A method for controlling the thickness of edge coating film, a coating nozzle, and a semiconductor coating device.

By using multi-stage variable diameter coating nozzles and precisely controlling the parameters of the scanning and removal stage, the problems of inaccurate film thickness control and poor consistency in edge coating are solved, thereby improving film integrity and product quality.

CN123113245APending Publication Date: 2026-11-17KINGSEMI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611515241.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies in edge coating processes suffer from insufficient precision in film thickness control, poor film integrity, and inconsistent film thickness across multiple cavities, making it difficult to achieve simultaneous improvements.

Method used

By employing a coating nozzle with a multi-stage variable diameter structure, and by controlling the motor rotation speed, robotic arm movement speed, and motor rotation duration during the scanning and removal phase, combined with adjusting the coating nozzle position and motor switching time, the liquid output state is optimized to achieve precise film thickness control and multi-cavity consistency.

Benefits of technology

It significantly improves the integrity of the adhesive film and product yield of edge coating, reduces coating defects, reduces the sensitivity of film thickness to cavity wind pressure, and improves the consistency of film thickness in multiple cavities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113245A_ABST
    Figure CN123113245A_ABST
Patent Text Reader

Abstract

This application belongs to the field of semiconductor manufacturing technology and relates to a method for controlling the thickness of edge photoresist coating, a photoresist coating nozzle, and a semiconductor photoresist coating apparatus. The control method includes at least: applying photoresist to the wafer edge using a photoresist coating nozzle with at least two variable diameter sections; and controlling at least one of the following during the scanning and removal stage of the photoresist coating process: the rotational speed of the motor during scanning and removal, the moving speed of the scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal. This application optimizes the liquid discharge state through a multi-section variable diameter photoresist nozzle and simultaneously achieves precise control of film thickness and improved consistency across multiple cavities by adjusting process parameters during the scanning and removal stage. This effectively improves the integrity of the photoresist coating at the edge, reduces the sensitivity of film thickness to cavity air pressure, avoids photoresist defects, and significantly improves wafer edge protection and product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of semiconductor manufacturing technology, and relates to a wafer edge coating method, and more particularly to a method for controlling the thickness of the edge coating film, a coating nozzle, and a semiconductor coating apparatus. Background Technology

[0002] In integrated circuit manufacturing processes, the patterns in the wafer edge region are easily damaged after multiple etching and deposition steps, affecting the electrical performance of devices and product yield. To protect the wafer edge, edge coating (EC) is often used. This involves coating the wafer edge with a high-viscosity protective adhesive to form an edge protection layer of specific thickness and width. This isolates defects such as film peeling and chemical etching outside the effective area, while also reducing cavity particle contamination, extending maintenance cycles, stabilizing the edge chip structure, and indirectly increasing the number of effective chips.

[0003] Specifically, the quality of edge coating processes is mainly measured by three dimensions: the uniformity of film thickness in a single wafer, the integrity of the coating pattern within the wafer, and the consistency of film thickness across multiple cavities. Among these, film thickness uniformity significantly affects stress buffering capacity and protection duration; uneven thickness may cause localized protection failure or uneven surfaces in subsequent processes. Poor coating patterns within the wafer can lead to localized underprotection or adhesive splashing into the wafer interior, resulting in the loss of usable chips. Poor film thickness consistency across multiple cavities will cause differences in protection capabilities between multiple wafers during subsequent etching, thereby affecting the batch-to-batch stability of chips.

[0004] Edge coating processes typically consist of five stages: pre-discharge of solvent, scanning and wetting, spot application, scanning and removal for film formation, and main rotation for film formation. The scanning and removal stage is a crucial step in pre-film formation; the motor speed, robotic arm speed, and motor rotation duration all affect the film thickness by influencing the solvent evaporation state. The main rotation stage is critical for controlling the overall film thickness. Furthermore, the structure and material of the coating nozzle directly affect the solvent discharge state; improper nozzle backflow parameters can easily generate air bubbles, leading to poor coating or jagged streaks during the spot application stage.

[0005] Regarding the issue of poor film thickness consistency across multiple cavities, those skilled in the art generally believe it is related to fluctuations in cavity air pressure, formulation parameter settings, and consistency in motor control speed change time. Furthermore, ambient air pressure can affect film thickness by influencing the solvent evaporation rate in the photoresist. However, the sealing performance of each coating unit often varies, making it difficult to troubleshoot and improve air pressure changes caused by these differences. When cavity air pressure is consistent, variations in control and manual adjustment during the scanning and removal stage can easily lead to deviations in dwell time and trimming position. Improper motor control can shorten or increase the rotation time in this step, essentially causing the film to enter the main rotation speed period that determines film thickness earlier or later. Positional differences can cause overall film drift, resulting in film thickness measurements falling at different positions on a sloping film, thus causing inter-cavity film thickness variations.

[0006] It is evident that existing technologies lack a systematic understanding of how parameters at each stage of edge coating process affect film thickness and morphology, and have limited means of controlling film thickness consistency across multiple cavities, making it difficult to simultaneously achieve precise film thickness control, ensure film integrity, and synergistic improvement in multi-cavity consistency. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the purpose of this application is to provide a method for controlling the thickness of edge coating film, a coating nozzle, and a semiconductor coating device, so as to solve the technical problems of insufficient film thickness control accuracy, poor film integrity, and poor film thickness consistency in multi-cavity processes.

[0008] To achieve this objective, the present application adopts the following technical solution:

[0009] In a first aspect, this application provides a method for controlling the thickness of an edge photoresist coating, comprising at least: applying photoresist to the edge of a wafer using a coating nozzle having at least two variable diameter sections; and controlling at least one of the following during the scanning and removal stage of the coating process: the rotational speed of a motor during scanning and removal, the moving speed of a scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal.

[0010] In this application, the motor in the terms "motor rotation speed during scanning and removal" and "motor rotation duration" specifically refers to the spindle motor for adsorbing the wafer.

[0011] This application optimizes the liquid dispensing state by using a multi-stage variable diameter coating nozzle, reducing bubble generation and coating defects, and lowering the sensitivity of film thickness to cavity air pressure. At the same time, by adjusting the rotation speed of the motor, the movement speed of the robotic arm, and the rotation duration of the motor during the scanning and removal stage, it achieves precise control of film thickness and improves the consistency of multiple cavities, effectively improving the integrity of the adhesive film at the edge, avoiding coating defects, and significantly improving the wafer edge protection effect and product yield.

[0012] And / or, the adhesive nozzle has a three-section variable diameter structure.

[0013] And / or, the material of the adhesive nozzle includes soluble polytetrafluoroethylene.

[0014] And / or, the rotational speed of the motor is 300~500 rpm when the scan is removed.

[0015] And / or, the scanning removal robotic arm moves at a speed of 6~10 mm / s.

[0016] And / or, the duration of the motor rotation during the scan removal is 1.3~3.8s.

[0017] And / or, the control method further includes: adjusting the position of the adhesive nozzles to make the actual performance value of the cut edge width of each adhesive cavity consistent.

[0018] And / or, the control method further includes: controlling the transition time of the drive motor of each coating cavity to be consistent between the scanning removal stage and the main speed stage.

[0019] And / or, the control method is applied to the edge coating process of three-dimensional and non-flash memory chips.

[0020] Secondly, this application provides a coating nozzle used in the control method described in the first aspect, the coating nozzle having at least two variable diameter sections and being made of soluble polytetrafluoroethylene.

[0021] Thirdly, this application provides a semiconductor coating apparatus, which includes at least the coating nozzle as described in the second aspect, and a control module connected to the coating nozzle.

[0022] The control module is used to control at least one of the following during the scanning and removal stage of the adhesive coating process: the rotation speed of the motor during scanning and removal, the moving speed of the scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal.

[0023] Compared with the prior art, this application has the following advantages:

[0024] This application optimizes the liquid dispensing state by using a multi-stage variable diameter coating nozzle, reducing bubble generation and coating defects, and lowering the sensitivity of film thickness to cavity air pressure. At the same time, by adjusting the rotation speed of the motor, the movement speed of the robotic arm, and the rotation duration of the motor during the scanning and removal stage, it achieves precise control of film thickness and improves the consistency of multiple cavities, effectively improving the integrity of the adhesive film at the edge, avoiding coating defects, and significantly improving the wafer edge protection effect and product yield. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of the three-section variable diameter PFA coating nozzle structure used in Example 1.

[0026] Figure 2 This is a flowchart of the edge adhesive application method provided in Example 1.

[0027] Figure 3 This is a schematic diagram of the single-diameter variable PTFE coating nozzle structure used in Comparative Example 1. Detailed Implementation

[0028] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0029] One embodiment of this application provides a method for controlling the thickness of an edge photoresist coating, which includes at least: applying photoresist to the edge of a wafer using a coating nozzle having at least two variable diameter sections; and controlling at least one of the following during the scanning and removal stage of the coating process: the rotational speed of a motor, the moving speed of a scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal.

[0030] This application optimizes the liquid dispensing state by using a multi-stage variable diameter coating nozzle, reducing bubble generation and coating defects, and lowering the sensitivity of film thickness to cavity air pressure. At the same time, by adjusting the rotation speed of the motor, the movement speed of the robotic arm, and the rotation duration of the motor during the scanning and removal stage, it achieves precise control of film thickness and improves the consistency of multiple cavities, effectively improving the integrity of the adhesive film at the edge, avoiding coating defects, and significantly improving the wafer edge protection effect and product yield.

[0031] In some embodiments, the adhesive nozzle has a three-section variable diameter structure.

[0032] In some embodiments, the adhesive nozzle is made of soluble polytetrafluoroethylene (PFA).

[0033] In this application, PFA material has transparent properties, which makes it easier to observe and adjust the nozzle back suction state compared to opaque polytetrafluoroethylene (PTFE) material. At the same time, the three-stage variable diameter structure is less likely to generate bubbles during the back suction process. The shorter nozzle length allows the front-end photoresist with bubbles to be ejected in the liquid pre-discharge stage, thereby significantly reducing the foam generated in the subsequent scanning and fixed-point liquid dispensing stages, and making it less likely to produce poor coating and splashing film defects.

[0034] In addition, the three-section variable diameter PFA coating nozzle can reduce the sensitivity of the average film thickness to air pressure by optimizing the liquid outlet state, and has a positive effect on improving the cavity differences introduced by changes in air pressure.

[0035] In some embodiments, the rotational speed of the motor during the scan removal is 300~500 rpm, for example, it can be 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm, 400 rpm, 420 rpm, 440 rpm, 460 rpm, 480 rpm or 500 rpm, but is not limited to the listed values, other unlisted values ​​within this range are also applicable.

[0036] In this application, the scanning and removal stage is a pre-film formation process. Increasing the rotation speed in this stage is equivalent to achieving pre-film formation earlier and entering the main rotation speed stage. This allows the film to form earlier, thereby reducing the impact of wind pressure during the pre-film formation stage, i.e., significantly reducing wind pressure sensitivity. Simultaneously, increasing the scanning and removal rotation speed aligns with the principle that increasing the main rotation speed reduces film thickness, enabling precise control of film thickness. If the motor rotation speed during scanning and removal is below 300 rpm, the pre-film formation speed is too slow, prolonging the time the film is affected by wind pressure, increasing the film thickness's sensitivity to wind pressure, and resulting in a higher film thickness. If the motor rotation speed during scanning and removal is above 500 rpm, excessively high speeds can easily lead to sputtering defects, affecting the integrity of the film morphology.

[0037] In some embodiments, the scanning removal robotic arm moves at a speed of 6 to 10 mm / s, for example, 6 mm / s, 6.4 mm / s, 6.8 mm / s, 7.2 mm / s, 7.6 mm / s, 8 mm / s, 8.4 mm / s, 8.8 mm / s, 9.2 mm / s, 9.6 mm / s, or 10 mm / s, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0038] In this application, as the robotic arm's moving speed increases during the scanning and removal stage, the amount of photoresist deposited at the wafer edge decreases, resulting in a reduction in the average film thickness. Fine-tuning of the film thickness can be achieved by controlling the robotic arm's moving speed. If the robotic arm's moving speed is below 6 mm / s, excessive photoresist deposits at the wafer edge lead to a higher film thickness and reduced uniformity. If the robotic arm's moving speed is above 10 mm / s, insufficient photoresist application can easily cause localized underprotection, affecting the integrity of the photoresist film morphology.

[0039] In some embodiments, the duration of the motor rotation during the scan removal is 1.3 to 3.8 s, for example, it can be 1.3 s, 1.5 s, 1.8 s, 2.0 s, 2.3 s, 2.5 s, 2.8 s, 3.0 s, 3.3 s, 3.5 s or 3.8 s, but is not limited to the listed values, other unlisted values ​​within this range are also applicable.

[0040] In this application, the scanning and removal stage is a pre-film formation process. The longer this step lasts, the more time the adhesive film has to form a thin surface film. Due to the partial curing affecting the volatile state, a thicker film will form, thus requiring a higher master rotation speed to achieve a lower target film thickness. Experiments show that for every 0.1s increase in the motor rotation duration during scanning and removal, the film thickness changes by approximately 160 angstroms. Therefore, the motor rotation duration during scanning and removal is a significant factor affecting film thickness, and strictly controlling the duration of this step is crucial for precise film thickness control and multi-cavity consistency. If the motor rotation duration during scanning and removal is less than 1.3s, the pre-film formation is insufficient, and the film morphology is unstable; if the motor rotation duration during scanning and removal is longer than 3.8s, the film is over-cured, resulting in an excessively thick film that is difficult to adjust to the target value using the master rotation speed.

[0041] In some embodiments, the control method further includes: adjusting the position of the adhesive nozzles to make the actual performance value of the cut edge width of each adhesive application cavity consistent.

[0042] In this application, for edge coating, the shape of the prepared film exhibits two adjacent peaks from the inside to the outside of the wafer: a high peak closer to the inside and a low peak immediately following. Both peaks are relatively close to the center of the wafer, and the film thickness gradually increases towards the outside. When the formulation is fixed, the resulting film shapes are roughly similar. When the film width decreases, the measurement points remain fixed, but the film thickness decreases. Experiments show that for every 0.1 mm increase in actual edge width, the film thickness increases by approximately 40 angstroms. Therefore, for the coating unit, it is necessary to strictly control the actual value of the edge width to ensure strict consistency across multiple cavities, thereby improving the consistency of the average film thickness across multiple cavities. Edge films produced using the same formulation have almost identical shapes; differences in film thickness often arise from measurements taken at different locations on the film with a certain slope. Therefore, adjusting the position of the coating nozzle to ensure that the edge width of each coating cavity is consistent is an important way to achieve film thickness consistency across multiple cavities.

[0043] The statement that "the actual value of the cut edge width of each adhesive coating cavity is consistent" specifically means that the actual value of the cut edge width of each adhesive coating cavity is exactly the same.

[0044] In some embodiments, the control method further includes: controlling the transition time of the drive motors of each coating cavity to be consistent between the scanning removal stage and the main speed stage.

[0045] In this application, based on the influence of the dwell time in the pre-film formation stage on film thickness, an increase in the scanning and removal dwell time tends to increase the film thickness. Due to differences in motor control across chambers, the transition time between the scanning and removal stage and the main rotation speed stage may vary, which is equivalent to a deviation in the timing of each chamber entering the main rotation speed film formation stage, further exacerbating the inter-chamber differences in film thickness. Therefore, strictly controlling the consistency of the motor duration in the scanning and removal step across multiple chambers can significantly improve the consistency of the average film thickness across multiple chambers.

[0046] In some embodiments, the adhesive application process further includes a scanning and moving stage, wherein the motor speed in the scanning and moving stage is 300~350 rpm, for example, 300 rpm, 305 rpm, 310 rpm, 315 rpm, 320 rpm, 325 rpm, 330 rpm, 335 rpm, 340 rpm, 345 rpm, or 350 rpm, and the robotic arm moving speed in the scanning and moving stage is 6~10 mm / s, for example, 6 mm / s, 6.5 mm / s, 7 mm / s, 7.5 mm / s, 8 mm / s, 8.5 mm / s, 9 mm / s, 9.5 mm / s, or 10 mm / s, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0047] In this application, since the scanning and transfer stage is a pre-wetting stage, the parameters of this stage mainly affect the morphology of the photoresist film, while having a relatively small impact on the film thickness. As the motor speed and robotic arm movement speed increase during the scanning and transfer stage, poor coating can easily occur, resulting in a poor photoresist film morphology. This is because the photoresist and wafer are mainly coated during the scanning and transfer stage, and excessively high rotation speed and robotic arm movement speed make it difficult to coat the photoresist evenly.

[0048] In some embodiments, the control method is applied to the edge coating process of 3D NAND chips.

[0049] In this application, the edge coating process can be used in 3D NAND chips to solve the problems of high-layer stacking and high-stress thin film deposition, thereby effectively preventing the thin film from peeling and cracking at the edge and avoiding the generation of moving particles that could contaminate the entire wafer or cavity.

[0050] One embodiment of this application also provides a glue-applying nozzle used in the control method described in any of the above embodiments, the glue-applying nozzle having at least two variable diameter sections and being made of soluble polytetrafluoroethylene.

[0051] One embodiment of this application also provides a semiconductor coating apparatus, which includes at least the coating nozzle described in any of the above embodiments, and a control module connected to the coating nozzle.

[0052] In some embodiments, the control module is used to control at least one of the following during the scanning and removal phase of the coating process: the rotational speed of the motor during scanning and removal, the moving speed of the scanning and removal robotic arm, or the duration of the motor's rotation during scanning and removal.

[0053] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0054] Example 1

[0055] This embodiment provides a method for controlling the thickness of the adhesive film at the edge, specifically including the following steps:

[0056] (1) Provide a wafer to be coated and load it into four identical coating unit cavities. Set the exhaust air pressure of each cavity to 13Pa, 14Pa, 15Pa, 16Pa and 17Pa respectively (that is, set five exhaust air pressure values ​​for each cavity in sequence).

[0057] (2) Use a three-section variable diameter PFA coating nozzle (see Figure 1 Edge coating is performed, and five stages are executed sequentially: liquid pre-drainage, scanning and wetting, fixed-point liquid dispensing, scanning and film formation, and main rotation speed film formation (see...). Figure 2 );

[0058] (3) During the scanning and moving-in stage, the motor speed is set to 300 rpm and the robotic arm moving speed is 6 mm / s; during the scanning and moving-out stage, the motor speed is set to 300 rpm, the robotic arm moving speed is 10 mm / s, and the motor rotation duration is 1.3 s.

[0059] (4) By adjusting the position of the glue-applying nozzles in each cavity, the actual value of the cut edge width of the four cavities is 4.3mm;

[0060] (5) After the coating is completed, the wafer is baked to obtain the edge-coated wafer.

[0061] Example 2

[0062] This embodiment provides a method for controlling the thickness of the edge coating film. Except for the setting of the motor speed to 400 rpm, the robotic arm movement speed to 8 mm / s, the motor rotation duration to 2.3s in the scanning and removal stage in step (3), and the actual value of the cutting edge width to 4.5 mm in step (4), the other steps and conditions are the same as in embodiment 1, so they will not be repeated here.

[0063] Example 3

[0064] This embodiment provides a method for controlling the thickness of the edge coating film. Except for the setting of the motor speed to 500 rpm, the robotic arm movement speed to 6 mm / s, the motor rotation duration to 3.8 s in step (3) during the scanning and removal stage, and the actual value of the cutting edge width to 5.1 mm in step (4), the other steps and conditions are the same as in embodiment 1, so they will not be repeated here.

[0065] Example 4

[0066] This embodiment provides a method for controlling the thickness of the edge adhesive film. Four adhesive coating cavities are used to apply adhesive to the edges simultaneously. Except for adjusting the position of the adhesive nozzles in each cavity so that the actual value of the cut edge width of the four cavities is 4.4mm, and calibrating the drive motors of each cavity so that the transition time between the scanning removal stage and the main speed stage is consistent, the other steps and conditions are the same as in Embodiment 1, so they will not be described in detail here.

[0067] Comparative Example 1

[0068] This comparative example provides a method for controlling the thickness of the adhesive film at the edge, except that a single-diameter PTFE adhesive nozzle is used in step (2) (see...). Figure 3 Apart from the above, the remaining steps and conditions are the same as in Example 1, so they will not be repeated here.

[0069] Comparative Example 2

[0070] This comparative example provides a method for controlling the thickness of the edge coating film. Except for setting the motor speed to 200 rpm in the scanning and moving-out stage in step (3), the other steps and conditions are the same as in Example 1, so they will not be repeated here.

[0071] Comparative Example 3

[0072] This comparative example provides a method for controlling the thickness of the edge coating film. Except for the motor rotation duration of 4.5s in step (3) during the scanning and removal stage, the other steps and conditions are the same as in Example 1, so they will not be described in detail here.

[0073] Comparative Example 4

[0074] This comparative example provides a method for controlling the thickness of the edge coating film. Four coating cavities are used to apply the coating to the edge simultaneously. Except that the actual values ​​of the cut edge widths of the four cavities are 4.3mm, 4.5mm, 4.7mm and 5.1mm respectively and the drive motor conversion time is not calibrated, the other steps and conditions are the same as in Example 4, so they will not be described again here.

[0075] Performance testing

[0076] (1) Average film thickness: The film thickness of the wafer edge after coating was measured using a film thickness gauge from Zhongke Feice. 49 measurement points were selected at equal intervals on the circumference of the wafer edge, and the arithmetic mean of the film thickness of all measurement points was taken as the average film thickness. Test conditions: After coating, the wafer was baked at 100℃ for 90s and then cooled to room temperature before measurement.

[0077] (2) Wind pressure sensitivity: Edge coating was performed under exhaust air pressures of 13 Pa, 14 Pa, 15 Pa, 16 Pa, and 17 Pa respectively. The average film thickness under each air pressure condition was measured using the above-mentioned average film thickness test method. The slope of the linear fit of the average film thickness with the change of air pressure was taken as the wind pressure sensitivity, with the unit being Å / Pa. The lower the wind pressure sensitivity, the less the film thickness is affected by the fluctuation of air pressure in the cavity.

[0078] (3) Integrity of the adhesive film: The state of the adhesive film coating on the edge of the wafer after coating is observed by an automated optical inspection (AOI) machine. The total number of coating defects, serrated stripes, splatter defects and spherical defects appearing on the edge of each wafer is counted. At the same time, a high-speed camera is used to collect the liquid discharge state of the nozzle and observe whether bubbles are generated during the liquid discharge process.

[0079] (4) Multi-cavity film thickness consistency: Four coating cavities were simultaneously coated with adhesive under the same formulation conditions. The average film thickness of the wafers obtained from the four cavities was measured using the above-mentioned average film thickness test method. The difference between the maximum and minimum values ​​of the average film thickness of the four cavities was taken as the multi-cavity film thickness difference, with the unit being angstroms. The smaller the multi-cavity film thickness difference, the better the multi-cavity film thickness consistency.

[0080] The relevant test results are shown in Table 1 below.

[0081] Table 1

[0082]

[0083] As shown in Table 1:

[0084] (1) By comparing Examples 1 to 3, it can be seen that within a limited range, changing the motor speed, the robotic arm moving speed, and the duration of motor rotation during scanning and removal can change the average film thickness and wind pressure sensitivity, but has little effect on the coating state of the adhesive film and the consistency of the multi-cavity.

[0085] (2) By comparing Example 1 and Example 4, it can be seen that changing the actual width of the coating by 0.1 mm can change the film thickness by about 40 angstroms.

[0086] (3) By comparing Example 1 and Comparative Example 1, it can be seen that changing the nozzle to a multi-section variable diameter structure can reduce the number of defective pieces of the adhesive film, and at the same time reduce the cavity wind pressure sensitivity from 66 Å / Pa to 54 Å / Pa.

[0087] (4) By comparing Example 1 and Comparative Example 2, it can be seen that reducing the motor speed during the scanning removal stage can increase the film thickness and increase the wind pressure sensitivity. It can also be seen that the factor affecting the wind pressure sensitivity in Examples 1 to 3 is the motor speed during the scanning removal stage.

[0088] (5) By comparing Example 1 and Comparative Example 3, it can be seen that increasing the duration of motor rotation during the scanning removal stage only affects the film thickness, and the film thickness increases by about 160 angstroms for every 0.1s increase.

[0089] (6) By comparing Example 4 with Comparative Example 4, and by comparing Example 1 with Comparative Example 3, it can be seen that the difference in multi-cavity film thickness is consistent with the actual performance value of adjusting the cutting edge width and the conversion time of the calibration drive motor in the scanning removal and main rotation stages is completely consistent.

[0090] Therefore, this application optimizes the liquid dispensing state by using a multi-stage variable diameter coating nozzle, reducing bubble generation and coating defects, and lowering the sensitivity of film thickness to cavity air pressure. At the same time, by adjusting the rotation speed of the motor, the movement speed of the robotic arm, and the rotation duration of the motor during the scanning and removal stage, it achieves precise control of film thickness and improves the consistency of multiple cavities, effectively improving the integrity of the adhesive film in edge coating, avoiding coating defects, and significantly improving the wafer edge protection effect and product yield.

[0091] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for controlling the thickness of an edge-coated adhesive film, characterized in that, The control method includes at least: applying photoresist to the wafer edge using a coating nozzle with at least two variable diameter sections; and controlling at least one of the following during the scanning and removal stage of the coating process: the rotational speed of the motor, the moving speed of the scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal.

2. The method for controlling the thickness of the edge coating film according to claim 1, characterized in that, The adhesive nozzle has a three-section variable diameter structure; And / or, the material of the adhesive nozzle includes soluble polytetrafluoroethylene.

3. The method for controlling the thickness of the edge adhesive film according to claim 1, characterized in that, The motor rotates at a speed of 300-500 rpm during the scanning process.

4. The method for controlling the thickness of the edge adhesive film according to claim 1, characterized in that, The scanning and removal robotic arm moves at a speed of 6~10 mm / s.

5. The method for controlling the thickness of the edge coating film according to claim 1, characterized in that, The duration of the motor rotation during the scanning process is 1.3 to 3.8 seconds.

6. The method for controlling the thickness of the edge adhesive film according to any one of claims 1 to 5, characterized in that, The control method further includes: adjusting the position of the adhesive nozzles to make the actual performance value of the cut edge width of each adhesive application cavity consistent.

7. The method for controlling the thickness of the edge adhesive film according to any one of claims 1 to 5, characterized in that, The control method further includes: controlling the transition time of the drive motor of each coating cavity to be consistent between the scanning removal stage and the main speed stage.

8. The method for controlling the thickness of the edge adhesive film according to any one of claims 1 to 5, characterized in that, The control method is applied to the edge coating process of 3D and non-flash memory chips.

9. A glue-applying nozzle used in the control method according to any one of claims 1 to 8, characterized in that, The adhesive nozzle has at least two variable diameter sections and is made of soluble polytetrafluoroethylene.

10. A semiconductor coating apparatus, characterized in that, It includes at least the adhesive application nozzle as described in claim 9, and a control module connected to the adhesive application nozzle; The control module is used to control at least one of the following during the scanning and removal stage of the adhesive coating process: the rotation speed of the motor during scanning and removal, the moving speed of the scanning and removal robotic arm, or the rotation duration of the motor during scanning and removal.