A multifunctional marine recycled polyester ultrafine filament and its preparation method

By using core-shell functional particles and calcined magnesium-aluminum composite metal oxides, the problem of fiber strength decline during the antibacterial, UV aging resistance and coloring process of marine recycled polyester microfiber filaments has been solved. This has achieved high-efficiency compatibility between functional components and polyester, reduced the breakage rate and diameter dispersion, and is suitable for automotive interior and outdoor textiles.

CN123108780APending Publication Date: 2026-11-17CHANGZHOU XINZHANJIANG SPECIAL FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611631003.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing marine recycled polyester microfilaments suffer from problems such as residual chemical reagents, decreased fiber strength, high filament breakage rate, low automation, and poor compatibility between functional components and polyester. In particular, the unstable intrinsic viscosity of marine recycled PET bottle flakes and the impact of residual chloride ions on melt processing stability are particularly problematic.

Method used

By mixing core-shell functional particles and calcined magnesium-aluminum composite metal oxides with a polyester matrix, and isolating the zinc oxide core and polyester chain through a mesoporous rutile phase titanium dioxide shell, combined with an integrated functional masterbatch preparation method, antibacterial, UV aging resistant and coloring functions can be achieved simultaneously.

Benefits of technology

It effectively reduces the catalytic degradation of polyester by zinc oxide, maintains fiber strength, reduces fiber breakage rate and diameter dispersion, and avoids the discharge of dyeing wastewater, thus meeting the application requirements of automotive interior and outdoor textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108780A_ABST
    Figure CN123108780A_ABST
Patent Text Reader

Abstract

This invention discloses a multifunctional marine recycled polyester ultrafine filament and its preparation method. The raw materials for this ultrafine filament include a polyester matrix, core-shell functional particles, calcined magnesium-aluminum composite metal oxide, coloring masterbatch, and a dispersant. The polyester matrix is ​​composed of marine recycled polyethylene terephthalate (PET) flakes and virgin PET flakes. The core-shell functional particles consist of a zinc oxide core and a mesoporous rutile titanium dioxide shell coating the zinc oxide core. The calcined magnesium-aluminum composite metal oxide is obtained by calcining a layered bimetallic hydroxide precursor. This invention significantly reduces the direct contact between the zinc oxide core and the recycled polyester molecular chains through the spatial confinement effect of the mesoporous shell, and adsorbs and fixes residual chlorine-containing species from the marine recycled material through the calcined magnesium-aluminum composite metal oxide, thereby endowing the filament with antibacterial, UV-resistant, and solution-dyed properties while maintaining the fiber's mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of recycled textile new materials and functional chemical fiber preparation technology, specifically relating to a multifunctional marine recycled polyester ultrafine filament and its preparation method. Background Technology

[0002] Marine plastic pollution is a major challenge in global ecological and environmental governance. PET flakes, obtained from the recycling and crushing of waste polyethylene terephthalate (PET) bottles from the ocean, are high-quality recycled fiber raw materials that can replace virgin petroleum-based PET in the production of polyester fibers. However, marine-recycled PET flakes differ significantly from land-based recycled flakes in three key aspects: First, prolonged contact with seawater allows sodium, magnesium, calcium, and chloride ions to penetrate the flake surface and remain in microcracks and degradation layers. The moisture, salinity, and trace metal ions in the seawater environment promote hydrolysis and aging of the PET surface, leading to a decrease in molecular weight and an increase in end-carboxyl group content. Second, the surface is contaminated with oil, salt, and marine biological residue, resulting in significant fluctuations in the raw material's moisture content. Third, the batch-to-batch intrinsic viscosity exhibits large dispersion, leading to poor raw material performance stability. These characteristics make marine-recycled PET flakes extremely sensitive to any additional degradation during subsequent processing.

[0003] Existing marine recycled polyester production technologies have the following shortcomings: First, the pretreatment process often uses alkaline or surfactant chemical cleaning, which leaves chemical reagent residues after impurity removal, and high-temperature alkaline washing will further aggravate the degradation of PET molecular chains; simple physical cleaning has the problems of incomplete impurity removal and salt and chloride ion residues. Existing physical cleaning processes do not set control indicators for the extractable chloride ion content of bottle flakes.

[0004] Second, existing dyeing methods for recycled fibers mostly employ post-treatment high-temperature and high-pressure dyeing, resulting in large wastewater discharge and low color fastness. While the solution of using masterbatch dosing for dyeing can avoid dyeing wastewater, the dispersion and synergy of multi-component functional powders and pigments in polyester melt still need to be improved.

[0005] Third, when imparting antibacterial and UV-resistant properties to fibers, inorganic functional powders such as nano-zinc oxide and nano-titanium dioxide are commonly added directly to the polyester melt, or introduced through chemical grafting or post-treatment impregnation. However, nano-zinc oxide has catalytic activity on the alcoholysis and thermal degradation of polyester, and the addition of nano-titanium dioxide reduces the molecular weight and strength of the polyester. Furthermore, the photogenerated carriers generated by anatase titanium dioxide under UV irradiation oxidize the polyester matrix, leading to fiber yellowing and strength reduction. Chemical grafting, on the other hand, damages the fiber molecular chains. Therefore, existing technologies often sacrifice mechanical properties while imparting antibacterial and UV-resistant properties to recycled polyester.

[0006] Fourth, existing solutions have not identified or controlled the residual chloride ions unique to marine recycled materials. These residual chloride ions and other chloride-containing impurities may exacerbate zinc migration and reduce the stability of polyester melt during the melt processing.

[0007] Fifth, the existing recycled fiber production lines lack sufficient automation, process parameters cannot be adaptively adjusted in real time, and the breakage rate and diameter dispersion of ultra-fine denier filaments are too high.

[0008] In summary, there is a lack in the field of technology for preparing recycled polyester microfilaments that can simultaneously achieve antibacterial, UV aging resistance, and solution dyeing functions while maintaining the molecular weight and mechanical properties of recycled polyester fibers, and can adapt to the high degradation sensitivity of marine recycled materials. Summary of the Invention

[0009] The purpose of this invention is to provide a multifunctional marine recycled polyester ultrafine filament and its preparation method, in order to solve the problems of melt degradation, fiber strength reduction and filament breakage rate caused by residual chloride ions and degradation sensitivity of marine recycled PET bottle flakes when introducing antibacterial and UV aging resistant functional components. At the same time, it can achieve solution coloring and avoid post-dyeing wastewater.

[0010] To achieve the above objectives, the technical solution adopted by the present invention is: a multifunctional marine recycled polyester ultrafine filament, wherein the raw materials of the ultrafine filament include polyester matrix, core-shell functional particles, calcined magnesium-aluminum composite metal oxide, coloring masterbatch and dispersant; Based on 100 parts by weight of the polyester matrix, the polyester matrix is ​​composed of 70-90 parts by weight of marine recycled polyethylene terephthalate bottle flakes and 10-30 parts by weight of virgin polyethylene terephthalate chips. In addition to the polyester matrix, it also includes the following components: 0.8-3.0 parts by weight of core-shell functional particles, 0.3-1.5 parts by weight of calcined magnesium-aluminum composite metal oxide, 1.5-4.0 parts by weight of coloring masterbatch, and 0.1-0.5 parts by weight of dispersant. The core-shell functional particle is composed of a zinc oxide core and a mesoporous rutile phase titanium dioxide shell covering the zinc oxide core. The calcined magnesium-aluminum composite metal oxide has the composition shown in general formula (I): Mg 1-x Al x O 1+x / 2 In general formula (I), x is selected from 0.20 to 0.33.

[0011] In general formula (I), x corresponds one-to-one with the Mg:Al molar ratio of the calcined precursor, i.e., Mg:Al = (1-x):x; x = 0.20, 0.25, and 0.33 correspond to Mg:Al molar ratios of 4:1, 3:1, and 2:1, respectively.

[0012] Furthermore, in the core-shell functional particles, the average particle size of the zinc oxide core is 20-80 nm, the thickness of the mesoporous rutile phase titanium dioxide shell is 5-25 nm, and the mass fraction of rutile phase in the mesoporous rutile phase titanium dioxide shell is not less than 90%.

[0013] Furthermore, the mesoporous rutile titanium dioxide shell has a mesopore size of 2–5 nm and a pore volume of 0.10–0.40 cm³. 3 / g, the BET specific surface area of ​​the core-shell functional particles is 60-200 m² / g. 2 / g.

[0014] Furthermore, the core-shell functional particles are 1.0 to 2.5 parts by mass, the calcined magnesium-aluminum composite metal oxide is 0.5 to 1.2 parts by mass, the coloring masterbatch is 2.0 to 3.5 parts by mass, and the dispersant is 0.2 to 0.4 parts by mass.

[0015] Furthermore, the core-shell functional particles are prepared by a method comprising the following steps: A1. Disperse zinc oxide powder with an average particle size of 20-80 nm in a mixed solvent of ethanol and water to obtain a zinc oxide core suspension. A2. Add rutile titanium dioxide seed crystals to the zinc oxide core suspension, then prepare a solution by mixing tetrabutyl titanate and ethanol at a mass ratio of 1:1 to 1:3, and add the solution dropwise at a uniform rate over 2 to 8 hours. Simultaneously, add a template agent, and react at 40 to 70°C with pH adjusted to 6.5 to 7.5 using 0.1 mol / L nitric acid or 0.1 mol / L sodium hydroxide solution to obtain zinc oxide composite particles coated with titanium dioxide precursor. The amount of rutile titanium dioxide seed crystals is 2% to 8% of the mass of the zinc oxide powder, the molar ratio of titanium in the tetrabutyl titanate to zinc in the zinc oxide powder is 0.15 to 0.60:1, the molar ratio of water in the mixed solvent to titanium in the tetrabutyl titanate is 4 to 12:1, and the amount of template agent is 5% to 15% of the mass of the tetrabutyl titanate. A3. Place the zinc oxide composite particles obtained in step A2 into a hydrothermal reactor and hydrothermally treat them at 120-180℃ for 4-24 hours to obtain the hydrothermal product. A4. Remove the template agent from the hydrothermal products, and obtain the core-shell functional particles by washing, solid-liquid separation, drying and pulverizing.

[0016] Furthermore, the calcined magnesium-aluminum composite metal oxide is obtained by calcining the precursor represented by general formula (II): [Mg 1-x Al x [(OH)2](CO3) x / 2·mH2O, in general formula (II), x is selected from 0.20 to 0.33, and m is 0 to 4; the calcination temperature is 450 to 600℃, and the time is 2 to 6 hours; the saturated adsorption capacity of the calcined magnesium-aluminum composite metal oxide for chloride ions is not less than 120 mg / g, and the BET specific surface area is not less than 120 m². 2 / g, the moisture content before use should not exceed 0.3%.

[0017] A method for preparing a multifunctional marine recycled polyester ultrafine filament includes the following steps: S1. Marine recycled polyethylene terephthalate bottle flakes are sequentially subjected to near-infrared spectroscopy sorting, high-pressure spraying and ultrasonic vibration combined cleaning, and hot air drying to obtain pretreated bottle flakes. S2. The precursor shown in general formula (II) is calcined at 450-600℃ for 2-6 hours to obtain the calcined magnesium-aluminum composite metal oxide, where x in general formula (II) is selected from 0.20-0.33 and m is 0-4; S3. Disperse zinc oxide powder with an average particle size of 20-80 nm in a mixed solvent of ethanol and water, add rutile titanium dioxide seed crystals, prepare a solution by mixing tetrabutyl titanate and ethanol at a mass ratio of 1:1 to 1:3, add a template agent at a uniform rate of 5% to 15% of the mass of tetrabutyl titanate over 2-8 hours, react at 40-70 °C with pH adjusted to 6.5-7.5 using 0.1 mol / L nitric acid or 0.1 mol / L sodium hydroxide solution, and then hydrothermally treat at 120-180 °C for 4-24 hours. After removing the template agent, pulverize to obtain the core-shell functional particles. S4. The core-shell functional particles, the calcined magnesium-aluminum composite metal oxide, the coloring masterbatch and the dispersant are mixed with the first part of the recycled polyethylene terephthalate powder obtained by crushing the first part of the pretreated bottle flakes and then melt-extruded and granulated to obtain an integrated functional masterbatch. S5. The integrated functional masterbatch, the second part of pretreated bottle flakes, and virgin polyethylene terephthalate chips are mixed to obtain a mixture with an intrinsic viscosity of 0.58-0.65 dL / g, which is then melt-spun to obtain nascent fibers; the ratio of the sum of the mass of the first part of pretreated bottle flakes and the second part of pretreated bottle flakes to the mass of the virgin polyethylene terephthalate chips is 70-90:10-30; S6. The nascent fibers are stretched and heat-set to obtain the multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 5-10 μm.

[0018] Further, in step S1, the wavelength of the near-infrared spectral sorting is 1100–1300 nm, and the sorting speed is 1.5–2.5 m / min; the pressure of the high-pressure spray is 0.3–0.8 MPa; the power of the ultrasonic oscillation is 300–800 W, the frequency is 20–40 kHz, and the time is 10–20 min; the temperature of the hot air drying is 100–120 °C, and the drying is carried out until the moisture content of the pretreated bottle flakes is not higher than 0.05%; the extractable chloride ion content of the pretreated bottle flakes is not higher than 50 mg / kg.

[0019] Furthermore, in step S3, the amount of rutile phase titanium dioxide seed crystals is 2% to 8% of the mass of zinc oxide powder, and the molar ratio of titanium in tetrabutyl titanate to zinc in zinc oxide powder is 0.15 to 0.60:1. In step S4, the temperature of the melt extrusion granulation is 240–270°C, and the first portion of recycled polyethylene terephthalate powder accounts for 55%–75% of the mass of the integrated functional masterbatch. In step S5, the temperature of the melt spinning is 265-285℃, the side blowing speed is 1.0-1.5m / s, and the air temperature is 20-28℃. In step S6, the stretching ratio is 3.0 to 4.0 times, the heat setting temperature is 110 to 130°C, and the winding speed is 3000 to 4200 m / min.

[0020] A multifunctional marine recycled polyester ultrafine filament, wherein the single filament diameter is 5-10 μm, the linear density is 0.27-1.08 dtex, and the coefficient of variation of the single filament diameter is not greater than 2%.

[0021] In the above scheme, the mesoporous rutile titanium dioxide shell provides spatial isolation for the zinc oxide core. Its 2-5 nm mesoporous structure reduces the probability of direct contact between the polyester macromolecular chains and the zinc oxide core, while providing migration channels for water, oxygen, and antibacterial-related small molecules or ions, thus achieving a balance between inhibiting polyester catalytic degradation and maintaining antibacterial activity. The rutile titanium dioxide phase has lower photocatalytic activity than the anatase phase, which is beneficial for reducing the photo-oxidation of the polyester matrix under ultraviolet irradiation. The calcined magnesium-aluminum composite metal oxide has a high specific surface area and can undergo local hydration reconstruction in the presence of trace amounts of water, thereby reducing the impact of residual chlorine-containing species on the melt processing stability of polyester and the stability of the zinc component through surface adsorption and anion fixation.

[0022] Compared with the prior art, the beneficial effects of the present invention are: First, the core-shell functional particles significantly reduce the direct contact between the zinc oxide core and the recycled polyester molecular chain by utilizing the spatial confinement effect of the mesoporous shell, thereby reducing the catalytic effect of zinc oxide on the polyester ester bond. This significantly reduces the intrinsic viscosity during melt processing and lowers the carboxyl content at the fiber end, thus introducing antibacterial function without sacrificing the fiber's breaking strength and reducing the breakage rate and diameter dispersion of ultrafine denier spinning.

[0023] Secondly, the pore size window of the mesoporous shell can restrict the polyester macromolecules from approaching the zinc oxide core while retaining the migration channels of small molecules and ionic species, thus maintaining antibacterial activity.

[0024] Third, the shell is limited to the rutile phase, which inhibits the photo-oxidative degradation of the polyester matrix by titanium dioxide under ultraviolet light, so that the fiber still maintains a high breaking strength retention rate after artificial accelerated aging.

[0025] Fourth, calcined magnesium-aluminum composite metal oxides can fix residual chlorine-containing species in marine recycled materials through surface adsorption and local hydration reconstruction under trace water conditions, and also have a certain hygroscopic effect, thereby helping to improve the stability of polyester melt processing and reduce the migration of zinc components.

[0026] Fifth, all functional components are added at once after being integrated with the coloring masterbatch to form an integrated functional masterbatch, so that coloring and functionalization are completed simultaneously, eliminating the need for post-dyeing and finishing processes and eliminating dyeing wastewater discharge; the fiber has three functions: antibacterial, UV aging resistant and coloring, which can meet the application requirements of automotive interior and outdoor textiles. Attached Figure Description

[0027] Figure 1 The X-ray diffraction (XRD) patterns of the core-shell functional particles of Example 1, the mesoporous anatase phase titanium dioxide shell particles of Comparative Example 3, and the uncoated zinc oxide cores are shown.

[0028] Figure 2 The figures show the pore size distribution curves of the core-shell functional particles in Embodiment 1, Comparative Example 2, and Comparative Example 6 of this invention.

[0029] Figure 3 The X-ray diffraction (XRD) patterns of the Mg-Al-CO3 layered bimetallic hydroxide precursor, the calcined magnesium-aluminum composite metal oxide, and the product after chloride ion adsorption in Example 1 of this invention are shown.

[0030] Figure 4 The Fourier transform infrared (FTIR) spectra of the Mg-Al-CO3 layered bimetallic hydroxide precursor, the calcined magnesium-aluminum composite metal oxide, and the product after chloride ion adsorption in Example 1 of this invention are shown. Detailed Implementation

[0031] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] The following examples are used to illustrate the present invention, but are not intended to limit the scope of protection of the present invention. Unless otherwise stated, all parts mentioned in the examples are parts by weight, and are based on 100 parts by weight of polyester matrix; percentages are by weight unless otherwise specified.

[0033] Proportioning and raw material specifications: The polyester matrix consists of marine-recycled polyethylene terephthalate (PET) bottle flakes and virgin PET chips, totaling 100.00 parts by weight. Core-shell functional particles, calcined magnesium-aluminum composite metal oxides, coloring masterbatch, and dispersant are added separately from the polyester matrix. When preparing the integrated functional masterbatch, the carrier used is the first portion of recycled PET powder taken from the aforementioned marine-recycled PET bottle flakes. This carrier powder is included in the total amount of the polyester matrix and is not deducted from it. The carrier powder used in step S4 is obtained by pulverizing the first portion of pretreated bottle flakes, and the second portion of pretreated bottle flakes used in step S5 is the remaining amount after deducting the first portion. The ratio of the sum of their masses to the mass of the virgin PET chips is 70–90:10–30.

[0034] The raw material specifications are as follows: recycled marine PET bottle flakes, intrinsic viscosity 0.58–0.62 dL / g, extractable chloride ion content not exceeding 50 mg / kg; virgin PET chips, intrinsic viscosity 0.64–0.70 dL / g, fiber grade; zinc oxide powder, average particle size 20–80 nm, purity not less than 99.0%; rutile phase titanium dioxide seed crystals, average particle size 5–15 nm, rutile phase mass fraction not less than 98%; tetrabutyl titanate, purity not less than 98%. The template agent is hexadecyltrimethylammonium bromide or polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer; the Mg-Al-CO3 layered bimetallic hydroxide precursor is a commercially available product with a Mg:Al molar ratio of 2:1 to 4:1 and a dry basis purity of not less than 95%; both nitric acid and sodium hydroxide are analytical grade; the coloring masterbatch is a PET carrier color masterbatch with a pigment content of 20% to 30% and a pigment heat resistance temperature of not less than 300℃; the dispersant is oxidized polyethylene wax or pentaerythritol stearate.

[0035] The two types of matrix resins mentioned above should also meet the following technical indicators and material selection criteria so that those skilled in the art can determine the specific selection of raw materials.

[0036] The above-mentioned marine recycled PET bottle flakes are bottle flakes obtained by crushing and sorting drinking water bottles and beverage bottles collected from the marine environment through seawater immersion or marine environment. They do not include oil bottles, pesticide bottles and chemical packaging bottles. The flake size is 3-12mm and meets all the indicators listed in Table 1.

[0037] Table 1

[0038] The above-mentioned virgin PET chips are fiber-grade glossy chips, free of matting agents, and meet all the indicators listed in Table 2.

[0039] Table 2

[0040] The selection criteria for the two types of matrix resins are as follows.

[0041] Intrinsic viscosity is the most basic and commonly used indicator of polyester fiber raw materials, but two types of raw materials with the same intrinsic viscosity cannot guarantee consistent performance of the resulting filaments. Even after long-term immersion in seawater, marine recycled bottle flakes, while having an intrinsic viscosity comparable to virgin flakes, may still exhibit several times differences in terminal carboxyl group content, extractable chloride ion content, and iron and other metal ion content. These parameters correspond to the sensitivity to hydrolysis and alcoholysis during melt processing, the loading of chloride-containing species, and catalytic degradation activity, directly affecting whether the technical problem described in this invention can be solved. Therefore, this invention uses criteria P1 to P4 to determine the selection of two types of matrix resins: P1 (Viscosity Matching): The intrinsic viscosity difference ΔIV = IV(virgin) - IV(bottled) of virgin PET chips and recycled PET bottle flakes from the ocean is 0.02–0.12 dL / g. The difference between the calculated and measured intrinsic viscosity of the mixture, calculated using a weighted ratio of 70–90:10–30, should not exceed 0.02 dL / g, and the intrinsic viscosity of the mixture should fall within the range of 0.58–0.65 dL / g. When ΔIV is less than 0.02 dL / g, the compensating effect of virgin chips on the degradation of recycled materials is insufficient, and the intrinsic viscosity of the mixture is likely to be lower than 0.58 dL / g, leading to an increased breakage rate in ultrafine denier spinning. When ΔIV is greater than 0.12 dL / g, the viscosities of the two components are mismatched, and the melt is prone to unstable flow at the spinneret exit, increasing the coefficient of variation of the single filament diameter.

[0042] P2 (Terminal Carboxyl Group Matching): The terminal carboxyl group content of the mixture should not exceed 29 mol / t. Calculated using a weighted ratio of 70–90:10–30, when the terminal carboxyl group content of the bottle flakes is 30 mol / t and the virgin PET chips are 20 mol / t, the calculated value of the terminal carboxyl group content of the mixture is 27–29 mol / t, which aligns with the indices in Tables 1 and 2. When the terminal carboxyl group content of marine recycled PET bottle flakes exceeds 30 mol / t, it should first undergo solid-phase thickening treatment (220℃, vacuum degree not exceeding 100 Pa, treatment for 4 hours) to reduce it to below 30 mol / t, or its ratio should be reduced to 70 parts while simultaneously increasing the virgin PET chips to 30 parts before use. Bottle flakes with a terminal carboxyl group content greater than 35 mol / t should not be directly used in this invention.

[0043] P3 (Chlorine-containing species matching): The extractable chloride ion content of the bottle flakes after pretreatment in step S1 is no more than 50 mg / kg; the amount m of calcined magnesium-aluminum composite metal oxide (based on 100 parts by mass of polyester matrix) is calculated according to m≥2×10-2×w, where w is the extractable chloride ion content (mg / kg) of the pretreated bottle flakes; the coefficient is determined as follows: based on 100 parts by mass of matrix, the total chloride ion content is 0.1w mg, and based on a saturated adsorption capacity of 120 mg / g, the amount required for complete fixation is 8.3×10-4w parts by mass, and taking a safety factor of 4, we get 2×10-2w. When w is 50 mg / kg, the calculated value is 0.17 parts by mass, so the lower limit of 0.3 parts by mass has a margin of more than 1.8 times; the surplus capacity corresponding to the upper limit of 1.5 parts by mass is used to fix the newly generated chlorides from the reaction of trace chlorine-containing species with terminal carboxyl groups during melt extrusion and spinning, and to inhibit the migration of zinc components to the fiber surface.

[0044] P4 (Moisture content and cleanliness matching): The moisture content of the bottle flakes after pretreatment in step S1 is not greater than 0.05%, the moisture content of the virgin PET chips after drying is not greater than 50 mg / kg, and the dew point of the drying hot air is not higher than -40℃; the amount of polyvinyl chloride mixed in the bottle flakes is not greater than 30 mg / kg, and the amount of other heterogeneous resins mixed in is not greater than 100 mg / kg.

[0045] Raw materials that simultaneously meet the requirements of Tables 1 and 2 and criteria P1 to P4 belong to the two types of matrix resins applicable to this invention. Conversely, if a recycled material falls within the range of Table 1 in terms of intrinsic viscosity, but its terminal carboxyl group content, extractable chloride ion content, or impurity resin content exceeds the above indicators, then those skilled in the art can determine, based on the description in this specification, that it cannot achieve the technical effects described in this invention, and therefore does not fall within the raw material selection range of this invention.

[0046] The correspondence between the above raw material parameters and the technical problems solved by this invention, the countermeasures taken, and the technical effects is shown in Table 3.

[0047] Table 3

[0048] The methods for determining structural parameters and raw material indicators are as follows: Extractable chloride ion content was determined by ion chromatography. 10.0 g of shredded PET bottle flakes were added to 100 mL of deionized water, and the mixture was extracted at 60℃ with shaking for 2 h. After filtration through a 0.45 μm filter membrane, the Cl- concentration was determined. The average core particle size and shell thickness of zinc oxide were determined by transmission electron microscopy, with at least 30 particles randomly counted. The BET specific surface area, pore size, and pore volume of core-shell functional particles were determined using nitrogen adsorption-desorption at 77 K. The sample was degassed under vacuum at 120℃ for 6 h. The specific surface area was calculated using the BET method, the mesopore size was calculated using the BJH desorption branch, and the total pore volume was calculated at a P / P0 ratio of approximately 0.99. The titanium dioxide crystal phase was determined using Cu Kα... X-ray diffraction and Rietveld refinement were performed, and the mass fraction of rutile phase was calculated after normalization of each phase of titanium dioxide. The saturated chloride ion adsorption capacity of calcined magnesium-aluminum composite metal oxide was tested by static adsorption using a series of sodium chloride solutions ranging from 200 to 3000 mg / L, with a solid-liquid ratio of 1.0 g / L, at 25℃ and oscillation at 150 r / min for 24 h. The chloride ion concentration in the equilibrium solution was determined by ion chromatography, and the plateau value of the adsorption isotherm was used as the saturated adsorption capacity. The moisture content was determined by drying at 105℃ to constant weight. The diameter of 50 filaments was randomly measured, and the average value and coefficient of variation were calculated. The linear density was determined according to GB / T14343.

[0049] Example 1

[0050] Step S1: Take a sufficient amount of marine recycled PET bottle flakes, sort them by near-infrared spectroscopy at a wavelength of 1200nm and a speed of 2.0m / min, clean them by a combination of high-pressure spraying at 0.5MPa and ultrasonic vibration at 500W and 28kHz for 15min, and dry them with hot air at 110℃ to a moisture content of 0.04%, to obtain pretreated bottle flakes with an extractable chloride ion content of 18mg / kg and a moisture content of 0.04%. Weigh out 80 portions for subsequent steps.

[0051] Step S2, [Mg:Al molar ratio of 3:1] 0.75 Al 0.25 [(OH)2](CO3) 0.125 The mH2O precursor was calcined at 520℃ for 4 h to obtain calcined magnesium-aluminum composite metal oxide (hereinafter referred to as CLDH, x=0.25), which has a saturated adsorption capacity of 142 mg / g for chloride ions and a BET specific surface area of ​​186 m². 2 / g; after cooling to 50℃ under nitrogen protection, seal and dry at 130℃ for 3h before use, with a moisture content of 0.2%.

[0052] Step S3: Take 100 parts of zinc oxide powder with an average particle size of 50 nm and disperse it in a mixed solvent of 1000 parts anhydrous ethanol and 62 parts deionized water, and ultrasonically disperse for 30 min; add 5 parts of rutile phase titanium dioxide seed crystals, and prepare a solution by mixing tetrabutyl titanate and anhydrous ethanol at a mass ratio of 1:2 (molar ratio of titanium to zinc 0.35:1, molar ratio of water to titanium 8:1), and add it dropwise at a uniform rate over 6 h, while simultaneously adding hexadecyltrimethylammonium bromide in an amount equal to the mass of tetrabutyl titanate. The zinc oxide content was 5.4%. The pH was maintained at 7.0 at 55℃ using 0.1 mol / L nitric acid or 0.1 mol / L sodium hydroxide solution. After the addition was complete, the mixture was aged for 4 hours. It was then transferred to a hydrothermal reactor and hydrothermally treated at 160℃ for 12 hours. The template agent was removed by Soxhlet extraction with anhydrous ethanol for 8 hours. The mixture was then centrifuged (8000 r / min, 10 min), washed three times with anhydrous ethanol, dried at 100℃ for 6 hours, and air-jet milled to a D50 of 180 nm to obtain core-shell functional particles. The obtained particles had an average zinc oxide core diameter of 50 nm, a shell thickness of 14 nm, a mesopore diameter of 3.6 nm, a pore volume of 0.25 cm³ / g, and a BET specific surface area of ​​132 m². 2 / g, rutile phase mass fraction 94%.

[0053] Step S4: Take 1.8 parts of core-shell functional particles, 0.8 parts of CLDH, 2.8 parts of coloring masterbatch, and 0.3 parts of dispersant oxidized polyethylene wax, and mix them with 13.3 parts of recycled PET powder from the first part of the pretreated bottle flakes (total functional components 5.7 parts, total masterbatch 19.0 parts, carrier accounts for 70.0% of masterbatch), and granulate by twin-screw melt extrusion at 255℃ to obtain integrated functional masterbatch.

[0054] In step S5, 19.0 parts of integrated functional masterbatch, 66.7 parts of pretreated bottle flakes from the second part, and 20 parts of virgin PET chips are mixed (total matrix 100.0 parts, intrinsic viscosity of the mixture 0.62dL / g), and melt-spun at 275℃ with a side-blowing air velocity of 1.2m / s and an air temperature of 24℃ to obtain nascent fibers.

[0055] Step S6: 3.5 times stretching, heat setting at 125℃, and winding speed of 3600m / min to obtain a multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 6.4μm, a linear density of 0.44dtex, and a single filament diameter variation coefficient of 1.2%.

[0056] Example 2

[0057] Following the raw materials and steps of Example 1, with only the following adjustments: 70 parts of marine recycled PET bottle flakes, 30 parts of virgin PET chips; 0.8 parts of core-shell functional particles, 0.3 parts of CLDH, 1.5 parts of coloring masterbatch, and 0.1 parts of dispersant oxidized polyethylene wax; 6.3 parts of recycled PET powder in the first part (total functional components 2.7 parts, total masterbatch 9.0 parts, carrier accounting for 70.0% of masterbatch); 63.7 parts of pretreated bottle flakes and 30 parts of virgin PET chips in the second part, with a mixture intrinsic viscosity of 0.63 dL / g; CLDH x=0.20, calcination temperature 460℃, time 6h, saturated adsorption capacity 126mg / g, and BET specific surface area 164m2 / g. Other conditions were the same as in Example 1, yielding a multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 8.7μm, a linear density of 0.82dtex, and a single filament diameter variation coefficient of 1.7%.

[0058] Example 3

[0059] Following the raw materials and steps of Example 1, with only the following adjustments: 90 parts of recycled PET bottle flakes from the ocean, 10 parts of virgin PET chips; 3.0 parts of core-shell functional particles, 1.5 parts of CLDH, 4.0 parts of coloring masterbatch, and 0.5 parts of dispersant oxidized polyethylene wax; 11.0 parts of recycled PET powder in the first part (total functional components 9.0 parts, total masterbatch 20.0 parts, carrier accounting for 55.0% of masterbatch); 79.0 parts of pretreated bottle flakes in the second part, 10 parts of virgin PET chips, with an intrinsic viscosity of 0.61. The CLDH concentration was set to x=0.33, the calcination temperature was 580℃, the time was 2h, the saturated adsorption capacity was 158mg / g, and the BET specific surface area was 138m2 / g. In step S3, the molar ratio of titanium to zinc was adjusted to 0.55:1, the molar ratio of water to titanium was adjusted to 10:1, the amount of deionized water was adjusted to 122 parts, the amount of template agent was 8.0% of the mass of tetrabutyl titanate, the dropping time was 7h, and the hydrothermal treatment was adjusted to 170℃ for 18h. The resulting shell thickness was 22nm and the mesopore diameter was 4.8nm. The remaining conditions were the same as in Example 1, resulting in a multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 5.8μm, a linear density of 0.36dtex, and a single filament diameter variation coefficient of 1.3%.

[0060] Example 4

[0061] The raw materials and steps of Example 1 were adjusted only as follows: the dispersant was replaced with 0.3 parts of pentaerythritol stearate; the core-shell functional particles were 2.2 parts; in step S3, the average particle size of zinc oxide powder was 30 nm, the molar ratio of titanium to zinc was adjusted to 0.20:1, the molar ratio of water to titanium was adjusted to 5:1, the amount of deionized water was adjusted to 22 parts, the amount of template agent was 5.0% of the mass of tetrabutyl titanate, the dropping time was 4 h, and the hydrothermal treatment was adjusted to 140 °C for 8 h, resulting in a shell thickness of 9 nm, a mesopore diameter of 2.4 nm, and a rutile phase mass fraction of 91%; the first part consisted of 14.2 parts of recycled PET powder (6.1 parts of functional components, 20.3 parts of masterbatch, and 70.0% of the carrier in the masterbatch); the second part consisted of 65.8 parts of pretreated bottle flakes. Under the same conditions as in Example 1, a multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 6.6 μm, a linear density of 0.47 dtex, and a single filament diameter variation coefficient of 1.4% was obtained.

[0062] The following comparative examples are based on the raw materials, proportions, and process steps of Example 1. Only one variable is changed each time to illustrate the impact of that variable on the technical effect.

[0063] Comparative Example 1 In steps S3 to S4, 1.8 parts of core-shell functional particles were replaced with a physical mixture of 1.17 parts of uncoated nano-zinc oxide and 0.63 parts of rutile titanium dioxide (totaling 1.80 parts, of which 1.17 parts contain zinc oxide, the same as the zinc oxide core content in the core-shell particles of Example 1). The remaining components and steps were the same as in Example 1. This comparative example was used to control the morphology of the functional particles.

[0064] Comparative Example 2 The core-shell functional particles were replaced with dense shell particles with no pores (average zinc oxide core diameter 50 nm, dense rutile titanium dioxide shell thickness 14 nm, BET specific surface area 28 m²). 2 / g (mesopore diameter and pore volume not measured), dosage 1.8 parts, the rest is the same as in Example 1. This comparative example is used to compare the presence or absence of shell pores.

[0065] Comparative Example 3 The core-shell functional particles were replaced with mesoporous anatase titanium dioxide shell particles (zinc oxide core average particle size 50 nm, shell thickness 14 nm, mesopore diameter 3.6 nm, pore volume 0.25 cm³). 3 / g, rutile phase mass fraction 5%), amount 1.8 parts, the rest is the same as in Example 1. This comparative example is used to control the crystal phase of the shell.

[0066] Comparative Example 4 0.8 parts of calcined magnesium-aluminum composite metal oxide were removed. The first part of recycled PET powder remained at 13.3 parts, and the second part of pretreated bottle flakes remained at 66.7 parts. The rest was the same as in Example 1. At this time, the total functional components were 4.9 parts, the total masterbatch was 18.2 parts, and the carrier accounted for 73.1% of the masterbatch. This comparative example was used to control the presence or absence of calcined magnesium-aluminum composite metal oxide.

[0067] Comparative Example 5 Replace 0.8 parts of calcined magnesium-aluminum composite metal oxide with uncalcined [Mg] 0.75 Al 0.25 [(OH)2](CO3) 0.125 0.8 parts of layered bimetallic hydroxide (mH2O) were used, with the remainder the same as in Example 1. This comparative example was used to check whether the precursor was activated by calcination.

[0068] Comparative Example 6 The core-shell functional particles were replaced with macroporous shell particles (zinc oxide core with an average particle size of 50 nm, shell thickness of 14 nm, macropore diameter of 60–120 nm, and pore volume of 0.25 cm³). 3 / g, BET specific surface area 126m² 2 / g), the amount used is 1.8 parts, and the rest is the same as in Example 1. According to the pore classification of the International Union of Pure and Applied Chemistry, pores with a diameter greater than 50 nm are classified as macropores, therefore the shell of this comparative example does not belong to the mesoporous shell.

[0069] Performance testing methods: The filaments obtained in the examples and comparative examples were tested using the following method. All samples were conditioned to humidity for 24 hours at a temperature of 20℃±2℃ and a relative humidity of 65%±4% before testing.

[0070] I. Melt intrinsic viscosity drop Δ[η]: determined according to GB / T14190. The solvent was a mixture of phenol and 1,1,2,2-tetrachloroethane in a mass ratio of 1:1, the temperature was 25℃±0.05℃, an Ubbelohde viscometer was used, and the sample mass concentration was 0.005 g / mL. The intrinsic viscosity of the melt before spinning in step S5 and the filament obtained in step S6 were measured separately, and the difference between the two was Δ[η]. Each group was measured in triplicate, and the arithmetic mean was taken.

[0071] II. Terminal carboxyl group content: determined by titration method specified in Appendix of GB / T14190, using potassium hydroxide-ethanol standard titration solution. The results are expressed as mol / t. Each group was measured in triplicate and the arithmetic mean was taken.

[0072] III. Breaking strength and elongation at break: Tested according to GB / T14344, using an electronic strength tester with constant speed elongation, clamping distance of 500 mm, tensile speed of 500 mm / min, and pre-tension of 0.05 cN / dtex. Each group was tested 30 times and the arithmetic mean was taken.

[0073] IV. Antibacterial rate: Determined by the shaking method according to GB / T20944.3, using Escherichia coli ATCC25922 and Staphylococcus aureus ATCC6538, with an inoculum concentration of 1×10⁻⁶. 5 CFU / mL, oscillation frequency 150r / min, temperature 37℃, contact time 18h; before testing, each filament was made into a knitted sample with the same linear density and uniform mass per unit area; the knitted sample made with the same raw materials and processes as the core-shell functional particles was used as the control sample. The antibacterial rate was the percentage of the difference between the colony count of the control sample and the sample colony count to the colony count of the control sample. Each group was measured in parallel 3 times and the arithmetic mean was taken.

[0074] V. Antibacterial rate after washing: First, wash 50 times at 40℃ according to the 4N procedure specified in GB / T8629. Hang to dry after each wash, and then determine the antibacterial rate according to the above method.

[0075] VI. Fracture strength retention rate after artificial accelerated aging: According to GB / T16422.2 Xenon arc lamp artificial climate aging method, the irradiance is 0.51W / m2 (340nm), the black panel temperature is 65℃±3℃, the relative humidity is 50%±5%, and the light irradiation is alternated with spraying for 102min and 18min for 100h in total; the fracture strength retention rate is measured after aging.

[0076] VII. Color difference ΔE: Measured according to GB / T7921, using D65 standard light source, 10° field of view, and CIELAB color space. The color of the same sample before artificial accelerated aging is used as the standard value. The color difference after 100 hours of artificial accelerated aging is measured. The arithmetic mean of 5 positions is taken for each sample.

[0077] Performance test results The performance test results of the examples and comparative examples are shown in Table 4.

[0078] Table 4

[0079] As shown in Table 4, all embodiments exhibited a small decrease in intrinsic viscosity and a low level of terminal carboxyl groups during melt processing, while maintaining high fracture strength and elongation at break. They also demonstrated good initial antibacterial properties, wash-resistant antibacterial properties, retention of mechanical properties after artificial aging, and color stability, indicating a good synergistic effect between the core-shell functional particles and the calcined magnesium-aluminum composite metal oxide. In contrast, the control example using uncoated zinc oxide showed more significant polyester thermal degradation and a decrease in mechanical properties, indicating that the mesoporous titanium dioxide shell effectively weakens the catalytic degradation caused by direct contact between zinc oxide and polyester molecular chains. While the dense shell maintained good melt stability and mechanical properties, the antibacterial properties, especially the retention of antibacterial properties after washing, were significantly reduced. The significant decrease indicates that a suitable mesoporous structure plays an important role in the migration of antibacterial active species. Samples using anatase shells showed relatively small changes in initial overall performance, but their mechanical property retention after artificial aging decreased significantly, indicating that rutile shells are more effective in inhibiting photocatalytic aging under UV irradiation. Removing calcined magnesium-aluminum composite metal oxides or using uncalcined precursors increased polyester degradation and decreased mechanical properties and antibacterial durability, indicating that calcined and activated magnesium-aluminum composite metal oxides help fix residual chlorine-containing species and improve the stability of polyester melt processing. Furthermore, when using macroporous shells, the overall performance was inferior to samples with suitable mesoporous structures, further illustrating that the shell pore size needs to strike a balance between isolating polyester macromolecules and ensuring the migration of antibacterial active species. Therefore, the variation patterns presented in the data of each group in Table 4 are basically consistent with the single-factor design objectives of each comparative example and the mechanism of action described in this invention.

[0080] like Figure 1 As shown, the uncoated zinc oxide core exhibits characteristic diffraction peaks of the zinc oxide crystalline phase. In the diffraction pattern of the core-shell functional particle of Example 1, while retaining the characteristic diffraction peaks of the zinc oxide core, a distinct rutile phase titanium dioxide characteristic diffraction peak appears around 27°, indicating the presence of highly crystalline rutile phase titanium dioxide in the composite particle of Example 1. Combined with the shell thickness measured by the transmission electron microscope, its rutile phase titanium dioxide coating structure can be confirmed. In contrast, Comparative Example 3 exhibits a more distinct anatase phase titanium dioxide characteristic diffraction peak around 25°, and its diffraction peak distribution is significantly different from that of Example 1.

[0081] like Figure 2As shown, the pore size of the core-shell functional particles obtained in Example 1 is mainly concentrated in the range of 2 to 5 nm, and a significant main distribution peak is formed at about 3 to 4 nm, which is consistent with the mesoporous pore size measured in Example 1, indicating that its titanium dioxide shell has a relatively concentrated mesoporous structure; Comparative Example 2 uses a dense titanium dioxide shell, and its pore size distribution curve is close to the baseline as a whole, without forming a significant mesoporous distribution peak, indicating that its shell lacks effective through-pores; Comparative Example 6 shows a significant macroporous distribution peak in the range of tens to hundreds of nanometers, and its main pore size is significantly beyond the mesoporous range.

[0082] like Figure 3 As shown, the Mg-Al-CO3 layered bimetallic hydroxide precursor exhibits obvious layered structure diffraction peaks in the low-angle region, indicating that it has a typical ordered layered structure. After calcination, the low-angle layered structure characteristic peaks of the precursor are significantly weakened or disappear, and corresponding broadened diffraction peaks appear in the calcined magnesium-aluminum composite oxide, indicating that the calcination process destroys the original laminations and interlayer structure and forms magnesium-aluminum composite metal oxide. When the calcined magnesium-aluminum composite metal oxide comes into contact with a chlorine-containing system, the low-angle layered structure characteristic peaks reappear, indicating that the material undergoes hydration reconstruction and reforms the layered structure.

[0083] like Figure 4 As shown, the Mg-Al-CO3 layered bimetallic hydroxide precursor exhibits a broad hydroxyl stretching vibration absorption band in the high wavenumber region, while interlayer water, carbonate, and metal-oxygen bond related absorption characteristics can be observed in the mid-to-low wavenumber region. After calcination, the hydroxyl and interlayer anion related absorptions are significantly weakened, indicating that interlayer water and some oxygen-containing anions are removed, which is consistent with the process of the layered bimetallic hydroxide transforming into magnesium-aluminum composite metal oxides after heat treatment. After the calcined material adsorbs chloride ions, the hydroxyl and bound water related absorptions in the high wavenumber region are re-enhanced, and the morphology of some absorption bands also changes, indicating that the material undergoes structural reconstruction during hydration and anion adsorption.

[0084] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A multifunctional marine recycled polyester ultrafine filament, characterized in that, The raw materials for the ultrafine filaments include polyester matrix, core-shell functional particles, calcined magnesium-aluminum composite metal oxide, coloring masterbatch, and dispersant. Based on 100 parts by weight of the polyester matrix, the polyester matrix is ​​composed of 70-90 parts by weight of marine recycled polyethylene terephthalate bottle flakes and 10-30 parts by weight of virgin polyethylene terephthalate chips. In addition to the polyester matrix, it also includes the following components: 0.8-3.0 parts by weight of core-shell functional particles, 0.3-1.5 parts by weight of calcined magnesium-aluminum composite metal oxide, 1.5-4.0 parts by weight of coloring masterbatch, and 0.1-0.5 parts by weight of dispersant. The core-shell functional particle is composed of a zinc oxide core and a mesoporous rutile phase titanium dioxide shell covering the zinc oxide core. The calcined magnesium-aluminum composite metal oxide has the composition shown in general formula (I): Mg 1-x Al x O 1+x / 2 In general formula (I), x is selected from 0.20 to 0.33; The diameter of the single filament of the ultrafine filament is 5 to 10 μm.

2. The multifunctional marine recycled polyester ultrafine filament according to claim 1, characterized in that, In the core-shell functional particles, the average particle size of the zinc oxide core is 20-80 nm, the thickness of the mesoporous rutile phase titanium dioxide shell is 5-25 nm, and the mass fraction of rutile phase in the mesoporous rutile phase titanium dioxide shell is not less than 90%.

3. The multifunctional marine recycled polyester ultrafine filament according to claim 2, characterized in that, The mesoporous rutile titanium dioxide shell has a mesopore size of 2–5 nm and a pore volume of 0.10–0.40 cm³. 3 / g, the BET specific surface area of ​​the core-shell functional particles is 60-200 m² / g. 2 / g.

4. The multifunctional marine recycled polyester ultrafine filament according to claim 1, characterized in that, The core-shell functional particles are 1.0 to 2.5 parts by mass, the calcined magnesium-aluminum composite metal oxide is 0.5 to 1.2 parts by mass, the coloring masterbatch is 2.0 to 3.5 parts by mass, and the dispersant is 0.2 to 0.4 parts by mass.

5. The multifunctional marine recycled polyester ultrafine filament according to claim 2, characterized in that, The core-shell functional particles are prepared by a method comprising the following steps: A1. Disperse zinc oxide powder with an average particle size of 20-80 nm in a mixed solvent of ethanol and water to obtain a zinc oxide core suspension. A2. Add rutile titanium dioxide seed crystals to the zinc oxide core suspension, then prepare a solution by mixing tetrabutyl titanate and ethanol at a mass ratio of 1:1 to 1:3, and add the solution dropwise at a uniform rate over 2 to 8 hours. Simultaneously, add a template agent, and react at 40 to 70°C with pH adjusted to 6.5 to 7.5 using 0.1 mol / L nitric acid or 0.1 mol / L sodium hydroxide solution to obtain zinc oxide composite particles coated with titanium dioxide precursor. The amount of rutile titanium dioxide seed crystals used is 2% to 8% of the mass of zinc oxide powder; the molar ratio of titanium in tetrabutyl titanate to zinc in zinc oxide powder is 0.15 to 0.60:1; the molar ratio of water in the mixed solvent to titanium in tetrabutyl titanate is 4 to 12:1; and the amount of template agent used is 5% to 15% of the mass of tetrabutyl titanate. A3. Place the zinc oxide composite particles obtained in step A2 into a hydrothermal reactor and hydrothermally treat them at 120-180℃ for 4-24 hours to obtain the hydrothermal product. A4. Remove the template agent from the hydrothermal products, and obtain the core-shell functional particles by washing, solid-liquid separation, drying and pulverizing.

6. The multifunctional marine recycled polyester ultrafine filament according to claim 1, characterized in that, The calcined magnesium-aluminum composite metal oxide is obtained by calcining the precursor represented by general formula (II): [Mg 1-x Al x [(OH)2](CO3) x / 2 ·mH2O, in general formula (II), x is selected from 0.20 to 0.33, and m is 0 to 4; the calcination temperature is 450 to 600℃, and the time is 2 to 6 hours; the saturated adsorption capacity of the calcined magnesium-aluminum composite metal oxide for chloride ions is not less than 120 mg / g, and the BET specific surface area is not less than 120 m². 2 / g, the moisture content before use should not exceed 0.3%.

7. The multifunctional marine recycled polyester ultrafine filament according to claim 1, characterized in that, The ultrafine filament has a single filament diameter of 5–10 μm, a linear density of 0.27–1.08 dtex, and a single filament diameter variation coefficient of no more than 2%. The dispersant is selected from oxidized polyethylene wax or pentaerythritol stearate; The marine recycled polyethylene terephthalate (PET) bottle flakes are bottle flakes from drinking water bottles or beverage bottles, and their extractable chloride ion content is no higher than 50 mg / kg.

8. A method for preparing multifunctional marine recycled polyester ultrafine filament as described in claim 1, characterized in that, Includes the following steps: S1. Marine recycled polyethylene terephthalate bottle flakes are sequentially subjected to near-infrared spectroscopy sorting, high-pressure spraying and ultrasonic vibration combined cleaning, and hot air drying to obtain pretreated bottle flakes. S2. The precursor shown in general formula (II) is calcined at 450-600℃ for 2-6 hours to obtain the calcined magnesium-aluminum composite metal oxide, where x in general formula (II) is selected from 0.20-0.33 and m is 0-4; S3. Disperse zinc oxide powder with an average particle size of 20-80 nm in a mixed solvent of ethanol and water, add rutile titanium dioxide seed crystals, prepare a solution by mixing tetrabutyl titanate and ethanol at a mass ratio of 1:1 to 1:3, add a template agent at a uniform rate of 5% to 15% of the mass of tetrabutyl titanate over 2-8 hours, react at 40-70 °C with pH adjusted to 6.5-7.5 using 0.1 mol / L nitric acid or 0.1 mol / L sodium hydroxide solution, and then hydrothermally treat at 120-180 °C for 4-24 hours. After removing the template agent, pulverize to obtain the core-shell functional particles. S4. The core-shell functional particles, the calcined magnesium-aluminum composite metal oxide, the coloring masterbatch and the dispersant are mixed with the first part of the recycled polyethylene terephthalate powder obtained by crushing the first part of the pretreated bottle flakes and then melt-extruded and granulated, wherein the first part of the recycled polyethylene terephthalate powder accounts for 55% to 75% of the mass of the integrated functional masterbatch, to obtain the integrated functional masterbatch. S5. The integrated functional masterbatch, the second part of pretreated bottle flakes, and virgin polyethylene terephthalate chips are mixed to obtain a mixture with an intrinsic viscosity of 0.58-0.65 dL / g, which is then melt-spun to obtain nascent fibers; the ratio of the sum of the mass of the first part of pretreated bottle flakes and the second part of pretreated bottle flakes to the mass of the virgin polyethylene terephthalate chips is 70-90:10-30; S6. The nascent fibers are stretched and heat-set to obtain the multifunctional marine recycled polyester ultrafine filament with a single filament diameter of 5-10 μm.

9. The preparation method according to claim 8, characterized in that, In step S1, the wavelength of the near-infrared spectral sorting is 1100–1300 nm, and the sorting speed is 1.5–2.5 m / min; the pressure of the high-pressure spraying is 0.3–0.8 MPa; the power of the ultrasonic oscillation is 300–800 W, the frequency is 20–40 kHz, and the time is 10–20 min; the temperature of the hot air drying is 100–120 °C, and the drying is carried out until the moisture content of the pretreated bottle flakes is not higher than 0.05%; the extractable chloride ion content of the pretreated bottle flakes is not higher than 50 mg / kg.

10. The preparation method according to claim 8, characterized in that, In step S3, the amount of rutile phase titanium dioxide seed crystals is 2% to 8% of the mass of zinc oxide powder, and the molar ratio of titanium in tetrabutyl titanate to zinc in zinc oxide powder is 0.15 to 0.60:

1. In step S4, the temperature of the melt extrusion granulation is 240–270°C, and the first portion of recycled polyethylene terephthalate powder accounts for 55%–75% of the mass of the integrated functional masterbatch; In step S5, the temperature of the melt spinning is 265-285℃, the side blowing speed is 1.0-1.5m / s, and the air temperature is 20-28℃. In step S6, the stretching ratio is 3.0 to 4.0 times, the heat setting temperature is 110 to 130°C, and the winding speed is 3000 to 4200 m / min.