A fatigue-resistant nickel alloy material for printing screens and its preparation method

By preparing fatigue-resistant nickel alloy materials containing nitrogen-doped graphene and Ni(Co) solid solution, the problem of insufficient fatigue resistance of electroformed nickel screen printing plates during long-term cyclic printing was solved, and the high strength and durability of the material were achieved.

CN123108673APending Publication Date: 2026-11-17SHANGHAI SHIYUGUANG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611511364.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electroformed nickel screen printing plates have insufficient fatigue resistance during long-term cyclic printing, making them prone to fatigue cracks, which can lead to screen breakage and reduced printing accuracy.

Method used

A fatigue-resistant nickel alloy material was prepared by electroforming and heat treatment using an electroforming solution composed of nickel sulfamate, nickel chloride, boric acid, cobalt sulfamate, sodium hypophosphite, nitrogen-doped graphene, and polyethylene glycol. This process formed Ni(Co) solid solution, nanotwins, and Zener pinning structures, thereby enhancing the material's fatigue resistance.

Benefits of technology

It significantly improves the fatigue resistance of printing screens, extends their service life, and ensures the stability and reliability of printing accuracy.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides a fatigue-resistant nickel alloy material for printing screens and its preparation method. The method includes the following steps: using a master mold as the cathode, electroforming is performed in a nickel sulfamate electroforming solution, wherein the nickel sulfamate electroforming solution uses water as a solvent and contains: 200-500 g / L nickel sulfamate, 5-50 g / L nickel chloride, 25-45 g / L boric acid, 1.0-3.0 g / L sodium saccharin, 10-20 g / L cobalt sulfamate, 2.5-3 g / L sodium hypophosphite, 0.1-0.3 g / L nitrogen-doped graphene, and 0.1-0.5 g / L polyethylene glycol; the electroformed nickel alloy layer is completely peeled off from the master mold to obtain the fatigue-resistant nickel alloy material for printing screens. A multi-level anti-fatigue system consisting of "solid solution strengthening - interface anchoring - grain boundary pinning" was constructed using cobalt sulfamate, sodium hypophosphite, and nitrogen-doped graphene / PEG. The "solute segregation pinning" of phosphorus and the "surface confinement" of nitrogen-doped graphene complement each other, jointly inhibiting grain growth and crack propagation under cyclic loading, and significantly improving the fatigue resistance of printing screens under cyclic loading.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electroforming technology, and in particular to a fatigue-resistant nickel alloy material for printing screens and its preparation method. Background Technology

[0002] Screen printing is a core component for printing fine circuitry in fields such as solar cells, printed circuit boards, and display panels. Electroformed nickel screens are gradually replacing traditional etched screens due to their advantages such as high aperture precision, smooth aperture walls, and good ink flow. Currently, electroformed nickel screens mostly use pure nickel or Ni-Co alloy systems. Pure nickel has low strength and limited fatigue resistance; while Ni-Co alloys can improve strength through solid solution strengthening, excessive cobalt content significantly increases internal stress, leading to difficulties in demolding and dimensional instability. Furthermore, during long-term cyclic printing, electroformed nickel screens are subjected to repeated squeegee pressure and ink friction, making them prone to fatigue crack initiation and propagation, resulting in screen damage and decreased printing accuracy. Therefore, improving the fatigue resistance of electroformed nickel screens is crucial for extending their service life. Thus, there is an urgent need for an electroforming material and preparation method that can improve the fatigue resistance of printing screens. Summary of the Invention

[0003] The present invention aims to solve the technical problem of insufficient fatigue resistance of existing electroformed nickel screen printing plates, and provides a fatigue-resistant nickel alloy material for printing screen printing plates and its preparation method.

[0004] This invention provides a method for preparing a fatigue-resistant nickel alloy material for printing screens, comprising the following steps: Using a master mold as the cathode, electroforming is performed in a nickel sulfamate electroforming solution. The nickel sulfamate electroforming solution contains: 200-500 g / L nickel sulfamate, 5-50 g / L nickel chloride, 25-45 g / L boric acid, 1.0-3.0 g / L sodium saccharin, 10-20 g / L cobalt sulfamate, 2.5-3 g / L sodium hypophosphite, 0.1-0.3 g / L nitrogen-doped graphene, and 0.1-0.5 g / L polyethylene glycol. The electroformed nickel alloy layer is completely peeled off from the master mold to obtain a fatigue-resistant nickel alloy material for printing screens.

[0005] The functions of each component in the electroforming solution are as follows.

[0006] Nickel sulfamate is the most commonly used main salt in electroforming nickel, and its core function is to provide Ni²⁺ ions required for deposition during the electroforming process. Nickel chloride's core function is to provide chloride ions, acting as an anodic activator to promote the normal dissolution of the nickel anode and prevent anode passivation. Boric acid's core function is to act as a pH buffer, stabilizing the pH value at the cathode interface during electroforming. Sodium saccharin has both grain refinement and stress relief functions, providing a structural basis for cobalt solid solution strengthening and nanotwin formation by refining the grains.

[0007] Cobalt sulfamate provides Co²⁺, allowing cobalt atoms to dissolve into the nickel FCC lattice via substitution, forming a Ni(Co) solid solution. This lattice distortion effectively hinders dislocation movement and enhances alloy strength. This invention controls the cobalt sulfamate concentration within the range of 10-20 g / L, corresponding to a cobalt content of approximately 7%-15% in the alloy. Its core advantage is the balance between strength and internal stress. This concentration range promotes nanotwin formation through solid solution strengthening and reduced SFE, while avoiding a sharp increase in internal stress caused by excessively high cobalt content, ensuring demolding feasibility and dimensional stability.

[0008] Sodium hypophosphite provides the phosphorus source, and under the induced co-deposition of Ni / Co, phosphorus atoms co-deposit with Ni and Co to form a Ni-Co-P alloy. The electrodeposited plating structure is a supersaturated solid solution of phosphorus in the Ni-Co matrix. Some phosphorus atoms segregate at twin boundaries and stacking faults during electrodeposition, forming solute drag pinning and stabilizing the nanocrystalline structure. The sodium hypophosphite concentration is set at 2.5-3 g / L, matched with the high concentration of cobalt sulfamate, to ensure that the phosphorus supply rate and cobalt deposition rate are synergistic, forming a sufficient amount of Ni3P reinforcing phase.

[0009] The pyridine nitrogen and graphitic nitrogen sites on the surface of nitrogen-doped graphene (NG) exhibit differential anchoring behavior for Ni²⁺ and Co²⁺, lowering the nucleation energy barrier of metal ions and guiding preferential and uniform nucleation of Ni-Co alloys on the NG surface, thus significantly refining the grain size. NG sheets, acting as a two-dimensional reinforcing phase, construct nanoscale physical barriers within the matrix, achieving surface-confined strengthening: confining dislocation motion, deflecting crack propagation, transferring interfacial loads, and inhibiting grain growth.

[0010] Polyethylene glycol (PEG), as a nonionic dispersant, ensures uniform dispersion of NG in the electroforming bath through steric hindrance, preventing lamellar agglomeration. Its nonionic nature makes it unaffected by the pH and electric field of the plating bath, and it exhibits good stability in aminosulfonate systems. The addition of PEG guarantees that the anchoring effect and surface confinement strengthening effect of NG are uniform and consistent throughout the electroforming process.

[0011] The electroforming solution uses deionized water as a solvent, and the components are dissolved sequentially according to the concentrations mentioned above. NG needs to be pre-dispersed with PEG in deionized water using ultrasonication for 30-60 minutes until homogeneous before mixing with the base electroforming solution. After preparation, adjust the pH to 3.8-4.2.

[0012] Furthermore, the electroforming solution has a pH of 3.8-4.2, an electroforming temperature of 40-55 °C, and a current density of 1.0-5.0 A / dm².

[0013] Furthermore, the process after exfoliation includes heat treatment: first, holding at 175-200 °C for 1-4 hours, and then holding at 300-550 °C for 1-2 hours. The first step, holding at 175-200 °C for 1-4 hours, drives phosphorus segregation towards the grain boundaries and NG interface, while simultaneously releasing residual internal stress from electroforming. The second step, holding at 300-550 °C for 1-2 hours, precipitates nanoscale Ni3P deposits, which preferentially nucleate at the NG interface, achieving a synergistic structure of "NG surface confinement + Ni3P point pinning." After heat treatment, the furnace is cooled to room temperature.

[0014] Furthermore, the electroforming solution also includes a wetting agent of 0.1-1 g / L, wherein the wetting agent is at least one of sodium dodecyl sulfate, sodium n-octyl sulfate, and sodium dodecylbenzene sulfonate.

[0015] Furthermore, the electroforming solution also includes 0.5-2 g / L of sodium citrate. The complexation stability of citrate with Co²⁺ is higher than that of Ni²⁺, preferentially "locking in" Co²⁺ and continuously inhibiting the abnormal preferential deposition of cobalt. This makes the cobalt deposition rate of the bottom layer and the main layer more consistent, thereby eliminating the composition gradient, buffering the pH at the cathode interface, and assisting in the dispersion of NG. Ultimately, a casting layer with uniform composition, fine grains, and low internal stress along the thickness direction is obtained.

[0016] Furthermore, the electroforming process is divided into a bottom layer stage and a main layer stage. Sodium citrate is added at the beginning of the main layer stage. The thickness of the nickel alloy layer formed in the bottom layer stage is 1 / 5 to 2 / 5 of the total thickness of the electroformed nickel alloy layer. Bottom layer stage: No sodium citrate or NG is added; DC electroforming is used with a current density of 1.0-2.0 A / dm² and a temperature of 45-55 °C, resulting in a deposition thickness of 1 / 5 to 2 / 5 of the total thickness. This stage yields a high-toughness, low-stress pure Ni-Co bottom layer, ensuring a controllable weak bond with the master mold, facilitating complete peeling. More preferably, the main layer stage uses bidirectional pulse electroforming with a forward current density of 2.5-3.5 A / dm² and a reverse current density of 0.1-0.5 A / dm². The main layer stage uses ultrasonic-assisted electroforming with an ultrasonic power of 40-60 W and a frequency of 40-80 kHz.

[0017] Main layer stage: Sodium citrate (0.5-2 g / L) is added, and bidirectional pulse electroforming is used with a forward current density of 2.5-3.5 A / dm² and a reverse current density of 0.1-0.5 A / dm², at a temperature of 25-35 °C, while ultrasonic assistance is applied (power 40-60 W, frequency 40-80 kHz). The reverse pulse dissolves weakly adsorbed phosphorus atoms and impurities on the cathode surface, promoting phosphorus segregation at twin boundaries and stacking faults; the ultrasonic cavitation effect breaks up NG aggregates, exposing more nitrogen active sites and enhancing the differential anchoring efficiency.

[0018] This invention also provides a fatigue-resistant nickel alloy material for printing screens prepared by the above method. This material is a nickel-cobalt-phosphorus alloy, in which nitrogen-doped graphene is uniformly dispersed, with its sheets acting as a two-dimensional reinforcing phase to achieve planar confinement strengthening; phosphorus segregates at grain boundaries, generating a Zener pinning effect; and high-density nanotwins and stacking faults are also present. The synergistic effect of the "planar confinement" of nitrogen-doped graphene and the "point pinning" of Ni3P effectively suppresses grain growth and crack propagation under cyclic loading, significantly improving fatigue resistance and making it suitable for long-life printing screens.

[0019] The present invention has the following beneficial effects: A multi-level fatigue resistance system consisting of "solid solution strengthening—interface anchoring—grain boundary pinning" was constructed using cobalt sulfamate (10-20 g / L), sodium hypophosphite (2.5-3 g / L), and nitrogen-doped graphene (0.1-0.3 g / L) / PEG (0.1-0.5 g / L). Specifically, cobalt atoms replace Ni lattice to form a stable face-centered cubic Ni(Co) solid solution. The cobalt content is controlled at 10-20 g / L, which promotes nanotwin formation through solid solution strengthening and reduction of stacking fault energy, while avoiding excessive cobalt content that would lead to a sharp increase in internal stress, thus ensuring demolding feasibility and dimensional stability. The pyridine nitrogen / graphitic nitrogen sites in nitrogen-doped graphene can coordinate and anchor Ni²⁺ and Co²⁺, lowering their nucleation energy barrier and guiding Ni²⁺ and Co²⁺ to preferentially nucleate and grow into Ni-Co grains near the nitrogen-doped graphene sites. Its sheets act as a two-dimensional reinforcing phase, forming numerous parallel physical interfaces in the matrix to confine dislocation movement, deflect crack propagation, transfer interfacial loads, and inhibit grain growth, achieving planar confinement strengthening. Sodium hypophosphite co-deposits under Ni / Co induction, forming a Ni-Co-P supersaturated solid solution. During deposition, some phosphorus atoms segregate at twin boundaries and stacking faults, forming solute segregation pinning. Ultimately, the phosphorus "solute segregation pinning" and the nitrogen-doped graphene "planar confinement" complement each other, jointly inhibiting grain growth and crack propagation under cyclic loading, significantly improving the fatigue resistance of printing screens under cyclic loading.

[0020] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures particularly pointed out in the written description. Detailed Implementation

[0022] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0023] The preparation method of the fatigue-resistant nickel alloy material for printing screens of the present invention will be further described below with reference to embodiments.

[0024] All raw materials used in the following examples are commercially available. Nickel sulfamate can be electroplating grade nickel sulfamate (purity ≥99%), nickel chloride can be analytical grade nickel chloride, boric acid can be analytical grade boric acid, sodium saccharin can be electroplating grade or food grade sodium saccharin, cobalt sulfamate can be electroplating grade cobalt sulfamate, sodium hypophosphite can be analytical grade sodium hypophosphite, nitrogen-doped graphene can be a commercially available research-grade product with a nitrogen content of 2-5 wt% and a sheet diameter of 0.5-5 μm, polyethylene glycol can be chemically pure polyethylene glycol with a number average molecular weight of 2000-6000, sodium dodecyl sulfate can be analytical grade sodium dodecyl sulfate, sodium citrate can be analytical grade sodium citrate, pure nickel plate can be electroplating grade pure nickel anode, and the master mold can be a stainless steel plate or a nickel alloy plate.

[0025] The test criteria for each performance index in the following examples are as follows: tensile strength was determined according to GB / T 228.1-2021 "Metallic materials, tensile testing - Part 1: Test at room temperature"; fatigue limit was determined according to GB / T 3075-2021 "Metallic materials, fatigue testing - Axial force control method", with a cycle base of 10. 7 The stress ratio R = -1 was applied. Output linewidth drift was determined according to IEC 60068-2-14:2009 "Environmental testing - Part 2-14: Test N: Temperature variation" Test Na, cyclically 100 times between 20 and 80 °C, with each cycle lasting 30 minutes. Before and after each cycle, the linewidth and mesh pitch of ≥50 lines at the same coordinate were measured, and the linewidth drift was recorded. Example 1 Three groups were set up to investigate the effects of parameter changes in nitrogen-doped graphene and polyethylene glycol on the preparation method.

[0026] Group 1-1: Nitrogen-doped graphene 0.1 g / L, polyethylene glycol 0.1 g / L.

[0027] Group 1-2: Nitrogen-doped graphene 0.2 g / L, polyethylene glycol 0.3 g / L.

[0028] Groups 1-3: Nitrogen-doped graphene 0.3 g / L, polyethylene glycol 0.5 g / L.

[0029] The remaining parameters are as follows: nickel sulfamate 400 g / L, nickel chloride 25 g / L, boric acid 35 g / L, sodium saccharin 2.0 g / L, cobalt sulfamate 15 g / L, sodium hypophosphite 2.75 g / L, sodium dodecyl sulfate 0.5 g / L; the pH of the electroforming solution is 4.0, the electroforming temperature is 30 °C, and the current density is 3.0 A / dm².

[0030] The test results are shown in the table below. Group Tensile strength (MPa) Fatigue limit (MPa) Linewidth drift (μm) 1-1 720 262 2.0 1-2 780 308 1.2 1-3 750 289 1.5 Table 1 shows that Group 1-2 exhibits the best overall performance. In Group 1-3, the NG concentration is relatively high, leading to a corresponding increase in PEG content. Excessive PEG may introduce organic inclusions, and the NG sheets at high concentrations show a slight tendency to agglomerate, resulting in decreased dispersion uniformity and a slight reduction in performance. Linewidth drift is directly related to grain size and residual stress; the fine-grained structure and low internal stress of Group 1-2 minimize dimensional changes during temperature cycling. Example

[0031] Three groups were set up to investigate the effect of parameter changes on the preparation method of sodium hypophosphite.

[0032] Group 2-1: Sodium hypophosphite 2.5 g / L.

[0033] Group 2-2: Sodium hypophosphite 2.75 g / L.

[0034] Group 2-3: Sodium hypophosphite 3.0 g / L.

[0035] The remaining parameters are as follows: nickel sulfamate 400 g / L, nickel chloride 25 g / L, boric acid 35 g / L, sodium saccharin 2.0 g / L, cobalt sulfamate 15 g / L, nitrogen-doped graphene 0.2 g / L, polyethylene glycol 0.3 g / L, sodium dodecyl sulfate 0.5 g / L; pH of the electroforming solution 4.0, electroforming temperature 30 °C, and current density 3.0 A / dm².

[0036] The test results are shown in the table below.

[0037] Group Tensile strength (MPa) Fatigue limit (MPa) Linewidth drift (μm) 2-1 750 289 1.5 2-2 780 308 1.2 2-3 760 284 1.6 As shown in the table above, group 2-2 exhibits the best performance. At this concentration, the phosphorus supply rate matches the cobalt deposition rate well, resulting in a moderate phosphorus content in the coating. Phosphorus segregation at twin boundaries and stacking faults is sufficient, forming effective solute drag pinning. Group 2-1 has a low phosphorus content (approximately 0.8%), insufficient grain boundary segregation and pinning effect, and a lower fatigue limit. Group 2-3 has a high phosphorus content (approximately 2.5%), and excessive phosphorus may lead to increased coating brittleness, increased internal stress, and increased linewidth drift. Example

[0038] Three groups were set up to investigate the effect of parameter changes of cobalt aminosulfonate on the preparation method.

[0039] Group 3-1: Cobalt aminosulfonate 10 g / L.

[0040] Group 3-2: Cobalt aminosulfonate 15 g / L.

[0041] Group 3-3: Cobalt aminosulfonate 20 g / L.

[0042] The remaining parameters are as follows: nickel aminosulfonate 400 g / L, nickel chloride 25 g / L, boric acid 35 g / L, sodium saccharin 2.0 g / L, sodium hypophosphite 2.75 g / L, nitrogen-doped graphene 0.2 g / L, polyethylene glycol 0.3 g / L, sodium dodecyl sulfate 0.5 g / L; the pH of the electroforming solution is 4.0, the electroforming temperature is 30 °C, and the current density is 3.0 A / dm².

[0043] The test results are shown in the table below.

[0044] Group Tensile strength (MPa) Fatigue limit (MPa) Linewidth drift (μm) 3-1 730 274 1.8 3-2 780 308 1.2 3-3 800 306 1.4 As shown in the table above, group 3-3 exhibits the highest tensile strength, which is consistent with the strengthening effect of increased cobalt content on solid solution strengthening. In the system of this invention, the internal stress of group 3-3 increases with increasing cobalt content, while the linewidth drift slightly recovers (1.4 μm). Group 3-2 (cobalt sulfamate 15 g / L) achieves the best balance between strength and internal stress, with the highest fatigue limit (308 MPa). Group 3-1 has a relatively low cobalt content, resulting in insufficient solid solution strengthening and nanotwin promotion effects, leading to the lowest tensile strength and fatigue limit, and the largest linewidth drift. Example

[0045] Five groups were set up to investigate the effects of nickel aminosulfonate, nickel chloride, boric acid, sodium saccharin, pH, temperature, and current density on the preparation method.

[0046] Five groups were set up to investigate the effects of nickel aminosulfonate, nickel chloride, boric acid, sodium saccharin, pH, temperature, and current density on the preparation method.

[0047] Group 4-1: Nickel sulfamate 200 g / L, nickel chloride 5 g / L, boric acid 25 g / L, sodium saccharin 1.0 g / L, pH 3.8, temperature 40°C, current density 1.0 A / dm².

[0048] Group 4-2: Nickel sulfamate 300 g / L, nickel chloride 15 g / L, boric acid 30 g / L, sodium saccharin 1.5 g / L, pH 3.8, temperature 45 °C, current density 2.0 A / dm².

[0049] Group 4-3: Nickel sulfamate 400 g / L, nickel chloride 25 g / L, boric acid 35 g / L, sodium saccharin 2.0 g / L, pH 4.0, temperature 50 °C, current density 3.0 A / dm².

[0050] Group 4-4: Nickel sulfamate 450 g / L, nickel chloride 35 g / L, boric acid 40 g / L, sodium saccharin 2.5 g / L, pH 4.0, temperature 52 °C, current density 4.0 A / dm².

[0051] Groups 4-5: Nickel sulfamate 500 g / L, nickel chloride 50 g / L, boric acid 45 g / L, sodium saccharin 3.0 g / L, pH 4.2, temperature 55 °C, current density 5.0 A / dm².

[0052] The remaining parameters are: cobalt aminosulfonate 15 g / L, sodium hypophosphite 2.75 g / L, nitrogen-doped graphene 0.2 g / L, polyethylene glycol 0.3 g / L, and sodium dodecyl sulfate 0.5 g / L.

[0053] The test results are shown in the table below.

[0054] Group Tensile strength (MPa) Fatigue limit (MPa) Linewidth drift (μm) 4-1 690 204 2.8 4-2 700 253 1.8 4-3 780 308 1.2 4-4 760 292 1.5 4-5 710 267 2.2 As shown in the table above, Group 4-3 exhibits the best overall performance. Group 4-1 uses low values ​​for all parameters; the low nickel sulfamate concentration leads to insufficient deposition rate and a loose casting layer. The boric acid buffering capacity is weak, and the low current density results in coarse grains, leading to relatively poor tensile strength and linewidth drift. Group 4-5 uses high values ​​for all parameters; the high nickel sulfamate concentration is beneficial for deposition efficiency, but excessively high current density and temperature increase internal stress. Simultaneously, excessively high nickel chloride concentration may accelerate anodic dissolution, producing sludge inclusions. Although tensile strength decreases, the linewidth drift recovers to 2.2 μm. Example

[0055] Six groups were set up to investigate the effects of changes in sodium citrate concentration, bidirectional pulse current density, ultrasonic power, and frequency on the preparation method.

[0056] Group 5-1: Sodium citrate 0.5 g / L.

[0057] Group 5-2: Sodium citrate 2.0 g / L.

[0058] Group 5-3: Sodium citrate 1.0 g / L, bidirectional pulse forward current density 2.5 A / dm², reverse current density 0.1 A / dm².

[0059] Group 5-4: Sodium citrate 1.0 g / L, bidirectional pulse forward current density 3.5 A / dm², reverse current density 0.5 A / dm².

[0060] Group 5-5: Sodium citrate 1.0 g / L, ultrasonic power 40 W, frequency 40 kHz.

[0061] Groups 5-6: Sodium citrate 1.0 g / L, ultrasonic power 60 W, frequency 80 kHz.

[0062] The remaining parameters are as follows: nickel sulfamate 400 g / L, nickel chloride 25 g / L, boric acid 35 g / L, sodium saccharin 2.0 g / L, cobalt sulfamate 15 g / L, sodium hypophosphite 2.75 g / L, nitrogen-doped graphene 0.2 g / L, polyethylene glycol 0.3 g / L, sodium dodecyl sulfate 0.5 g / L; the pH of the electroforming solution is 4.0, the electroforming temperature is 30 °C, and the current density is 3.0 A / dm².

[0063] The test results are shown in the table below.

[0064] Group Tensile strength (MPa) Fatigue limit (MPa) Linewidth drift (μm) 5-1 750 289 1.5 5-2 760 292 1.8 5-3 740 277 1.6 5-4 770 296 1.4 5-5 745 287 1.7 5-6 785 310 1.1 As shown in the table above, group 5-6 exhibits the best overall performance. Under these parameters, the reverse pulse effectively dissolves weakly adsorbed phosphorus atoms and impurities on the cathode surface, promoting phosphorus segregation at twin boundaries and stacking faults. The high-power, high-frequency ultrasonic cavitation effect thoroughly breaks down NG aggregates, exposing more pyridine nitrogen / graphite nitrogen active sites, resulting in the finest grains. Therefore, tensile strength, fatigue limit, and linewidth drift are all optimal. Group 5-4 shows the second best performance; higher current density is beneficial for deposition efficiency and grain refinement, but excessively high reverse current may cause slight damage to the deposited layer. Group 5-2 indicates that while excessive sodium citrate can more effectively suppress abnormal cobalt deposition, excessive complexation may reduce the deposition rate and affect NG anchoring efficiency. Group 5-3 has a low current density, slow deposition rate, and insufficient grain refinement effect, resulting in relatively low performance. Group 5-5 has low ultrasonic power and frequency, limiting NG dispersion effect, and its performance is lower than group 5-6.

[0065] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for preparing a fatigue-resistant nickel alloy material for printing screens, characterized in that, Includes the following steps: Using a master mold as the cathode, electroforming is performed in a nickel sulfamate electroforming solution. The nickel sulfamate electroforming solution contains 200-500 g / L nickel sulfamate, 5-50 g / L nickel chloride, 25-45 g / L boric acid, 1.0-3.0 g / L sodium saccharin, 10-20 g / L cobalt sulfamate, 2.5-3 g / L sodium hypophosphite, 0.1-0.3 g / L nitrogen-doped graphene, and 0.1-0.5 g / L polyethylene glycol. The electroformed nickel alloy layer is completely peeled off from the master mold to obtain a fatigue-resistant nickel alloy material for printing screens.

2. The preparation method according to claim 1, characterized in that, The electroforming solution has a pH of 3.8-4.2, an electroforming temperature of 40-55 °C, and a current density of 1.0-5.0 A / dm².

3. The preparation method according to claim 1, characterized in that, The stripping process also includes heat treatment: first, heat treatment at 175-200°C for 1-4 hours, and then heat treatment at 300-550°C for 1-2 hours.

4. The preparation method according to claim 1, characterized in that, The nickel aminosulfonate electroforming solution also includes a wetting agent of 0.1-1 g / L.

5. The preparation method according to claim 4, characterized in that, The wetting agent is at least one of sodium dodecyl sulfate, sodium n-octyl sulfate, and sodium dodecylbenzene sulfonate.

6. The preparation method according to claim 1, characterized in that, The nickel aminosulfonate electroforming solution also includes 0.5-2 g / L of sodium citrate.

7. The preparation method according to claim 6, characterized in that, The electroforming process is divided into a bottom layer stage and a main layer stage. Sodium citrate is added at the beginning of the main layer stage. The thickness of the nickel alloy layer formed in the bottom layer stage is 1 / 5 to 2 / 5 of the thickness of the nickel alloy layer formed by electroforming.

8. The preparation method according to claim 7, characterized in that, The main layer stage employs bidirectional pulse electroforming with a forward current density of 2.5-3.5 A / dm² and a reverse current density of 0.1-0.5 A / dm².

9. The preparation method according to claim 7, characterized in that, The main layer stage employs ultrasonic-assisted electroforming with an ultrasonic power of 40-60 W and a frequency of 40-80 kHz.

10. A fatigue-resistant nickel alloy material for printing screens, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 10.