Nitrogen-doped fullerene-derived Fe-NC electrocatalysts and their preparation methods
By preparing nitrogen-doped fullerene-derived Fe-NC electrocatalysts, the problems of insufficient activity and low selectivity of existing electrocatalysts in the two-electron oxygen reduction reaction were solved, achieving efficient hydrogen peroxide generation. The raw materials are readily available and low in cost.
Patent Information
- Application Number
- CN202611537660.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electrocatalysts suffer from high cost, insufficient active site density, and low selectivity for hydrogen peroxide in the two-electron oxygen reduction reaction. In particular, noble metal-based catalysts are expensive, transition metal catalysts tend to promote the four-electron oxygen reduction reaction or hydrogen peroxide decomposition, while ordinary carbon materials have insufficient activity.
A method for preparing nitrogen-doped fullerene-derived Fe-NC electrocatalysts was adopted. By first constructing a nitrogen-doped carbon precursor and then introducing an iron source for high-temperature pyrolysis, a defect-rich carbon matrix and a nitrogen-doped structure were formed, which improved the contact and fixation of iron species with the carbon matrix and formed a catalyst with two-electron oxygen reduction performance.
It achieves a highly selective and efficient two-electron oxygen reduction reaction, improves the selectivity of hydrogen peroxide production, and has readily available raw materials, a simple preparation process, and low cost.
Smart Images

Figure CN123108636A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrocatalytic hydrogen peroxide production technology, and particularly to nitrogen-doped fullerene-derived Fe-NC electrocatalysts and their preparation methods. Background Technology
[0002] Hydrogen peroxide is an important green oxidant with wide applications in paper bleaching, wastewater treatment, medical disinfection, electronic cleaning, and fine chemical synthesis. Currently, industrial hydrogen peroxide is mainly produced centrally using the anthraquinone process. This process involves multiple steps, including organic working fluid circulation, hydrogenation, and oxidation, and is accompanied by the storage and transportation of high-concentration hydrogen peroxide. This process suffers from drawbacks such as a long workflow, high energy consumption, and unsuitability for small-scale on-site production. Therefore, developing a mild, safe, simple, and distributed hydrogen peroxide production method is of great significance.
[0003] Hydrogen peroxide can be synthesized directly from oxygen, water, and electricity under mild conditions via the two-electron oxygen reduction reaction (OOR), and can be coupled with renewable electricity. During the OOR reaction, the electrocatalyst significantly influences the adsorption mode of oxygen molecules, the stability of the *OOH intermediate, and whether the OO bond is broken. Therefore, the composition and structure of the electrocatalyst play a crucial role in the generation of hydrogen peroxide.
[0004] Existing noble metal-based electrocatalysts typically suffer from high costs; some transition metal electrocatalysts tend to promote the four-electron oxygen reduction reaction to produce water, or cause further decomposition of the generated hydrogen peroxide; while ordinary carbon materials offer advantages such as low cost and good conductivity, they often suffer from insufficient active site density and low selectivity for hydrogen peroxide. Therefore, how to prepare non-noble metal electrocatalysts that combine metal active centers, defective carbon structures, and high two-electron oxygen reduction selectivity remains a problem to be solved in the electrochemical preparation of hydrogen peroxide. Summary of the Invention
[0005] The purpose of this invention is to provide a nitrogen-doped fullerene-derived Fe-NC electrocatalyst, its preparation method, and its application. By first constructing a nitrogen-doped carbon precursor, and then introducing an iron source for a second high-temperature pyrolysis, the iron source and the fullerene-derived carbon matrix are fully contacted and combined, thereby obtaining an Fe-NC electrocatalyst with two-electron oxygen reduction performance.
[0006] In one aspect of the present invention, a nitrogen-doped fullerene-derived Fe-NC electrocatalyst is provided. The electrocatalyst uses fullerene as a carbon source, melamine as a nitrogen source, and ferric nitrate nonahydrate as an iron source; the mass ratio of fullerene to melamine is 1:1 or 2:1, and the mass ratio of the NC precursor to ferric nitrate nonahydrate is 10:1.
[0007] The fullerene undergoes pyrolysis and carbon skeleton reconstruction during high-temperature pyrolysis, forming a defect-rich carbon matrix. Nitrogen-containing species generated from melamine pyrolysis can participate in carbon skeleton construction and form nitrogen-doped structures. The formed nitrogen-doped structures can serve as potential binding sites for iron species, facilitating contact and fixation between iron species and the carbon matrix. Ferric nitrate nonahydrate forms an iron-containing component after a second high-temperature pyrolysis.
[0008] In another aspect, the present invention provides a method for preparing the above-mentioned nitrogen-doped fullerene-derived Fe-NC electrocatalyst. The preparation method includes the following steps:
[0009] Fullerene and melamine are mixed evenly according to a set ratio;
[0010] The resulting mixture was subjected to a first high-temperature pyrolysis in a tube furnace under an inert atmosphere to obtain the NC precursor.
[0011] The NC precursor and ferric nitrate nonahydrate are mixed uniformly in a set ratio;
[0012] The obtained iron-containing precursor was subjected to a second high-temperature pyrolysis in a tubular furnace under an inert atmosphere to obtain iron-containing pyrolysis products.
[0013] The iron-containing pyrolysis product was acid-washed, filtered, and washed with water. After washing with water until the filtrate was neutral, it was dried to obtain the nitrogen-doped fullerene-derived Fe-NC electrocatalyst.
[0014] In some embodiments of the present invention, the mass ratio of fullerene to melamine is 1:1 or 2:1, and the two raw materials are uniformly contacted by one or more of the following methods: grinding, stirring, ultrasonic dispersion, or solvent-assisted impregnation.
[0015] In some embodiments of the present invention, both the first and second high-temperature pyrolysis are carried out under a nitrogen atmosphere, and the pyrolysis temperature is 900℃~1000℃, preferably 900℃. The first high-temperature pyrolysis is used to construct the nitrogen-doped fullerene-derived NC precursor, and the second high-temperature pyrolysis is used to thermally decompose the iron source, which is beneficial for the contact between the iron species and the nitrogen-doped carbon matrix and improves their fixation degree.
[0016] In some embodiments of the present invention, the amount of ferric nitrate nonahydrate added is determined based on the actual mass of the NC precursor obtained from the first high-temperature pyrolysis. The mass ratio of the NC precursor to ferric nitrate nonahydrate is 10:1, and the ferric nitrate nonahydrate and the NC precursor are fully mixed by impregnation, stirring, ultrasonication, or grinding.
[0017] In some embodiments of the present invention, the acid washing is performed by treating the iron-containing pyrolysis product with an acid solution to remove some of the insufficiently fixed iron species and soluble inorganic impurities; after acid washing, the product is filtered and washed with deionized water until the filtrate is neutral, and finally dried to obtain the nitrogen-doped fullerene-derived Fe-NC electrocatalyst.
[0018] In another aspect of the invention, the present invention provides the application of the above-described nitrogen-doped fullerene-derived Fe-NC electrocatalyst. According to embodiments of the invention, the nitrogen-doped fullerene-derived Fe-NC electrocatalyst is used for electrocatalytic oxygen reduction reactions.
[0019] In some embodiments of the present invention, the nitrogen-doped fullerene-derived Fe-NC electrocatalyst is used to electrosynthesize hydrogen peroxide via a two-electron oxygen reduction reaction. It can be loaded onto a glassy carbon electrode, carbon paper, carbon cloth, or a gas diffusion electrode, and applied to a three-electrode system or a flow electrolyzer.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] This invention uses fullerene as a carbon source, which is then subjected to high-temperature pyrolysis and carbon skeleton reconstruction to form a carbon matrix with certain structural defects. This provides a reaction interface and carbon-based active sites for the oxygen reduction reaction, which is beneficial to improving the performance of the two-electron oxygen reduction reaction.
[0022] Melamine provides nitrogen doping sites, while ferric nitrate nonahydrate provides the iron source. The nitrogen-doped structure formed by the pyrolysis of melamine can provide potential binding sites for iron species, which is beneficial for the contact and fixation of iron species with the fullerene-derived carbon matrix.
[0023] This invention employs a two-step tubular furnace high-temperature pyrolysis process: first preparing the NC precursor, then introducing ferric nitrate nonahydrate. This process first forms a nitrogen-doped carbon framework and potential anchoring sites, followed by the introduction of an iron source for a second high-temperature pyrolysis. This improves the contact between the iron source and the nitrogen-doped carbon matrix and promotes the fixation of iron species within the carbon matrix. Compared to a one-step co-pyrolysis sample, FeNC-900-2 exhibits higher H₂O₂ selectivity, indicating that the process of first preparing the nitrogen-doped NC precursor and then introducing an iron source for a second high-temperature pyrolysis is beneficial for obtaining Fe-NC electrocatalysts with high two-electron oxygen reduction selectivity.
[0024] The pyrolysis temperature affects the structural characteristics and catalytic performance of the fullerene-derived carbon framework. Compared with the 800℃ comparative sample and the 1000℃ sample, the 900℃ sample exhibited superior two-electron oxygen reduction performance. XRD results showed that all samples were mainly composed of amorphous or low-degree graphitized carbon structures, and no large-sized crystalline iron-based particles reaching the conventional XRD detection limit were observed. Raman results further indicated that the sample obtained at 900℃ had obvious D and G peaks. The value is approximately 1.03, indicating that the obtained carbon material has a certain degree of structural defects and disorder.
[0025] Compared with the graphene-900-2 control sample, the optimal sample FeNC-900-2 exhibited a more positive oxygen reduction initiation potential and a larger disk current, and maintained approximately 90% H2O2 selectivity in the range of 0.2–0.65 V (vs. RHE). The H2O2 selectivity of the graphene control sample was significantly lower and decreased significantly with increasing potential, indicating that the fullerene-derived FeNC material has superior two-electron oxygen reduction performance.
[0026] Pickling can remove some of the insufficiently fixed iron species and soluble inorganic residues, thereby obtaining the pickled Fe-NC electrocatalyst. The raw materials used in this invention are readily available, and the preparation process mainly includes mixing, two high-temperature pyrolysis in a tubular furnace, and pickling and filtration, with a clear process route. Attached Figure Description
[0027] Figure 1 This is a flowchart of the two-step high-temperature pyrolysis preparation process of the nitrogen-doped fullerene-derived Fe-NC electrocatalyst in a tubular furnace according to the present invention.
[0028] Figure 2 X-ray diffraction patterns of nitrogen-doped fullerene-derived Fe-NC electrocatalysts obtained under different pyrolysis temperatures and fullerene to melamine mass ratios.
[0029] Figure 3 Raman spectra of FeNC-900-1 and FeNC-900-2 samples.
[0030] Figure 4 A comparison of hydrogen peroxide selectivity for samples FeNC-800-1, FeNC-900-1, and FeNC-1000-1.
[0031] Figure 5 A comparison of hydrogen peroxide selectivity for samples FeNC-800-2, FeNC-900-2, and FeNC-1000-2.
[0032] Figure 6 The LSV (linear sweep voltammetry) curves are for samples FeNC-800-1, FeNC-900-1, and FeNC-1000-1.
[0033] Figure 7 The LSV (linear sweep voltammetry) curves are for samples FeNC-800-2, FeNC-900-2, and FeNC-1000-2.
[0034] Figure 8RRDE linear sweep voltammetric curves of FeNC-900-2, graphene-900-2 and one-step co-pyrolysis samples are shown.
[0035] Figure 9 The graph shows a comparison of hydrogen peroxide selectivity for FeNC-900-2, graphene-900-2, and one-step co-pyrolysis samples.
[0036] Figure 10 The hydrogen peroxide yield and Faraday efficiency of FeNC-900-2 electrocatalyst at different electrode potentials in a flow electrolyzer are shown. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0038] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.
[0039] Example 1: A method for preparing a nitrogen-doped fullerene-derived Fe-NC electrocatalyst, comprising the following steps:
[0040] (1) Weigh the raw materials according to the mass ratio of fullerene to melamine of 1:1, wherein the amount of fullerene is 150 mg and the amount of melamine is 150 mg. Grind the fullerene and melamine evenly to obtain the first mixture.
[0041] (2) The first mixture was placed in a tube furnace and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere and held for 1 h. Then it was naturally cooled to room temperature to obtain the NC-900 precursor.
[0042] (3) Weigh 150 mg of the NC-900 precursor obtained in step (2), add 15 mg of ferric nitrate nonahydrate at a mass ratio of 10:1 between the NC-900 precursor and ferric nitrate nonahydrate, and use a grinding method to fully mix the NC-900 precursor and ferric nitrate nonahydrate to obtain an iron-containing precursor.
[0043] (4) The iron-containing precursor is placed in a tube furnace and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere and held for 1 h. Then it is naturally cooled to room temperature to obtain the iron-containing pyrolysis product.
[0044] (5) The iron-containing pyrolysis product was added to a 0.5 mol / L H2SO4 solution and acid-washed at 80°C for 6 h. Then it was filtered and washed with deionized water until the filtrate was neutral. After that, it was dried at 80°C for 12 h to obtain a nitrogen-doped fullerene-derived Fe-NC electrocatalyst. The obtained sample was named FeNC-900-1.
[0045] Example 2: This example provides a method for preparing a nitrogen-doped fullerene-derived Fe-NC electrocatalyst, which is the same as in Example 1, except that the initial mass ratio of fullerene to melamine is 2:1, wherein the amount of fullerene is 200 mg and the amount of melamine is 100 mg. The resulting nitrogen-doped fullerene-derived Fe-NC electrocatalyst is designated FeNC-900-2.
[0046] Example 3: This example provides a method for preparing a nitrogen-doped fullerene-derived Fe-NC electrocatalyst, which is the same as in Example 1, except that the temperatures of the first and second high-temperature pyrolysis are both 1000℃. The resulting nitrogen-doped fullerene-derived Fe-NC electrocatalyst is designated FeNC-1000-1.
[0047] Example 4: This example provides a method for preparing a nitrogen-doped fullerene-derived Fe-NC electrocatalyst, which is the same as in Example 3, except that the initial mass ratio of fullerene to melamine is 2:1, wherein the amount of fullerene is 200 mg and the amount of melamine is 100 mg. The resulting nitrogen-doped fullerene-derived Fe-NC electrocatalyst is designated FeNC-1000-2.
[0048] To further compare the effects of different high-temperature pyrolysis temperatures, different carbon sources, and different high-temperature pyrolysis processes on the obtained electrocatalysts, the following comparative examples were set up.
[0049] Comparative Example 1: This comparative example was prepared according to the preparation method of Example 1, except that the temperature of the first high-temperature pyrolysis and the second high-temperature pyrolysis was adjusted to 800℃, while other conditions remained unchanged. The resulting comparative sample was denoted as FeNC-800-1.
[0050] Comparative Example 2: This comparative example was prepared according to the preparation method of Example 2, except that the temperature of the first high-temperature pyrolysis and the second high-temperature pyrolysis was adjusted to 800℃, while other conditions remained unchanged. The resulting comparative sample was denoted as FeNC-800-2.
[0051] Comparative Example 3: In this comparative example, graphene was used instead of fullerene in Example 2. 200 mg of graphene and 100 mg of melamine were weighed and mixed at a mass ratio of 2:1. Except for using graphene instead of fullerene as the carbon source, the amounts of ferric nitrate nonahydrate added, high-temperature pyrolysis, acid washing, water washing, and drying conditions were the same as in Example 2. The resulting sample was designated as Graphene-900-2.
[0052] Comparative Example 4: This comparative example uses a one-step co-pyrolysis process. 200 mg of fullerene, 100 mg of melamine and 15 mg of ferric nitrate nonahydrate were weighed, mixed thoroughly and placed in a tube furnace. The temperature was raised to 900 °C at a rate of 10 °C / min under a nitrogen atmosphere and held for 1 h. Then it was naturally cooled to room temperature to obtain the one-step co-pyrolysis product.
[0053] The one-step co-pyrolysis product was processed according to the acid washing, filtration, water washing and drying conditions in Example 2, and the resulting sample was recorded as the one-step co-pyrolysis sample.
[0054] Based on Examples 1-4 and Comparative Examples 1-4 above, the obtained samples were characterized structurally and tested for electrocatalytic performance to compare the effects of different pyrolysis temperatures, different carbon sources and different pyrolysis processes on the structure and two-electron oxygen reduction performance of the obtained nitrogen-doped fullerene-derived Fe-NC electrocatalysts.
[0055] like Figure 2 As shown, samples FeNC-900-1, FeNC-900-2, FeNC-1000-1, and FeNC-1000-2 all exhibit broadened diffraction peaks related to carbon materials in the 2θ range of approximately 22°–27°, with a weaker broad peak near approximately 43°–45°, indicating that the obtained samples are predominantly amorphous or low-graphitized carbon structures. Compared to the 900°C sample, the 1000°C sample shows a sharper peak near approximately 26°, indicating that increasing the pyrolysis temperature can promote the partial ordering of carbon structures. No obviously sharp diffraction peaks of crystalline iron-containing species were observed in the testing range of 10°–80°, indicating that large-sized, highly crystalline iron-based particles reaching the conventional XRD detection limit were not formed in the samples.
[0056] ICP-OES analysis was performed on the acid-washed FeNC-900-2 sample. 0.0477 g of sample was weighed, digested, and diluted to 25 mL. Three parallel determinations were performed, and the results are shown in Table 1. Table 1 shows that the Fe content in Fe-NC was 0.1480 ± 0.0028 wt%, corresponding to an Fe content of 1480.4 ± 27.8 mg·kg⁻¹. -1 The relative standard deviation of parallel measurements was 1.88%. ICP-OES results showed that Fe could still be detected in the acid-washed nitrogen-doped fullerene-derived Fe-NC electrocatalyst.
[0057] Table 1. ICP-OES test results of FeNC-900-2 electrocatalyst
[0058] Parallel measurements Fe concentration (mg / L) Fe content (mg / kg) Fe mass fraction (wt%) 1 2.777789 1455.86 0.1456% 2 2.813901 1474.79 0.1475% 3 2.882177 1510.58 0.1511% Mean ± Standard Deviation 2.824622±0.053014 1480.41±27.78 0.1480%±0.0028% RSD 1.88% 1.88% 1.88%
[0059] To compare the effects of different carbon sources and pyrolysis processes on the two-electron oxygen reduction performance, graphene-900-2 and a one-step co-pyrolysis sample were selected as control samples and compared with FeNC-900-2 under the same RRDE test system and test conditions.
[0060] like Figure 3 As shown, FeNC-900-1 and FeNC-900-2 samples were at approximately 1350 cm⁻¹. -1 and 1590 cm -1 Distinct D and G peaks were observed at all locations. The D peak is mainly related to structural defects and disordered structures in carbon materials, while the G peak primarily originates from sp... 2 In-plane vibrations of the hybrid carbon framework. FeNC-900-1 and FeNC-900-2 samples. The values are all approximately 1.03, indicating that the obtained carbon materials all have a certain degree of structural defects and disorder. Moreover, at the same pyrolysis temperature, the carbon skeleton defects of the samples obtained from the two fullerene-melamine feeding ratios are relatively similar. Combined with the XRD results, it can be seen that the obtained Fe-NC samples are mainly composed of amorphous or low-graphitized carbon structures, and have obvious defective carbon structure characteristics.
[0061] like Figure 4 and Figure 5 As shown, the hydrogen peroxide selectivity of samples obtained at different high-temperature pyrolysis temperatures varies. Compared with the corresponding 800℃ comparative example and 1000℃ sample, the FeNC-900-1 and FeNC-900-2 samples obtained at 900℃ exhibit better hydrogen peroxide selectivity. Figure 6 and Figure 7 The LSV curves of samples FeNC-800-1, FeNC-900-1, and FeNC-1000-1, and samples FeNC-800-2, FeNC-900-2, and FeNC-1000-2 are shown respectively. Combined with... Figures 4-7 It can be seen that the high temperature of pyrolysis affects the two-electron oxygen reduction performance of the obtained electrocatalyst. Compared with the 800℃ comparative sample and the 1000℃ sample, the 900℃ sample showed better two-electron oxygen reduction performance.
[0062] Weigh 5 mg of electrocatalyst, add 980 μL of isopropanol and 20 μL of Nafion solution, and sonicate for 15 min to obtain catalyst ink. Take 5 μL of catalyst ink and drop-coat it onto the surface of a rotating ring-disk electrode glassy carbon disk. Apply 0.1 mol·L⁻¹ -1 KOH was used as the electrolyte, and high-purity O2 was bubbled through the electrode for at least 15 minutes until oxygen saturation was achieved. A three-electrode system was used, with RRDE as the working electrode, Ag / AgCl as the reference electrode, and a graphite rod as the counter electrode. The test rotation speed was 1600 rpm, and the scan rate was 10 mV·s. -1 The ring electrode potential is maintained at 0.236 V (vs. Ag / AgCl, corresponding to 1.20 V vs. RHE) for oxidation and detection of H2O2 generated by the disk electrode.
[0063] like Figure 8 As shown, the disk current curves of FeNC-900-2 and the one-step co-pyrolysis sample are generally similar, and both are significantly better than those of graphene-900-2; FeNC-900-2 exhibits a slightly higher disk current in the low potential region. Figure 9 As shown, within the range of 0.2 to 0.65 V (vs. RHE), the H2O2 selectivity of FeNC-900-2 is generally higher than that of the one-step co-pyrolysis sample and graphene-900-2; the H2O2 selectivity of the one-step co-pyrolysis sample is generally higher than that of graphene-900-2, but lower than that of FeNC-900-2, indicating that the two-step pyrolysis process is beneficial to improving the two-electron oxygen reduction selectivity of the electrocatalyst.
[0064] like Figure 10 As shown, in the flow electrolyzer test, at 0.1 mol·L⁻¹ -1 KOH was used as the electrolyte, Ag / AgCl as the reference electrode, carbon paper coated with electrocatalyst as the cathode, and a ruthenium-iridium-titanium plate as the anode. The test potential was converted to the RHE scale. At −0.6 V, −0.4 V, −0.2 V, 0 V, and 0.2 V (vs. RHE), the hydrogen peroxide yields were 955.78, 530.09, 488.56, 384.73, and 280.90 mg·L⁻¹, respectively. -1 ·h -1 The corresponding Faraday efficiencies are 79.03%, 74.62%, 86.65%, 82.71%, and 86.27%, respectively.
[0065] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing nitrogen-doped fullerene-derived Fe-NC electrocatalysts, characterized in that, Includes the following steps: Fullerene and melamine were mixed and subjected to a first high-temperature pyrolysis under an inert atmosphere to obtain the NC precursor. The NC precursor was mixed with ferric nitrate nonahydrate and subjected to a second high-temperature pyrolysis under an inert atmosphere to obtain an iron-containing pyrolysis product. The iron-containing pyrolysis product was acid-washed, filtered, and washed with water until the filtrate was neutral before drying to obtain the nitrogen-doped fullerene-derived Fe-NC electrocatalyst.
2. The preparation method according to claim 1, characterized in that, The mass ratio of fullerene to melamine is 1:1 or 2:
1.
3. The preparation method according to claim 2, characterized in that, The mass ratio of the NC precursor to ferric nitrate nonahydrate is 10:
1.
4. The preparation method according to claim 3, characterized in that, Both the first and second high-temperature pyrolysis were carried out under a nitrogen atmosphere, and the temperatures of both the first and second high-temperature pyrolysis were 900℃~1000℃.
5. The preparation method according to claim 4, characterized in that, The temperatures of the first and second high-temperature pyrolysis were both 900℃.
6. The preparation method according to any one of claims 1 to 5, characterized in that, The pickling process involves treating the iron-containing pyrolysis products with an acid solution to remove some of the insufficiently fixed iron species and soluble inorganic impurities. The water washing process uses deionized water.
7. A nitrogen-doped fullerene-derived Fe-NC electrocatalyst, characterized in that, The electrocatalyst was prepared using the method described in claim 1.
8. The application of the nitrogen-doped fullerene-derived Fe-NC electrocatalyst of claim 7 in the electrosynthesis of hydrogen peroxide via a two-electron oxygen reduction reaction.