Grey board paper and its preparation method
By optimizing the production process of grey board paper through high-concentration ONP/OCC pulp mixing and thermal dispersion technology, the problems of high cost and high energy consumption in traditional grey board paper production have been solved, realizing low-cost and high-quality grey board paper production, and improving fiber resource utilization and environmental benefits.
Patent Information
- Application Number
- CN202611313564.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
In traditional greyboard paper production, the surface pulp relies on DIP deinking pulp, which is costly, has low yield, high energy consumption, and the ONP/OCC waste paper fiber resources are not fully utilized.
High-concentration ONP/OCC pulp is mixed, and energy consumption is reduced by strengthening fiber dissociation and thermal dispersion technology to prepare high-quality surface pulp. Recycled slag and sludge are used as core pulp, and the papermaking process is optimized to improve paper quality.
This method enables the low-cost production of high-quality grey board paper, reduces energy consumption, improves fiber utilization, and reduces anionic waste, thus possessing both economic and environmental value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of papermaking technology, and in particular to a grey board paper and its preparation method. Background Technology
[0002] Grey board is a rigid paperboard made primarily from recycled waste paper (such as ONP / OCC) through processes including pulping, refining, pressing, and drying. Domestic grey board production capacity exceeds 80 million tons per year. Traditionally, the surface pulp relies on DIP deinking pulp, which suffers from high costs, low yield (70%–75%), and high energy consumption. In contrast, ONP / OCC, as a major source of domestic waste paper, offers advantages such as a wide availability of fiber, lower prices, and complementary strengths. Summary of the Invention
[0003] In view of the above problems, this application provides a method for preparing greyboard paper surface layer pulp using ONP / OCC. The method uses high-concentration ONP / OCC pulp mixture to enhance fiber dissociation, reduce energy consumption, and reduce anionic waste. It can prepare high-quality surface layer pulp at low cost, and has both economic and environmental value.
[0004] The first aspect of this application provides a method for preparing grey board paper, comprising the following steps:
[0005] Preparation of slurry:
[0006] Using waste book paper as raw material, the pulp undergoes shredding, high-consistency slag removal, fine screening, heavy slag removal, and multi-plate concentration to obtain ONP pulp.
[0007] Pulp preparation:
[0008] Mix 50% OCC pulp with 50% ONP pulp, then spiral concentrate, preheat, thermally disperse, and finally grind in a disc mill to obtain the surface layer pulp for grey board paper.
[0009] The ONP pulp has a hue of L: 80-85, an a value of 0-1, and a B value of 3-5; the OCC pulp has a hue of L: 63-65, an a value of 4-5, and a B value of 14-16; the grey board paper surface layer pulp has a hue of L: 70-71, an a value of 3-3.9, and a B value of 10-12.
[0010] The first and second core layer pulps of greyboard paper are made of 34% wood pulp, 37% OCC pulp, 22% recycled slag pulp, and 7% recycled sludge.
[0011] Use 30% OCC long fiber pulp and 70% OCC short fiber pulp as the bottom pulp for grey board paper;
[0012] Copy:
[0013] The pulp is dewatered and shaped in the wire section, laminated with the face liner and core bottom, pressed and dewatered in the pressing section, and dried in the drying section before being made into paper.
[0014] The thermal disperser uses the relative movement between the rotor and stator to knead the high-concentration slurry heated by steam, dispersing heat-fusible impurities such as adhesives and paraffin into fine particles without affecting the paper machine system or the quality of the finished paper.
[0015] Unlike existing technologies, OCC and ONP pulps are mixed in a thermal dispersion system. This process transforms hard-to-remove adhesives, paraffin wax, and other substances in the pulp into fine particles, which are then evenly dispersed in the pulp. This reduces the impact of the pulp on the paper and improves the quality of the finished paper.
[0016] Furthermore, the pulping is performed intermittently, with a pulp concentration of 3-5%, a pulping time of 12 minutes, and a pulping temperature of 70°C.
[0017] Intermittent pulping provides high controllability of the pulp, allowing for independent and precise setting of pulping time, temperature, and concentration. Process parameters are consistent for each batch, resulting in uniform fiber disintegration and the absence of unpulped paper scraps and pulp clumps. Furthermore, intermittent hydraulic pulpers offer superior impurity removal, ensuring complete separation of impurities.
[0018] Furthermore, the concentration of the high-concentration slag remover is 3.0% to 5.0%. As a pre-treatment coarse slag remover, the high-concentration slag remover removes metals and stones in advance, preventing damage to subsequent equipment.
[0019] Furthermore, the concentration of the fine screening is 1.0% to 2.0%. The purpose of fine screening is to remove fine adhesives, hot melt adhesive particles, plastic film fragments, and other small harmful impurities, which helps to improve the appearance of the paper.
[0020] Furthermore, the concentration of the heavy slag removal process is 0.8% to 1.2%. The purpose of heavy slag removal is to specifically remove fine, high-density, hard impurities, protect all equipment, significantly reduce spare parts wear, and further eliminate paper quality defects.
[0021] Furthermore, the multi-disc thickener has a processing concentration of 0.8–1.2% and an outlet concentration of 8–12%. The multi-disc thickener concentrates low-concentration slurry to a medium concentration for subsequent equipment processing.
[0022] Furthermore, the inlet concentration of the spiral concentrator is 12-18%, and the outlet concentration is 28-30%.
[0023] Furthermore, the preheating and thermal dispersion temperature is 90–105°C. The high-concentration slurry heated with steam is kneaded to disperse heat-fusible impurities such as adhesives and paraffin into fine particles, while simultaneously enhancing the mixing effect.
[0024] Furthermore, the concentration of the disc mill is 3-5%; the inlet freeness of the disc mill is 30-35°SR, and the outlet freeness is 40-45°SR. The disc mill causes the pulp fibers to separate and filamentize; the toothed discs shear and knead the fibers, peeling away the outer layer of the fiber walls to produce a large number of microfibers. At the same time, the mechanical force causes the fibers to absorb water and swell, changing the pulp's water filtration performance.
[0025] The second aspect of this application provides a grey board paper, wherein the high-flatness grey board paper is prepared using the method described in the first aspect of this application.
[0026] The above description of the invention is merely an overview of the technical solution of this application. In order to enable those skilled in the art to better understand the technical solution of this application and to implement it based on the textual description, and to make the above-mentioned objectives and other objectives, features and advantages of this application easier to understand, the following description is based on the specific embodiments of this application. Detailed Implementation
[0027] To explain in detail the technical content, structural features, objectives, and effects of the technical solution, the following detailed description is provided in conjunction with specific embodiments.
[0028] To illustrate the possible application scenarios, technical principles, implementable specific solutions, and achievable objectives and effects of this application in detail, the following description is provided in conjunction with the specific embodiments listed. The embodiments described herein are merely illustrative of the technical solutions of this application and are therefore intended only as examples, not as limiting the scope of protection of this application.
[0029] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.
[0030] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.
[0031] In the description of this application, the term "and / or" is used to describe the logical relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A exists, B exists, and A and B exist simultaneously. Additionally, the character " / " in this document generally indicates that the preceding and following objects have an "or" logical relationship.
[0032] In this application, terms such as “first” and “second” are used only to distinguish one entity or operation from another, and do not necessarily require or imply any actual quantity, hierarchy or order relationship between these entities or operations.
[0033] Unless otherwise specified, the use of terms such as “comprising,” “including,” “having,” or other similar expressions in this application is intended to cover non-exclusive inclusion, which does not exclude the presence of additional elements in a process, method, or product that includes the stated elements, such that a process, method, or product that includes a list of elements may include not only those defined elements but also other elements not expressly listed, or elements inherent to such a process, method, or product.
[0034] As understood in the Examination Guidelines, in this application, expressions such as "greater than," "less than," and "exceeding" are understood to exclude the stated number; expressions such as "above," "below," and "within" are understood to include the stated number. Furthermore, in the description of the embodiments in this application, "multiple" means two or more (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups" and "multiple times," unless otherwise explicitly specified.
[0035] The reusable sludge described in this application is a type of sludge that has undergone a series of treatments, such as filtration, fermentation and deodorization, and white water thickening, to make it more active and better adsorbed onto fibers before being reused in waste paper pulp.
[0036] The first aspect of this application provides a method for preparing grey board paper, comprising the following steps:
[0037] Preparation of slurry:
[0038] Using waste book paper as raw material, the pulp undergoes shredding, high-consistency slag removal, fine screening, heavy slag removal, and multi-plate concentration to obtain ONP pulp.
[0039] Pulp preparation:
[0040] Mix 50% OCC pulp with 50% ONP pulp, then concentrate in a spiral, thermally disperse, and finally mill in a disc to obtain the surface layer pulp for grey board paper.
[0041] The ONP pulp has a hue of L: 80-85, an a value of 0-1, and a B value of 3-5; the OCC pulp has a hue of L: 63-65, an a value of 4-5, and a B value of 14-16; the grey board paper surface layer pulp has a hue of L: 70-71, an a value of 3-3.9, and a B value of 10-12.
[0042] The first and second core layer pulps of greyboard paper are made of 34% wood pulp, 37% OCC pulp, 22% recycled slag pulp, and 7% recycled sludge.
[0043] Use 30% OCC long fiber pulp and 70% OCC short fiber pulp as the bottom pulp for grey board paper;
[0044] Copy:
[0045] The pulp is dewatered and shaped in the wire section, laminated with the face liner and core bottom, pressed and dewatered in the pressing section, and dried in the drying section before being made into paper.
[0046] The thermal disperser uses the relative movement between the rotor and stator to knead the high-concentration slurry heated by steam, dispersing heat-fusible impurities such as adhesives and paraffin into fine particles without affecting the paper machine system or the quality of the finished paper.
[0047] Unlike existing technologies, OCC and ONP pulps are mixed in a thermal dispersion system. This process transforms hard-to-remove adhesives, paraffin wax, and other substances in the pulp into fine particles, which are then evenly dispersed in the pulp. This reduces the impact of the pulp on the paper and improves the quality of the finished paper.
[0048] Furthermore, using domestic waste OCC as raw material, OCC pulp is obtained after being crushed, descaled at high concentration, coarsely screened, and descaled at low concentration in a pulping OCC line. The OCC pulp is then separated into short fibers and long fibers by a sieve. The long fibers are then finely screened, concentrated in multiple discs, and then milled to obtain OCC long fiber pulp. The short fibers are then descaled at light concentration and concentrated in multiple discs to obtain OCC short fiber pulp.
[0049] Furthermore, wood chips and refined wood chips are used as raw materials, and wood chips are produced by feeding, hot grinding, pulping, screening, and concentration.
[0050] Furthermore, paper pulp residue is used as raw material, and recycled pulp residue is obtained through disc milling, low-consistency slag removal, fine screening, concentration, and disc milling.
[0051] Furthermore, the pulping is performed intermittently, with a pulp concentration of 3-5%, a pulping time of 12 minutes, and a pulping temperature of 70°C.
[0052] Intermittent pulping provides high controllability of the pulp, allowing for independent and precise setting of pulping time, temperature, and concentration. Process parameters are consistent for each batch, resulting in uniform fiber disintegration and the absence of unpulped paper scraps and pulp clumps. Furthermore, intermittent hydraulic pulpers offer superior impurity removal, ensuring complete separation of impurities.
[0053] Furthermore, the concentration of the high-concentration slag remover is 3.0% to 5.0%. As a pre-treatment coarse slag remover, the high-concentration slag remover removes metals and stones in advance, preventing damage to subsequent equipment.
[0054] Furthermore, the concentration of the fine screening is 1.0% to 2.0%. The purpose of fine screening is to remove fine adhesives, hot melt adhesive particles, plastic film fragments, and other small harmful impurities, which helps to improve the appearance of the paper.
[0055] Furthermore, the concentration of the heavy slag removal process is 0.8% to 1.2%. The purpose of heavy slag removal is to specifically remove fine, high-density, hard impurities, protect all equipment, significantly reduce spare parts wear, and further eliminate paper quality defects.
[0056] Furthermore, the multi-disc thickener has a processing concentration of 0.8–1.2% and an outlet concentration of 8–12%. The multi-disc thickener concentrates low-concentration slurry to a medium concentration for subsequent equipment processing.
[0057] Furthermore, the inlet concentration of the spiral concentrator is 12-18%, and the outlet concentration is 28-30%.
[0058] Furthermore, the temperature for thermal dispersion is 90–105°C. The high-concentration slurry heated with steam is kneaded to disperse heat-fusible impurities such as adhesives and paraffin wax into fine particles, while simultaneously enhancing the mixing effect.
[0059] Furthermore, the concentration of the disc mill is 3-5%; the inlet freeness of the disc mill is 30-35°SR, and the outlet freeness is 40-45°SR. The disc mill causes the pulp fibers to separate and filamentize; the toothed discs shear and knead the fibers, peeling away the outer layer of the fiber walls to produce a large number of microfibers. At the same time, the mechanical force causes the fibers to absorb water and swell, changing the pulp's water filtration performance.
[0060] Furthermore, a dry strength agent is added to the pulp at a rate of 10–20 kg / t.
[0061] Furthermore, the difference in dryness between the core layer before lamination and the liner layer before lamination is less than 3%.
[0062] The second aspect of this application provides a grey board paper, wherein the high-flatness grey board paper is prepared using the method described in the first aspect of this application.
[0063] Furthermore, the thickness of the grey board paper per 100 square meters is ≥17 mils, the interlayer bonding strength is ≥130J / ㎡, the hue L: 64-66, the a value is 2~3, and the b value is 9.5~11.5.
[0064] In this embodiment, the vacuum and pulp pump frequencies were optimized, and the core layer dewatering was adjusted, with the water line maintained in the second and third low-vacuum dewatering tanks. The core layer high vacuum was set at -18 to -30 kPa, the liner layer high vacuum at -20 to 40 kPa, the liner layer pulp pump frequency at 62%, the core layer pulp pump frequency at 59%, the wire speed ratio of the surface layer, liner layer, and core layer at 0.98, and the bottom layer wire speed ratio at 0.96. This achieved reduced wire density, enhanced dewatering, and ensured good paper uniformity. Furthermore, the dryness before core layer lamination was 17.5%, and the dryness before liner layer lamination was 15.9%, with a lamination dryness difference of <3%, which is beneficial for layer-to-layer lamination and results in optimal strength.
[0065] In this embodiment, the linear pressure of the wire section is 20 bar for roller 1, 30 bar for roller 2, 35 bar for roller 2, 63 bar for roller 3, 68 bar for roller 4, and 72 bar for roller 5. Sufficient linear pressure ensures the flatness of the paper.
[0066] Example:
[0067] ONP pulping process: Using domestic waste book paper as raw material, the pulp undergoes disintegration, high-consistency deslagging (slagging concentration set at 3-5%), fine screening (concentration 1-2%), heavy deslagging (concentration 0.6-1.2%), and multi-plate concentration (inlet concentration 0.8-1.2%) to obtain ONP pulp with a concentration of 12%. The ONP pulp has a hue of L: 80-85, a value of 0-1, and a B value of 3-5. Intermittent pulping is used, with a pulp concentration of 3-5%, a disintegration time of 12 minutes, and a disintegration temperature of 70℃.
[0068] OCC pulping process: Using domestic waste OCC as raw material, the pulp undergoes crushing, slag removal, drum screen screening, high-consistency sand remover, coarse screening, flotation slag remover, impurity separation by impurity separator, and low-consistency slag removal in the OCC pulping line to obtain OCC pulp. The OCC pulp is then separated into short fibers and long fibers using a sieve. The short fibers undergo light slag removal by a light slag remover and multi-disc concentration to obtain OCC short fiber pulp. The long fibers undergo three-stage fine screening, multi-disc concentration, and disc milling to obtain OCC long fiber pulp. The OCC pulp has a hue of L: 63-65, a value of 4-5, and a B value of 14-16.
[0069] Wood pulp preparation
[0070] Using branch wood chips and refined wood chips as raw materials, a wood pulp mixture is prepared through feeding, hot grinding of wood chips, pulping, screening, and concentration. Specifically:
[0071] Wood chip conveying: 20% branch wood chips and 80% eucalyptus wood chips with a moisture content of 40-50% are conveyed from the silo to the oscillating screen via a double screw conveyor and belt conveyor;
[0072] Crushing and impurity removal: The wood chips are screened by a vibrating screen to remove bark and large wood blocks. The screened wood chips are then crushed by a drum crusher and sent to the wood chip cooking system by a bucket elevator and belt conveyor.
[0073] Steam cooking: High-pressure steam cooking of wood chips increases the moisture content of the wood and softens the wood chips again;
[0074] Wood chip hot milling: After being cooked in the cooking chamber, the wood chips are fed into the hot mill through the feeding screw, and the hot mill grinds the wood chips into single fibers;
[0075] Hot grinding pulp dilution: The hot-ground wood pulp mixture is adjusted to the concentration by a dilution screw and sent to the anti-submersion tank;
[0076] Hot refining and de-flaking: After de-flaking, the wood pulp is thickened and sent to a disc mill for refining;
[0077] Disc milling: The thermo-refined pulp is refined using a dual-disc mill to cut and dissociate fibers to achieve the pulping requirements;
[0078] Fine screening: The pulp from the double-disc mill outlet is diluted and thickened, and then sent to the wood pulp fine screen for screening to obtain wood pulp.
[0079] Preparation of recycled pulp residue:
[0080] Using paper pulp residue as raw material, recycled pulp residue is obtained through disc milling, low-consistency residue removal, fine screening, concentration, and disc milling.
[0081] The low-concentration slag remover is a three-stage type, with the following parameters:
[0082]
[0083] The fine screening is a two-stage process:
[0084] First-stage fine screening: bar gap: 0.27mm, feed slurry concentration: 1.09%, feed pressure: 0.15-0.3MPa, slag discharge rate: 24-28%;
[0085] Two-stage fine screening: bar gap 0.27mm, feed slurry concentration: 1.08%, feed pressure 0.15-0.3MPa, slag discharge rate 24-28%.
[0086] Greyboard paper preparation
[0087] Mix 18% OCC pulp and 18% ONP pulp in a 1:1 ratio, spiral concentrate to a mixed pulp concentration of 28-30%, then heat the mixed pulp to 90-105℃, followed by thermal dispersion and disc milling. The disc milling treatment concentration is 3-5%. The inlet freeness of the disc mill is 30-35°SR, and the outlet freeness is 40-45°SR. Add 10-20 kg / t of dry strength agent to obtain greyboard paper surface layer pulp. The hue of the greyboard paper surface layer pulp is L: 70-71, a value: 3-3.9, and B value: 10-12.
[0088] The pulp consists of 34% wood pulp, 37% OCC pulp, 22% recycled slag pulp, and 7% recycled sludge; 10-20 kg / t of dry strength agent is added as the first and second core layer pulps for grey board paper.
[0089] Use 30% OCC long fiber pulp, 70% OCC short fiber pulp, and add 10-20 kg / t of dry strength agent as the bottom pulp for grey board paper;
[0090] Copy:
[0091] The above pulp is dewatered and shaped in the wire section, laminated with the face and core, pressed and dewatered in the pressing section, and dried in the drying section to produce high-flatness grey board paper.
[0092] Copy:
[0093] The pulp is dewatered and shaped in the wire section, laminated with the face liner and core bottom, pressed and dewatered in the pressing section, and dried in the drying section before being made into paper.
[0094] By adjusting the process, a high-concentration blend of ONP / OCC was used to prepare the surface layer pulp for grey board paper. The color met the requirements. This eliminates the traditional reliance on DIP deinking pulp for grey board paper surface layers. Our plant has an annual grey board paper production capacity of 200,000 tons; surface layer pulp accounts for 10%. The surface layer pulp consumption is 20,000 tons, which translates to a waste paper demand of 24,000 tons, half of which is OCC waste paper and half is ONP book paper. Saving 300 yuan per ton of waste paper generates a benefit of 3.6 million yuan.
[0095] Finally, it should be noted that although the above embodiments have been described in the description of this application, this should not limit the scope of patent protection of this application. Any technical solutions that are based on the essential concept of this application, utilize the content described in this application's description to make equivalent structural or procedural substitutions or modifications, or directly or indirectly implement the technical solutions of the above embodiments in other related technical fields, are all included within the scope of patent protection of this application.
Claims
1. A method for preparing grey board paper, characterized in that, Includes the following steps: Preparation of slurry: Using waste book paper as raw material, the pulp undergoes shredding, high-consistency slag removal, fine screening, heavy slag removal, and multi-plate concentration to obtain ONP pulp. Pulp preparation: Mix 50% OCC pulp with 50% ONP pulp, then spiral concentrate, preheat, thermally disperse, and finally grind in a disc mill to obtain the surface layer pulp for grey board paper. The ONP pulp has a hue of L: 80-85, an a value of 0-1, and a B value of 3-5; the OCC pulp has a hue of L: 63-65, an a value of 4-5, and a B value of 14-16; the grey board paper surface layer pulp has a hue of L: 70-71, an a value of 3-3.9, and a B value of 10-12. The first and second core layer pulps of grey board paper are made of 34% wood pulp, 37% OCC pulp, 22% recycled slag pulp, and 7% recycled sludge. Use 30% OCC long fiber pulp and 70% OCC short fiber pulp as the bottom pulp for grey board paper; Copy: The above pulp is dewatered and shaped in the wire section, laminated with the face liner and core bottom, pressed and dewatered in the pressing section, and dried in the drying section before being made into paper.
2. The preparation method according to claim 1, characterized in that, The pulping process is intermittent, with a pulp concentration of 3-5%, a pulping time of 12 minutes, and a pulping temperature of 70℃.
3. The preparation method according to claim 1, characterized in that, The concentration of the high-concentration slag removal agent is 3.0–5.0%.
4. The preparation method according to claim 1, characterized in that, The concentration used for fine screening is 1.0–2.0%.
5. The preparation method according to claim 1, characterized in that, The concentration of the heavy slag removal process is 0.8–1.2%.
6. The preparation method according to claim 1, characterized in that, The multi-disc concentration has a processing concentration of 0.8-1.2% and an outlet concentration of 8-12%.
7. The preparation method according to claim 1, characterized in that, The spiral concentrator has an inlet concentration of 12-18% and an outlet concentration of 28-30%.
8. The preparation method according to claim 1, characterized in that, The preheating and heat dispersion temperatures are 90–105°C.
9. The preparation method according to claim 1, characterized in that, The concentration obtained from the disc mill is 3-5%; the inlet percussion degree of the disc mill is 30-35°SR, and the outlet percussion degree is 40-45°SR.
10. A type of grey board paper, characterized in that, The high-flatness grey board paper is prepared using the method described in any one of claims 1 to 9.