Liquid crystal display device and method for manufacturing liquid crystal display device
By using an electrostatic discharge (ESD) layer composed of a specific material between the array substrate and the opposing substrate, the problems of low productivity and high cost of embedded touch LCD devices are solved, achieving a more efficient manufacturing process and lower manufacturing cost, while maintaining touch sensitivity and image quality.
Patent Information
- Application Number
- CN202611242209.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-11
- Filing Date
- 2020-11-10
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional embedded touch LCD devices suffer from low productivity and high manufacturing costs, mainly due to the need to form additional inorganic insulating layers and expensive polarizers to prevent static electricity and gate metal reflections.
An electrostatic discharge layer is formed using In2O3 and SnO2 as the main materials and at least one of SiO2, ZrO2, HfO2, Nb2O5 and Ta2O5 as the dopant material. The thin-film resistance is in the range of 106.5 Ω/sq to 109 Ω/sq. It is used between the array substrate and the opposite substrate to replace the traditional inverted panel structure.
It improved productivity, reduced manufacturing costs, and maintained the accuracy of touch sensing and image brightness, avoiding additional equipment investment.
Smart Images

Figure CN123113189A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese Patent Application No. 202011247762.3, filed on November 10, 2020, entitled "Liquid Crystal Display Apparatus and Method for Manufacturing Liquid Crystal Display Apparatus".
[0002] Cross-references to related applications
[0003] This application claims priority to Korean Patent Application No. 10-2019-0143396, filed on November 11, 2019, in the Republic of Korea, the entire contents of which are incorporated herein by reference for all purposes, as if fully set forth herein. Technical Field
[0004] This invention relates to liquid crystal display (LCD) devices, and more particularly to touch LCD devices. Background Technology
[0005] With the rapid transition to the information society, the demand for display devices for displaying images is increasing in various forms, and recently, various flat panel display devices such as liquid crystal display (LCD) devices, plasma display panel (PDP) devices, and organic light-emitting diode (OLED) devices are being used in various fields.
[0006] LCD devices, one type of flat panel display, have technical advantages such as small size, light weight, thinness and low power consumption, and are widely used in many applications.
[0007] Recently, touch sensing functionality has become increasingly necessary for various information display electronic devices such as laptops and smartphones, leading to the application of touch sensors in LCD devices. In particular, in-cell touch LCD devices, in which an LCD panel equipped with a touch sensor is incorporated, are becoming widely used.
[0008] Typically, conventional embedded touch LCD devices are configured with an inverted panel structure. In this structure, an array substrate is positioned adjacent to the display surface to which touch events are input, while a counter substrate is positioned at the bottom of the LCD device. A transparent conductive layer is formed on the outer surface of the counter substrate to prevent electrostatic discharge (ESD) during automated probe testing, and a polarizing plate with an ESD protection layer is attached to the outer surface of the array substrate for touch sensing and ESD protection. Furthermore, in the inverted panel structure, an inorganic insulating layer is additionally formed to prevent the user from recognizing reflections from the gate metal.
[0009] For conventional inverted panel structure touch LCD devices, it is necessary to form an additional inorganic insulating layer and fabricate a very expensive polarizing plate with electrostatic discharge protection, as well as additional equipment for inverting the panel. Therefore, conventional touch LCD devices suffer from problems such as low productivity and high manufacturing costs. Summary of the Invention
[0010] Therefore, the present invention relates to an LCD device that substantially eliminates one or more problems caused by the limitations and disadvantages of related technologies.
[0011] The purpose of this invention is to provide a touch LCD device that can effectively increase productivity and reduce manufacturing costs.
[0012] Additional features and advantages of this disclosure will be set forth in the description which follows, and will be apparent in part from that description, or may be learned by practice of this disclosure. The advantages of this disclosure will be realized and obtained by means of the structures particularly pointed out in the written description, claims, and drawings.
[0013] To achieve these and other advantages, and in accordance with the purposes of the invention, as embodied and broadly described herein, a liquid crystal display device includes: an array substrate comprising a first substrate disposed adjacent to a backlight source and thin-film transistors and touch electrodes disposed on the first substrate; and a opposing substrate comprising a second substrate facing the first substrate and an electrostatic discharge (ESD) layer deposited on the outer surface of the second substrate, wherein a liquid crystal layer is interposed between the first substrate and the second substrate, wherein the ESD layer is formed of a host material comprising at least one of In₂O₃ and SnO₂ and a dopant material comprising at least one of SiO₂, ZrO₂, HfO₂, Nb₂O₅, and Ta₂O₅, and the ESD layer has a density of approximately 10 μm. 6.5 Ω / sq to approximately 10 9 Thin-film resistance in Ω / sq.
[0014] In another aspect, a method of manufacturing a liquid crystal display device includes: manufacturing an array substrate comprising a first substrate disposed adjacent to a backlight source and thin-film transistors and touch electrodes disposed on the first substrate; and manufacturing a counter substrate comprising a second substrate facing the first substrate and an electrostatic discharge (ESD) layer deposited on the outer surface of the second substrate, wherein a liquid crystal layer is inserted between the first substrate and the second substrate, wherein the ESD layer is formed of a host material comprising at least one of In₂O₃ and SnO₂ and a dopant material comprising at least one of SiO₂, ZrO₂, HfO₂, Nb₂O₅ and Ta₂O₅, and the ESD layer has a density of approximately 10 μm. 6.5 Ω / sq to approximately 10 9Thin-film resistance in Ω / sq.
[0015] It should be understood that both the foregoing general description and the following detailed description are exemplary and illustrative, and are intended to provide further explanation of the claimed invention. Attached Figure Description
[0016] The accompanying drawings are included to provide a further understanding of this disclosure and are incorporated in and form a part of this specification. The drawings illustrate embodiments of the disclosure and, together with the description, serve to explain the principles of the disclosure. In the drawings:
[0017] Figure 1 This is a schematic plan view of a touch LCD device according to an embodiment of the present invention;
[0018] Figure 2 This is a schematic plan view of a liquid crystal panel according to an embodiment of the present invention;
[0019] Figure 3 This is a plan view showing a portion of the touch block of the array substrate of an LCD device according to an embodiment of the present invention;
[0020] Figure 4 This is a cross-sectional view showing a portion of the touch block of an LCD device according to an embodiment of the present invention;
[0021] Figures 5 to 7 This is a schematic cross-sectional view illustrating the process of manufacturing a touch LCD device relative to a substrate according to an embodiment of the present invention;
[0022] Figure 8 This is a graph showing the change of thin-film resistance over time in a comparative experiment;
[0023] Figure 9 and Figure 10 This is a graph showing the change of the thin-film resistance over time in Experiment 1 of the present invention;
[0024] Figure 11 This is a graph showing the transmittance versus wavelength obtained in Experiment 1 of the present invention;
[0025] Figure 12 This is a graph showing the results of the thin-film resistance obtained from the chemical resistance test in Experiment 1 of the present invention;
[0026] Figures 13 to 15 This is a graph showing the change of the thin-film resistance over time in Experiment 2 of the present invention;
[0027] Figures 16(a) to 16(f) are graphs showing the thin-film resistivity obtained from heat treatment stability and chemical resistance tests in Experiment 3 of the present invention; and
[0028] Figures 17(a) to 17(f) are graphs showing the sheet resistance obtained according to the 6090 reliability and chemical resistance test in Experiment 3 of the present invention. Detailed Implementation
[0029] Reference will now be made in detail to the embodiments, examples of which are shown in the accompanying drawings. The same or similar reference numerals may be used throughout the drawings to refer to the same or similar parts.
[0030] The touch LCD device according to the present invention may have an embedded structure in which a touch sensor is provided in the liquid crystal panel, and may operate in various capacitive touch sensing methods (e.g., self-capacitance sensing method and mutual capacitance sensing method).
[0031] In the embodiments described below, for the sake of brevity, a touch LCD device operating in a self-capacitance manner will be described by way of example.
[0032] Figure 1 This is a schematic plan view of a touch LCD device according to an embodiment of the present invention, and Figure 2 This is a schematic plan view of a liquid crystal panel according to an embodiment of the present invention.
[0033] Reference Figure 1 and Figure 2 The touch LCD device 10 according to this embodiment may include: a liquid crystal panel 100 configured to display images and provided with a touch device; and a cover window CW attached to the front surface of the liquid crystal panel 100, which serves as an image display surface (referred to as the display surface).
[0034] Although not shown in detail, the backlight unit may be located below the liquid crystal panel 100 to provide light to the liquid crystal panel 100.
[0035] An edge-lit backlight unit in which a light source (e.g., a light-emitting diode (LED)) is disposed adjacent to the liquid crystal panel 100 in the lateral direction, or a direct-lit backlight unit in which the light source is disposed below the liquid crystal panel 100, can be used as a backlight unit.
[0036] In this embodiment, the liquid crystal panel 100 may have an embedded structure, wherein a touch electrode 151, one of the self-capacitive touch devices, is provided in the panel. For example, the touch electrode 151 may be provided in one of the two substrates AS and OS of the liquid crystal panel 100.
[0037] In the embedded liquid crystal panel 100, a common voltage can be applied to the touch electrode 151, which has a touch sensing function, during the image display period of the liquid crystal panel 100, so that the touch electrode 151 serves as a common electrode 151. During the touch sensing period between image display periods, a touch drive signal can be applied to the touch electrode 151, and in this case, the touch electrode 151 can serve as a touch sensing electrode.
[0038] The embedded liquid crystal panel 100 may include: an array substrate AS disposed adjacent to a backlight unit to serve as a lower substrate; a relative substrate OS disposed adjacent to an image display surface to serve as an upper substrate opposite to the array substrate AS; and a liquid crystal layer disposed between the array substrate AS and the relative substrate OS.
[0039] In one embodiment, the liquid crystal panel 100 may be configured to have an array substrate AS, wherein pixel electrodes and touch electrodes 151 (i.e., common electrodes 151) are formed as electrodes for generating an electric field for driving the liquid crystal layer.
[0040] For example, a liquid crystal panel operating in in-plane switching (IPS) or advanced high-performance IPS (AH-IPS) mode can be used as liquid crystal panel 100. In this embodiment, for the sake of simplicity, a liquid crystal panel operating in AH-IPS mode to generate edge fields will be referred to as an example of liquid crystal panel 100.
[0041] The liquid crystal panel 100 may include a display area AA for displaying images and a non-display area NA disposed adjacent to the display area AA. The display area AA may include a plurality of pixel areas arranged in a matrix shape along the row and column directions.
[0042] The liquid crystal panel 100 may have multiple touch blocks TB, and in this embodiment, the touch blocks TB may be arranged in a matrix shape along the row and column directions. Each touch block TB may be composed of multiple pixel regions that are adjacent to each other as a unit group along the row and column directions.
[0043] In the array substrate AS of the liquid crystal panel 100, the touch electrode 151 (i.e., the common electrode 151) can be patterned and formed in each touch block TB through a patterning process.
[0044] The common electrodes 151 in adjacent touch blocks TB can be physically spaced apart from each other, and therefore, the common electrodes 151 in each touch block TB can be set as an isolation pattern.
[0045] Therefore, the common electrode 151 in adjacent touch blocks TB can be electrically disconnected from each other, and thus, the touch blocks TB can be operated individually or independently.
[0046] Touch lines SL extending in a specific direction can be formed in the array substrate AS of the liquid crystal panel 100, and the touch lines SL can be connected to touch blocks TB respectively. For example, the touch lines SL can be formed parallel to the column direction or the vertical direction, which is the extension direction of the data lines.
[0047] Each touch line SL can be connected to the common electrode 151 in the corresponding touch block TB through a contact hole TCH formed in the corresponding touch block TB, and can be used to transmit a drive signal to the common electrode 151.
[0048] During an image display period (e.g., per frame), a common voltage can be applied to the common electrode 151 via the touch line SL. Therefore, in each pixel region of the touch block TB, an electric field can be generated between the pixel electrode and the common electrode 151, and such an electric field can be controlled to drive the liquid crystal layer and thus display an image.
[0049] During the touch sensing period between image display periods (e.g., the blank period between adjacent frames), a touch drive signal can be applied to the common electrode 151 (i.e., touch electrode 151) via the touch line SL.
[0050] Additionally, the sensing signal can be detected by the common electrode 151 and applied to the touch line SL, and in this case, a sensing signal is generated to contain information related to the change in electrostatic capacitance of each touch block TB caused by a touch event. The sensing signal can be used to determine whether a touch event provided by the user exists.
[0051] As described above, the common electrode 151 in the touch block TB can be used not only as an electrode for generating an electric field, but also as a touch electrode 151 for sensing touch events. Therefore, an embedded structure liquid crystal panel 100 can be realized and the thickness of the liquid crystal panel 100 can be reduced.
[0052] In this embodiment, the opposing substrate OS facing the array substrate AS can be configured to have a smaller size than the array substrate AS. For example, the opposing substrate OS can be configured to expose a portion of the edge region of the array substrate AS. Specifically, the opposing substrate OS may not cover the lower edge region of the array substrate AS in which the panel driving circuit 300 is disposed and which overlaps with the non-display region NA.
[0053] The panel driving circuit 300 can be manufactured, for example, in the form of an integrated circuit (IC), and can then be mounted on the non-display area NA of the array substrate AS in a chip-on-glass (COG) manner.
[0054] The panel driving circuit 300 can be configured to generate various driving signals required to operate the liquid crystal panel 100, and to provide such driving signals to the liquid crystal panel 100. In other words, the operation of the liquid crystal panel 100 can be controlled by the driving signals provided from the panel driving circuit 300.
[0055] For example, the panel driving circuit 300 can output a gate signal to a gate line and a data signal to a data line. Furthermore, the panel driving circuit 300 can output a common voltage or a touch driving signal to the touch line SL. The panel driving circuit 300 can receive a sensing signal generated in the common electrode 151 via the touch line SL.
[0056] The panel driving circuit 300 may include a data driving circuit, a gate driving circuit, and a touch sensing circuit, wherein the data driving circuit, the gate driving circuit, and the touch sensing circuit are configured to drive a data line, a gate line, and a touch line, respectively. In one embodiment, the data driving circuit, the gate driving circuit, and the touch sensing circuit may be configured as separate integrated circuits. In another embodiment, an integrated circuit in which at least two of these circuits are integrated may be used. In this embodiment, a single integrated circuit in which all the circuits of the data driving circuit, the gate driving circuit, and the touch sensing circuit are integrated may be used as the panel driving circuit 300.
[0057] As another example, the panel driving circuit 300, which is configured as an IC, can be mounted on a flexible circuit film and can be connected to the liquid crystal panel 100 through the flexible circuit film.
[0058] In the following text, reference will be made to Figures 3 to 4 The structure of the LCD device 10 according to this embodiment will be described in more detail.
[0059] Figure 3 This is a plan view showing a portion of the touch block of the array substrate of an LCD device according to an embodiment of the present invention. Figure 4 This is a cross-sectional view showing a portion of the touch block of an LCD device according to an embodiment of the present invention.
[0060] Reference Figure 3 and Figure 4An LCD device 10 according to an embodiment of the present invention may include a liquid crystal panel 100, a first polarizing plate 201 attached to the bottom surface of the liquid crystal panel 100, a second polarizing plate 202 attached to the top surface of the liquid crystal panel 100, and a cover window CW attached to the top surface of the second polarizing plate 202. Here, the bottom surface and the top surface of the liquid crystal panel 100 may be the outer surfaces of the liquid crystal panel 100 that are opposite to each other and positioned adjacent to the backlight unit and the image display surface, respectively.
[0061] Thin-film transistors T and touch electrodes 151 serving as common electrodes can be formed in the array substrate AS of the liquid crystal panel 100. In addition, color filter patterns 130 can be formed in the array substrate AS.
[0062] A gate line GL may be formed on the top or inner surface of the first substrate 101 to extend along a first direction (e.g., a row direction). A gate electrode 111 may be formed and connected to the gate line GL. The gate line GL and the gate electrode 111 may be formed from the same metal material using the same process. The gate line GL and the gate electrode 111 may be formed to have a single-layer or multi-layer structure, wherein the single-layer or multi-layer structure comprises at least one of, for example, aluminum (Al), aluminum alloys (e.g., AlNd), copper (Cu), molybdenum (Mo), molybdenum alloys (e.g., MoTi), and chromium (Cr).
[0063] A gate insulating layer 113, serving as an insulating layer, may be formed on the gate line GL and the gate electrode 111. The gate insulating layer 113 may be formed of at least one of inorganic insulating materials (e.g., silicon oxide and silicon nitride) or may include at least one of inorganic insulating materials (e.g., silicon oxide and silicon nitride).
[0064] A semiconductor layer 115 may be formed on the gate insulating layer 113 corresponding to the gate electrode 111. The semiconductor layer 115 may be formed of at least one of, for example, amorphous silicon and oxide semiconductor materials, or may include at least one of, for example, amorphous silicon and oxide semiconductor materials.
[0065] Source electrodes 121 and drain electrodes 123 spaced apart from each other can be formed on semiconductor layer 115. Data lines DL can be formed on gate insulating layer 113 to extend along a second direction (e.g., column direction) intersecting the first direction. Source electrodes 121, drain electrodes 123, and data lines DL can be formed from the same metal material using the same process. Data lines DL, source electrodes 121, and drain electrodes 123 can be formed to have a single-layer or multi-layer structure, wherein the single-layer or multi-layer structure comprises at least one of, for example, aluminum (Al), aluminum alloys (e.g., AlNd), copper (Cu), molybdenum (Mo), molybdenum alloys (e.g., MoTi), and chromium (Cr).
[0066] Multiple pixel regions P can be defined in a matrix shape by intersecting gate lines GL and data lines DL.
[0067] In each pixel region P, the gate electrode 111, the semiconductor layer 115, the source electrode 121, and the drain electrode 123 can form a thin film transistor T.
[0068] In this embodiment, an inverted interleaved or bottom-gate structure transistor is shown as an example of a thin-film transistor T. However, in this embodiment, a coplanar or top-gate structure thin-film transistor can be configured as thin-film transistor T, and in this case, the semiconductor layer can be formed of or include at least one of polycrystalline silicon or oxide semiconductor materials.
[0069] A first protective layer 125, serving as an insulating layer, can be formed over the entire area of the first substrate 101 to cover the thin-film transistor T. The first protective layer 125 can be formed of or include at least one of an inorganic insulating material or an organic insulating material. Here, the inorganic insulating material may include, for example, silicon oxide, silicon nitride, etc., and the organic insulating material may include photoacrylic acid materials, benzocyclobutene, etc.
[0070] On the first protective layer 125, a color filter pattern 130 can be formed corresponding to each pixel region P.
[0071] In the LCD panel 100, such as Figure 4 As exemplarily shown, pixel regions P of red (R), green (G) and blue (B) can be alternately arranged along a specific direction (e.g., row direction), and color filter patterns 130 of red (R), green (G) and blue (B) can be patterned and formed in the pixel regions P of red (R), green (G) and blue (B) to display their own colors.
[0072] In this embodiment, the LCD device 10 has been described as having a thin-film transistor on-chip (COT) structure in which a color filter pattern 130 is formed on a thin-film transistor T of an array substrate AS. As another example, the LCD device 10 may be configured to have a structure in which the color filter pattern 130 is set as part of a substrate OS.
[0073] A second protective layer 135, serving as an insulating layer, can be formed over the entire area of the first substrate 101 to cover the color filter pattern 130. The second protective layer 135 may be formed of at least one of inorganic insulating materials or organic insulating materials, or may include at least one of inorganic insulating materials or organic insulating materials.
[0074] A touch line SL can be formed on the second protective layer 135. In the touch block TB, the touch line SL can extend along the extension direction of the data line DL and can overlap with the data line DL. When the touch line SL is set to overlap with the data line DL, which is one of the non-display elements, the width of the touch line SL can be maximized without reducing the aperture ratio due to the presence of the touch line SL, thereby enabling the touch line SL to have reduced resistance.
[0075] A third protective layer 137, serving as an insulating layer, can be formed over the entire area of the first substrate 101 to cover the touch line SL. The third protective layer 137 may be formed of at least one of inorganic insulating materials or organic insulating materials, or may include at least one of inorganic insulating materials or organic insulating materials.
[0076] A pixel electrode 140 may be formed on the third protective layer 137 and in each pixel region P. Here, the pixel electrode 140 may be formed to be substantially plate-shaped in each pixel region P. The pixel electrode 140 may be connected to the drain electrode 123 of the thin-film transistor T in the corresponding pixel region P. For example, the pixel electrode 140 may contact and connect to the drain electrode 123 through a drain contact hole CHd formed to penetrate the first protective layer 125, the second protective layer 135, and the third protective layer 137.
[0077] A fourth protective layer 143, serving as an insulating layer, may be formed on the pixel electrode 140. The fourth protective layer 143 may be formed of at least one of inorganic insulating materials or organic insulating materials, or may include at least one of inorganic insulating materials or organic insulating materials.
[0078] Touch electrodes 151 (i.e., common electrodes 151) can be formed on the fourth protective layer 143 and in each touch block TB. The common electrodes 151, in combination with the pixel electrodes 140, can generate an edge field for changing the orientation of liquid crystal molecules.
[0079] In order to generate an edge field, the common electrode 151 may include a plurality of strip electrode patterns 152 facing the pixel electrode 140 corresponding to each pixel region P, and openings may be formed between the electrode patterns 152.
[0080] Regarding the arrangement or configuration of the common electrode 151 and the pixel electrode 140, in another embodiment, the common electrode 151 may be disposed in each touch block TB in a substantially plate-like manner, while the pixel electrode 140, which consists of multiple electrode patterns, may be disposed on the common electrode 151, wherein an insulating layer is inserted between the common electrode 151 and the pixel electrode 140.
[0081] In other embodiments, each of the common electrode 151 and the pixel electrode 140 may be formed with an electrode pattern, and the common electrode 151 and the pixel electrode 140 may be disposed on the same layer or may be disposed with an insulating layer inserted therebetween.
[0082] A first alignment layer 191 may be formed on the top surface of the array substrate AS to determine the initial orientation of the liquid crystal molecules. In other words, the first alignment layer 191 may be formed on the common electrode 151. The first alignment layer 191 may be formed of, for example, polyimide or include, for example, polyimide.
[0083] In this embodiment, the first polarizing plate 201 can be attached to the bottom surface or the outer surface of the array substrate AS. Here, the first polarizing plate 201 can be directly attached to the bottom surface of the first substrate 101 by means of an adhesive member.
[0084] For example, a typical polarizing plate can be used as the first polarizing plate 201, and in this case, the first polarizing plate 201 may include a polarizing layer and a protective layer disposed on opposite surfaces (i.e., bottom and top surfaces) of the polarizing layer, but an additional electrostatic discharge (ESD) prevention layer may not be required. The first polarizing plate 201 may have approximately 10 12 The sheet resistance is Ω / sq or higher, and in this case, the first polarizing plate 201 cannot be used as an electrostatic discharge prevention element because the first polarizing plate 201 has essentially insulating properties.
[0085] The relative substrate OS can be combined with the array substrate AS and can face the array substrate AS, wherein a liquid crystal layer 105 is inserted between the relative substrate OS and the array substrate AS. The relative substrate OS can be disposed adjacent to the display surface of the liquid crystal panel 100, which is used to display images and input touch events to the display surface of the liquid crystal panel 100.
[0086] The substrate OS may include columnar spacers 160 disposed on the bottom or inner surface of the second substrate 102, which are used to maintain the cell gaps or thickness of the liquid crystal layer 105. The columnar spacers 160 may be disposed corresponding to non-display elements (e.g., thin-film transistors T, data lines DL, gate lines GL, etc.) in the array substrate AS.
[0087] The columnar spacer 160 can be formed by a masking process, and for example by performing several processes including deposition, exposure, development, etching, and stripping. A heat treatment process can be performed on the columnar spacer 160 formed by the masking process.
[0088] The columnar spacer 160 can be formed to include black pigment, and in this case, the columnar spacer 160 can have a light-blocking function to prevent or suppress leaked light from entering adjacent pixel areas such as the black matrix.
[0089] A second alignment layer 192 may be formed on the inner surface of the second substrate 102 where the columnar spacer 160 is disposed. The second alignment layer 192 may be formed of, for example, polyimide or include, for example, polyimide.
[0090] The second orientation layer 192 can be formed by coating an orientation material, and thereafter, a heat treatment process can be performed. Similarly, the first orientation layer 191 can be formed by coating, and then a heat treatment process can be performed.
[0091] An anti-static layer 220 may be formed on the top or outer surface of the second substrate 102.
[0092] The electrostatic discharge (ESD) prevention layer 220 can be used to discharge static electricity generated during the manufacturing process of the LCD device 10 (e.g., including testing processes) to the outside. Since the ESD prevention layer 220 is disposed adjacent to the display surface of the LCD device 10, it must be configured to suppress interference from the electrostatic capacitance between the user's finger and the touch electrode 151 when a touch event is input through the display surface of the LCD device 10.
[0093] To achieve electrostatic discharge prevention without interfering with the touch-sensing capacitance, the electrostatic discharge prevention layer 220 in this embodiment can preferably have a depth of about 10. 6.5 Ω / sq to approximately 10 9 Thin-film resistance in the range of Ω / sq.
[0094] Regarding the appropriate range of sheet resistance, if the sheet resistance is less than 10... 6.5 If the resistance is less than Ω / sq, the anti-static layer 220 can act as a conductor, causing interference with the electrostatic capacitance generated by touch events, which may lead to difficulty in recognizing touch events. In contrast, if the layer resistance is greater than 10Ω / sq, the anti-static layer 220 can act as a conductor, thus causing interference with the electrostatic capacitance generated by touch events, and this may result in difficulty in recognizing touch events. 9 If the static electricity level is Ω / sq, then the anti-static layer 220 can act as an insulator, thereby preventing static electricity from being discharged to the outside, and therefore, defects caused by static electricity may occur.
[0095] Therefore, the electrostatic discharge (ESD) prevention layer 220 can preferably be configured as: a dielectric material that prevents interference with the touch sensing capacitance when a touch event occurs; and a conductor that prevents electrostatic discharge when an electrostatic problem exists. For example, the ESD prevention layer 220 is configured to have approximately 10 6.5 Ω / sq to approximately 10 9 Thin-film resistance in Ω / sq.
[0096] Furthermore, preferably, since the anti-static layer 220 in this embodiment is disposed adjacent to the display surface, the anti-static layer 220 can have a sufficiently high transmittance without causing any substantial change in the brightness of the image. For example, the anti-static layer 220 is configured to have a transmittance of about 97% or higher.
[0097] In order to enable the electrostatic discharge (ESD) layer 220 formed on the substrate OS to have reliable thin-film resistance and transmittance characteristics, the ESD layer 220 in this embodiment can preferably be formed of a host material containing at least one of In2O3 and SnO2 and a dopant material containing at least one of SiO2, ZrO2, HfO2, Nb2O5 and Ta2O5.
[0098] The antistatic layer 220 formed from the material may have a thickness of about 100 Å to about 300 Å.
[0099] In the anti-static layer 220, the content of the dopant material can be in the range of about 9 wt% to 15 wt%, and the content of the host material, given by subtracting the content of the dopant material from the total content, can be in the range of about 85 wt% to 91 wt%.
[0100] When one of In2O3 and SnO2 is used as the host material, the content of the dopant material can be in the range of about 12 wt% to about 15 wt%, and the content of the host material can be in the range of about 85 wt% to about 88 wt%.
[0101] When a mixture of In2O3 and SnO2 is used as the host material, the content of the dopant material can be in the range of about 9 wt% to about 11 wt%, and the content of the host material can be in the range of about 89 wt% to about 91 wt%.
[0102] As mentioned above, the content of the dopant material can vary depending on the composition of the host material, and therefore, the content of the host material can be changed.
[0103] Meanwhile, as the content of the dopant material increases, the sheet resistance of the electrostatic discharge (ESD) layer 220 increases. Even under such circumstances, by adjusting the content of the dopant material, the sheet resistance of the ESD layer 220 can be controlled within the range required by the LCD device 10.
[0104] Furthermore, by adjusting the oxygen partial pressure in the processing chamber during the process of depositing the electrostatic discharge layer 220 on the second substrate 102, the sheet resistance of the electrostatic discharge layer 220 can be controlled within the range required by the LCD device 10, which will be described in more detail below.
[0105] The second polarizing plate 202 can be attached to the top surface or the outer surface of the substrate OS where the electrostatic discharge layer 220 is provided. Here, the second polarizing plate 202 can be directly attached to the top surface of the electrostatic discharge layer 220 by means of an adhesive member.
[0106] For example, similar to the first polarizing plate 201, a typical polarizing plate can be used as the second polarizing plate 202. In this case, the second polarizing plate 202 may include a polarizing layer and a protective layer disposed on opposite surfaces (i.e., the bottom surface and the top surface) of the polarizing layer, but an additional electrostatic discharge (ESD) prevention layer may not be required. The second polarizing plate 202 may have approximately 10 12 The sheet resistance is Ω / sq or higher, and in this case, the second polarizing plate 202 cannot be used as an electrostatic discharge prevention element because the second polarizing plate 202 has essentially insulating properties.
[0107] The cover window CW can be attached to the top or outer surface of the second polarizing plate 202, and it is disposed on the top or display surface of the liquid crystal panel 100 to which the first polarizing plate 201 and the second polarizing plate 202 are attached. Here, the cover window CW can be directly attached to the top surface of the second polarizing plate 202 by means of an adhesive member.
[0108] As described above, in the embedded structure touch LCD device 10 according to this embodiment, an electrostatic discharge (ESD) layer 220 formed of a body material comprising at least one of In₂O₃ and SnO₂ and a dopant material comprising at least one of SiO₂, ZrO₂, HfO₂, Nb₂O₅, and Ta₂O₅ can be formed on the outer surface of the substrate OS. When the ESD layer 220 is formed of the aforementioned material, approximately 10 6.5 Ω / sq to approximately 10 9 A thin-film resistance of Ω / sq is necessary to prevent electrostatic problems and interference with touch-sensitive capacitance, and can effectively ensure a transmittance of about 97% or higher, which is required to keep image brightness at the desired level.
[0109] Therefore, the relative substrate OS can be disposed adjacent to the display surface or top surface of the liquid crystal panel 100, and thus, the embedded touch LCD device can be configured to have a non-inverted panel structure.
[0110] Therefore, the technical problems encountered in conventional inverted panel structures can be effectively overcome. For example, it is unnecessary to form an additional inorganic insulating layer to reduce the recognition of reflections from the gate metal in the inverted panel structure. Furthermore, it is unnecessary to provide expensive polarizing plates with electrostatic discharge protection near the display surface, and typical polarizing plates can be used cost-effectively in inverted panel structures. Additionally, no additional equipment is required for inverted panels.
[0111] In addition, an existing sputtering system can be used to form the electrostatic discharge layer 220, which is also used to form a transparent conductive layer on the outer surface of the substrate, so there is no additional cost of preparing a new system.
[0112] Therefore, according to this embodiment, productivity can be increased and manufacturing costs can be reduced.
[0113] In the following text, reference will be made to Figures 5 to 7 A method for manufacturing a touch LCD device with an embedded structure and the aforementioned features is described in more detail.
[0114] Figures 5 to 7 This is a schematic cross-sectional view illustrating the process of manufacturing a touch LCD device relative to a substrate according to an embodiment of the present invention.
[0115] Reference Figure 5 The second substrate 102 relative to the substrate OS can be placed in the sputtering deposition chamber 400, and a sputtering process can be performed on the outer surface of the second substrate 102 to form an electrostatic anti-electrostatic layer 220 on the entire outer surface of the second substrate 102.
[0116] During sputtering, the target, serving as the deposition source, can be composed of a host material and a dopant material used to form the electrostatic discharge layer 220. In embodiments, the host material may include at least one of In2O3 and SnO2, and the dopant material may include at least one of SiO2, ZrO2, HfO2, Nb2O5, and Ta2O5.
[0117] Since the target is used for the sputtering process, the host material and dopant material can be deposited to form the electrostatic discharge (ESD) layer 220, and in an embodiment, the ESD layer 220 can be formed to have a thickness of, for example, about 100 Å to 300 Å.
[0118] Even after subsequent processing on the substrate OS, the electrostatic discharge (ESD) prevention layer 220 can still stably maintain the approximately 10 required by the LCD device 10. 6.5 Ω / sq to approximately 10 9 The thin-film resistance range is Ω / sq. Therefore, electrostatic discharge (ESD) protection characteristics can be ensured and interference from electrostatic capacitance caused by touch events can be prevented. Furthermore, for the ESD protection layer 220 with the aforementioned characteristics, the transmittance can be stably maintained at a value of approximately 97% or higher, thereby ensuring the desired image brightness of the touch LCD device.
[0119] To stably ensure the thin-film resistance characteristics in the electrostatic discharge layer 220, the content of the dopant material can be in the range of about 9 wt% to about 15 wt%, and the content of the host material can be in the range of about 85 wt% to about 91 wt%.
[0120] When one of In2O3 and SnO2 is used as the host material, the content of the dopant material can be in the range of about 12 wt% to about 15 wt%, and the content of the host material can be in the range of about 85 wt% to about 88 wt%.
[0121] When a mixture of In₂O₃ and SnO₂ is used as the host material, the content of the dopant material can range from about 9 wt% to about 11 wt%, and the content of the host material can range from about 89 wt% to about 91 wt%. In this case, the content of SnO₂ in the host material can preferably be higher than the content of In₂O₃, and for example, the content of SnO₂ can range from about 50 wt% to about 70 wt%, and In₂O₃ can have a surplus content.
[0122] Here, as the content of the dopant material increases, the sheet resistance also increases. Considering this relationship between content and sheet resistance, the required sheet resistance of the LCD device 10 can be ensured by adjusting the content of the dopant material within the above-mentioned range.
[0123] Meanwhile, the electrostatic discharge prevention layer 220 can be a layer first deposited on the second substrate 102, and can be deposited at room temperature or high temperature.
[0124] When using a mixture of In₂O₃ and SnO₂ as the host material, the SnO₂ content ratio in high-temperature deposition can be higher than that in room-temperature deposition. In other words, the SnO₂ content ratio in high-temperature deposition can be higher than that in room-temperature deposition.
[0125] For example, when the deposition process is performed at room temperature conditions of approximately 15°C to 100°C, the SnO2 content can be in the range of 50 wt% to 60 wt%. In contrast, when the deposition process is performed at high temperature conditions of approximately 100°C to 300°C, the SnO2 content can be in the range of 60 wt% to 70 wt%.
[0126] Meanwhile, the sheet resistance can be changed according to the amount of oxygen (or oxygen partial pressure) supplied to the sputtering deposition chamber 400, and with this in mind, the amount of oxygen can be adjusted during the sputtering process performed on the electrostatic anti-static layer 220 to ensure the sheet resistance range required by the LCD device 10.
[0127] Specifically, as the oxygen content increases during deposition, the sheet resistance of the deposited material decreases. In other words, the sheet resistance can be inversely proportional to the oxygen content. Conversely, as mentioned above, the sheet resistance can be proportional to the dopant content. Due to these relationships, when the dopant content is high, the desired sheet resistance characteristics can be achieved by increasing the oxygen content, while when the dopant content is low, the desired sheet resistance characteristics can be achieved by decreasing the oxygen content.
[0128] Here, the amount of oxygen or oxygen flow rate used to ensure the resistance of the thin film of the antistatic layer 220 can be in the range of about 5 sccm to 20 sccm, but is not limited to this range.
[0129] Next, refer to Figure 6 After forming the electrostatic discharge (ESD) layer 220, columnar spacers 160 may be formed on the inner surface of the second substrate 102. The columnar spacers 160 may correspond to those formed on the array substrate (see, for example, [reference needed]). Figure 4 Non-display elements are formed in the AS, and the non-display elements may include thin-film transistors (e.g., Figure 4 T in the middle), data cable (e.g.) Figure 4 DL in the middle) and gate lines (e.g. Figure 3 (GL in the text).
[0130] The columnar spacer 160 can be formed via a masking process. For example, the formation of the columnar spacer 160 may include a process of depositing an organic material for the columnar spacer, a process of coating a photoresist layer, a process of exposing the photoresist layer using a photomask, a process of developing the exposed photoresist layer, an etching process of patterning the deposited organic material, and a process of stripping the photoresist layer. A heat treatment process or a first heat treatment process may be performed after the masking process.
[0131] Here, the heat treatment process on the columnar spacer 160 can be a process of curing organic materials, and can be performed at a high temperature for a specific time (e.g., performed at about 230°C for about 20 minutes).
[0132] In one embodiment, the columnar spacer 160 may be formed to contain black pigment (e.g., carbon), and in this case, the columnar spacer 160 may have a light-blocking function to prevent or suppress leaked light from entering adjacent pixel areas such as the black matrix.
[0133] Next, refer to Figure 7 The second alignment layer 192 can be formed by coating an alignment material onto the inner surface of the second substrate 102 where the columnar spacers 160 are provided, and then a heat treatment process or a second heat treatment process can be performed on the alignment material. For example, polyimide can be used as the material of the second alignment layer 192.
[0134] In one embodiment, a cleaning process can be performed on the second substrate 102 before the alignment material is coated.
[0135] Here, the heat treatment process on the second orientation layer 192 can be a process of curing the orientation material, and can be performed at a high temperature for a specific time (e.g., performed at about 230°C for about 15 minutes).
[0136] As a result of the aforementioned process, a relative substrate OS having an electrostatic discharge prevention layer 220 can be manufactured.
[0137] In the aforementioned process of manufacturing the substrate OS, the electrostatic discharge (ESD) prevention layer 220 can be formed before the formation of the columnar spacer 160 and the second alignment layer 192, and therefore, the ESD prevention layer 220 can be exposed to subsequent processes. That is, the characteristics of the ESD prevention layer 220 may be affected by subsequent processes.
[0138] Therefore, considering that the electrostatic discharge (ESD) layer 220 is exposed to subsequent processes, before the formation of the columnar spacer 160 and the second orientation layer 192, the ESD layer 220 can be formed from a host material and a dopant material, wherein the content ratio of the host material and the dopant material is within the aforementioned appropriate range. Therefore, even when the ESD layer 220 is exposed to the process environment used for subsequent processes (e.g., the developing solution (e.g., KOH) for forming the columnar spacer 160, the heat treatment process on the columnar spacer 160, and the cleaning solution (e.g., LGD-900) before the formation of the second orientation layer 192, and the heat treatment process on the second orientation layer 192), stable 10 6.5 Ω / sq up to 10 9 A suitable range of sheet resistance (Ω / sq) and a suitable transmittance of approximately 97% or higher.
[0139] LCD panels (e.g.) Figure 4 100 in the above process can be achieved by bonding the relative substrate OS manufactured through the above process to a separately manufactured array substrate (e.g., Figure 4 The process involves fabricating an array substrate (OS) with a liquid crystal layer (e.g., an AS) inserted between the opposing substrate OS and the array substrate. Figure 4 105 in the middle).
[0140] First polarizing plate and second polarizing plate (e.g.) Figure 4 201 and 202 in the above process can be attached to the bottom and top surfaces of the liquid crystal panel manufactured by the above process, and then, the cover window (e.g.) Figure 4 The CW in the image can be attached to the top surface of the second polarizer. Therefore, LCD devices (e.g., ...) can be manufactured. Figure 4 10 in the middle).
[0141] Based on experiments used to evaluate chemical resistance and reliability characteristics, the electrostatic discharge (ESD) layer 220 of the LCD device according to this embodiment exhibits sheet resistance and transmittance characteristics maintained at appropriate levels. These experiments will be described in more detail below. The table below includes sheet resistance values for multiple samples. In the table, the sheet resistance values are expressed as the logarithm of the sheet resistance to base 10.
[0142] 1. Comparative Experiment (GZTO Antistatic Layer)
[0143] In the comparative experiment, unlike the present invention, the embedded touch LCD device has a non-inverted panel structure and includes an opposing substrate, wherein the electrostatic discharge (ESD) layer is made of GZTO. A substrate with a GZTO ESD layer was prepared as the experimental sample for the comparative experiment.
[0144] The results of the comparative experiment 1 are summarized in Table 1 below. Figure 8 middle.
[0145] Table 1
[0146]
[0147] In the comparative experiment, 6090 reliability tests (temperature 60°C and humidity 90%) were performed on three samples 1-1, 1-2, and 1-3 (for an oxygen partial pressure of 1.1% in the test sputtering deposition chamber) and three samples 2-1, 2-2, and 2-3 (for an oxygen partial pressure of 4%). The sheet resistance characteristics of the samples were measured after the sputtering deposition process, after two heat treatment processes, and when certain preset times had elapsed under the 6090 reliability test conditions.
[0148] In Table 1, the expression “230℃, 20 minutes” represents the processing conditions for the heat treatment process performed on the columnar spacer, and the expression “230℃, 15 minutes” represents the processing conditions for the heat treatment process performed on the second orientation layer.
[0149] exist Figure 8 In the figure, the y-axis represents the exponent of the sheet resistance to base 10 (i.e., the logarithm of the sheet resistance to base 10).
[0150] Refer to Table 1 and Figure 8 In the comparative experiment, the sheet resistance decreased by approximately 10 ohms 24 hours after the completion of the two heat treatment processes. 1.5 Ω / sq up to 10 2 Ω / sq decreased by approximately 10 after 300 hours. 1.8 Ω / sq up to 10 2.8 The Ω / sq value exhibits saturation characteristics, but increases in the opposite direction after 800 hours.
[0151] The results show that, in the comparative experiments, the electrostatic discharge layer of GTZO did not have good film quality, exhibited unstable thin-film resistance characteristics, and could not guarantee 10 6.5 Ω / sq up to 10 9 Appropriate thin-film resistance of Ω / sq.
[0152] This means that the anti-static layer made of GTZO cannot be applied to touch LCD devices.
[0153] 2. Experiment 1 of the present invention (electrostatic prevention layer, wherein Nb2O5 and SnO2 are used as dopants and the host, respectively)
[0154] In Experiment 1 of this invention, the embedded touch LCD device has a non-inverted panel structure and includes a counter substrate and an electrostatic discharge (ESD) layer on the outer surface of the counter substrate. The ESD layer is formed using Nb₂O₅ and SnO₂ as dopant and host materials, respectively. A substrate with ESD layers of Nb₂O₅ and SnO₂ is prepared as the experimental sample for Experiment 1 of this invention.
[0155] The results of Experiment 1 are summarized in Table 2 below, and the data in Table 2 are visually presented. Figure 9 and Figure 10 middle.
[0156] Table 2
[0157]
[0158] In Experiment 1, 6090 reliability testing was performed on samples with dopant content ratios of 10 wt%, 11 wt%, and 12.5 wt%, and the test for each sample was performed under oxygen partial pressure conditions of 5%, 6%, and 7% in the test sputtering deposition chamber. The sheet resistance of the samples was measured when the sputtering deposition process was completed, when two heat treatment processes were completed, and when certain preset times had elapsed under the 6090 reliability test conditions.
[0159] Meanwhile, in Experiment 1, an anti-static layer was formed through a deposition process at room temperature (50°C).
[0160] Figure 9 The sheet resistance of the samples is shown (for 5% oxygen partial pressure and dopant content ratios of 10 wt%, 11 wt%, and 12.5 wt%), and Figure 10 The sheet resistance of the samples is shown (for a dopant content ratio of 12.5 wt% and oxygen partial pressures of 5%, 6% and 7%).
[0161] Refer to Table 2 and Figure 9 and Figure 10In Experiment 1, when the sample had a dopant content of 12.5 wt%, the sheet resistance was 10 Ω·cm. 6.5 Ω / sq up to 10 9 The sheet resistance is within the appropriate range of Ω / sq, but when the sample has a dopant content ratio of 10wt% and 11wt%, the sheet resistance is not within the appropriate range.
[0162] The transmittance measured in Experiment 1 and the film resistivity measured in the chemical resistance assessment are summarized in Tables 3 and 4 below, respectively, and the data in Tables 3 and 4 are visually illustrated. Figure 11 and Figure 12 middle.
[0163] Table 3
[0164]
[0165] Table 4
[0166]
[0167] Table 3 and Figure 11 The results show the transmittance versus wavelength obtained for samples with dopant content ratios of 10wt%, 11wt%, and 12.5wt% when the oxygen partial pressure is 5%, 6%, and 7%.
[0168] Table 4 and Figure 12 The sheet resistance is shown in Table 4, as measured by chemical resistance tests on a sample with a dopant content ratio of 12.5 wt%, at oxygen partial pressures of 5%, 6%, and 7%. Figure 12 In the process, the sheet resistance of the antistatic layer was measured after the deposition process, after a heat treatment process under heat treatment conditions for columnar spacers (“230°C, 20 min”), after a development solution treatment process under development solution conditions for columnar spacers (“KOH (0.04%), 6 min”), and after a cleaning solution treatment process under cleaning solution conditions (“LGD-900, 6 min”) before coating the alignment layer. The development solution treatment process and the cleaning solution treatment process correspond to chemical resistance testing, and the conditions used for the development solution treatment process and the cleaning solution treatment process are set to be more stringent than the actual conditions used for the relevant processes.
[0169] Table 3 and Figure 11 As shown, for the sample, a suitable transmittance of 97% or higher can be ensured within the visible wavelength range (e.g., from 380 nm to 760 nm).
[0170] Table 4 and Figure 12 As shown, the film resistance measured in the chemical resistance test is within the appropriate film resistance range. This means that the sample can have the desired chemical resistance properties.
[0171] 3. Experiment 2 of the present invention (electrostatic discharge layer, wherein SiO2 and In2O3+SnO2 are used as dopants and host, and the electrostatic discharge layer is deposited at room temperature)
[0172] In Experiment 2 of the present invention, the embedded touch LCD device has a non-inverted panel structure and includes an opposing substrate and an electrostatic discharge (ESD) layer on the outer surface of the opposing substrate. The ESD layer is formed by a deposition process performed at room temperature (50°C) in which SiO2 and In2O3+SnO2 are used as the dopant material and the host material, respectively. A substrate with the ESD layer of SiO2 and In2O3+SnO2 is prepared as the experimental sample for Experiment 2 of the present invention.
[0173] The results of Experiment 2 are summarized in Table 5 below, and the data in Table 5 are visually presented. Figures 13 to 15 middle.
[0174] Table 5
[0175]
[0176] In Experiment 2, a 6090 reliability test was performed on the samples, with a dopant content of 9 wt% and a SnO2 content of 40 wt%, 50 wt%, and 60 wt% in the bulk. This test was performed for each sample under oxygen partial pressures of 5%, 6%, and 7% in the test sputtering deposition chamber. The sheet resistance of the samples was measured after the sputtering deposition process, after the developing solution treatment process, after two heat treatment processes, and when certain preset times had elapsed under the 6090 reliability test conditions.
[0177] Figure 13 , Figure 14 and Figure 15 Each of the figures shows the sheet resistance of the sample, with SnO2 content ratios of 40wt%, 50wt%, and 60wt% in the bulk sample.
[0178] Refer to Table 5 and Figures 13 to 15 In Experiment 2, when the samples had SnO2 content ratios of 50 wt% and 60 wt%, the sheet resistance was at 10 Ω·cm. 6.5 Ω / sq up to 10 9 The appropriate sheet resistance is within the range of Ω / sq, but when the sample has a content ratio of 40wt%, the sheet resistance is not within the appropriate range.
[0179] Table 6 below shows the transmittance of the samples in Experiment 2 as measured by chemical resistance and reliability tests.
[0180] Table 6
[0181]
[0182] Table 6 shows the transmittance of samples with SnO2 content ratios of 40 wt%, 50 wt%, and 60 wt%, respectively, measured in chemical resistance and reliability tests.
[0183] Referring to Table 6, in the chemical resistance and reliability tests, the samples exhibited 97% or higher transmittance within an appropriate transmittance range. This means that the samples in Experiment 2 of this study can possess sufficient chemical resistance and reliability.
[0184] 4. Experiment 3 of the present invention (static discharge prevention layer, wherein SiO2 and In2O3+SnO2 are used as dopants and host, and the static discharge prevention layer is deposited at high temperature)
[0185] In Experiment 3 of the present invention, the embedded touch LCD device has a non-inverted panel structure and includes an opposing substrate and an electrostatic discharge (ESD) layer on the outer surface of the opposing substrate. The ESD layer is formed by a deposition process in which SiO2 and In2O3+SnO2 are used as dopant and host materials, respectively, and performed at a high temperature (200°C). A substrate with the ESD layer of SiO2 and In2O3+SnO2 is prepared as the experimental sample for Experiment 3 of the present invention.
[0186] The results of Experiment 3 are summarized in Figures 16(a) to 16(f) and Figures 17(a) to 17(f).
[0187] In Experiment 3, when the oxygen partial pressure in the test sputtering deposition chamber was 3%, 4%, 5%, 6%, and 7%, the samples were subjected to heat treatment stability test, chemical resistance test, and 6090 reliability test, with dopant content ratios of 9wt%, 10wt%, and 11wt% and SnO2 content ratio in the bulk of 60wt%.
[0188] In Figures 16(a) to 16(f), the results of the heat treatment stability test are shown in (a), (b), and (c), and the combined results of the heat treatment stability test and the chemical resistance test are shown in (d), (e), and (f). Here, the results of the heat treatment stability test are the sheet resistance measured after two heat treatment processes (230°C, 20 minutes; 230°C, 15 minutes), and the combined results of the heat treatment stability test and the chemical resistance test are the sheet resistance measured after two heat treatment processes and two chemical resistance treatment processes (KOH, 90 seconds; LGD-900, 70 seconds).
[0189] In Figures 17(a) through 17(f), the results of the 6090 reliability test are shown in (a), (b), and (c), and the combined results of the 6090 reliability test and the chemical resistance test are shown in (d), (e), and (f). Here, the results of the 6090 reliability test are the sheet resistance measured after the 6090 reliability test, and the combined results of the 6090 reliability test and the chemical resistance test are the sheet resistance measured after the 6090 reliability treatment and the chemical resistance treatment.
[0190] Referring to Figures 16(a) to 16(f) and Figures 17(a) to 17(f), the results obtained in Experiment 3 show that when the SnO2 content ratio is 60 wt% and the dopant content ratio is 9 wt%, 10 wt%, and 11 wt%, the 10 wt% can be ensured by adjusting the oxygen partial pressure. 6.5 Ω / sq up to 10 9 The appropriate sheet resistance is Ω / sq. In detail, the sheet resistance increases with the increase of the SiO2 content ratio, and even in this case, the appropriate sheet resistance can be ensured by increasing the oxygen partial pressure when the SiO2 content ratio increases.
[0191] The chemical resistance treatment results in a very small change in the film resistivity, which means that the film resistivity characteristics before chemical resistance treatment are essentially the same as those after chemical resistance treatment.
[0192] Tables 7 and 8 below show the transmittance of the samples in Experiment 3 as measured by reliability and chemical resistance tests.
[0193] Table 7
[0194]
[0195] Table 8
[0196]
[0197] Tables 7 and 8 show the transmittance of samples with a SnO2 content ratio of 60 wt% as measured in reliability and chemical resistance tests, respectively.
[0198] Based on these results, the samples have a transmittance of 97% or higher within an appropriate range, which means that the samples in Experiment 3 can have sufficient reliability and chemical resistance.
[0199] The experimental results show that, according to embodiments of the present invention, appropriate sheet resistance and transmittance ranges can be ensured for the electrostatic discharge (ESD) layer formed on the outer surface of the opposing substrate. Meanwhile, in the experiments, for convenience, process conditions associated with the amount of oxygen during the deposition of the ESD layer are expressed in terms of oxygen partial pressure; however, these conditions can be expressed in terms of oxygen quantity. For example, the oxygen flow rate for appropriate sheet resistance and transmittance ranges can be in the range of approximately 5 sccm to 20 sccm.
[0200] As described above, in the embedded structure touch LCD device according to an embodiment of the present invention, an electrostatic discharge layer formed of a host material comprising at least one of In2O3 and SnO2 and a dopant material comprising at least one of SiO2, ZrO2, HfO2, Nb2O5 and Ta2O5 can be formed on the outer surface of the substrate.
[0201] Therefore, it can effectively ensure approximately 10 6.5 Ω / sq to approximately 10 9 A thin-film resistance of Ω / sq is necessary to prevent static electricity and interference with touch-sensitive capacitance, and can effectively ensure a transmittance of about 97% or higher, which is required to keep image brightness at the desired level.
[0202] Therefore, the substrate can be disposed adjacent to the display surface or top surface of the liquid crystal panel 100, and thus, the embedded touch LCD device can be configured to have a non-inverted panel structure.
[0203] Therefore, the problems in conventional inverted panel structures can be effectively overcome. For example, it is unnecessary to form an additional inorganic insulating layer to reduce the recognition of reflections from the gate metal in the inverted panel structure. Furthermore, it is unnecessary to provide expensive polarizing plates with electrostatic discharge protection near the display surface, and typical polarizing plates can be used cost-effectively in inverted panel structures. Additionally, no additional equipment is required for inverted panels.
[0204] In addition, an existing sputtering system can be used to form an electrostatic discharge layer, which is also used to form a transparent conductive layer on the outer surface of the substrate, so there is no additional cost to prepare a new system.
[0205] Therefore, productivity can be increased and manufacturing costs can be reduced.
[0206] In the embedded structure of the touch LCD device according to the present invention, an anti-static layer formed of a host material comprising at least one of In2O3 and SnO2 and a dopant material comprising at least one of SiO2, ZrO2, HfO2, Nb2O5 and Ta2O5 can be formed on the outer surface of the opposite substrate.
[0207] Therefore, it can effectively ensure approximately 10 6.5 Ω / sq to approximately 10 9 A thin-film resistance of Ω / sq is necessary to prevent static electricity and interference with touch-sensitive capacitance, and can effectively ensure a transmittance of about 97% or higher, which is required to keep image brightness at the desired level.
[0208] Therefore, the substrate can be disposed adjacent to the display surface or top surface of the liquid crystal panel 100, and thus, the embedded touch LCD device can be configured to have a non-inverted panel structure.
[0209] Therefore, the problems in conventional inverted panel structures can be effectively overcome. For example, it is unnecessary to form an additional inorganic insulating layer to reduce the recognition of reflections from the gate metal in the inverted panel structure. Furthermore, it is unnecessary to provide expensive polarizing plates with electrostatic discharge protection near the display surface, and typical polarizing plates can be used cost-effectively in inverted panel structures. Additionally, no additional equipment is required for inverted panels.
[0210] In addition, an existing sputtering system can be used to form an electrostatic discharge layer, which is also used to form a transparent conductive layer on the outer surface of the substrate, so there is no additional cost to prepare a new system.
[0211] Therefore, productivity can be increased and manufacturing costs can be reduced.
[0212] It will be apparent to those skilled in the art that various modifications and variations can be made to the display device of the present invention without departing from the spirit or scope of this disclosure. Therefore, the present invention is intended to cover modifications and variations of this disclosure, provided that such modifications and variations fall within the scope of the appended claims and their equivalents.
[0213] This disclosure includes, but is not limited to, the following schemes.
[0214] 1. A liquid crystal display device, comprising:
[0215] An array substrate, the array substrate including a first substrate disposed adjacent to a backlight source and thin-film transistors and touch electrodes disposed on the first substrate; and
[0216] The opposing substrate includes a second substrate facing the first substrate and an electrostatic discharge (ESD) layer deposited on the outer surface of the second substrate, wherein a liquid crystal layer is inserted between the first substrate and the second substrate.
[0217] The electrostatic discharge (ESD) layer is formed of a host material comprising at least one of In₂O₃ and SnO₂, and a dopant material comprising at least one of SiO₂, ZrO₂, HfO₂, Nb₂O₅, and Ta₂O₅, and the ESD layer has a density of 10. 6.5 Ω / sq up to 10 9 Thin-film resistance in Ω / sq.
[0218] 2. The liquid crystal display device according to claim 1, wherein the content ratio of the dopant material is in the range of 9 wt% to 15 wt%, and
[0219] The content ratio of the main material is in the range of 85wt% to 91wt%.
[0220] 3. The liquid crystal display device according to claim 2, wherein when the host material is one of In2O3 and SnO2, the content ratio of the dopant material is in the range of 12wt% to 15wt% and the content ratio of the host material is in the range of 85wt% to 88wt%, and
[0221] When the host material is In2O3 and SnO2, the content ratio of the dopant material is in the range of 9wt% to 11wt% and the content ratio of the host material is in the range of 89wt% to 91wt%.
[0222] 4. The liquid crystal display device according to Scheme 3, wherein when the main material is In2O3 and SnO2, the SnO2 content ratio is in the range of 50wt% to 70wt%.
[0223] 5. The apparatus according to Scheme 4, wherein the dopant material is SiO2.
[0224] 6. The liquid crystal display device according to claim 1, wherein the thickness of the electrostatic discharge protection layer is in the range of 100 Å to 300 Å.
[0225] 7. The liquid crystal display device according to claim 1, wherein the electrostatic discharge layer has a transmittance of 97% or higher.
[0226] 8. The liquid crystal display device according to claim 1, wherein the opposing substrate comprises:
[0227] Columnar spacers on the inner surface of the second substrate; and
[0228] An alignment layer on the inner surface of the columnar spacer and the second substrate.
[0229] 9. The liquid crystal display device according to Scheme 1 further includes:
[0230] A polarizing plate, the polarizing plate being attached to the top surface of the anti-static layer; and
[0231] A cover window is attached to the top surface of the polarizing plate.
[0232] 10. The liquid crystal display device according to claim 1, wherein the array substrate includes pixel electrodes and color filter patterns formed in the pixel region, and
[0233] During the image display period, an electric field is generated between the pixel electrode and the touch electrode to drive the liquid crystal layer.
[0234] 11. A method for manufacturing a liquid crystal display device, comprising:
[0235] Manufacturing an array substrate, the array substrate including a first substrate disposed adjacent to a backlight source and thin-film transistors and touch electrodes disposed on the first substrate; and
[0236] A counter substrate is manufactured, the counter substrate comprising a second substrate facing the first substrate and an electrostatic discharge (ESD) layer deposited on the outer surface of the second substrate, wherein a liquid crystal layer is inserted between the first substrate and the second substrate.
[0237] The electrostatic discharge (ESD) layer is formed of a host material comprising at least one of In₂O₃ and SnO₂, and a dopant material comprising at least one of SiO₂, ZrO₂, HfO₂, Nb₂O₅, and Ta₂O₅, and the ESD layer has a density of 10. 6.5 Ω / sq up to 10 9 Thin-film resistance in Ω / sq.
[0238] 12. The method according to claim 11, wherein the fabrication of the opposing substrate comprises:
[0239] The electrostatic anti-electrostatic layer is deposited on the outer surface of the second substrate using a sputtering method;
[0240] A masking process, including a development process, is performed to form columnar spacers on the inner surface of the second substrate to which the electrostatic discharge layer is deposited, and then a first heat treatment process is performed.
[0241] A cleaning process is performed after the first heat treatment process;
[0242] An orientation layer is applied after the cleaning process, and then a second heat treatment process is performed.
[0243] 13. The method according to claim 11 or 12, wherein the content ratio of the dopant material is in the range of 9 wt% to 15 wt%, and
[0244] The content ratio of the main material is in the range of 85wt% to 91wt%.
[0245] 14. The method according to Scheme 13, wherein when the host material is one of In2O3 and SnO2, the content ratio of the dopant material is in the range of 12wt% to 15wt% and the content ratio of the host material is in the range of 85wt% to 88wt%, and
[0246] When the host material is In2O3 and SnO2, the content ratio of the dopant material is in the range of 9wt% to 11wt% and the content ratio of the host material is in the range of 89wt% to 91wt%.
[0247] 15. The method according to Scheme 14, wherein when the main materials are In2O3 and SnO2, the SnO2 content ratio is in the range of 50wt% to 70wt%.
[0248] 16. The method according to Scheme 15, wherein when the antistatic layer is deposited at a temperature below 100°C, the SnO2 content ratio is in the range of 50wt% to 60wt%.
[0249] When the antistatic layer is deposited at a temperature of 100°C or higher, the SnO2 content ratio is in the range of 60wt% to 70wt%, and
[0250] The dopant material is SiO2.
[0251] 17. The method according to Scheme 12, wherein when the electrostatic anti-electrostatic layer is deposited, the oxygen flow rate in the deposition chamber is in the range of 5 sccm to 20 sccm.
[0252] 18. The method according to Scheme 11 or 12, wherein the thickness of the electrostatic anti-electrostatic layer is in the range of 100 Å to 300 Å.
[0253] 19. The method according to claim 11 or 12, wherein the antistatic layer has a transmittance of 97% or higher.
Claims
1. A liquid crystal display device, comprising: Backlight unit; The first substrate above the backlight unit; Thin-film transistors above the first substrate; Color filter pattern above the thin-film transistor; Touch electrodes above the color filter pattern; The liquid crystal layer above the touch electrode; A second substrate above the liquid crystal layer; as well as An anti-static layer on the outer surface of the second substrate. The color filter pattern is disposed between the touch electrode and the first substrate, and the touch electrode is disposed between the liquid crystal layer and the color filter pattern. wherein the electrostatic prevention layer is formed of a host material including at least one of In2O3 and SnO2 and a dopant material including at least one of ZrO2, HfO2, Nb2O5, and Ta2O5, and has a thin layer resistance of 10 6.5 Ω / sq to 10 9 Ω / sq. The content ratio of the dopant material is in the range of 9 wt% to 15 wt%, and the content ratio of the host material is in the range of 85 wt% to 91 wt%.
2. The liquid crystal display device according to claim 1, wherein The color filter pattern overlaps with another color filter pattern whose color is different from that of the color filter pattern above the thin-film transistor.
3. The liquid crystal display device according to claim 1, further comprising a pixel electrode connected to the thin-film transistor. wherein, The pixel electrode is disposed between the touch electrode and the color filter pattern, and the color filter pattern is disposed between the pixel electrode and the first substrate.
4. The liquid crystal display device according to claim 3, further comprising a touch line connected to the touch electrode. wherein The touch line is disposed between the touch electrode and the color filter pattern, and the pixel electrode is disposed between the touch electrode and the touch line.
5. The liquid crystal display device according to claim 4, further comprising a data line connected to the thin-film transistor and overlapping the touch line. wherein The data line is disposed between the color filter pattern and the first substrate, and the color filter pattern is disposed between the touch line and the data line.
6. The liquid crystal display device according to claim 5, further comprising a columnar spacer on the inner surface of the second substrate. wherein The columnar spacer overlaps with the touch line and the data line.
7. The liquid crystal display device according to claim 1, wherein When the host material is either In₂O₃ or SnO₂, the content ratio of the dopant material is in the range of 12 wt% to 15 wt%, and the content ratio of the host material is in the range of 85 wt% to 88 wt%. When the host material is In2O3 and SnO2, the content ratio of the dopant material is in the range of 9wt% to 11wt%, and the content ratio of the host material is in the range of 89wt% to 91wt%.
8. The liquid crystal display device according to claim 7, wherein When the main materials are In2O3 and SnO2, the SnO2 content ratio is in the range of 50wt% to 70wt%.
9. The liquid crystal display device according to claim 1, wherein The thickness of the electrostatic anti-static layer is in the range of 100 Å to 300 Å.
10. The liquid crystal display device according to claim 1, wherein The antistatic layer has a transmittance of 97% or higher.
11. The liquid crystal display device according to claim 1, further comprising: Columnar spacers on the inner surface of the second substrate; as well as An orientation layer of the columnar spacer is applied to the inner surface of the second substrate.
12. The liquid crystal display device according to claim 11, wherein The columnar spacer overlaps with the thin-film transistor.
13. The liquid crystal display device according to claim 1, further comprising: a polarizing plate attached to a top surface of the static electricity prevention layer; and a cover window attached to a top surface of the polarizing plate.
Citation Information
Patent Citations
Salt, acid generator, resist composition and method for producing resist pattern
KR1020190143396A