A copper nanowire composite gas diffusion electrode, its preparation method and application
By designing a copper nanowire composite gas diffusion electrode, the problems of stability and adaptability to low concentration CO2 under high current density of traditional electrodes are solved, realizing the efficient preparation of multi-carbon products by CO2 electroreduction, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202611069829.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-17
- Publication Date
- 2026-11-17
Smart Images

Figure CN123108602A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of preparing multi-carbon products by electroreduction of carbon dioxide, specifically to a copper nanowire composite gas diffusion electrode, its preparation method, and its application. Background Technology
[0002] Electrocatalytic carbon dioxide reduction (ECO2RR) technology can utilize renewable and clean energy to convert CO2 into high-value-added multi-carbon products (C60, ethanol, acetic acid, and propanol) under mild conditions. 2+ product).
[0003] However, transforming the laboratory research results of ECO2RR into industrially applicable technology requires an electrolytic system operating at ampere-level current densities (>0.5 A cm⁻¹). -2 Stable operation under these conditions far exceeds the capabilities of traditional H-type electrolyzers (current density below 60 mA cm⁻¹). -2 The emergence of flow electrolyzers equipped with gas diffusion electrodes (GDEs) has significantly overcome the aforementioned limitations by constructing a three-phase interface where gaseous CO2, liquid electrolyte, and solid catalyst coexist. This allows for a substantial increase in local CO2 supply, easily enabling current densities to exceed 200 mA cm⁻¹. -2 Inside the gas diffusion electrode, CO2 must first pass through the gas diffusion layer (GDL) to reach the catalyst layer (CL). Therefore, the efficiency of this mass transfer path is the core factor determining the overall performance of CO2RR.
[0004] However, currently available gas diffusion electrodes generally use commercial carbon-based gas diffusion electrodes (GDEs). The microporous layer (MPL) of GDEs has a narrow pore size, which not only severely hinders the rapid mass transfer of CO2, but also easily causes blockage of the pores of powder catalysts. At the same time, the carbon substrate cannot avoid electrowetting. As electrolysis proceeds, the electrolyte continues to wet and penetrate, especially under alkaline conditions, it will react with CO2 to form carbonates or bicarbonates and cause salting out, further blocking the mass transfer of CO2, destroying the gas-liquid-solid three-phase interface, leading to a series of problems such as the aggravation of hydrogen evolution reaction (HER) and a significant decrease in the reduction stability of CO2.
[0005] If hydrophobic polytetrafluoroethylene (PTFE) is used as the electrode substrate to overcome the wetting problem, the same issue arises: PTFE itself is an insulating material, and when powdered catalyst is directly loaded onto its surface, a continuous conductive network cannot be formed between the particles, resulting in the overall conductivity of the electrode failing and making it difficult to meet the requirements of electrocatalytic reactions. To address this problem, existing technologies propose modifying the conductivity of PTFE surfaces by magnetron sputtering copper nanoparticles. However, this approach relies on precision vacuum equipment, resulting in a cumbersome and complex process with poor controllability, making it unsuitable for large-scale industrial production.
[0006] Furthermore, none of the currently disclosed gas diffusion electrodes can meet the industrial-scale current density (0.5 A cm⁻¹). -2 The stability of CO2 electroreduction technology is limited by its rapid deactivation and drastic drop in selectivity under high current conditions. Furthermore, it can only operate in high-purity CO2, and is rarely suitable for actual working conditions such as low-concentration CO2 flue gas or simulated flue gas in industrial applications. This greatly restricts the industrial application scope of CO2 electroreduction technology. Summary of the Invention
[0007] This invention provides a copper nanowire composite gas diffusion electrode to solve the problem that existing gas diffusion electrodes cannot meet the requirements for stable operation at industrial current densities.
[0008] In a first aspect, the present invention provides a copper nanowire composite gas diffusion electrode, comprising: A PTFE substrate with a microporous structure, and a catalytic layer disposed on the PTFE substrate, wherein the catalytic layer is a three-dimensional network of copper nanowires coated with Nafion.
[0009] Nafion is a perfluorosulfonic acid resin, one of the most representative commercial ion exchange materials in the field of electrochemical energy and separation, with CAS number 31175-20-9.
[0010] In one optional embodiment, the pore size of the microporous structure is 0.1-5.0 μm, preferably 0.1-0.6 μm.
[0011] In one optional embodiment, the loading of the catalyst layer on the PTFE substrate is 0.5-5.0 mg cm⁻¹. 2 Preferably 1-3 mg cm 2 .
[0012] In one alternative embodiment, the mass ratio of the copper nanowires to Nafion is 9:(1-11), preferably 9:(5-11).
[0013] In one optional embodiment, the diameter of the copper nanowire is less than 500 nm, preferably less than 100 nm; and the length of the copper nanowire is more than 100 μm.
[0014] In one alternative implementation, the three-dimensional network has a 500–900 nm interconnect structure.
[0015] Secondly, the present invention also provides a method for preparing a copper nanowire composite gas diffusion electrode, comprising: Preparation of copper nanowires: Cu precursor and reducing agent were subjected to wet chemical synthesis and surface ligand replacement to obtain a precipitate. The precipitate was purified and acid-treated to obtain copper nanowires. Nafion coating: Copper nanowires were mixed with Nafion solution and then coated. After coating, they were centrifuged and washed to obtain Nafion-coated copper nanowires. Vacuum filtration loading: Nafion-coated copper nanowires were dispersed in a solvent and loaded onto a microporous PTFE substrate using vacuum filtration. After drying, a copper nanowire composite gas diffusion electrode was obtained.
[0016] The wet chemical synthesis and surface ligand replacement process includes: dissolving Cu precursor and reducing agent in water to obtain precursor solution; mixing ligand reagent with organic solvent to prepare ligand solution; adding ligand solution dropwise to precursor solution under first stirring condition; adding water to precursor solution under second stirring condition; heating to reaction temperature and holding at constant temperature for hydrothermal treatment; cooling after hydrothermal treatment and obtaining precipitate.
[0017] The Cu precursor includes one or more of CuCl2, Cu(NO3)2, CuSO4, and Cu(CH3COO)2; The reducing agent is a non-strong reducing system, including one or more of glucose, ascorbic acid, and organic amines; The ligand reagent includes one or more of oleic acid, oleylamine, C12-C18 long-chain hydrocarbon primary amine, ethylenediamine, polyvinylpyrrolidone, hexadecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride, and the organic solvent in the ligand solution is one or more of anhydrous ethanol, acetone, isopropanol, n-hexane, and toluene. The reaction temperature is below 100°C, preferably 40-60°C; The hydrothermal treatment is carried out in a high-pressure reactor lined with stainless steel and PTFE, and the treatment temperature is 100-240℃, preferably 110-130℃.
[0018] The precipitation purification process includes washing with ethanol-water solution, pure ethanol, and n-hexane in sequence; the volume ratio of ethanol to water in the ethanol-water solution is 1:1, the ethanol-water solution is used for washing twice, pure ethanol is used for washing once, and n-hexane is used for washing four times.
[0019] In this invention, the purified copper nanowires can be dispersed in n-hexane to obtain a stable dispersion for later use; alternatively, the purified copper nanowires can be directly subjected to subsequent acid treatment steps.
[0020] The acid treatment process includes: removing the surface coating agent of the prepared purified copper nanowires by using a lactic acid-methanol washing method to obtain copper nanowires; The process of the lactic acid-methanol washing method includes: taking the purified copper nanowires, adding lactic acid and methanol to make the copper nanowires uniformly dispersed and remove the surface oil amine, then shaking and mixing, and then washing with methanol by centrifugation to obtain copper nanowires.
[0021] The coating process includes: stirring followed by settling, repeating this stirring-set-settling process 1-4 times to achieve uniform coating of Nafion on copper nanowires. After coating, the nanowires are washed with methanol by centrifugation to remove excess Nafion from the solution.
[0022] Thirdly, the present invention also provides an application of a copper nanowire composite gas diffusion electrode in the cathode for the preparation of multi-carbon products by electroreduction reaction of carbon dioxide reactants.
[0023] In one alternative embodiment, the multicarbon product includes one or more of ethylene, ethanol, acetic acid, and propanol; The carbon dioxide reactant has a carbon dioxide concentration greater than 15%; the carbon dioxide reactant is industrial flue gas with a carbon dioxide concentration greater than 15%.
[0024] In one optional embodiment, the current density of the carbon dioxide electroreduction reaction is >0.5 A cm⁻¹. -2 Preferably, it is 0.5-1.2 A cm. -2 .
[0025] The technical solution of this invention has the following advantages: 1. The copper nanowire composite gas diffusion electrode provided by this invention can completely overcome the problems of mass transfer blockage in the microporous layer and water flooding failure caused by electrowetting under high current in traditional carbon-based gas diffusion electrodes, maintaining a more stable gas transport channel, thereby effectively improving the transport efficiency of carbon dioxide inside the electrode and improving the long-term operational stability of the electrode. Specifically, the electrode uses a hydrophobic porous PTFE film instead of traditional carbon paper or carbon-based gas diffusion layer, avoiding mass transfer blockage caused by the small pore size of traditional microporous layers, reducing carbon dioxide diffusion resistance, and enabling carbon dioxide to be transported from the gas side to the catalyst layer more quickly. Furthermore, PTFE has good hydrophobicity and resistance to electrolyte penetration, which can alleviate the electrowetting and water flooding problems that are prone to occur in traditional carbon-based gas diffusion electrodes under alkaline high current density conditions. At the same time, the three-dimensional interconnected conductive network constructed by the copper nanowires themselves enables the catalyst layer to simultaneously possess carbon dioxide electroreduction activity, electron transport capability, and open pore structure, without the need for additional reliance on traditional carbon paper current collectors or a large amount of carbon-based conductive additives. This structure not only reduces the complexity of the electrode structure but also avoids the densification problem of the catalyst layer caused by the accumulation of traditional powder catalysts, which is beneficial to improving the utilization rate of active sites within the catalyst layer. Furthermore, by introducing a Nafion ionomer coating layer on the surface of the copper nanowires, continuous ion conduction channels and a gas-liquid-solid three-phase reaction interface can be formed on the catalyst surface, enabling the synergistic transport of carbon dioxide, electrons, and ions on the copper nanowire surface. In summary, this application utilizes Nafion-coated copper nanowires to form a three-dimensional network catalyst layer on a microporous PTFE substrate, which can maintain a more stable gas transport channel at higher current densities, thereby meeting the requirements for the preparation of multi-carbon products by the electroreduction reaction of carbon dioxide at ampere-level high current densities and improving the long-term operational stability of the electrode. The copper nanowire composite gas diffusion electrode of this invention was verified at 0.8 Acm... 2 At a current density of [value missing], this electrode can operate stably for more than 13 hours, while traditional carbon paper-based electrodes are prone to electrolyte penetration and performance degradation in a short period of time, indicating that the electrode of this invention has significant advantages in resisting flooding and maintaining stable operation at high current.
[0026] 2. The copper nanowire composite gas diffusion electrode provided by this invention can operate stably with a low overpotential even under ampere-level high current densities, thereby improving the electroreduction of CO2 to C. 2+ The purpose of this electrode is to improve the energy efficiency of the product. In addition, it can efficiently convert CO2 into high-value-added multi-carbon products such as ethylene, ethanol, and propanol, thereby improving the economic efficiency of the entire CO2 electrocatalytic conversion system.
[0027] 3. The copper nanowire composite gas diffusion electrode provided by this invention further optimizes the pore size and catalyst loading of the microporous structure in the PTFE substrate. A PTFE substrate with a suitable pore size can increase carbon dioxide flux while preventing electrolyte infiltration; a copper nanowire catalyst layer of suitable thickness (i.e., a suitable loading) can provide sufficient active sites while avoiding insufficient carbon dioxide mass transfer. Therefore, the solution of this invention can solve the mass transfer bottleneck in ampere-level carbon dioxide electroreduction from the overall structure of the gas diffusion layer and catalyst layer, resulting in superior performance.
[0028] 4. The preparation process provided by this invention is simple, the parameters are controllable, and it is easy to scale up for mass production, which greatly reduces the preparation and operation costs of CO2 electroreduction technology. It can be mainly achieved through copper nanowire preparation, Nafion coating, and vacuum filtration loading, without the need for a complex high-temperature sintering process. This method can control the electrode area, catalyst layer thickness, and catalyst loading by adjusting the copper nanowire concentration, Nafion dosage, filtration volume, PTFE membrane area, and PTFE membrane pore size, and has good repeatability and potential for large-scale preparation.
[0029] 5. In the applications provided by this invention, the copper nanowire composite gas diffusion electrode exhibits excellent performance in the electroreduction of carbon dioxide to prepare multi-carbon products. Under preferred conditions, this electrode can achieve a multi-carbon product Faraday efficiency of 88.1% and a flux density of 1.19 A / cm². 2 The current density of the multi-carbon products indicates that the electrode can efficiently generate high-value-added multi-carbon products such as ethylene, ethanol, and n-propanol at ampere-level current densities.
[0030] 6. In the application provided by this invention, the copper nanowire composite gas diffusion electrode can still achieve a diffusion rate of 0.4 A cm⁻¹ under simulated flue gas conditions of 15% carbon dioxide. 2 Maintaining a multi-carbon product Faraday efficiency of 71.9% indicates that this electrode can reduce dependence on high-purity carbon dioxide feed or carbon dioxide pre-concentration processes. Therefore, it is suitable for both high-purity CO2 electrolytic reduction scenarios and can be directly adapted to reaction systems simulating 15% low-concentration CO2 industrial flue gas. It eliminates the need for complex CO2 capture, purification, and concentration processes, enabling the direct resource conversion of industrial waste CO2 and the efficient production of high-value-added C products such as ethylene and ethanol. 2+ Multi-carbon chemicals are suitable for resource utilization scenarios of low-concentration CO2 waste gases such as industrial tail gas and fermentation tail gas, which helps to reduce the energy consumption and cost of carbon dioxide capture and conversion coupling process.
[0031] 7. In the applications provided by this invention, the copper nanowire composite gas diffusion electrode can be adapted to the coupled operation of renewable energy power generation systems such as photovoltaic, wind power, and tidal power. It uses intermittent green electricity to drive the CO2 resource utilization reaction, without relying on high-purity CO2 gas sources and complex equipment operation and maintenance. It can achieve low-cost, long-term, and continuous green conversion of carbon dioxide, which greatly promotes the practical application of CO2 electroreduction technology from laboratory research to industrial systems and equipment. Attached Figure Description
[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0033] Figure 1 This is an electron imaging image of the copper nanowire composite gas diffusion electrode in Example 1.
[0034] Figure 2 The image shows the XPS spectrum of the copper nanowire composite gas diffusion electrode in Example 1.
[0035] Figure 3 The graph shows the overall performance of the composite gas diffusion electrode in CO2 reduction electrocatalysis in Examples 1, 1, and 2.
[0036] Figure 4 The graph shows the catalytic performance, compatibility, and stability test results for different Cu NWs and Nafion coating ratios in Example 2.
[0037] Figure 5 The figure shows the test results of catalytic performance, compatibility and stability of PTFE substrates with different pore sizes in Example 3.
[0038] Figure 6 The graph shows the test results of catalytic performance, compatibility and stability of different Cu NWs@Nafion loadings in Example 4. Detailed Implementation
[0039] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.
[0040] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0041] Example 1 A method for preparing a copper nanowire composite gas diffusion electrode includes: 1. Preparation of copper nanowires Dissolve 1.60 mmol CuCl2·2H2O and 1.76 mmol glucose in 32 mL of deionized water; dissolve 3.2 mL oleylamine and 32 μL oleic acid in 5.6 mL of anhydrous ethanol in a test tube, and then add the mixture dropwise to an Erlenmeyer flask while stirring vigorously with a magnetic stirrer at 1000 rpm. Next, slowly add 120 mL of deionized water to the Erlenmeyer flask. The resulting mixture is stirred continuously at 400 rpm, heated to 50 °C, and allowed to stand at this temperature for 12 h.
[0042] The mixture was then transferred to a PTFE-lined stainless steel high-pressure reactor and hydrothermally treated at 120 °C for 6 h. After the system cooled naturally to room temperature, the upper yellow suspension was discarded, and the reddish-brown copper nanowire precipitate at the bottom was collected. After centrifugation, the purified copper nanowires were obtained by washing twice with a 1:1 volume ratio ethanol-water solution, once with pure ethanol, and four times with n-hexane.
[0043] Based on the target requirements, an appropriate amount (approximately 9 mg in this example) of purified copper nanowires was placed in a small centrifuge tube with a capacity of 2.0 mL. 1.5 mL of lactic acid and 0.5 mL of methanol were added to uniformly disperse the copper nanowires and remove surface oil amines. The dispersion was placed in a shaking mixer (MSK-SFM-12M, Hefei Kejing Materials Technology Co., Ltd.) and ultrasonically treated for 3 min. Then, it was washed 4 times by centrifugation with methanol to obtain copper nanowires (Cu NWs).
[0044] 2. Nafion coating Based on the target coating amount of copper nanowires:Nafion at a mass ratio of 9:7, Nafion was mixed with copper nanowires and solvent; for example, 140 μL of Nafion® D520 solution (7 mg after drying) was mixed with copper nanowires (9 mg) and methanol was added to bring the volume to 2 mL. The suspension was circulated in a shaker for 4 cycles (stirring for 3 min and letting stand for 5 min per cycle) to ensure that Nafion uniformly coated the surface of the copper nanowires. Excess Nafion in the solution was removed by washing with methanol centrifugation to obtain Nafion-coated copper nanowires (Cu NWs@Nafion).
[0045] 3. Vacuum filtration load 27 mg of Cu NWs@Nafion was dispersed in methanol and the volume was adjusted to 4.0 mL. The dispersion was then vacuum filtered using a 0.45 μm PTFE membrane as the gas diffusion layer (GDL) to obtain a catalyst loading of 3.0 mg cm⁻¹. 2 Copper nanowire composite gas diffusion electrode.
[0046] Obtain electron imaging images of the copper nanowire composite gas diffusion electrode prepared in this embodiment, such as... Figure 1 As shown in the figures, a) is a scanning electron microscope (SEM) image showing that the prepared copper nanowires (Cu NWs) self-assemble into a highly porosity, randomly oriented three-dimensional interconnected network structure. Each nanowire has a diameter of approximately 70 nm and a length exceeding 100 μm, and this structure can construct continuous conductive pathways. b) is an optical image of the electrode. c) is a cross-sectional SEM image of the electrode, clearly showing a bilayer structure, with a catalyst layer thickness of approximately 16.7 μm and a PTFE substrate thickness of approximately 13.0 μm. d) is a transmission electron microscope (TEM) image of Cu NWs@Nafion, showing that Cu NWs@Nafion exhibits a regular coaxial core-shell structure, with the dark metallic Cu core completely encapsulated by a uniform light-colored coating layer, confirming that Nafion achieves uniform coating of the nanowires. e is a high-resolution transmission electron microscope (HRTEM) image of Cu NWs@Nafion, showing that the lattice spacing of the Cu nanowire core region is 0.208 nm, corresponding to the (111) crystal plane of face-centered cubic Cu; the lattice spacing of the nanowire surface region is 0.245 nm, belonging to the (111) crystal plane of Cu2O, indicating that the nanowire is composed of a Cu core and a surface Cu2O layer. f is the selected area electron diffraction (SAED) pattern of Cu NWs@Nafion, which shows characteristic fivefold symmetric diffraction spots, with an angle of approximately 72° between adjacent diffraction spot clusters, which is a characteristic of the inherent fivefold twin structure of copper nanowires. This structure is conducive to ECO2RR to C 2+ Product selectivity. High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) images of Cu NWs@Nafion clearly show the core-shell configuration of the nanowires; TEM-EDS elemental mapping images show that F, C, S, and O (characteristic elements of Nafion) are uniformly distributed along the radial and axial directions of the copper-nanowire, Cu is enriched in the core region, and the Cu2O phase is uniformly distributed at the interface between Cu and Nafion, proving that the components are uniformly distributed.
[0047] Obtain the XPS spectrum of the copper nanowire composite gas diffusion electrode prepared in this embodiment, as shown below. Figure 2As shown in the figure; where a is the X-ray diffraction (XRD) pattern of Cu NWs@Nafion, the figure shows that Cu NWs@Nafion is dominated by sharp Bragg diffraction peaks of face-centered cubic metal Cu (PDF card number: 04-0836), confirming that the Nafion coating process does not destroy the bulk crystal structure of the material; a weak but clearly identifiable Cu2O diffraction peak is also superimposed in the spectrum (PDF card number: 04-0836), which is consistent with the HRTEM characterization results; a broad diffuse peak appears at about 18°, which is consistent with the characteristic peak of the Nafion ionomer backbone, proving that Nafion has been successfully incorporated into the material. b is the Cu K-edge X-ray absorption near-edge structure (XANES) spectrum of Cu NWs@Nafion, the absorption curve of which is in high agreement with that of Cu foil, indicating that Cu0 is the main form present in the material, and a significantly enhanced edge front peak appears at about 8981 eV, which is the characteristic spectral fingerprint signal of Cu2O. c shows the EXAFS Fourier transform spectrum of CuNWs@Nafion. A strong coordination peak appears at 2.2 Å, corresponding to Cu-Cu bonds, and its peak shape is highly similar to that of the Cu foil, indicating that the core local coordination environment of Cu NWs was not altered by the Nafion coating. A weak Cu-O bond coordination peak appears at 1.5 Å, corresponding to Cu-O coordination in the surface Cu₂O, further confirming the presence of a trace oxide layer on the surface, and that this oxide layer did not change significantly during the coating process. d shows the high-resolution Cu 2p X-ray photoelectron spectroscopy (XPS) spectrum of CuNWs@Nafion. The XPS shows that the spectrum contains Cu₀ / Cu₂O bonds. + Characteristic peaks, along with accompanying peak signals, confirm the presence of metallic Cu and Cu. + Coexistence, this result is consistent with the above. Figure 2 The Cu LMM Auger spectral characterization results in e corroborate each other. f is the high-resolution C 1s XPS spectrum of Cu NWs@Nafion. The spectrum shows that the peaks can be fitted to three different chemical environments: the peak at 284.8 eV corresponds to the C of the aliphatic carbon backbone. The C bond at 286.7 eV belongs to the C-chain of the perfluoroalkyl vinyl ether side chain. O C-ether bond, C-terminal of the perfluorinated backbone at 292.0 eV. The F2 bond signal confirms the intact chemical structure of Nafion. g shows the high-resolution S 2p XPS spectrum of CuNWs@Nafion, which exhibits the broad S-band characteristic of sulfonic acid groups. The O signal indicates that the sulfonic acid group is the proton-conducting functional group of Nafion, which can promote ion transport between the gas, liquid, and solid phases during CO2RR. h is the high-resolution F 1s spectrum of Cu NWs@Nafion, showing a strong characteristic peak at 688.5 eV, corresponding to the CF bond in Nafion, further verifying the successful coating of Nafion onto the Cu NWs surface. i is the high-resolution O 1s XPS spectrum of Cu NWs@Nafion, which can be fitted with three peaks: the peak at 530.2 eV represents lattice oxygen (O2O) of Cu2O. 2- At 531.8 eV, it belongs to the Nafion sulfonic acid group ( The oxygen in SO3H is present at 533.9 eV, which is the C atom of the Nafion main chain. O The presence of oxygen in the C ether bond directly confirms the simultaneous presence of Cu2O and Nafion on the material surface, and is completely consistent with all the aforementioned characterization data.
[0048] Example 2 A method for preparing a copper nanowire composite gas diffusion electrode includes: 1. Preparation of copper nanowires Dissolve 1.60 mmol CuCl2·2H2O and 1.76 mmol glucose in 32 mL of deionized water; dissolve 3.2 mL oleylamine and 32 μL oleic acid in 5.6 mL of anhydrous ethanol in a test tube, and then add the mixture dropwise to an Erlenmeyer flask while stirring vigorously with a magnetic stirrer at 1000 rpm. Next, slowly add 120 mL of deionized water to the Erlenmeyer flask. The resulting mixture is stirred continuously at 400 rpm, heated to 50 °C, and allowed to stand at this temperature for 12 h.
[0049] The mixture was then transferred to a PTFE-lined stainless steel high-pressure reactor and hydrothermally treated at 120 °C for 6 h. After the system cooled naturally to room temperature, the upper yellow suspension was discarded, and the reddish-brown copper nanowire precipitate at the bottom was collected. After centrifugation, the purified copper nanowires were obtained by washing twice with a 1:1 volume ratio ethanol-water solution, once with pure ethanol, and four times with n-hexane.
[0050] Take an appropriate amount (approximately 9 mg) of purified copper nanowires and place them in a 2.0 mL centrifuge tube. Add 1.5 mL of lactic acid and 0.5 mL of methanol to uniformly disperse the copper nanowires and remove surface oil amines. Place the dispersion in a shaker (MSK-SFM-12M, Hefei Kejing Materials Technology Co., Ltd.) and sonicate for 3 min. Then, wash the dispersion four times with methanol by centrifugation to obtain copper nanowires (Cu NWs). Sufficient copper nanowires (Cu NWs) can be obtained by multiple preparations or proportional scaling-up.
[0051] 2. Nafion coating Based on the target coating amounts of copper nanowires to Nafion at mass ratios of 9:0, 9:1, 9:3, 9:5, 9:7, 9:9, and 9:11, Nafion was mixed with copper nanowires and a solvent. For example, different volumes of Nafion® D520 solution were mixed with copper nanowires (9 mg) according to the required dried mass of 0 mg, 1 mg, 3 mg, 5 mg, 7 mg, 9 mg, and 11 mg, respectively, and methanol was added to bring the volume to 2 mL. The suspension was circulated in a shaker for 4 cycles (stirring for 3 min and letting stand for 5 min per cycle) to ensure that Nafion uniformly coated the surface of the copper nanowires. Excess Nafion in the solution was removed by washing with methanol centrifugation to obtain Nafion-coated copper nanowires (Cu NWs@Nafion). Depending on the required amount for subsequent steps, multiple preparations or proportional scaling up of the amounts of Nafion, copper nanowires, and solvent could be used to obtain sufficient Nafion-coated copper nanowires (Cu NWs@Nafion).
[0052] 3. Vacuum filtration load A total of 27 mg of Cu NWs@Nafion was dispersed in methanol and brought to a final volume of 4.0 mL. The dispersion was then vacuum-filtered using a 0.45 μm PTFE membrane as the gas diffusion layer (GDL) to obtain a catalyst loading of 3.0 mg / cm³. 2 Copper nanowire composite gas diffusion electrode.
[0053] Example 3 A method for preparing a copper nanowire composite gas diffusion electrode includes: 1. Preparation of copper nanowires Dissolve 1.60 mmol CuCl2·2H2O and 1.76 mmol glucose in 32 mL of deionized water; dissolve 3.2 mL oleylamine and 32 μL oleic acid in 5.6 mL of anhydrous ethanol in a test tube, and then add the mixture dropwise to an Erlenmeyer flask while stirring vigorously with a magnetic stirrer at 1000 rpm. Next, slowly add 120 mL of deionized water to the Erlenmeyer flask. The resulting mixture is stirred continuously at 400 rpm, heated to 50 °C, and allowed to stand at this temperature for 12 h.
[0054] The mixture was then transferred to a PTFE-lined stainless steel high-pressure reactor and hydrothermally treated at 120 °C for 6 h. After the system cooled naturally to room temperature, the upper yellow suspension was discarded, and the reddish-brown copper nanowire precipitate at the bottom was collected. After centrifugation, the purified copper nanowires were obtained by washing twice with a 1:1 volume ratio ethanol-water solution, once with pure ethanol, and four times with n-hexane.
[0055] Take an appropriate amount (approximately 9 mg) of purified copper nanowires and place them in a 2.0 mL centrifuge tube. Add 1.5 mL of lactic acid and 0.5 mL of methanol to uniformly disperse the copper nanowires and remove surface oil amines. Place the dispersion in a shaker (MSK-SFM-12M, Hefei Kejing Materials Technology Co., Ltd.) and sonicate for 3 min. Then, wash the dispersion four times with methanol by centrifugation to obtain copper nanowires (Cu NWs). Sufficient copper nanowires (Cu NWs) can be obtained by multiple preparations or proportional scaling-up.
[0056] 2. Nafion coating Based on the target coating amount of copper nanowires:Nafion at a mass ratio of 9:7, 140 μL of Nafion® D520 solution (7 mg after drying) was mixed with copper nanowires (9 mg), and methanol was added to bring the volume to 2 mL. The suspension was circulated in a shaker for 4 cycles (stirring for 3 min and letting stand for 5 min per cycle) to ensure that Nafion uniformly coated the surface of the copper nanowires. Excess Nafion in the solution was removed by washing with methanol centrifugation to obtain Nafion-coated copper nanowires (Cu NWs@Nafion); sufficient amounts of Nafion-coated copper nanowires (CuNWs@Nafion) were obtained by multiple preparations or proportional scaling-up.
[0057] 3. Vacuum filtration load A total of 27 mg of Cu NWs@Nafion was dispersed in methanol and brought to a final volume of 4.0 mL. The dispersion was then vacuum-filtered using PTFE membranes with pore sizes of 0.10 μm, 0.22 μm, 0.45 μm, 1.0 μm, and 5.0 μm as gas diffusion layers (GDLs), yielding a catalyst loading of 3.0 mg / cm³. 2 Copper nanowire composite gas diffusion electrode.
[0058] Example 4 A method for preparing a copper nanowire composite gas diffusion electrode includes: 1. Preparation of copper nanowires Dissolve 1.60 mmol CuCl2·2H2O and 1.76 mmol glucose in 32 mL of deionized water; dissolve 3.2 mL oleylamine and 32 μL oleic acid in 5.6 mL of anhydrous ethanol in a test tube, and then add the mixture dropwise to an Erlenmeyer flask while stirring vigorously with a magnetic stirrer at 1000 rpm. Next, slowly add 120 mL of deionized water to the Erlenmeyer flask. The resulting mixture is stirred continuously at 400 rpm, heated to 50 °C, and allowed to stand at this temperature for 12 h.
[0059] The mixture was then transferred to a PTFE-lined stainless steel high-pressure reactor and hydrothermally treated at 120 °C for 6 h. After the system cooled naturally to room temperature, the upper yellow suspension was discarded, and the reddish-brown copper nanowire precipitate at the bottom was collected. After centrifugation, the purified copper nanowires were obtained by washing twice with a 1:1 volume ratio ethanol-water solution, once with pure ethanol, and four times with n-hexane.
[0060] Take an appropriate amount (approximately 9 mg) of purified copper nanowires and place them in a 2.0 mL centrifuge tube. Add 1.5 mL of lactic acid and 0.5 mL of methanol to uniformly disperse the copper nanowires and remove surface oil amines. Place the dispersion in a shaker (MSK-SFM-12M, Hefei Kejing Materials Technology Co., Ltd.) and sonicate for 3 min. Then, wash the dispersion four times with methanol by centrifugation to obtain copper nanowires (Cu NWs). Sufficient copper nanowires (Cu NWs) can be obtained by multiple preparations or proportional scaling-up.
[0061] 2. Nafion coating Based on the target coating amount of copper nanowires:Nafion at a mass ratio of 9:7, 140 μL of Nafion® D520 solution (7 mg after drying) was mixed with copper nanowires (9 mg), and methanol was added to bring the volume to 2 mL. The suspension was circulated in a shaker for 4 cycles (stirring for 3 min and letting stand for 5 min per cycle) to ensure that Nafion uniformly coated the surface of the copper nanowires. Excess Nafion in the solution was removed by washing with methanol centrifugation to obtain Nafion-coated copper nanowires (Cu NWs@Nafion); sufficient amounts of Nafion-coated copper nanowires (CuNWs@Nafion) were obtained by multiple preparations or proportional scaling-up.
[0062] 3. Vacuum filtration load A total of 27 mg of Cu NWs@Nafion was dispersed in methanol and brought to a final volume of 4.0 mL. The dispersion was then vacuum-filtered using a 0.45 μm PTFE membrane as the gas diffusion layer (GDL) to obtain catalyst loadings of 0.5 mg / cm³. 2 1.0 mg cm 2 2 mg cm 2 3.0 mg cm 2 4.0 mg cm 2 5.0 mg cm 2 Copper nanowire composite gas diffusion electrode.
[0063] Comparative Example 1 A method for preparing a copper nanowire composite gas diffusion electrode includes: 1. Preparation of copper nanowires Dissolve 1.60 mmol CuCl2·2H2O and 1.76 mmol glucose in 32 mL of deionized water; dissolve 3.2 mL oleylamine and 32 μL oleic acid in 5.6 mL of anhydrous ethanol in a test tube, and then add the mixture dropwise to an Erlenmeyer flask while stirring vigorously with a magnetic stirrer at 1000 rpm. Next, slowly add 120 mL of deionized water to the Erlenmeyer flask. The resulting mixture is stirred continuously at 400 rpm, heated to 50 °C, and allowed to stand at this temperature for 12 h.
[0064] The mixture was then transferred to a PTFE-lined stainless steel high-pressure reactor and hydrothermally treated at 120 °C for 6 h. After the system cooled naturally to room temperature, the upper yellow suspension was discarded, and the reddish-brown copper nanowire precipitate at the bottom was collected. After centrifugation, the purified copper nanowires were obtained by washing twice with a 1:1 volume ratio ethanol-water solution, once with pure ethanol, and four times with n-hexane.
[0065] Take an appropriate amount (about 9 mg) of purified copper nanowires and place them in a small centrifuge tube with a capacity of 2.0 mL. Add 1.5 mL of lactic acid and 0.5 mL of methanol to uniformly disperse the copper nanowires and remove the surface oil amine. Place the dispersion in a shaking mixer (MSK-SFM-12M, Hefei Kejing Materials Technology Co., Ltd.) and sonicate for 3 min. Then wash with methanol by centrifugation 4 times to obtain copper nanowires (Cu NWs).
[0066] 2. Nafion coating Based on the target coating amount of copper nanowires:Nafion at a mass ratio of 9:7, 140 μL of Nafion® D520 solution (7 mg after drying) was mixed with copper nanowires (9 mg), and methanol was added to bring the volume to 2 mL. The suspension was circulated in a shaker for 4 cycles (stirring for 3 min and letting stand for 5 min per cycle) to ensure that Nafion uniformly coated the surface of the copper nanowires. Excess Nafion in the solution was removed by washing with methanol centrifugation to obtain Nafion-coated copper nanowires (Cu NWs@Nafion).
[0067] 3. Vacuum filtration load A total of 27 mg of Cu NWs@Nafion was dispersed in methanol and brought to a final volume of 4.0 mL. Using CP as the gas diffusion layer (GDL), the dispersion was vacuum filtered to obtain a catalyst loading of 3.0 mg cm⁻¹. 2 A copper nanowire composite gas diffusion electrode. The CP is commercial carbon paper (YLS-30T, Suzhou Sainuoer Co., Ltd.).
[0068] Comparative Example 2 A method for preparing a copper nanoparticle composite gas diffusion electrode includes: 1. Preparation of Copper Nanoparticle (NPs) Dispersion The NPs were commercial Cu NPs (purchased from Shanghai Maclean Company, with a purity of 99.9% based on metal content and a particle size of 60-100 nm). A Cu NPs dispersion was prepared by dispersing 5 mg of Cu NPs in 550 μL of Nafion isopropanol solution. The preparation process of Nafion isopropanol solution was as follows: add isopropanol to 50 μL of 5wt% Nafion solution and bring the volume to 550 μL.
[0069] 2. Drop-coating load Using CP as the gas diffusion layer (GDL), the above Cu NPs dispersion was drop-coated onto CP to obtain a catalyst layer with a loading of 2.0 mg cm⁻¹. 2 The copper nanoparticle composite gas diffusion electrode; the CP is commercial carbon paper (YLS-30T, Suzhou Sainuoer Co., Ltd.).
[0070] Experimental Example 1 The composite gas diffusion electrodes obtained in the examples and comparative examples were used as cathodes in a gas diffusion flow electrolysis cell. 1.0 M KOH was used as the cathode electrolyte, and pure CO2 or 15% low-concentration CO2 simulated industrial flue gas was used as the reaction gas source. The system underwent optimization of electrode formulation and structural parameters, as well as testing of catalytic performance, compatibility, and stability. The test results are as follows: Figures 3-5 As shown.
[0071] The optimal Cu NWs to Nafion ratio (9:7), 0.45 μm PTFE gas diffusion layer pore size, and 3.0 mg cm⁻¹ in Example 1 were used. -2 Under the given catalyst loading conditions, the overall electrocatalytic CO2 reduction performance of this composite electrode is summarized as follows: Figure 3 As shown. Where 'a' indicates that the electrode is in... 1.0 V vs It can be achieved at RHE potential. 0.95 A cm -2Total current density; when the total current density is 1 A cm⁻¹ -2 At that time, C 2+ The product Faraday efficiency can reach 88.1%; the maximum peak value C 2+ The partial current density is 1.19 A cm⁻¹ -2 Optimal C 2+ The C1 selectivity reached 11.44, and the CO2 conversion rate was as high as 9.75%. Furthermore, the optimal electrode was used under low-concentration CO2 conditions to explore its industrial suitability. The performance of this electrode in a 15% CO2 simulated industrial flue gas environment is shown in Figure b. The electrode at 0.4 Acm... -2 It can still maintain 71.9% of C at current density. 2+ The product exhibits a Faraday efficiency while suppressing the hydrogen evolution side reaction to 13.2%, demonstrating its application potential in direct electrolysis of industrial flue gas. For industrial applications, as shown by c, the optimal electrode is at 0.8 A cm⁻¹. -2 Under constant current conditions, it can operate stably for more than 13 hours, and there is no significant decay in catalytic activity and product selectivity during operation, which can meet the requirements for long-term industrial electrolysis. In contrast, the catalytic activity and product selectivity of Comparative Examples 1 and 2 decayed significantly during operation, and could only operate for a maximum of 1 hour.
[0072] In Example 2, the fixed catalyst loading was 2.0 mg cm⁻¹. -2 The PTFE substrate was fixed with a pore size of 0.45 μm. The overall electrocatalytic CO2 reduction performance of this composite electrode is summarized as follows: Figure 4 As shown in the figure, a and b are the CO2RR linear sweep voltammetric curves for electrodes with different ratios. From a and b, it can be seen that the 9:7 ratio electrode has a significantly higher output current density at the same potential than other ratio samples. ci is the current-dependent product Faraday efficiency curve for electrodes with different ratios, and the relationship between total current density and C. 2+ The graph shows the variation of partial current density with pore size, and the total current density of the unmodified copper nanowire electrode with C. 2+ With extremely low selectivity, electrode C was optimized to a 9:7 ratio. 2+ Selectivity is significantly improved, and the hydrogen evolution process of the side reaction is effectively suppressed; further increasing the ratio results in a plateau period with essentially no change.
[0073] In Example 3, the Cu NWs to Nafion coating ratio was fixed at 9:7, and the catalyst loading was 3.0 mg cm⁻¹. -2 The overall electrocatalytic CO2 reduction performance of this composite electrode is summarized as follows: Figure 5As shown in the figure, a represents the LSV polarization curves of electrodes assembled on substrates with five pore sizes: 0.10 μm, 0.22 μm, 0.45 μm, 1.0 μm, and 5.0 μm. The 0.45 μm pore size electrode exhibits the highest catalytic current density. bf describes the current-dependent product Faradaic efficiency curves for the electrodes on substrates with pore sizes from 0.10 μm to 5.0 μm, as well as the relationship between total current density and C. 2+ The variation of partial current density with pore size shows that as the PTFE pore size increases, the CO2 mass transfer efficiency improves, and the overall catalytic performance of the electrode gradually improves. However, when the pore size exceeds 0.45 μm, the reduced water pressure resistance of the PTFE substrate makes it easier for the electrolyte to penetrate the gas diffusion layer, causing electrode flooding. This results in a decrease in the catalytic performance of the 1.0 μm and 5.0 μm large-pore-size electrodes. Based on the comprehensive electrochemical test results, 0.45 μm was determined to be the optimal PTFE gas diffusion layer pore size for the CO2RR reaction.
[0074] In Example 4, the Cu NWs to Nafion coating ratio was fixed at 9:7, and the PTFE filter membrane pore size was 0.45 μm. The overall electrocatalytic CO2 reduction performance of this composite electrode is summarized as follows: Figure 6 As shown in the figure, a represents the linear sweep voltammetric curves of CO2RR for electrodes with different loading amounts, where the total catalytic current density gradually increases with increasing loading amount; bf describes the current-dependent product Faradaic efficiency curves for electrodes with different loading amounts, and the relationship between total current density and C. 2+ The variation of partial current density with load: As the load gradually increases from 0.5 mg to 3.0 mg cm⁻¹ -2 When the loading is 3.0 mg cm -2 The performance reached its optimal level at a certain loading point; however, with further increases in loading, the performance declined as CO2 could not diffuse to deeper catalyst layers, leading to a greater likelihood of hydrogen evolution side reactions occurring at deeper catalyst layers. Based on the combined results of various electrochemical tests, the optimal loading was determined to be 3.0 mg cm⁻¹. -2 To achieve a suitable loading that balances catalytic activity and product selectivity.
[0075] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A copper nanowire composite gas diffusion electrode, characterized in that, It includes a PTFE substrate with a microporous structure, and a catalytic layer disposed on the PTFE substrate, wherein the catalytic layer is a three-dimensional network of copper nanowires coated with Nafion.
2. The copper nanowire composite gas diffusion electrode according to claim 1, characterized in that, The pore size of the microporous structure is 0.1-5.0 μm, preferably 0.1-0.6 μm; And / or, the loading of the catalyst layer on the PTFE substrate is 0.5-5.0 mg cm⁻¹. 2 Preferably 1-3 mg cm 2 ; And / or, the mass ratio of the copper nanowires to Nafion is 9:(1-11), preferably 9:(5-11).
3. The preparation method according to claim 1 or 2, characterized in that, The diameter of the copper nanowire is less than 500 nm, preferably less than 100 nm; the length of the copper nanowire is more than 100 μm. And / or, the three-dimensional network has a 500–900 nm interconnected hole structure.
4. A method for preparing a copper nanowire composite gas diffusion electrode according to any one of claims 1-3, comprising: Preparation of copper nanowires: Cu precursor and reducing agent were subjected to wet chemical synthesis and surface ligand replacement to obtain a precipitate. The precipitate was purified and acid-treated to obtain copper nanowires. Nafion coating: Copper nanowires were mixed with Nafion solution and then coated. After coating, they were centrifuged and washed to obtain Nafion-coated copper nanowires. Vacuum filtration loading: Nafion-coated copper nanowires were dispersed in a solvent and loaded onto a microporous PTFE substrate using vacuum filtration. After drying, a copper nanowire composite gas diffusion electrode was obtained.
5. The preparation method according to claim 4, characterized in that, The wet chemical synthesis and surface ligand replacement process includes: dissolving Cu precursor and reducing agent in water to obtain precursor solution; mixing ligand reagent with organic solvent to prepare ligand solution; adding ligand solution dropwise to precursor solution under first stirring condition; adding water to precursor solution under second stirring condition; heating to reaction temperature and holding at constant temperature for standing; performing hydrothermal treatment; cooling after hydrothermal treatment and obtaining precipitate. And / or, the purification process of the precipitate includes: washing sequentially with an ethanol-water solution, pure ethanol, and n-hexane; And / or, the acid treatment process includes: removing the ligand reagent coated on the surface of the prepared purified copper nanowires by a lactic acid-methanol washing method to obtain copper nanowires.
6. The preparation method according to claim 5, characterized in that, The ligand reagent includes one or more of oleic acid, oleylamine, C12-C18 long-chain hydrocarbon primary amine, ethylenediamine, polyvinylpyrrolidone, hexadecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride, and the organic solvent in the ligand solution is one or more of anhydrous ethanol, acetone, isopropanol, n-hexane, and toluene. The reaction temperature is below 100°C, preferably 40-60°C; The hydrothermal treatment is carried out in a high-pressure reactor lined with stainless steel and the treatment temperature is 100-240℃, preferably 110-130℃. The process of the lactic acid-methanol washing method includes: taking the purified copper nanowires, adding lactic acid and methanol to make the copper nanowires uniformly dispersed and remove the surface oil amine, then performing a shaking and mixing treatment, and then washing with methanol by centrifugation to obtain copper nanowires.
7. The preparation method according to claim 4, characterized in that, The coating process includes: stirring and then letting stand, repeating the stirring and standing process 1-4 times; after coating, washing to remove excess Nafion from the solution.
8. The application of the copper nanowire composite gas diffusion electrode according to any one of claims 1-3 in the cathode for the preparation of multi-carbon products by electroreduction reaction of carbon dioxide reactants.
9. The application according to claim 8, characterized in that, The multicarbon products include one or more of ethylene, ethanol, acetic acid, and propanol; The carbon dioxide reactant has a carbon dioxide concentration greater than 15%.
10. The application according to claim 8, characterized in that, The current density of the carbon dioxide electroreduction reaction is >0.5 A cm⁻¹. -2 Preferably, it is 0.5-1.2 A cm. -2 .