A method for preparing extinction monofilaments

By preparing core-shell structured matte monofilaments, and utilizing the melt blending of porous silica microspheres with a thermoplastic elastomer matrix and multi-stage stretching treatment, the problems of strong plastic feel and lack of matte appearance of the monofilaments were solved, achieving a soft matte effect and high strength and toughness.

CN123108775APending Publication Date: 2026-11-17FUJIAN JINJIANG HUAYU WEAVING
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611482319.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing monofilaments have a strong plastic feel and lack a matte finish when made into fabrics, thus lacking matte characteristics.

Method used

Surface-modified porous silica matte microspheres were melt-blended with a thermoplastic elastomer matrix to prepare core-shell structured monofilaments. Through multi-stage stretching and heat setting treatment, a uniform scattering network was formed to achieve a soft matte effect.

Benefits of technology

It achieves a soft matte finish on the monofilament, avoids spinneret clogging, ensures spinning continuity, and improves fiber toughness and strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of fiber processing technology and provides a method for preparing matte monofilaments, which solves the defects of existing monofilaments that have a strong plastic feel and lack a matte appearance when made into fabric. The method includes the following steps: S1. Preparing matte masterbatch; S2. Drying raw materials; S3. Core-sheath composite spinning; S4. Cooling and stretching; S5. Heat setting and oiling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fiber processing technology, and in particular to a method for preparing matte monofilaments. Background Technology

[0002] Chinese Patent No. 201610561819.4 discloses a multi-purpose core-sheath composite monofilament, its production method, and its applications. The monofilament consists of a sheath and a core layer, with the sheath covering the outside of the core layer. The core layer is composed of polypropylene (PP), polyurethane elastic composite material (TPU), or polyester elastic composite material (TPEE), while the sheath layer is composed of polyethylene (PE), rubber-plastic elastic composite material (POE), polyurethane elastic composite material (TPU), or polyester elastic composite material (TPEE). The melting point of the sheath layer is 120-170 degrees Celsius, and the melting point of the core layer is 150-210 degrees Celsius. The sheath component accounts for 30-70% of the total composition, and the core layer component accounts for 70-30%. It can be used in the substrates of woven mesh, window screens, curtains, sunshades, light-diffusing cloth, mosquito nets, anti-smog mesh, filter cloth, shoe material mesh, and power transmission belts. Since its core structure is made of ordinary material and has not undergone modification treatment, it does not have matting characteristics. The monofilament of this material has good permeability but also a strong plastic feel, and its appearance quality is relatively ordinary. Summary of the Invention

[0003] Therefore, in view of the above problems, the present invention provides a method for preparing matte monofilament, which solves the defects of existing monofilaments that have a strong plastic feel and do not have a matte appearance when made into fabric.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: a method for preparing extinction monofilaments, comprising the following steps: S1. Preparation of matting masterbatch: Surface-modified porous silica matting microspheres are melt-blended and granulated with a thermoplastic elastomer matrix in a twin-screw extruder to obtain matting masterbatch with a matting microsphere weight ratio of 10-15 wt%; the average particle size D of the matting microspheres is... 50 The micrometer diameter is 0.4~3.0 μm, the porosity is 45~72%, and the surface is modified by silane coupling agent or C12~C22 fatty acid ester grafting. S2. Raw material drying: The core material and the matting masterbatch obtained in step S1 are vacuum dried separately to control the moisture content to be below 100 ppm; S3. Core-Sheath Composite Spinning: A core-sheath composite spinneret is used, in which the core material and sheath material are independently metered and fed into the spinneret, and are combined in a molten state to form a core-sheath structure filament; wherein, the sheath material is a mixture of the matte masterbatch and the thermoplastic elastomer matrix in a weight ratio of 5-15:85-95; the core material is a thermoplastic elastomer matrix; the weight ratio of the core material to the sheath material is 65-80:20-35; S4. Cooling and stretching: The extruded core-sheath structure filaments are cooled by side blowing and then subjected to multi-stage stretching, with a total stretching ratio of 2 to 5.0 times; S5. Heat setting and oiling: The stretched core-sheath structure filaments are relaxed and heat-set at 155~175℃, and then oiled and wound to obtain the matte thermoplastic elastomer monofilament.

[0005] Furthermore, the thermoplastic elastomer matrix is ​​TPEE or TPU.

[0006] Furthermore: when the thermoplastic elastomer matrix is ​​TPEE, its hard segment content is 30-55wt%, and the melt temperature of the core-sheath composite spinning in step S3 is 235~255℃.

[0007] Furthermore: when the thermoplastic elastomer matrix is ​​TPU, its hardness is 95A-50D, and the melt temperature of the core-sheath composite spinning in step S3 is 185~215℃.

[0008] Furthermore: the multi-stage stretching in step S4 includes primary stretching and secondary stretching; the primary stretching ratio is 2.2 to 2.8 times, and the stretching temperature is 110 to 130°C; the secondary stretching ratio is 1.3 to 1.8 times, and the stretching temperature is 145 to 165°C.

[0009] Furthermore: the vacuum drying temperature in step S2 is 80~110℃, the vacuum degree is ≤-0.08 MPa, and the drying time is 6~12 h.

[0010] Furthermore: the side-blowing cooling air temperature in step S4 is 18~28℃, and the air speed is 0.3~0.8 m / s.

[0011] Furthermore, the relaxation heat setting time described in step S5 is 30~120 s.

[0012] Furthermore, the concentration of the oiling agent is 5-15 wt%, and the oiling rate is 0.5-1.5%.

[0013] By adopting the aforementioned technical solution, the beneficial effects of the present invention are as follows: 1. This application uses surface-modified porous silica microspheres as a matting stop, combined with silane or fatty acid ester grafting treatment, which solves the defect of traditional matting agents being prone to agglomeration in melt spinning. The porous structure of the microspheres produces a soft matte effect through interfacial refraction. At the same time, the micron-sized structure avoids the clogging of the spinneret orifice and ensures the continuity of spinning.

[0014] 2. The matte monofilament of this application has a core-sheath structure. The core material is a thermoplastic elastomer matrix, which can provide high strength to the fiber. The sheath material is a mixture of matte masterbatch and thermoplastic elastomer matrix. The weight ratio of matte microspheres in the matte masterbatch in the sheath material is 10~15 wt%. The low concentration of matte microspheres gives the fiber a matte texture and good toughness. In addition, the core-sheath ratio is 65-80:20-35, which can avoid the whitening caused by bending due to excessively thick sheath and the insufficient matteness caused by excessively thin sheath.

[0015] 3. The stretching process employs multi-stage stretching, which induces the extinction microspheres to arrange themselves in an orderly manner along the axial direction in the cortex, forming a uniform scattering network. Furthermore, the use of two-stage gradient temperature stretching allows for gradient control of the crystallinity of the fiber filaments, preventing internal stress cracking. Detailed Implementation Example 1

[0016] A method for preparing an extinction monofilament includes the following steps: S1. Preparation of matting masterbatch: Surface-modified porous silica matting microspheres are melt-blended and granulated with a thermoplastic elastomer matrix in a twin-screw extruder to obtain a matting masterbatch with a matting microsphere weight ratio of 10 wt%; the average particle size D of the matting microspheres is... 50 The micrometer diameter is 0.4 μm, the porosity is 45%, and the surface is modified by silane coupling agent grafting; the above thermoplastic elastomer matrix is ​​TPEE, and its hard segment content is 3 wt%. S2. Raw material drying: The core layer material and the matting masterbatch obtained in step S1 are vacuum dried separately to control the moisture content to be below 100 ppm; the vacuum drying temperature is 80℃, the vacuum degree is -0.08 MPa, and the drying time is 6 h; S3. Core-Sheath Composite Spinning: A core-sheath composite spinneret is used, in which the core material and sheath material are independently metered and fed into the spinneret, and are combined in a molten state to form a core-sheath structure filament; wherein, the sheath material is a mixture of the matte masterbatch and the thermoplastic elastomer matrix in a weight ratio of 5:95; the core material is a thermoplastic elastomer matrix; the weight ratio of the core material to the sheath material is 65:35; the melt temperature of the core-sheath composite spinning is 235℃; S4. Cooling and Stretching: The extruded core-sheath structure filaments are cooled by side-blowing air and then subjected to multi-stage stretching with a total stretching ratio of 2. The side-blowing air temperature is 18℃ and the air velocity is 0.3 m / s. The multi-stage stretching includes primary stretching and secondary stretching. The primary stretching ratio is 2.2 times and the stretching temperature is 110℃. The secondary stretching ratio is 1.3 times and the stretching temperature is 145℃. S5. Heat setting and oiling: The stretched core-sheath structure filament is subjected to relaxation heat setting at 155°C for 30 seconds, followed by oiling and winding. The concentration of the oiling agent is 5 wt%, and the oiling rate is 0.5%, thus obtaining the matte thermoplastic elastomer monofilament. Example 2

[0017] A method for preparing an extinction monofilament includes the following steps: S1. Preparation of matting masterbatch: Surface-modified porous silica matting microspheres are melt-blended and granulated with a thermoplastic elastomer matrix in a twin-screw extruder to obtain a matting masterbatch with a matting microsphere weight ratio of 12 wt%; the average particle size D of the matting microspheres is... 50 The micrometer diameter is 1.5 μm, the porosity is 55%, and the surface is modified by grafting C12 fatty acid esters; the thermoplastic elastomer matrix is ​​TPU with a hardness of 95A. S2. Raw material drying: The core layer material and the matting masterbatch obtained in step S1 are vacuum dried separately to control the moisture content to be below 100 ppm; the vacuum drying temperature is 95℃, the vacuum degree is -0.1 MPa, and the drying time is 9h. S3. Core-Sheath Composite Spinning: A core-sheath composite spinneret is used, in which the core material and sheath material are independently metered and fed into the spinneret, and are combined in a molten state to form a core-sheath structure filament; wherein, the sheath material is a mixture of the matte masterbatch and the thermoplastic elastomer matrix in a weight ratio of 10:90; the core material is a thermoplastic elastomer matrix; the weight ratio of the core material to the sheath material is 72:28; the melt temperature of the core-sheath composite spinning is 200℃; S4. Cooling and Stretching: The extruded core-sheath structure filaments are cooled by side-blowing air and then subjected to multi-stage stretching with a total stretching ratio of 4 times. The multi-stage stretching includes primary stretching and secondary stretching. The primary stretching ratio is 2.5 times and the stretching temperature is 120℃. The secondary stretching ratio is 1.5 times and the stretching temperature is 155℃. The side-blowing air temperature is 23℃ and the air velocity is 0.5m / s. S5. Heat setting and oiling: The stretched core-sheath structure filament is subjected to relaxation heat setting at 165°C for 75 seconds, followed by oiling and winding. The oil concentration is 10 wt%, and the oiling rate is 1%. The matte thermoplastic elastomer monofilament is thus obtained. Example 3

[0018] A method for preparing an extinction monofilament includes the following steps: S1. Preparation of matting masterbatch: Surface-modified porous silica matting microspheres are melt-blended and granulated with a thermoplastic elastomer matrix in a twin-screw extruder to obtain a matting masterbatch with a matting microsphere weight ratio of 15 wt%; the average particle size D of the matting microspheres is... 50 The micrometer diameter is 3.0 μm, the porosity is 72%, and the surface is modified by grafting C22 fatty acid esters; the thermoplastic elastomer matrix is ​​TPU with a hardness of 50D. S2. Raw material drying: The core layer material and the matting masterbatch obtained in step S1 are vacuum dried separately to control the moisture content to be below 100 ppm; the vacuum drying temperature is 110℃, the vacuum degree is -0.09 MPa, and the drying time is 12 h; S3. Core-Sheath Composite Spinning: A core-sheath composite spinneret is used, in which the core material and sheath material are independently metered and fed into the spinneret, and are combined in a molten state to form a core-sheath structure filament; wherein, the sheath material is a mixture of the matte masterbatch and the thermoplastic elastomer matrix in a weight ratio of 5:85; the core material is a thermoplastic elastomer matrix; the weight ratio of the core material to the sheath material is 80:20; the melt temperature of the core-sheath composite spinning is 215℃; S4. Cooling and Stretching: The extruded core-sheath structure filaments are cooled by side-blowing air and then subjected to multi-stage stretching with a total stretching ratio of 5.0 times. The multi-stage stretching includes primary stretching and secondary stretching. The primary stretching ratio is 2.8 times and the stretching temperature is 130℃. The secondary stretching ratio is 1.8 times and the stretching temperature is 165℃. The side-blowing air temperature is 28℃ and the air velocity is 0.8 m / s. S5. Heat setting and oiling: The stretched core-sheath structure filament is subjected to relaxation heat setting at 175°C for 120 seconds, followed by oiling and winding. The concentration of the oiling agent is 15 wt%, and the oiling rate is 1.5%, thus obtaining the matte thermoplastic elastomer monofilament.

[0019] The properties of the extinction monofilaments obtained in Examples 1 to 3 of this application were tested, and the results are shown in the table below: Testing items Example 1 Example 2 Example 3 Elongation at break (%) 26 22 17 Light transmittance (%, 400-700nm) can be measured. 28 22 16 60º Specular Gloss (GU) 19 17 15 Although the invention has been specifically shown and described in conjunction with preferred embodiments, those skilled in the art should understand that various changes in form and detail may be made to the invention without departing from the spirit and scope of the invention as defined in the appended claims, all of which shall be within the scope of protection of the invention.

Claims

1. A method for preparing an extinction monofilament, characterized in that, Includes the following steps: S1. Prepare matting masterbatch: melt blend and granulate surface-modified porous silica matting microspheres and a thermoplastic elastomer matrix in a twin-screw extruder to obtain a matting masterbatch with a matting microsphere weight percentage of 10-15 wt%; the average particle size D 50 of the matting microspheres is 0.4-3.0 μm, the porosity is 45-72%, and the surface is modified by grafting with a silane coupling agent or a C12-C22 fatty acid ester; S2. Raw material drying: The core material and the matting masterbatch obtained in step S1 are vacuum dried separately to control the moisture content to be below 100 ppm; S3. Core-Sheath Composite Spinning: A core-sheath composite spinneret is used, in which the core material and sheath material are independently metered and fed into the spinneret, and are combined in a molten state to form a core-sheath structure filament; wherein, the sheath material is a mixture of the matte masterbatch and the thermoplastic elastomer matrix in a weight ratio of 5-15:85-95; the core material is a thermoplastic elastomer matrix; the weight ratio of the core material to the sheath material is 65-80:20-35; S4. Cooling and stretching: The extruded core-sheath structure filaments are cooled by side blowing and then subjected to multi-stage stretching, with a total stretching ratio of 2 to 5.0 times; S5. Heat setting and oiling: The stretched core-sheath structure filaments are relaxed and heat-set at 155~175℃, and then oiled and wound to obtain the matte thermoplastic elastomer monofilament.

2. The method for preparing an extinction monofilament according to claim 1, characterized in that: The thermoplastic elastomer matrix is ​​TPEE or TPU.

3. The method for preparing an extinction monofilament according to claim 2, characterized in that: When the thermoplastic elastomer matrix is ​​TPEE, its hard segment content is 30-55wt%, and the melt temperature of the core-sheath composite spinning in step S3 is 235~255℃.

4. The method for preparing an extinction monofilament according to claim 2, characterized in that: When the thermoplastic elastomer matrix is ​​TPU, its hardness is 95A-50D, and the melt temperature of the core-sheath composite spinning in step S3 is 185~215℃.

5. The method for preparing an extinction monofilament according to claim 3, characterized in that: The multi-stage stretching in step S4 includes primary stretching and secondary stretching; the primary stretching ratio is 2.2 to 2.8 times, and the stretching temperature is 110 to 130°C; the secondary stretching ratio is 1.3 to 1.8 times, and the stretching temperature is 145 to 165°C.

6. The method for preparing an extinction monofilament according to claim 1, characterized in that: The vacuum drying temperature in step S2 is 80~110℃, the vacuum degree is ≤-0.08 MPa, and the drying time is 6~12 h.

7. The method for preparing an extinction monofilament according to claim 1, characterized in that: The side-blowing cooling air temperature in step S4 is 18~28℃, and the air speed is 0.3~0.8 m / s.

8. The method for preparing an extinction monofilament according to claim 1, characterized in that: The relaxation heat setting time in step S5 is 30~120 s.

9. The method for preparing an extinction monofilament according to claim 1, characterized in that: The concentration of the oiling agent is 5-15 wt%, and the oiling rate is 0.5-1.5%.

Citation Information

Patent Citations

  • Multi-purpose sheath-core composite monofilament as well as production method and application thereof

    CN106048777A