Copper foil and its preparation method, current collector, negative electrode sheet, secondary battery

By adjusting the crystal texture coefficient and grain size of the copper foil, a thin copper foil with both high tensile strength and high elongation was prepared, which solved the problems of high temperature stability and processing stability of thin copper foil in the field of power batteries and improved the overall performance of the battery.

CN123108672APending Publication Date: 2026-11-17JIUJIANG TELFORD ELECTRONICS MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611357253.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing thin copper foils are difficult to balance high tensile strength and high elongation in the field of power batteries, and their high-temperature stability is poor. In particular, they are prone to problems such as foil breakage and cracking during high-speed winding of battery cells, electrode rolling and cyclic charging and discharging.

Method used

By adjusting the crystal texture coefficient and grain size of the copper foil, copper foil with a thickness of 3μm~6μm was prepared. The texture coefficient of the (220) crystal plane was greater than or equal to 0.5 and less than 1. The ratio of the texture coefficient of the (111) crystal plane to the texture coefficient of the (200) crystal plane was 1~5. The average grain size was controlled to be 0.22μm~0.60μm, and the difference between the maximum and minimum grain size did not exceed 2.30μm.

Benefits of technology

This achieves a balance between high tensile strength and high elongation of copper foil, improves the high-temperature stability and processing stability of copper foil, reduces the risk of electrode cracking and peeling, and improves the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108672A_ABST
    Figure CN123108672A_ABST
Patent Text Reader

Abstract

This application provides a copper foil and its preparation method, a current collector, a negative electrode sheet, and a secondary battery. The thickness of the copper foil is 3μm~6μm, and the texture coefficient of the (220) crystal plane in the copper foil is TC. (220) The texture coefficient of the (111) crystal plane is TC. (111) The texture coefficient of the (200) crystal plane is TC. (200) , with TC (220) TC (111) and TC (200) Based on the sum, TC (220) The proportion is greater than or equal to 0.5 and less than 1, and 1 ≤ TC (111) / TC (200) ≤5. The copper foil provided in this application has high tensile strength and elongation, as well as good stability, especially high-temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrochemical technology, and in particular to copper foil and its preparation method, current collector, negative electrode sheet, and secondary battery. Background Technology

[0002] Rechargeable batteries, represented by lithium-ion batteries, possess advantages such as high operating voltage, high energy density, good safety, and no memory effect, and have achieved great success in portable electronic devices, electric vehicles, and hybrid vehicles. Copper foil, as the current collector, has a significant impact on battery performance. Currently, in the field of power batteries, to continuously improve battery energy density, the industry is gradually pushing copper foil thickness from the traditional 8μm to 6μm and 5μm, and has gradually developed ultra-thin copper foils of 3μm to 3.5μm. However, reducing the thickness of the copper foil directly reduces the cross-sectional mechanical load-bearing capacity, especially during high-speed winding of the battery cell, electrode rolling, and volume deformation during cyclic charging and discharging. This easily leads to problems such as foil breakage, cracking, and copper layer peeling, making it difficult for current thin copper foils to simultaneously achieve high tensile strength and high elongation, and also resulting in poor stability, especially high-temperature stability. Therefore, how to develop thin copper foils with high tensile strength and high elongation, while also possessing good stability, especially high-temperature stability, is a pressing technical problem that needs to be solved. Summary of the Invention

[0003] Based on this, this application provides a copper foil and its preparation method, a current collector, a negative electrode sheet, and a secondary battery, aiming to improve the tensile strength and elongation of the thin copper foil, while also having good stability, especially high-temperature stability.

[0004] The first aspect of this application provides a copper foil with a thickness of 3μm to 6μm, wherein the texture coefficient of the (220) crystal plane in the copper foil is TC. (220) The texture coefficient of the (111) crystal plane is TC. (111) The texture coefficient of the (200) crystal plane is TC. (200) , with the TC (220) The TC (111) and the TC (200) Based on the sum of the TCs, (220) The proportion is greater than or equal to 0.5 and less than 1, and 1 ≤ TC (111) / TC (200) ≤5.

[0005] In some implementations, one or more of the following conditions are met:

[0006] (1) In the copper foil, the average grain size is φ, 0.22μm≤φ≤0.60μm;

[0007] (2) In the copper foil, the difference in grain size between the largest and smallest grains is Td, and Td≤2.30μm.

[0008] In some embodiments, the copper foil has a tensile strength ≥690MPa at 20℃~30℃, and may be 690MPa~810MPa.

[0009] In some implementations, one or more of the following conditions are met:

[0010] (1) The thickness of the copper foil is 3μm~3.5μm, and the elongation is ≥2.5%, which can be 2.5%~7%;

[0011] (2) The thickness of the copper foil is 4μm~5μm, and the elongation is ≥3.5%, which can be 3.5%~10%;

[0012] (3) The thickness of the copper foil is 5.5μm~6μm and the elongation is ≥5.5%, which can be 5.5%~13%.

[0013] In some embodiments, after the annealed copper foil is baked at 180°C for 10 minutes, one or more of the following conditions are met:

[0014] (1) The decrease in the tensile strength of the copper foil is ≤5%;

[0015] (2) The texture coefficient TC of the (220) crystal plane of the copper foil (200) The rate of change is <5%.

[0016] In some embodiments, after the annealed copper foil is baked at 200°C for 10 minutes, one or more of the following conditions are met:

[0017] (1) The decrease in the tensile strength of the copper foil is ≤8%;

[0018] (2) The texture coefficient TC of the (220) crystal plane of the copper foil (200) The rate of change is <10%.

[0019] A second aspect of this application provides a method for preparing copper foil, comprising:

[0020] Copper foil is prepared by electrolysis. The electrolyte used in the electrolysis method includes the following components: copper ions 70g / L~110g / L, sulfuric acid 90g / L~130g / L, chloride ions 10ppm~50ppm, Class A additives 60ppm~120ppm, Class B additives 14ppm~40ppm, and Class C additives 10ppm~25ppm.

[0021] The Class A additives include one or more of tetrahydrothiazothione and sodium thiazolinyl dithiopropane sulfonate; the Class B additives include Class B1 and Class B2 additives, wherein Class B1 additives include hydroxyethyl cellulose, and Class B2 additives include one or more of polyvinylpyrrolidone and polyvinylimidazolium; and the Class C additives include one or more of ethylene thiourea and polyethyleneimine.

[0022] A third aspect of this application provides a current collector comprising the copper foil described in the first aspect.

[0023] A fourth aspect of this application provides a negative electrode sheet, comprising a current collector as described in the third aspect and a negative electrode active layer disposed on at least one side of the current collector, the negative electrode active layer comprising a negative electrode active material.

[0024] In some embodiments, the negative electrode active material includes a silicon-based material.

[0025] The fifth aspect of this application provides a secondary battery, including the negative electrode sheet described in the fourth aspect.

[0026] The thin copper foil of the above thickness provided in this application is certified by TC. (220) The proportion of TC is greater than or equal to 50% and less than 100%. (111) / TC (200) The synergy of 1 to 5 can jointly regulate the morphology and orientation distribution of columnar crystals in copper foil, taking into account the mechanical strength, elongation and thermal recrystallization stability of copper foil. Attached Figure Description

[0027] Figure 1 The image shows the electron backscatter diffraction (EBSD) pattern of the copper foil prepared in Example 2.

[0028] Figure 2 Electron backscatter diffraction (EBSD) pattern of the copper foil prepared for Comparative Example 2.

[0029] Figure 3 The image shows the X-ray diffraction pattern of the copper foil prepared in Example 12. Detailed Implementation

[0030] To facilitate understanding of this application, a more complete description will be provided below. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.

[0031] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form a range not explicitly stated; and any lower limit can be combined with other lower limits to form a range not explicitly stated, just as any upper limit can be combined with any other upper limit to form a range not explicitly stated. Furthermore, although not explicitly stated, every point or individual value between the endpoints of the range is included within that range. Therefore, each point or individual value can be used as its own lower or upper limit and combined with any other point or individual value or with other lower or upper limits to form a range not explicitly stated.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. It should be noted that, unless otherwise stated, the term "and / or" as used herein includes any and all combinations of one or more of the associated listed items, "above," "below," includes the stated number, and "one or more" with "multiple" means two or more.

[0033] In this document, when referring to numerical intervals (i.e., numerical ranges), unless otherwise specified, the distribution of selectable values ​​within a numerical interval is considered continuous, and includes the two endpoints (i.e., the minimum and maximum values) of the numerical interval, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all subranges included therein. The "numerical value" in this numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include percentage intervals, ratio intervals, proportion intervals, and other numerical interval types.

[0034] In this document, for methods involving multiple steps, unless otherwise explicitly stated herein, there is no strict order constraint on the execution of these steps; they may be executed in any order other than those described. Moreover, any step may include multiple sub-steps or multiple stages, which are not necessarily completed at the same time, but may be executed at different times, and their execution order is not necessarily sequential, but may be executed in turn, alternately, or simultaneously with other steps or parts of the sub-steps or stages of other steps.

[0035] The foregoing description of this application is not intended to describe every disclosed implementation or method. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the application, guidance is provided through a series of embodiments that can be used in various combinations. The examples listed are representative only and should not be construed as exhaustive.

[0036] Currently, in the field of power batteries, to continuously improve battery energy density, the industry is gradually promoting the iteration of copper foil thickness from the traditional 8μm to 6μm and 5μm, and has gradually developed ultra-thin copper foils of 3μm to 3.5μm. However, thin copper foils usually have the following problems: First, high-strength copper foils, which emphasize tensile strength, generally have low elongation (e.g., less than 3%), making them prone to cracking and breakage during cell bending, electrode rolling, and thermal cycling deformation, and can only be used in low-stress conditions; second, high-elongation copper foils, which emphasize elongation, usually have low tensile strength (e.g., less than 650MPa), making it difficult to meet the tension requirements of high-speed mass production equipment. Therefore, current thin copper foils cannot achieve a balance between high strength and high elongation.

[0037] Furthermore, the aforementioned thin copper foils typically require tolerance to harsh environments such as annealing and prolonged baking at 180°C or higher during use, but current products exhibit significant shortcomings in thermal stability. Currently, high-strength thin copper foils primarily rely on metastable fine grains formed by electrodeposition and internal stress for strengthening. After complete annealing, the internal stress is released, and the grains coarsen, leading to a substantial decrease in tensile strength. Most products cannot maintain a strength above 690 MPa after annealing, making it difficult to guarantee reliability in subsequent use. To address this, the industry currently relies mainly on external methods such as adjusting the annealing process and adding anti-oxidation coatings to improve heat resistance. However, these modifications are not only costly but also damage conductivity and interfacial adhesion, failing to fundamentally solve the problem of high-temperature structural instability, resulting in poor stability of the copper foil, especially at high temperatures. Therefore, this application proposes the following technical solution.

[0038] In a first aspect, this application provides a copper foil with a thickness of 3μm to 6μm, wherein the texture coefficient of the (220) crystal plane in the copper foil is TC. (220) The texture coefficient of the (111) crystal plane is TC. (111) The texture coefficient of the (200) crystal plane is TC. (200) , with TC (220) TC (111) and TC (200) Based on the sum, TC (220) The proportion is greater than or equal to 0.5 and less than 1; and satisfies: 1≤TC (111) / TC (200) ≤5.

[0039] The thin copper foil of the above thickness provided in this application has a texture coefficient TC of the (220) crystal plane. (220) The proportion is greater than or equal to 0.5 and less than 1, and the ratio of the texture coefficient of the (111) crystal plane to the texture coefficient of the (200) crystal plane is TC. (111) / TC (200) The range is 1 to 5. Among them, TC (111) / TC (200) A value of 1 to 5 indicates that the (111) preferred orientation is dominant over the (200) preferred orientation in the copper foil. At this time, the copper foil has a sufficient number of movable slip systems, and the stress can be released in multiple directions during the deformation process, thus improving the elongation of the copper foil. At the same time, it can avoid the intensification of mechanical anisotropy caused by the excessive dominance of the (111) texture.

[0040] TC (220) The proportion is greater than or equal to 0.5 and less than 1, indicating that the (220) crystal plane of the copper foil has a moderate preferred orientation; combined with TC (111) / TC (200) With a constraint of 1 to 5, the copper foil can simultaneously maintain a high (111) crystal plane orientation level. This moderate (220) preferred orientation forms a columnar crystal structure extending along the thickness direction of the copper foil with approximately parallel grain boundaries; this columnar crystal structure makes the intrinsic {111} within the grains... <110> The uniform distribution of the Schmidt factor in the slip system facilitates the uniform initiation of slip during deformation and alleviates local stress concentration. The columnar crystal structure, accompanied by high-density grain boundaries and substructures, can suppress recrystallization nucleation, increase the critical recrystallization temperature of the copper foil, and improve the thermal stability of the copper foil.

[0041] Thus, under the above textured conditions, through TC (220) The proportion of TC is greater than or equal to 50% and less than 100%. (111) / TC (200) The synergistic effect of 1-5 allows copper foil grains to align in an orderly manner along a specific orientation, optimizing the slip system's activation capability. It also balances the proportions of two types of secondary crystal planes, reducing strength or plasticity limitations caused by enrichment in a single crystal orientation. This achieves high strength enhancement while retaining good plasticity, thus facilitating a balance between high strength and high elongation in copper foil. Simultaneously, it enhances the copper foil's grain boundary thermal stability. Its stable, preferred crystal orientation structure effectively suppresses abnormal grain growth and recrystallization at high temperatures (e.g., ≥100℃), effectively improving the stability of the copper foil's microstructure and properties in high-temperature environments, particularly its high-temperature stability. This is achieved through TC... (220) The proportion of TC is greater than or equal to 50% and less than 100%. (111) / TC (200) The synergy of 1 to 5 can jointly regulate the morphology and orientation distribution of columnar crystals in copper foil, taking into account the mechanical strength, elongation and thermal recrystallization stability of copper foil.

[0042] For example, TC (220) The percentage can be 0.5, 0.53, 0.60, 0.64, 0.70, 0.75, 0.80, 0.86, 0.90, 0.99, or within any range of the above values; TC (111) / TC (200) It can be 1, 2, 3, 4, 5, or any of the above values.

[0043] It is understood that the "texture coefficient of a crystal facet" in this application refers to a parameter used to quantify the degree of orientation concentration of a specific crystal facet in a polycrystalline material. It characterizes the intensity of the preferred orientation of a crystal facet by comparing the experimentally measured X-ray diffraction (XRD) intensity of a crystal facet (such as (220)) with the theoretical intensity of a randomly oriented sample. The "texture coefficient ratio of a crystal facet" represents the proportion of the texture coefficient of a crystal facet in the total coefficients of all measured crystal facets. It is used to compare the contribution of different crystal facet orientations to the overall texture. In X-ray diffraction analysis, the texture coefficient can be calculated by comparing the integral intensity of each diffraction peak with the intensity ratio of a standard powder sample, and then normalized to obtain the coefficient ratio of each crystal facet.

[0044] In some embodiments, the average grain size of the copper foil is φ, 0.22μm≤φ≤0.60μm. For example, φ can be 0.22μm, 0.26μm, 0.30μm, 0.34μm, 0.40μm, 0.45μm, 0.50μm, 0.56μm, 0.60μm, or within any range of the above values. The fact that the average grain size of the copper foil is within this range indicates that the grain distribution in the copper foil is uniform and refined. This uniform and refined grain distribution can improve the strength of the copper foil through the strengthening effect of fine grains, and can reduce or even avoid the brittleness problem caused by excessively fine local grains. Simultaneously, it can reduce or even eliminate grain boundary stress concentration points, which is beneficial for improving the bending and tearing resistance of the copper foil, and can solve the problems of large performance fluctuations between batches and easy failure of weak points in traditional high-strength copper foil.

[0045] In some embodiments, the difference in grain size between the largest and smallest grains in the copper foil is Td, where Td ≤ 2.3 μm. For example, Td can be 2.3 μm, 2 μm, 1.7 μm, 1.4 μm, 1.1 μm, 0.8 μm, 0.5 μm, 0.3 μm, 0.1 μm, 0.08 μm, 0.05 μm, 0.03 μm, 0.01 μm, etc.

[0046] The difference in grain size between the largest and smallest grains in the copper foil, Td, does not exceed 2.30 μm, indicating that the grain size difference in the copper foil is small and the grain size distribution is relatively uniform. This can reduce the problem of local stress concentration caused by uneven grain size distribution, thereby reducing brittle cracking and foil breakage, and improving the stability of the copper foil. At the same time, it can also reduce the problem of aggravated abnormal grain growth at high temperature caused by large differences in grain size, and improve the stability of the copper foil in high-temperature environments.

[0047] In some embodiments, the average grain size of the copper foil is φ, where 0.22 μm ≤ φ ≤ 0.60 μm; the difference in grain size between the largest and smallest grains is Td, where Td ≤ 2.3 μm. The synergy between the average grain size and the grain size difference Td in the copper foil allows for a uniform and refined grain distribution. The uniform and moderately refined grains can enhance the overall strength through grain refinement, reduce or even eliminate stress-weak areas, improve the copper foil's resistance to bending and tearing, and further enhance its high-temperature structural stability, reducing performance fluctuations.

[0048] In some embodiments, the copper foil has a thickness of 3μm to 6μm and a tensile strength of ≥690MPa at 20℃ to 30℃, optionally 690MPa to 810MPa. The aforementioned texture state of the copper foil, and further, the aforementioned grain size relationship, enable thin copper foils within this thickness range to possess a high tensile strength of ≥690MPa. This high tensile strength is beneficial for improving the copper foil's resistance to bending and tearing.

[0049] For example, the thickness of the copper foil can be 3μm, 4μm, 5μm, 6μm or within any range of the above values; the tensile strength at 20℃~30℃ can be 690MPa, 710MPa, 730MPa, 750MPa, 770MPa, 790MPa, 810MPa, etc.

[0050] In some embodiments, the copper foil has a thickness of 3 μm to 3.5 μm and an elongation of ≥2.5%, optionally 2.5% to 7%. For example, the thickness of the copper foil can be 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm or within any range of the above values; the elongation can be 2.5%, 4.5%, 4.5%, 5.5%, 6.5%, 7%, etc.

[0051] In some embodiments, the copper foil has a thickness of 4μm to 5μm and an elongation of ≥3.5%, optionally 3.5% to 10%. For example, the thickness of the copper foil can be 4μm, 4.2μm, 4.4μm, 4.6μm, 4.8μm, 5μm, or within any range of the above values; the elongation can be 3.5%, 4.5%, 5.5%, 6.5%, 7.5%, 8.5%, 9.5%, 10%, etc.

[0052] In some embodiments, the copper foil has a thickness of 5.5 μm to 6 μm and an elongation of ≥5.5%, optionally 5.5% to 13%. For example, the thickness of the copper foil can be 5.5 μm, 5.6 μm, 5.7 μm, 5.8 μm, 5.9 μm, 6 μm or within any range of the above values; the elongation can be 5.5%, 6.5%, 7.5%, 8.5%, 9.5%, 10%, 11%, 12%, 13%, etc.

[0053] The elongation of copper foil decreases with decreasing thickness. Thinner copper foils have a higher proportion of defects, making them more prone to stress concentration and microcracks during stretching. Furthermore, the scale effect is significant, and cracks can easily penetrate the foil rapidly, causing breakage before it can be fully and uniformly stretched, resulting in low elongation. To address this, this application improves the elongation of copper foil at thinner dimensions by adjusting the grain texture and, based on this, the grain size (see above). The above-mentioned thickness-elongation matching relationship was designed accordingly. This design precisely matches the processing tension and service deformation requirements of copper foils of different thicknesses. It ensures that the thin copper foil of this application does not break during high-speed winding and rolling processes, and effectively adapts to the volume expansion during silicon-based anode cycling, reducing or even avoiding electrode cracking and peeling, thus significantly improving electrode yield and battery cycle stability.

[0054] In some embodiments, the copper foil has a tensile strength ≥690MPa at 20℃~30℃, optionally 690MPa~810MPa; the copper foil thickness is 3μm~3.5μm, and the elongation is ≥2.5%, optionally 2.5%~7%; the copper foil thickness is 4μm~5μm, and the elongation is ≥3.5%, optionally 3.5%~10%; the copper foil thickness is 5.5μm~6μm, and the elongation is ≥5.5%, optionally 5.5%~13%.

[0055] This application achieves high strength in copper foil while simultaneously improving its elongation at thinner dimensions by adjusting the grain texture and, based on this, the aforementioned thickness-elongation matching relationship was designed. This design precisely matches the processing tension and service deformation requirements of copper foils of different thicknesses, which helps to solve the problems of insufficient overall strength of current ultra-thin copper foils, the difficulty in matching the processing and service conditions of copper foils of different thicknesses with a uniform elongation index, and the difficulty of adapting ultra-thin specifications to the volume deformation of silicon-based anodes. Among them, high tensile strength can resist the stress generated by high-speed winding and electrode rolling, while graded elongation can precisely adapt to the usage requirements of products of various thicknesses, effectively reducing the risk of electrode cracking and peeling, and improving processing yield and battery cycle life.

[0056] It should be noted that the "copper foil after annealing" in this application refers to the process of baking freshly electrolyzed copper foil at 60℃~90℃ for 20h~120h, then taking out a sample to test the warpage (e.g., using a disc sampler to measure the warpage). If the warpage is >10mm, it is determined that the annealing is not complete, and baking continues (the extension time is set according to the degree of warpage); if the warpage is ≤10mm, it is determined that the annealing is complete, and the copper foil at this time is the copper foil after annealing.

[0057] In some embodiments, after the annealed copper foil is baked at 180°C for 10 minutes, the decrease in tensile strength of the copper foil is ≤5%. For example, this decrease can be 1%, 2%, 3%, 4%, 5%, or within any of the above values.

[0058] In some embodiments, after the annealed copper foil is baked at 200°C for 10 minutes, the decrease in tensile strength of the copper foil is ≤8%. For example, this decrease can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, or within any of the above values.

[0059] In this application, the decrease in the tensile strength of the copper foil is equal to (σ... 烘烤前 -σ 烘烤后 ) / σ 烘烤前 ×100%; where σ 烘烤前 σ represents the tensile strength of the copper foil after annealing; 烘烤后 This represents the tensile strength of the copper foil after annealing and baking it at 180°C or 200°C for 10 minutes.

[0060] In some embodiments, after the annealed copper foil is baked at 180°C for 10 min, the texture factor TC of the (220) crystal plane of the copper foil is... (200)The rate of change is <5%, further ≤4.9%, and even further 1% to 4.9%. For example, the rate of change can be 1%, 2%, 3%, 4%, 4.9%, or within any of the above values.

[0061] In some embodiments, after the annealed copper foil is baked at 200°C for 10 minutes, the texture factor TC of the (220) crystal plane of the copper foil is... (200) The rate of change is <10%, further ≤9.9%, and even further 1% to 9.9%. For example, the rate of change can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 9.9%, or any of the above values.

[0062] In this application, the texture factor TC of the (220) crystal plane of the copper foil is... (200) The rate of change can be calculated using the following formula: Among them, TC (200) The texture factor of the (220) crystal plane of the copper foil before baking, TC, represents the texture factor of the copper foil after annealing. (200) The texture factor of the (220) crystal plane of the copper foil after baking represents the copper foil after annealing is baked at 180°C or 200°C for 10 minutes.

[0063] Traditional copper foil has random grain orientation and disordered grain boundary energy distribution. During high-temperature baking and annealing, grain recovery and recrystallization easily occur, causing the original preferred texture to rapidly disintegrate and grain orientation to become disordered, ultimately resulting in a significant decrease in mechanical properties. In contrast, the high (220) texture formed in this application possesses parallel and continuous columnar grain boundaries, with the grain boundaries pinning each other, significantly increasing the recrystallization critical temperature; and the high proportion of (220) texture (i.e., TC) (220) The proportion of 50% or more and less than 100% is combined with a specific texture coefficient ratio (i.e., 1 ≤ TC). (111) / TC (200) ≤5), can provide sufficient and uniform start-up {111} <110> The slip system, (111) and (200) grains can further divide columnar crystals and hinder high-temperature grain boundary migration. This allows the well-oriented columnar grain boundaries of the copper foil to continue to play a grain boundary strengthening role after annealing, making its microstructure similar to that before baking. Therefore, its texture change rate is small (i.e., the decrease in tensile strength after baking at 180℃ and 200℃ for 10 min is ≤5% and ≤8%, respectively), and the decrease in tensile strength is also small (i.e., after baking at 180℃ and 200℃ for 10 min, the texture coefficient TC of the (220) crystal plane is small). (200)The change rates are <5% and <10% respectively, indicating strong high-temperature mechanical stability. Thus, this copper foil can withstand harsh conditions such as downstream annealing processes, high-temperature service in automotive batteries, and high-frequency PCB bonding, reducing or even avoiding the precipitous performance decline caused by high-temperature microstructure degradation in traditional high-strength copper foil, thereby improving the reliability and lifespan of end products.

[0064] In a second aspect, this application provides a method for preparing copper foil, which can be used to prepare the copper foil of the first aspect, comprising: preparing copper foil by electrolysis, wherein the electrolyte used in the electrolysis method comprises the following components: copper ions 70 g / L~110 g / L, sulfuric acid 90 g / L~130 g / L, chloride ions 10 ppm~50 ppm, type A additives 60 ppm~120 ppm, type B additives 14 ppm~40 ppm, and type C additives 10 ppm~25 ppm; wherein type A additives include one or more of tetrahydrothiazolylthione (H1) and sodium thiazolinyl dithiopropane sulfonate (SH110); type B additives include type B1 additives and type B2 additives, type B1 additives include hydroxyethyl cellulose (HEC), type B2 additives include one or more of polyvinylpyrrolidone (PVP) and polyvinylimidazolium (PVI); and type C additives include one or more of ethylene thiourea (ETU) and polyethyleneimine (PEI).

[0065] In the above electrolyte, by combining appropriate types and concentrations of type A additives, type B additives, and type C additives, the grain deposition and growth process of copper foil can be reasonably controlled, thereby producing the copper foil of the first aspect of this application.

[0066] For example, the concentration of Class A additives in the electrolyte can be 60ppm, 70ppm, 80ppm, 90ppm, 100ppm, 110ppm, 120ppm or within any of the above values.

[0067] For example, the concentration of Class B additives in the electrolyte can be 14 ppm, 15 ppm, 20 ppm, 25 ppm, 30 ppm, 35 ppm, 40 ppm, or within any range of the above values.

[0068] For example, the concentration of Class C additives in the electrolyte can be 10 ppm, 13 ppm, 16 ppm, 19 ppm, 22 ppm, 25 ppm, or within any of the above values.

[0069] In some embodiments, the Class A additives include tetrahydrothiazothione (H1) and sodium thiazolinyl dithiopropane sulfonate (SH110). Further, in the electrolyte, the concentration of tetrahydrothiazothione (H1) is 25 ppm to 44 ppm, and the concentration of sodium thiazolinyl dithiopropane sulfonate (SH110) is 37 ppm to 64 ppm.

[0070] H1 and SH110, especially H1, are strong inducers for the (220) crystal plane. The higher the concentration of H1, the greater the adsorption coverage on the cathode surface. 2+ The faster the deposition rate on the (220) surface, the better. By compounding H1 and SH110 and controlling the concentration of Class A additives in the electrolyte within a suitable range, it is beneficial to promote the formation of the specific texture parameters of the copper foil mentioned above. At the same time, when the concentration of Class A additives is high, it can trigger instantaneous nucleation, resulting in a larger nucleation density and relatively fine and uniform grains; when the concentration of Class A additives decreases, the nucleation overpotential decreases, and the grains grow and their size distribution widens. Therefore, by controlling the concentration of Class A additives in the electrolyte within a suitable range in this application, it is beneficial to promote the formation of the specific grain size of the copper foil mentioned above.

[0071] In some embodiments, the Class B additives include hydroxyethyl cellulose (HEC) and polyvinylpyrrolidone (PVP). Further, the concentration of hydroxyethyl cellulose (HEC) in the electrolyte is 3.75 ppm to 8 ppm, and the concentration of polyvinylpyrrolidone (PVP) is 11 ppm to 24 ppm.

[0072] HEC, a type B1 additive, can promote (220) orientation. As a protective colloid, HEC can inhibit abnormal grain growth and reduce the grain size difference (Td) between the largest and smallest grains in the copper foil. PVP or PVI, type B2 additives, exhibit strong selective adsorption (including physical and chemical adsorption) of Cu(111), thus inhibiting (111) growth. By combining type B1 and type B2 additives and controlling the concentration of type B additives in the electrolyte within a suitable range, it is beneficial to promote the formation of the specific texture parameters of the copper foil mentioned above. Furthermore, when the concentration of type A additives is high, the induction of the (220) crystal plane by type A is dominant; when the concentration of type A additives is low, the inhibitory effect of type B on the (111) crystal plane is relatively enhanced. When the concentrations of both are controlled within suitable ranges, the TC(220) value of the copper foil mentioned above can be obtained through their synergistic effect.

[0073] In some embodiments, the Class C additive includes ethylene thiourea (ETU). Further, the concentration of ethylene thiourea (ETU) in the electrolyte is 10 ppm to 24 ppm.

[0074] Class C additives, especially ETU, can enhance the (111) texture by refining the grains and increasing the density of nanotwins. By controlling the concentration of Class C additives in the electrolyte within a suitable range, the increase of TC(111) / TC(200) can be promoted and the specific TC(111) / TC(200) value mentioned above can be obtained.

[0075] Thirdly, this application provides a current collector, comprising the copper foil of the first aspect or the copper foil prepared by the preparation method of the second aspect.

[0076] Fourthly, this application provides a negative electrode sheet, including a current collector as described in the third aspect and a negative electrode active layer disposed on at least one side of the current collector. The negative electrode active material in the negative electrode active layer includes a silicon-based material; optionally, the silicon-based material includes one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Silicon-based materials exhibit significant volume expansion during cycling. When used in conjunction with the copper foil of this application, the copper foil can withstand the volume expansion of the silicon-based negative electrode, as well as the heat generation and high temperatures during cycling, and is less prone to breakage, thereby improving the cycle life of the battery.

[0077] Fifthly, this application provides a secondary battery, including a third-party negative electrode sheet.

[0078] In some embodiments, the secondary battery also includes an electrolyte and a separator. During the charging and discharging process, ions move back and forth between the positive and negative electrodes, inserting and extracting. The electrolyte acts as a conductor of ions between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.

[0079] Fifthly, this application provides an electrical device, including the secondary battery of the fourth aspect of this application.

[0080] In some implementations, the type of electrical equipment is not particularly limited, and it can be any electronic device known in the prior art. For example, the electrical equipment may include, but is not limited to, power tools, electric vehicles, laptops, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, etc.

[0081] The following are specific embodiments, which describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations within the scope of the disclosure of this application will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.

[0082] In the following examples, "room temperature" or "normal temperature" refers to 20°C to 30°C, for example, 25°C.

[0083] Example 1

[0084] This embodiment provides an electrolytic copper foil with a thickness of 3μm, an annealed tensile strength of 761.5MPa at room temperature, an elongation of 3.29% after annealing (warpage ≤10mm is considered complete), and a purity ≥99.95%.

[0085] The preparation process of this copper foil is as follows: A copper rod with a purity of 99.9% and a diameter of 8 mm is dissolved in concentrated sulfuric acid, and air is introduced from the bottom side of the copper dissolving tank while hydrochloric acid is added. After passing through a diatomaceous earth filter and a security filter, the solution is mixed evenly with an aqueous solution of additives. Then, after passing through a precision filter and a plate heat exchanger, the electrolyte is obtained and injected into an electrolytic cell. The temperature of the electrolyte after the plate heat exchanger is controlled at 54℃. The electrolytic cell consists of a cathode roller and an anode plate. Current forms a closed loop through the anode plate-copper sulfate electrolyte-cathode roller, and copper foil is deposited on the surface of the cathode roller. After peeling and anti-oxidation treatment, and annealing treatment, electrolytic copper foil is obtained. The electrolyte contains 90 g / L~95 g / L copper ions, 100 g / L~110 g / L sulfuric acid, 25 ppm~35 ppm chloride ions, and additives. The types and concentrations of additives can be found in Table 1.

[0086] Example 2

[0087] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 3 μm, a room temperature tensile strength of 734.2 MPa, an elongation of 3.13%, and a purity of ≥99.95%.

[0088] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0089] Example 3

[0090] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 3.5 μm, a room temperature tensile strength of 765.8 MPa, an elongation of 3.65%, and a purity of ≥99.95%.

[0091] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0092] Example 4

[0093] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 3.5 μm, a room temperature tensile strength of 738.6 MPa, an elongation of 3.36%, and a purity of ≥99.95%.

[0094] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0095] Example 5

[0096] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 4.0 μm, a room temperature tensile strength of 772.3 MPa, an elongation of 4.34%, and a purity of ≥99.95%.

[0097] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0098] Example 6

[0099] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 4.0 μm, a room temperature tensile strength of 745.7 MPa, an elongation of 4.01%, and a purity of ≥99.95%.

[0100] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0101] Example 7

[0102] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 5.0 μm, a room temperature tensile strength of 770.1 MPa, an elongation of 5.13%, and a purity of ≥99.95%.

[0103] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0104] Example 8

[0105] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 5.0 μm, a room temperature tensile strength of 746.9 MPa, an elongation of 4.72%, and a purity of ≥99.95%.

[0106] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0107] Example 9

[0108] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 793.4 MPa, an elongation of 6.74%, and a purity of ≥99.95%.

[0109] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0110] Example 10

[0111] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 764.8 MPa, an elongation of 6.31%, and a purity of ≥99.95%.

[0112] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0113] Example 11

[0114] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 752.5 MPa, an elongation of 6.15%, and a purity of ≥99.95%.

[0115] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0116] Example 12

[0117] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 776.2 MPa, an elongation of 6.52%, and a purity of ≥99.95%.

[0118] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0119] Example 13

[0120] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 758.9 MPa, an elongation of 6.23%, and a purity of ≥99.95%.

[0121] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0122] Comparative Example 1

[0123] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 669.7 MPa, an elongation of 4.04%, and a purity of ≥99.95%.

[0124] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0125] Comparative Example 2

[0126] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 642.9 MPa, an elongation of 3.57%, and a purity of ≥99.95%.

[0127] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0128] Comparative Example 3

[0129] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 655.3 MPa, an elongation of 3.81%, and a purity of ≥99.95%.

[0130] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0131] Comparative Example 4

[0132] Unlike Example 1, this example provides an electrolytic copper foil with a thickness of 6.0 μm, a room temperature tensile strength of 674.1 MPa, an elongation of 4.16%, and a purity of ≥99.95%.

[0133] The preparation process of this copper foil differs from that of Example 1 in that the formulation of the additives is different, as detailed in Table 1.

[0134] The copper foils or batteries prepared according to the above embodiments and comparative examples were subjected to relevant performance tests, and the test results are shown in Tables 2 and 3 below.

[0135] The test conditions or standards for each performance test item are as follows:

[0136] (1) Grain orientation test of copper foil

[0137] The grain orientation in the copper foil was tested using an X-ray diffractometer, including the texture coefficient TC of the (220) crystal plane. (220) (111) Texture coefficient TC of crystal plane (111) and TC (200) The texture coefficient of the crystal plane can be derived as TC for the (200) crystal plane.(200) , and the ratio TC of the texture coefficient of the (111) crystal plane to the texture coefficient of the (200) crystal plane. (111) / TC (200) .

[0138] The formulas for calculating the texture coefficient of each crystal plane are as follows:

[0139]

[0140]

[0141] ;

[0142] TC (220) Percentage = TC (220) / (TC (220) +TC (111) +TC (200) ).

[0143] Texture coefficient TC of (220) crystal plane after baking (200) The rate of change is:

[0144] .

[0145] (2) Grain morphology test of copper foil

[0146] Grain morphology was tested by electron backscatter diffraction (EBSD): including the average grain size and the grain size difference Td between the largest and smallest grains.

[0147] (3) Tensile strength and elongation test of copper foil

[0148] Cut copper foil strips to a width of 15mm and a length of 10cm. Perform tensile testing using a universal testing machine. The gauge length is 50mm, and the tensile speed is 50mm / min. Unit conversion: 0.1kgf / mm² = 0.98MPa. When the load drops to 80% of the peak load, fracture is considered, and the test is stopped.

[0149] σ = Fmax / A;

[0150] σ represents tensile strength, with units of MPa;

[0151] Fmax represents the maximum load (N), which is read directly from the testing machine.

[0152] The decrease in the tensile strength of copper foil = (σ 烘烤前 -σ 烘烤后 ) / σ 烘烤前 ×100%.

[0153] Elongation calculation: △L=(L-L0) / L0*100% (where L0 is the initial length of the spline; L is the length after stretching).

[0154] (4) Battery performance test

[0155] Battery Preparation: ① Lithium cobalt oxide (LiCoO2), conductive carbon black SuperP, and polyvinylidene fluoride (PVDF) were thoroughly mixed in an appropriate amount of N-methylpyrrolidone (NMP) solvent at a weight ratio of 97:1.5:1.5 to form a uniform positive electrode slurry with a solid content of 73 wt%. This slurry was coated onto a 10 μm positive electrode current collector aluminum foil, dried at 85°C, cold-pressed, and slit to obtain the positive electrode sheet. ② Artificial graphite and silicon-carbon anode material were used as the negative electrode active material at a mass ratio of 90:10 (wherein the silicon-carbon anode material has an average silicon grain size of 1.5 nm, a silicon mass content of 35%, and a specific surface area of ​​2.8 m²). 2 / g; Porous carbon with an average pore size of 1.7nm and a BET of 2027m. 2 / g, pore volume 0.87cm 3 / g), the negative electrode active material, styrene-butadiene rubber, CMC, and carbon nanotubes are mixed evenly in an appropriate amount of distilled water at a weight ratio of 97:2:0.5:0.5 to obtain a negative electrode slurry. The negative electrode slurry is coated on the above copper foil, dried at 85°C, cold-pressed, and slit to obtain a negative electrode sheet. ③ The negative electrode sheet, separator, and positive electrode sheet are stacked and wound in sequence. The separator is made of polypropylene (PP) film. After welding the tabs, it is placed in an aluminum-plastic film packaging bag. Then, the electrolyte is injected. The electrolyte is a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) at a volume ratio of 1:1 and contains LiPF6 with a molar concentration of 1 mol / L. Finally, after vacuum sealing, standing, formation, shaping, and capacity testing, a soft-pack lithium-ion battery with a capacity of 8Ah is obtained.

[0156] Test conditions: At an ambient temperature of 25±3°C, the charge / discharge rate is 1.5C / 2C, and the voltage range is 3V~4.5V. The capacity retention rate of the battery is tested after 500 cycles. Then, the battery is discharged to 3.2V, and the soft-pack battery is disassembled to check for microcracks and broken strips on the negative electrode.

[0157] Table 1

[0158]

[0159] Table 2

[0160]

[0161] Table 3

[0162]

[0163] As can be seen from Tables 2 and 3, the copper foil thickness of all the samples in this application is relatively small, the (220) texture coefficient is relatively large, and the average grain size is relatively small. In the 3.0μm ultra-thin specification, the (220) texture coefficient reaches the highest of 0.71, corresponding to a stable tensile strength of over 700MPa at room temperature. Relying on the optimization effect of the high proportion of (220) preferred texture on the grain slip system, this product achieves enhanced tensile strength while retaining good plasticity, and can fully adapt to the usage requirements of different ultra-thin copper foils under the conditions of cell winding, electrode rolling and silicon-based anode volume deformation.

[0164] The comparative sample (220) had the highest texture coefficient of only 0.42, and the texture coefficient ratio TC (111) / TC (200) Deviating from the reasonable range of 1~5, and dominated by the (111) or (200) crystal orientation, not only are the room temperature tensile strengths all below 675MPa, but the elongation is also generally below 4.2%, exhibiting obvious brittleness, making it difficult to meet the requirements for high-end lithium battery copper foil. The cell cycle test results further confirmed the application impact of the mechanical performance differences: the sample of the example did not have any broken strips or microcracks during the cycle, and the cell capacity retention rate was ≥95%. In contrast, the comparative sample generally showed microcracks, and the highest capacity retention rate was only 88.2%, with some samples even below 85%, fully demonstrating the key role of the graded elongation rate and high strength performance of this application in the cycle stability of the battery.

[0165] As can be seen from the data in Tables 2 and 3, the average grain size φ of the sample in the example is concentrated between 0.27 μm and 0.56 μm, and the difference in grain size Td between the largest and smallest grains does not exceed 2.17 μm. The overall grain distribution is uniform and continuous. According to the theory of fine grain strengthening, moderately refined grains can increase the number of grain boundaries, hinder dislocation movement, and thus improve the overall strength of the material. At the same time, the uniform grain distribution can eliminate local stress concentration points and improve the bending and tearing resistance of the copper foil. In contrast, all comparative samples have a larger average grain size φ and a grain size difference Td greater than 2.51 μm. The grain distribution is highly dispersed, and stress-weak areas are easily formed inside the matrix. This not only results in lower mechanical properties at room temperature but also induces cracking and band breakage during processing. Meanwhile, the uniformity of grain size and the crystal texture work together to further affect the high-temperature service performance of copper foil. The sample in the example, with its uniform grains and highly stable (220) texture, can effectively suppress abnormal grain growth and grain boundary migration in high-temperature environments, providing microstructure support for thermal stability.

[0166] The high-temperature aging test results directly confirm the important role of microstructure in the thermal stability of copper foil. After the samples in this application were treated at 180℃ / 10min and 200℃ / 10min, the change rate of the (220) texture coefficient was less than 4.83% and 8.81%, respectively, and the tensile strength attenuation rate was less than 4.41% and 7.15%, respectively, which fully met the requirements of high temperature and low attenuation index. This is because the high proportion of (220) preferred texture has higher grain boundary migration energy, and the grain orientation is not easily disordered at high temperature. The superimposed constraint effect of uniform grain structure can suppress recrystallization behavior from the source. Even after annealing and long-term high-temperature baking, the microstructure and macroscopic mechanical properties of copper foil can still remain stable. The comparative sample was mainly composed of random mixed textures. The texture ratio was low and the grain boundary thermal stability was poor. Under high temperature conditions, not only did the grains coarsen and the orientation become disordered, but the organic additives remaining in the copper foil preparation process would also gradually decompose and destroy the grain boundary bonding force, ultimately resulting in a significant deterioration in performance. The tensile strength at 180℃ / 10min of the comparative sample all exceeded 14.62%, and the tensile strength at 200℃ / 10min all exceeded 25%. After high temperature treatment, the tensile strength of some samples was far below 600MPa, making it difficult to withstand harsh working conditions such as annealing, vehicle high temperature, and energy storage high temperature.

[0167] Example 2 (see Figure 1 The cross-sectional EBSD morphology of the copper foil shows that the grains are fine and highly uniformly distributed, with an average grain size φ of 0.34 μm. The grain size difference Td between the largest and smallest grains is only 1.26 μm, and there are no obvious coarse grains or stress-weak areas. The IPF orientation pattern shows that the grain boundaries are mainly high-stability, large-angle grain boundaries. Combined with the XRD pattern (see...), Figure 2 Verification showed that the texture factor TC of the (220) crystal plane of the copper foil in Example 12 reached 0.55, and the ratio of the texture factor of the (111) to that of the (200) crystal plane was 3.5. This microstructure directly supports the macroscopic performance: the copper foil of Example 12 has a room temperature tensile strength ≥700MPa, while maintaining a graded elongation of 2.98%~6.52%, and after baking at 200℃ / 10min, the change rate of the (220) texture factor is only 5.81%~7.54%, and the tensile strength decay rate is ≤7.15%.

[0168] In contrast, see Comparative Example 2 (see Figure 3 The grain size distribution of conventional copper foil is extremely uneven, with an average grain size φ of 0.64 μm and a grain size difference Td between the largest and smallest grains exceeding 2.51 μm. The texture coefficient (220) is only 0.34. This structural defect directly leads to the deterioration of its macroscopic performance: the tensile strength at room temperature is only 642.9 MPa, the elongation is only 3.57%, and after baking at 200℃ / 10min, the tensile strength decay rate is as high as 25.48%. Microcracks are prone to occur during the battery cell cycle, and the capacity retention rate is only 88.2%.

[0169] As can be seen from the comparison, this application constructs a preferred texture of "moderately refined grains + uniform distribution + high proportion (220) + stable large-angle grain boundaries" (see [reference]). Figure 1 Of all grain boundaries, those with a large angle greater than 10° accounted for 94.49%; while Figure 2 The integrated microstructure, which accounts for only 88.18% of the total, overcomes the antagonistic relationship between strength and elongation by relying on the synergistic effect of fine grain strengthening and (220) texture. It also suppresses grain coarsening at high temperatures by relying on high migration energy grain boundaries and stable texture. This fundamentally solves the industry pain points of insufficient mechanical properties and poor thermal stability of existing products, and provides solid microstructure support for the reliable application of copper foil in high energy density batteries.

[0170] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0171] The above embodiments merely illustrate several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A copper foil, characterized in that, The thickness of the copper foil is 3 μm-6 μm, a texture coefficient of a (220) crystal face in the copper foil is TC (220) , a texture coefficient of a (111) crystal face is TC (111) , and a texture coefficient of a (200) crystal face is TC (200) , wherein the sum of the TC (220) , the TC (111) , and the TC (200) is taken as a reference, the proportion of the TC (220) is greater than or equal to 0.5 and less than 1, and 1≤TC (111) / TC (200) ≤5.

2. The copper foil according to claim 1, characterized in that, One or more of the following conditions must be met: (1) In the copper foil, the average grain size is φ, 0.22μm≤φ≤0.60μm; (2) In the copper foil, the difference in grain size between the largest and smallest grains is Td, and Td≤2.30μm.

3. The copper foil according to claim 1 or 2, characterized in that, The copper foil has a tensile strength ≥690MPa at 20℃~30℃, and can be selected as 690MPa~810MPa.

4. The copper foil according to claim 3, characterized in that, One or more of the following conditions must be met: (1) The thickness of the copper foil is 3μm~3.5μm, and the elongation is ≥2.5%, which can be 2.5%~7%; (2) The thickness of the copper foil is 4μm~5μm, and the elongation is ≥3.5%, which can be 3.5%~10%; (3) The thickness of the copper foil is 5.5μm~6μm and the elongation is ≥5.5%, which can be 5.5%~13%.

5. The copper foil according to claim 1, 2 or 4, characterized in that, After the annealed copper foil is baked at 180°C for 10 minutes, one or more of the following conditions are met: (1) The decrease in the tensile strength of the copper foil is ≤5%; (2) the texture coefficient TC of the (220) crystal plane of the copper foil (200) of the change rate < 5%.

6. The copper foil according to claim 1, 2 or 4, characterized in that, After the copper foil has been annealed, it is baked at 200°C for 10 minutes, and one or more of the following conditions are met: (1) The decrease in the tensile strength of the copper foil is ≤8%; (2) The texture coefficient TC of the (220) crystal plane of the copper foil (200) The rate of change is <10%.

7. A method for preparing copper foil, characterized in that, include: Copper foil is prepared by electrolysis. The electrolyte used in the electrolysis method includes the following components: copper ions 70g / L~110g / L, sulfuric acid 90g / L~130g / L, chloride ions 10ppm~50ppm, Class A additives 60ppm~120ppm, Class B additives 14ppm~40ppm, and Class C additives 10ppm~25ppm. The Class A additives include one or more of tetrahydrothiazothione and sodium thiazolinyl dithiopropane sulfonate; the Class B additives include Class B1 and Class B2 additives, wherein Class B1 additives include hydroxyethyl cellulose, and Class B2 additives include one or more of polyvinylpyrrolidone and polyvinylimidazolium; and the Class C additives include one or more of ethylene thiourea and polyethyleneimine.

8. A current collector, characterized in that, Includes the copper foil as described in any one of claims 1 to 7.

9. A negative electrode sheet, characterized in that, It includes the current collector as described in claim 8 and a negative electrode active layer disposed on at least one side of the current collector, the negative electrode active layer comprising a negative electrode active material.

10. The negative electrode sheet according to claim 9, characterized in that, The negative electrode active material includes silicon-based materials.

11. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 9 or 10.