A catalyst for efficiently promoting electrochemical ammonia synthesis, its preparation method and application

By using a dispersed copper-supported cobalt tetroxide spinel catalyst, the problems of low efficiency and high cost in converting nitrates in water to ammonia were solved, achieving efficient and low-cost nitrate reduction to ammonia.

CN123108620APending Publication Date: 2026-11-17TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510621165.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient to efficiently and cost-effectively convert nitrates in water into high-value-added ammonia products, and traditional methods suffer from low efficiency and high energy consumption.

Method used

A dispersed copper-supported cobalt tetroxide spinel catalyst was used to form uniformly dispersed copper nanoparticles through hydrothermal reaction and high-temperature annealing. This process constructed active sites for Co and Cu, optimized the electronic structure, and promoted the electrochemical synthesis of ammonia.

Benefits of technology

It achieves efficient catalytic reduction of nitrate to ammonia under mild conditions, exhibiting good catalytic activity and stability, making it suitable for large-scale applications and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108620A_ABST
    Figure CN123108620A_ABST
Patent Text Reader

Abstract

This invention provides a catalyst for efficiently promoting electrochemical ammonia synthesis, its preparation method, and its application. The method includes the preparation of a mixed dispersion of cobalt salt and urea, the preparation of a spinel Co3O4 composite precursor, the preparation of a mixed ethanol dispersion of the spinel Co3O4 composite precursor and CuCl2·2H2O, and the preparation of the catalyst for efficiently promoting electrochemical ammonia synthesis. Copper nanoparticles exhibit good dispersibility and excellent loading on the surface of activated carbon materials, possessing a large number of catalytically active sites, which significantly increases the effective catalytic activity and inhibits the leakage of metal ions. This catalyst for efficiently promoting electrochemical ammonia synthesis helps to rapidly improve nitrate reduction kinetics; in a neutral solution containing 1000 ppm sodium nitrate, the ammonia yield can reach 1574.84 ± 46.70 μg / h in a three-electrode system over 2 hours. ‑ 1 mgcat ‑1 (-0.4V vs. RHE); In the electroreduction system of nitrate using this catalyst, the ammonia yield tends to increase with the increase of overpotential, and the ammonia yield tends to increase with the increase of nitrate concentration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochemical catalysis in environmental engineering, and more specifically to a catalyst that can efficiently promote the electrochemical synthesis of ammonia, its preparation method, and its application. Background Technology

[0002] In recent years, excessive nitrates in water have not only caused ecological imbalance but may also trigger a series of health problems. Nitrates entering the aquatic environment cause eutrophication, leading to the proliferation of algae and aquatic animals, resulting in a decline in water quality. Simultaneously, polluted water enters human living environments or the bodies of plants and animals directly or indirectly, accumulating through the food chain and impacting human health.

[0003] For decades, traditional nitrate treatment technologies, primarily physical, biological, and chemical methods, have been in use. Among these, electrochemical methods offer a more efficient and energy-efficient way to convert pollutants into NH3, N2O, N2, and NO. NH3, as an intermediate in the nitrogen cycle, is one of the most important industrial chemicals of our time and is considered essential for human nutrition. The electrocatalytic reduction of NO3 to NH3 is highly favored, as it represents a "win-win" process from an environmental perspective. This technology utilizes green energy to selectively convert nitrates into high-value-added ammonia products under mild conditions, achieving both environmental remediation and resource enhancement benefits.

[0004] Non-precious metals are widely used in NO3 due to their low cost, easy availability, and highly tunable electronic structure. - Electrochemical reduction reaction. Embedding isolated copper atoms into cobalt-based catalysts to construct asymmetric Cu-O-Co active sites is based on two core design advantages: the dynamic controllability of electronic orbital coupling and the spatial plasticity of the active site configuration. From the perspective of electronic interactions, the introduction of a single copper atom modulates the local coordination environment of Co3O4, resulting in strong coupling between the electronic orbitals of copper and cobalt, thus optimizing the electronic structure of the charge carriers. The coexistence of Cu and Co facilitates the realization of the high-spin state required for increased ammonia formation in Co. The cooperative coordination structure constructs an unobstructed upspin channel, enhancing NO3 production. - RR reaction kinetics. Furthermore, cobalt tetroxide possesses a typical three-dimensional framework structure of spinel oxides, which facilitates electron conduction between metal cations. After the addition of copper, the spinel structure did not change significantly, still providing sufficient space for electron interactions. Therefore, developing a copper-supported cobalt tetroxide spinel catalyst that is simple to prepare, inexpensive, and uniformly distributed is of great significance. Summary of the Invention

[0005] This invention overcomes the shortcomings of the prior art and provides a simple, low-cost, and highly efficient method for preparing and applying a dispersed copper-supported cobalt tetroxide spinel catalyst for the synthesis of ammonia from nitrates.

[0006] The objective of this invention is achieved through the following technical solution.

[0007] A catalyst that can efficiently promote the electrochemical synthesis of ammonia and its preparation method are carried out according to the following steps:

[0008] Step 1: Mix cobalt salt and urea (CO(NH2)2) into water and stir vigorously to break up the solid particles of cobalt salt and urea (CO(NH2)2) in the water, thereby obtaining a mixed dispersion of cobalt salt and urea, wherein the molar ratio of cobalt salt to urea (CO(NH2)2) is (0.1-1):1;

[0009] Step 2: The mixed dispersion of cobalt salt and urea obtained in Step 1 is transferred to a Teflon-lined autoclave and heated at high temperature to obtain a pink precipitate. The precipitate is purified with deionized water and ethanol, dried, and calcined at high temperature to obtain the spinel Co3O4 composite material precursor. The heating temperature for the high-temperature treatment is 150-850℃, and the heating time is 0-13h. The high-temperature calcination temperature is 200-1000℃, and the temperature is maintained for 1-3h after reaching the highest calcination temperature. The heating rate is 5-15℃·min. -1 ;

[0010] Step 3: After drying and ultrasonic treatment of the spinel Co3O4 composite material precursor prepared in Step 2, it is uniformly dispersed in ethanol to obtain an ethanol dispersion of the spinel Co3O4 composite material precursor. Then, a CuCl2·2H2O solution after strong ultrasonication is slowly added to the above ethanol dispersion to obtain a mixed ethanol dispersion of spinel Co3O4 composite material precursor and CuCl2·2H2O. The concentration of CuCl2·2H2O aqueous solution is 0.01-0.5M, the amount of CuCl2·2H2O aqueous solution used is [not specified], and the power of strong ultrasonication of CuCl2·2H2O aqueous solution is 30-60%.

[0011] Step 4: After drying the spinel Co3O4 composite material precursor prepared in Step 3 and the mixed ethanol dispersion of CuCl2·2H2O, the mixture is annealed at high temperature under the protection of an inert gas, washed with deionized water and dried to obtain a catalyst (xCu / Co3O4) that can efficiently promote the electrochemical synthesis of ammonia.

[0012] In step 1, the cobalt salt is cobalt chloride hexahydrate or cobalt nitrate hexahydrate, and the molar ratio of cobalt salt to urea is 0.2:1. Vigorous stirring is carried out using an ultrasonic pulverizer with a power of 30-60% and an ultrasonic time of 10 minutes. The vigorous stirring speed is 500-1000 rpm and the stirring time is 0-30 minutes.

[0013] In step 2, the volume of the Teflon-lined autoclave is 50-200 mL, the high-temperature heating treatment temperature is 200-800℃, the heating time is 0-12 h, the drying in a 60℃ vacuum drying oven is 12 h, the calcination temperature is 300℃, and after reaching the maximum calcination temperature, it is held for 3.5 h, with a heating rate of 5℃·min. -1 .

[0014] In step 3, the concentration of CuCl2·2H2O aqueous solution is 0.05M, the amount of CuCl2·2H2O aqueous solution used is 560μL, and the power of strong ultrasonic CuCl2·2H2O aqueous solution is 50%.

[0015] In step 4, the calcination temperature is 300℃, and after reaching the maximum calcination temperature, it is maintained for 3.5 hours, with a heating rate of 5℃·min. -1 .

[0016] The catalyst (xCu / Co3O4) can be used to efficiently promote the application of electrochemical ammonia synthesis catalyst in the catalytic reaction of nitrates and reduction intermediates in wastewater. The catalyst can be used to catalyze the synthesis of high-value-added ammonia products from nitrates and reduction intermediates in wastewater. The nitrates in the wastewater include one or a mixture of two of sodium nitrate, potassium nitrate, sodium nitrite and potassium nitrite composite salts.

[0017] This invention also discloses a method for catalytic synthesis of ammonia from nitrates under mild low pressure, comprising the following steps: mixing a catalyst (xCu / Co3O4) that can efficiently promote electrochemical ammonia synthesis, isopropanol, water, and Nafion to obtain a catalyst ink; ultrasonically treating the catalyst ink; and then uniformly coating it onto the surface of a working electrode, wherein the working electrode is a 1×1 cm... 2 A carbon cloth electrode was used, and after adding an electrolyte containing nitrates, a voltage of -0.4V vs. RHE was applied to carry out the degradation reaction. A platinum sheet electrode was used as the counter electrode, and an Ag / AgCl electrode was used as the reference electrode. 300μL of ink contained 5mg of a catalyst (xCu / Co3O4) that can efficiently promote the electrochemical synthesis of ammonia, 145μL of isopropanol, 145μL of water, and 10μL of Nafion. The ultrasonic treatment was carried out for no less than 1h at a power of 30-60%. The amount of catalyst ink coated on the surface of the working electrode was 24μL. The concentration of the nitrate electrolyte was 0.5M Na2SO4 solution, and the amount of nitrate electrolyte was 30-50mL.

[0018] The beneficial effects of this invention are as follows: 1. The preparation cycle is extremely short by using the technical solution of this invention. By using a simple hydrothermal reaction and high-temperature annealing, a catalyst (xCu / Co3O4) that can efficiently promote electrochemical ammonia synthesis is quickly prepared. The raw materials used are inexpensive and easy to purchase, which is conducive to large-scale production and application.

[0019] 2. The present invention provides a large three-dimensional structure that facilitates the successful preparation of an electrochemical ammonia synthesis catalyst (xCu / Co3O4), which can efficiently promote the successful preparation of the catalyst and form two catalytic sites, Co and Cu.

[0020] 3. By adopting the technical solution of the present invention, copper nanoparticles are well dispersed on the surface of activated carbon materials and have a better loading effect. They have a large number of catalytic active sites, which greatly improves the effective catalytic active sites and inhibits the leakage of metal ions.

[0021] 4. The technical solution of this invention can efficiently promote the electrochemical ammonia synthesis catalyst (xCu / Co3O4), which helps to rapidly improve the nitrate reduction kinetics. In a neutral solution containing 1000 ppm sodium nitrate, the ammonia yield can reach 1574.84 ± 46.70 μg / h in a three-electrode system over 2 hours. -1 mgcat -1 (-0.4V vs. RHE).

[0022] 5. By employing the technical solution of the present invention, the ammonia yield can be efficiently promoted in the electrochemical ammonia synthesis catalyst (xCu / Co3O4) electroreduction nitrate system as the overpotential increases.

[0023] 6. By adopting the technical solution of the present invention, the ammonia yield can be efficiently promoted in the electrochemical ammonia synthesis catalyst (xCu / Co3O4) electroreduction nitrate system as the nitrate concentration increases. Attached Figure Description

[0024] Figure 1 These are scanning electron microscope (SEM) images of Embodiment 1 and Comparative Examples 1-3 of the present invention;

[0025] Figure 2 These are the X-ray diffraction (XRD) patterns corresponding to Embodiment 1 and Comparative Examples 1-3 of the present invention;

[0026] Figure 3 This is a graph showing the electrochemical performance of different catalysts used in Example 2 of this invention to promote the electrochemical reduction of nitrate wastewater for ammonia synthesis.

[0027] Figure 4This is a graph showing the electrochemical performance of Cu / Co3O4-1 in Example 3 of the present invention at different potentials in promoting the electrochemical reduction of nitrate wastewater to synthesize ammonia.

[0028] Figure 5 This is a graph showing the continuous electrochemical performance of the Cu / Co3O4-1 catalyst in Example 4 of this invention in promoting the electrochemical reduction of nitrate wastewater to synthesize ammonia.

[0029] Figure 6 These are EPR diagrams of the catalysts in Example 1 and Comparative Example 1 of the present invention, where (a) is Co3O4 in Comparative Example 1 and (b) is Cu / Co3O4-1 in Example 1. Detailed Implementation

[0030] The technical solution of the present invention will be further described below through specific embodiments.

[0031] Example 1

[0032] This embodiment provides a method for preparing a cobalt tetroxide spinel (Cu / Co3O4-1) catalyst that can efficiently promote the electrochemical synthesis of ammonia, the steps of which are as follows:

[0033] Step 1: Mix 0.432g of cobalt chloride (CoCl2·6H2O) and 0.216g of urea (CO(NH2)2) into 30ml of water. The molar ratio of cobalt salt to urea is 1:3.

[0034] Step two: break up the solid particles by vigorous stirring to obtain a mixed dispersion.

[0035] Step 3: Transfer the dispersion from Step 2 to a 50mL Teflon-lined autoclave. Heat the solution at 105℃ for 6 hours. The resulting pink precipitate is purified three times with deionized water and ethanol, respectively. After drying, it is calcined at 300℃ for 3.5 hours to obtain the spinel Co3O4 composite material precursor.

[0036] Step 4: After drying the precursor obtained in Step 3, sonicate it for 30 minutes and then disperse it evenly in 50 mL of ethanol. Then slowly add 560 μL of 0.05 M CuCl2·2H2O after strong sonication.

[0037] Step 5: After drying the sample from Step 4, anneal it at 300℃ for 2 hours under an inert gas atmosphere (heating rate: 5℃·min). -1 After washing with deionized water, the sample was dried to obtain the final sample Cu / Co3O4-1.

[0038] Comparative Example 1

[0039] This embodiment provides a method for preparing a cobalt tetroxide spinel (Co3O4-0) catalyst that can efficiently promote the electrochemical synthesis of ammonia, the steps of which are as follows:

[0040] Step 1: Mix 0.432g of cobalt chloride (CoCl2·6H2O) and 0.216g of urea (CO(NH2)2) into 30ml of water. The molar ratio of cobalt salt to urea is 1:3.

[0041] Step two: break up the solid particles by vigorous stirring to obtain a mixed dispersion.

[0042] Step 3: Transfer the dispersion from Step 2 to a 50mL Teflon-lined autoclave. Heat the solution at 105℃ for 6 hours. The resulting pink precipitate is purified three times with deionized water and ethanol, respectively. After drying, it is calcined at 300℃ for 3.5 hours to obtain the spinel Co3O4 composite material precursor.

[0043] like Figure 3 It can be seen that, under the same conditions as Example 1 (i.e., nitrate content = 1000 ppm, nitrate concentration = 0.04 g·L⁻¹, voltage = -0.4 V vs. RHE, temperature = 25 °C), the ammonia yield decreased to 700.26 μg h⁻¹. -1 mg cat -1 , It is 89.20±2.77%.

[0044] Comparative Example 2

[0045] The preparation method of Cu / Co3O4-2 in this comparative example is similar to that in Example 1, except that the amount of copper chloride dihydrate added is 0.2M. The steps are as follows:

[0046] Step 1: Mix 0.432g of cobalt chloride (CoCl2·6H2O) and 0.216g of urea (CO(NH2)2) into 30ml of water. The molar ratio of cobalt salt to urea is 1:3.

[0047] Step two: break up the solid particles by vigorous stirring to obtain a mixed dispersion.

[0048] Step 3: Transfer the dispersion from Step 2 to a 50mL Teflon-lined autoclave. Heat the solution at 105℃ for 6 hours. The resulting pink precipitate is purified three times with deionized water and ethanol, respectively. After drying, it is calcined at 300℃ for 3.5 hours to obtain the spinel Co3O4 composite material precursor.

[0049] Step 4: After drying the precursor obtained in Step 3, sonicate it for 30 minutes and then disperse it evenly in 50 mL of ethanol. Then slowly add 560 μL of 0.2 M CuCl2·2H2O after strong sonication.

[0050] Step 5: After drying the sample from Step 4, anneal it at 300℃ for 2 hours under an inert gas atmosphere (heating rate: 5℃·min). -1 After washing with deionized water, the sample was dried to obtain the final sample Cu / Co3O4-2.

[0051] like Figure 3 It can be seen that this comparative example was conducted under the same conditions as Example 1, namely: nitrate content = 1000 ppm, nitrate content = 0.04 g·L⁻¹. -1 With voltage = -0.4V vs. RHE and temperature = 25℃, the ammonia yield decreased to 1207.97 μg / h. -1 mg cat -1 , It was 69.97 ± 1.30%.

[0052] Comparative Example 3

[0053] The preparation method of Cu / Co3O4-2 in this comparative example is similar to that in Example 1, except that the amount of copper chloride dihydrate added is 0.5M. The steps are as follows:

[0054] Step 1: Mix 0.432g of cobalt chloride (CoCl2·6H2O) and 0.216g of urea (CO(NH2)2) into 30ml of water. The molar ratio of cobalt salt to urea is 1:3.

[0055] Step two: break up the solid particles by vigorous stirring to obtain a mixed dispersion.

[0056] Step 3: Transfer the dispersion from Step 2 to a 50mL Teflon-lined autoclave. Heat the solution at 105℃ for 6 hours. The resulting pink precipitate is purified three times with deionized water and ethanol, respectively. After drying, it is calcined at 300℃ for 3.5 hours to obtain the spinel Co3O4 composite material precursor.

[0057] Step 4: After drying the precursor obtained in Step 3, sonicate it for 30 minutes and then disperse it evenly in 50 mL of ethanol. Then slowly add 560 μL of 0.2 M CuCl2·2H2O after strong sonication.

[0058] Step 5: After drying the sample from Step 4, anneal it at 300℃ for 2 hours under an inert gas atmosphere (heating rate: 5℃·min). -1 After washing with deionized water, the sample was dried to obtain the final sample Cu / Co3O4-3.

[0059] like Figure 1 Scanning electron microscopy (SEM) images of Co3O4, Cu / Co3O4-1, Cu / Co3O4-2, and Cu / Co3O4-3 show that the Co3O4 samples all exhibit irregular shapes under different copper content modifications. However, with increasing copper content, their diameter inevitably changes and aggregates. This may be due to changes in the nucleation and growth processes caused by introducing different copper contents.

[0060] like Figure 2 XRD was used to characterize Co3O4, Cu / Co3O4-1, Cu / Co3O4-2, and Cu / Co3O4-3. Cu / Co3O4-1 corresponds to the

[331] ,

[220] ,

[440] ,

[511] , and

[400] planes at 2θ = 37.0°, 31.4°, 65.5°, 59.6°, and 44.9°, respectively, consistent with the PDF card of standard cobalt tetroxide (JCPDS No.: 65-3103). All samples exhibit a cubic spinel structure characterized by the Fd-3m space group. No XRD diffraction peaks related to the crystalline phase of copper were observed in Cu / Co3O4-1, which may be due to the effective dispersion and uniform loading of copper in cobalt tetroxide. However, characteristic copper peaks appeared in Cu / Co3O4-2 with increasing copper content.

[0061] Example 2

[0062] This example describes the effect of different catalysts, such as Cu / Co3O4-1, on promoting the electrochemical reduction of nitrate wastewater to synthesize ammonia.

[0063] This Cu / Co3O4-1 catalyst was applied to promote the electrochemical reduction of nitrate wastewater to synthesize ammonia. The specific process was as follows: the catalyst ink consisted of 145 μL isopropanol, 145 μL water, 10 μL 5% Nafion solution, and 5 mg of catalyst. After ultrasonic treatment, 24 μL of the ink was evenly coated onto a 1×1 cm... 2 On a carbon cloth electrode (CC, hydrophilic treated). Using a Multi Autolab M204 workstation with an external voltage of -0.4V vs. RHE, the reaction was carried out in an H-type electrolytic cell equipped with a proton exchange membrane (Nafion 117). This electrolytic cell consisted of a three-electrode system (working electrode: the prepared modified electrode; counter electrode: a platinum sheet electrode; reference electrode: an Ag / AgCl electrode). All experiments were repeated three times under identical conditions to prevent excessive error.

[0064] like Figure 3 It can be seen that at -0.4V vs. RHE (electrolyte is 1000ppm NO3), -Under the conditions of 0.5 M Na₂SO₄, Cu-Co₃O₄⁻ exhibits the best performance because the metal species are atomically dispersed. This is more conducive to establishing efficient charge transfer kinetics between Cu and Co sites, thereby significantly improving NO₃⁻ performance. - RR catalytic activity. In comparison, Co3O4's... and The percentages were 89.2 ± 2.8% and 3.3 ± 0.2%, respectively.

[0065] Example 3

[0066] This embodiment describes the effect of Cu / Co3O4-1 catalyst on promoting the electrochemical reduction of nitrate wastewater to synthesize ammonia at different potentials.

[0067] This Cu / Co3O4-1 catalyst was applied to promote the electrochemical reduction of nitrate wastewater to synthesize ammonia. The specific process was as follows: the catalyst ink consisted of 145 μL isopropanol, 145 μL water, 10 μL 5% Nafion solution, and 5 mg of catalyst. After ultrasonic treatment, 24 μL of the ink was evenly coated onto a 1×1 cm... 2 On a carbon cloth electrode (CC, hydrophilic treated). Using a Multi Autolab M204 workstation with an external voltage of -0.4V vs. RHE, the reaction was carried out in an H-type electrolytic cell equipped with a proton exchange membrane (Nafion 117). This electrolytic cell consisted of a three-electrode system (working electrode: the prepared modified electrode; counter electrode: a platinum sheet electrode; reference electrode: an Ag / AgCl electrode). All experiments were repeated three times under identical conditions to prevent excessive error.

[0068] like Figure 4 It can be seen that when the electrolyte concentration is 1000 ppm NO3... - Under the conditions of 0.5M Na2SO4, Cu / Co3O4-1 Due to intensified competition with HER at high potentials, it exhibits a volcanic pattern, reaching a maximum of 96.4 ± 2.8% at -0.4 V vs. RHE, with a yield of 1574.84 ± 46.70 μg h. -1 mg cat -1 At -0.55V vs. RHE, the highest yield of NH3 reached 1739.31 ± 8.11 μg h⁻¹. -1 mg cat -1 .

[0069] Example 4

[0070] This embodiment describes the sustained effect of the Cu / Co3O4-1 catalyst in promoting the electrochemical reduction of nitrate wastewater for ammonia synthesis.

[0071] This Cu / Co3O4-1 catalyst was applied to promote the electrochemical reduction of nitrate wastewater to synthesize ammonia. The specific process was as follows: the catalyst ink consisted of 145 μL isopropanol, 145 μL water, 10 μL 5% Nafion solution, and 5 mg of catalyst. After ultrasonic treatment, 24 μL of the ink was evenly coated onto a 1×1 cm... 2 The reaction was carried out on a carbon cloth electrode (CC, hydrophilic treated). Using a Multi Autolab M204 workstation with an external voltage of -0.4V vs. RHE, the reaction was conducted in an H-type electrolytic cell equipped with a proton exchange membrane (Nafion 117). This electrolytic cell consisted of a three-electrode system (working electrode: the prepared modified electrode; counter electrode: a platinum sheet electrode; reference electrode: an Ag / AgCl electrode). All experiments were repeated three times under identical conditions to prevent excessive error.

[0072] like Figure 5 It can be seen that at -0.4V vs. RHE (electrolyte with 1000ppm NO3), - Under conditions of 0.5M Na2SO4, Cu / Co3O4-1 maintained good high performance in 8 consecutive tests (16 hours), with the Faraday efficiency remaining above 90%, indicating that Cu / Co3O4-1 effectively resists NO3-. - RR exhibits high stability.

[0073] Figure 6 These are the EPR diagrams of the catalysts in Example 1 and Comparative Example 1 of this invention. Compared to Co3O4, Cu-Co3O4 exhibits a stronger DMPO-H signal in the absence of NO3-. However, with the addition of NO3-... - Subsequently, the DMPO-H signal of Cu-Co3O4 decreased further, indicating that D-Cu-Co3O4 has a special ability to rapidly consume *H, thereby improving NO3- ionization. - Hydrogenation during the RR process.

[0074] The present invention has been described above by way of example. It should be noted that any simple modifications, alterations or other equivalent substitutions that can be made by those skilled in the art without creative effort without departing from the core of the present invention fall within the protection scope of the present invention.

Claims

1. A catalyst that can efficiently promote the electrochemical synthesis of ammonia, characterized in that: Follow these steps: Step 1: Mix cobalt salt and urea into water and stir vigorously to break up the solid particles of cobalt salt and urea in the water, thereby obtaining a mixed dispersion of cobalt salt and urea, wherein the molar ratio of cobalt salt to urea is (0.1-1):1; Step 2: The mixed dispersion of cobalt salt and urea obtained in Step 1 is transferred to a Teflon-lined autoclave and heated at high temperature to obtain a pink precipitate. The precipitate is purified with deionized water and ethanol, dried, and calcined at high temperature to obtain the spinel Co3O4 composite material precursor. The heating temperature for the high-temperature treatment is 150-850℃, and the heating time is 0-13h. The high-temperature calcination temperature is 200-1000℃, and the temperature is maintained for 1-3h after reaching the highest calcination temperature. The heating rate is 5-15℃·min. -1 ; Step 3: After drying and ultrasonic treatment, the spinel Co3O4 composite material precursor prepared in Step 2 is uniformly dispersed in ethanol to obtain an ethanol dispersion of the spinel Co3O4 composite material precursor. Then, a CuCl2·2H2O solution after strong ultrasonication is slowly added to the above ethanol dispersion to obtain a mixed ethanol dispersion of spinel Co3O4 composite material precursor and CuCl2·2H2O. The concentration of CuCl2·2H2O aqueous solution is 0.01-0.5M, the amount of CuCl2·2H2O aqueous solution used is 50μL-2.5mL, and the power of strong ultrasonication of CuCl2·2H2O aqueous solution is 30-60%. Step 4: After drying the spinel Co3O4 composite material precursor prepared in Step 3 and the mixed ethanol dispersion of CuCl2·2H2O, the mixture is annealed at high temperature under the protection of an inert gas, washed with deionized water and dried to obtain a catalyst that can efficiently promote the electrochemical synthesis of ammonia.

2. The catalyst for efficiently promoting electrochemical ammonia synthesis according to claim 1, characterized in that: In step 1, the cobalt salt is cobalt chloride hexahydrate or cobalt nitrate hexahydrate, and the molar ratio of cobalt salt to urea is 0.2:

1. Vigorous stirring is carried out using an ultrasonic pulverizer with a power of 30-60% and an ultrasonic time of 10 minutes. The vigorous stirring speed is 500-1000 rpm and the stirring time is 0-30 minutes.

3. The catalyst for efficiently promoting electrochemical ammonia synthesis according to claim 1, characterized in that: In step 2, the volume of the Teflon-lined autoclave is 50-200 mL, the high-temperature heating treatment temperature is 200-800℃, the heating time is 0-12 h, the drying in a 60℃ vacuum drying oven is 12 h, the calcination temperature is 200-500℃, and after reaching the maximum calcination temperature, it is held for 2-6 h, with a heating rate of 5℃·min. -1 .

4. The catalyst for efficiently promoting electrochemical ammonia synthesis according to claim 1, characterized in that: In step 3, the concentration of the CuCl2·2H2O aqueous solution was 0.05M, the volume of the CuCl2·2H2O aqueous solution was 560μL, and the power of the strong ultrasonic treatment of the CuCl2·2H2O aqueous solution was 50%; in step 4, annealing was carried out at 300℃ for 2 hours, with a heating rate of 5℃·min. -1 .

5. A method for preparing a catalyst that can efficiently promote electrochemical ammonia synthesis as described in any one of claims 1-4, characterized in that: Follow these steps: Step 1: Mix cobalt salt and urea into water and stir vigorously to break up the solid particles of cobalt salt and urea in the water, thereby obtaining a mixed dispersion of cobalt salt and urea, wherein the molar ratio of cobalt salt to urea is (0.1-1):1; Step 2: The mixed dispersion of cobalt salt and urea obtained in Step 1 is transferred to a Teflon-lined autoclave and heated at high temperature to obtain a pink precipitate. The precipitate is purified with deionized water and ethanol, dried, and calcined at high temperature to obtain the spinel Co3O4 composite material precursor. The heating temperature for the high-temperature treatment is 150-850℃, and the heating time is 0-13h. The high-temperature calcination temperature is 200-1000℃, and the temperature is maintained for 1-3h after reaching the highest calcination temperature. The heating rate is 5-15℃·min. -1 ; Step 3: After drying and ultrasonic treatment, the spinel Co3O4 composite material precursor prepared in Step 2 is uniformly dispersed in ethanol to obtain an ethanol dispersion of the spinel Co3O4 composite material precursor. Then, a CuCl2·2H2O solution after strong ultrasonication is slowly added to the above ethanol dispersion to obtain a mixed ethanol dispersion of spinel Co3O4 composite material precursor and CuCl2·2H2O. The concentration of CuCl2·2H2O aqueous solution is 0.01-0.5M, the amount of CuCl2·2H2O aqueous solution used is 50μL-2.5mL, and the power of strong ultrasonication of CuCl2·2H2O aqueous solution is 30-60%. Step 4: After drying the spinel Co3O4 composite material precursor prepared in Step 3 and the mixed ethanol dispersion of CuCl2·2H2O, the mixture is annealed at high temperature under the protection of an inert gas, washed with deionized water and dried to obtain a catalyst that can efficiently promote the electrochemical synthesis of ammonia.

6. The method for preparing a catalyst that can efficiently promote electrochemical ammonia synthesis according to claim 5, characterized in that: In step 1, the cobalt salt is cobalt chloride hexahydrate or cobalt nitrate hexahydrate, and the molar ratio of cobalt salt to urea is 0.2:

1. Vigorous stirring is carried out using an ultrasonic pulverizer with a power of 30-60% and an ultrasonic time of 10 minutes. The vigorous stirring speed is 500-1000 rpm and the stirring time is 0-30 minutes.

7. The method for preparing a catalyst that can efficiently promote electrochemical ammonia synthesis according to claim 5, characterized in that: In step 2, the volume of the Teflon-lined autoclave is 50-200 mL, the high-temperature heating treatment temperature is 200-800℃, the heating time is 0-12 h, the drying in a 60℃ vacuum drying oven is 12 h, the calcination temperature is 300℃, and after reaching the maximum calcination temperature, it is held for 3.5 h, with a heating rate of 5℃·min. -1 .

8. The method for preparing a catalyst that can efficiently promote electrochemical ammonia synthesis according to claim 5, characterized in that: In step 3, the concentration of the CuCl2·2H2O aqueous solution is 0.05M, the amount of CuCl2·2H2O aqueous solution used is [missing information], and the power of the strong ultrasonic treatment of the CuCl2·2H2O aqueous solution is 50%; in step 4, annealing is carried out at 300℃ for 2 hours, with a heating rate of 5℃·min. -1 .

9. The application of the catalyst for efficiently promoting electrochemical ammonia synthesis as described in any one of claims 1-4 in the catalytic reaction of nitrates and reduction intermediates in wastewater, characterized in that: The above-mentioned catalyst can be used to catalyze the nitrates and reduction reaction intermediates in wastewater to synthesize high-value-added ammonia products. The nitrates in the wastewater include one or a mixture of two of sodium nitrate, potassium nitrate, sodium nitrite, and potassium nitrite complex salts.

10. A method for catalyzing the synthesis of ammonia from nitrates using any one of the catalysts described in claims 1-4 of claim 1, characterized in that: Follow these steps: A catalyst ink was prepared by mixing a highly efficient catalyst for electrochemical ammonia synthesis (xCu / Co3O4), isopropanol, water, and Nafion. This catalyst ink was then ultrasonically treated and uniformly coated onto the surface of a working electrode (1×1 cm²). 2 The carbon cloth electrode was added to an electrolyte containing nitrates, and a voltage of -0.3 to -0.5V vs. RHE was applied to carry out the degradation reaction. The counter electrode was a platinum sheet electrode, and the reference electrode was an Ag / AgCl electrode. The 300μL ink contains 5mg of a catalyst (xCu / Co3O4) that can efficiently promote the electrochemical synthesis of ammonia, 145μL of isopropanol, 145μL of water, and 10μL of Nafion. The ultrasonic treatment lasts for at least 1 hour at a power of 30-60%. The amount of catalyst ink coated on the working electrode surface is 24μL. The concentration of the nitrate electrolyte is 0.5M Na2SO4 solution, and the amount of nitrate electrolyte is 30-50mL.