capability A transparent observation window was installed on the anode flow field plate to make the anode flow field visible. A high-speed camera (Revealer M230M) equipped with a macro lens was used to capture in-situ images of the gas-liquid two-phase flow within the anode flow field at a frame rate of 500 fps and an exposure time of 500 μs. The electrolytic cell structure, electrolyte concentration, operating temperature, and anode electrolyte flow rate used in the visualization test were consistent with those used in the electrochemical performance test.
[0085] At 1.0 A cm -2 The bubble motion within the anolyte flow field corresponding to Comparative Example 1 and Example 1 was recorded at different current densities. At each current density, photography began after the electrolytic cell voltage and the bubble state within the anolyte flow field had basically stabilized, while maintaining consistent camera position, observation area, magnification, frame rate, and exposure time. Figure 14 and Figure 15 Select 1.0 A cm -2 Compare representative images below.
[0086] like Figure 14 As shown, in Comparative Example 1, the original electrode corresponds to a anolyte flow field containing numerous large bubbles and long plug-like bubbles; for example... Figure 15 As shown, the hierarchical porous transport electrode in Example 1 reduces the number of large bubbles and long plug-like bubbles in the anode flow field, and the bubble distribution is more dispersed. These results indicate that the hierarchical porous transport electrode and its corresponding structure in the anode flow field are beneficial for suppressing bubble coalescence and flow field blockage, and for promoting bubble discharge.
[0087] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of this invention.
Claims
1. A hierarchical porous transport electrode for electrode-flow field synergistic defoaming, characterized in that, It includes a porous metal electrode, on one side of which an electrode microchannel is formed, and the electrode microchannel corresponds to the anolyte flow field channel formed on the anolyte flow field plate in the water electrolysis cell; the porous skeleton surface of the porous metal electrode and the electrode microchannel surface have superhydrophobic micro / nano structures.
2. The graded porous transport electrode for electrode-flow field synergistic defoaming as described in claim 1, characterized in that, The electrode microchannels are arranged in a serpentine pattern.
3. The graded porous transport electrode for electrode-flow field synergistic defoaming as described in claim 1, characterized in that, The width of the electrode microchannel is 400~600 μm.
4. The graded porous transport electrode for electrode-flow field synergistic defoaming according to claim 1, characterized in that, The porous metal electrode is a sintered 316L stainless steel porous metal electrode.
5. The method for preparing the graded porous transport electrode with electrode-flow field synergistic defoaming as described in any one of claims 1 to 4, characterized in that, include: (1) Laser processing is performed on one side of the porous metal electrode to form an electrode microchannel, thus obtaining a laser-etched electrode; (2) The laser-etched electrode is immersed in an aqueous solution of oxalic acid for chemical etching to obtain a hierarchical porous transport electrode.
6. The method for preparing a hierarchical porous transport electrode with electrode-flow field synergistic defoaming according to claim 5, characterized in that, The temperature for the chemical etching is 60~80 ℃.
7. The method for preparing a hierarchical porous transport electrode with electrode-flow field synergistic defoaming according to claim 5, characterized in that, The chemical etching time is 80-100 min.
8. The method for preparing a hierarchical porous transport electrode with electrode-flow field synergistic defoaming according to claim 5, characterized in that, The oxalic acid aqueous solution has a mass fraction of 15%.
9. A water electrolysis cell, characterized in that, include: The anode flow field plate and the graded porous transport electrode for electrode-flow field synergistic defoaming as described in any one of claims 1 to 4, which is disposed opposite to the anode flow field plate; An anode flow field channel is provided on one side of the anode flow field plate, and the electrode microchannel in the hierarchical porous transfer electrode is aligned with the anode flow field channel along the flow path direction.
10. The water electrolysis cell according to claim 9, characterized in that, The width of the electrode microchannel is smaller than the width of the anode flow field channel.
Citation Information
Patent Citations
Microchannel with three-dimensional composite wettability surface and preparation method of microchannel
CN113731771A
A high-activity super-hydrophilic and gas-repellent electrode used in low-pressure environment, and a preparation method and application thereof
CN121373806B
Self-exhaust porous electrode with amphiphilic interface and application of self-exhaust porous electrode
CN121528969A