An overlay marking structure, its fabrication and overlay measurement method, and a semiconductor device.

By designing high aspect ratio trenches in the overlay marking structure and combining them with optically effective depth detection decoupling, the shadowing effect problem of the overlay marking structure during metal deposition is solved, enabling more accurate overlay measurement, simplifying the etching process and reducing costs.

CN123113252APending Publication Date: 2026-11-17UNITED NOVA TECH - XIANFENG (SHAOXING) CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611209561.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing overlay marking structures are prone to shadowing effects during metal deposition, causing the effective optical center of the metal at the top of the mark to shift from the geometric center at the bottom, and the measurement results cannot truly reflect the actual overlay deviation.

Method used

Design an overlay marking structure, including a first dielectric layer and a second dielectric layer stacked from bottom to top, with trenches penetrating the second dielectric layer and located inside the first dielectric layer, having an aspect ratio of 0.4-0.5. The high aspect ratio trenches form closed cavities through the pre-sealing effect during the metal deposition process, and the effective optical detection depth is less than the trench depth, thereby achieving deep decoupling between the measurement signal and the bottom asymmetric topography.

Benefits of technology

It effectively reduced overlay measurement errors, improved the measurement accuracy of overlay marks, reduced the difficulty of etching control, and enabled rapid application on existing production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113252A_ABST
    Figure CN123113252A_ABST
Patent Text Reader

Abstract

This invention relates to the field of semiconductor manufacturing technology, and discloses an overlay marking structure, a preparation and overlay measurement method, and a semiconductor device. The overlay marking structure includes a marking layer with trenches, the depth of which is less than the thickness of the marking layer. The preparation method includes: providing a marking layer, the marking layer including a first dielectric layer and a second dielectric layer stacked sequentially from bottom to top; forming a photoresist layer on the marking layer, and defining a trench pattern by exposure and development; using the photoresist layer as a mask, etching the second dielectric layer, and continuing to etch a portion of the thickness of the first dielectric layer to form trenches, such that the bottom of the trenches is located inside the first dielectric layer. The technical solution of this invention aims to reduce the deviation in overlay measurement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing technology, and particularly to an overlay marking structure, a method for its fabrication and measurement, and a semiconductor device. Background Technology

[0002] In the manufacturing process of semiconductor integrated circuits, overlay accuracy is a key indicator for measuring the alignment quality of multilayer lithography. To ensure that the circuit patterns of each layer can be accurately superimposed, special overlay marks are usually set on the wafer. Optical measurement equipment is used to detect the relative positional deviation of the upper and lower layer marks, thereby monitoring and correcting the alignment error of the lithography machine in real time.

[0003] Existing traditional overlay markers are typically designed as trench structures. In the manufacturing process, an etching stop layer is usually provided at the bottom of the marker to control the etching depth. Subsequently, metal is filled into the marker trench using processes such as physical vapor deposition. Finally, the overlay accuracy is evaluated by measuring the relative offset between the center position of the metal at the top of the marker and the lithographic pattern of the top layer metal.

[0004] However, the aforementioned existing technologies have significant drawbacks in practical applications. Due to the small aspect ratio and large opening of the existing markers, shading effects are easily generated during metal deposition, especially in the region near the wafer edge. The tilted incident angle results in a thicker metal layer deposited on the positive side of the marker and a thinner metal layer deposited on the negative side. This asymmetric metal deposition causes the effective optical center of the metal at the top of the marker to shift from the geometric center at the bottom, making the measurement results unable to accurately reflect the actual overlay deviation. Summary of the Invention

[0005] The main objective of this invention is to provide an overlay marking structure, a preparation and overlay measurement method, and a semiconductor device, with the aim of reducing the deviation in overlay measurement.

[0006] To achieve the above objectives, the present invention proposes an overlay marking structure, wherein the overlay marking structure includes a marking layer and the marking layer is provided with grooves;

[0007] The marking layer includes a first dielectric layer and a second dielectric layer stacked sequentially from bottom to top;

[0008] The trench penetrates the second dielectric layer, and the bottom of the trench is located inside the first dielectric layer.

[0009] In some embodiments of the present invention, the depth-to-width ratio of the trench is 0.4-0.5.

[0010] In some embodiments of the present invention, the width of the trench is 1.7 μm-2.3 μm.

[0011] In some embodiments of the present invention, the depth of the trench is 0.8 μm - 1.0 μm.

[0012] In some embodiments of the present invention, the material of the marking layer is silicon oxide, silicon oxynitride, or silicon nitride.

[0013] The present invention also provides a method for preparing an overlay marking structure, the method comprising:

[0014] A marking layer is provided, the marking layer comprising a first dielectric layer and a second dielectric layer stacked sequentially from bottom to top;

[0015] A photoresist layer is formed on the marking layer, and the trench pattern is defined by exposure and development.

[0016] Using the photoresist layer as a mask, the second dielectric layer is etched, and a portion of the thickness of the first dielectric layer is further etched to form a trench, such that the bottom of the trench is located inside the first dielectric layer.

[0017] The depth-to-width ratio of the groove is 0.4-0.5.

[0018] In some embodiments of the present invention, the width of the trench is 1.7 μm-2.3 μm.

[0019] The present invention also provides an overlay measurement method, the overlay measurement method comprising:

[0020] Provide the overlay marking structure;

[0021] A metal layer is deposited within the trench;

[0022] The wafer with the deposited metal layer is planarized to remove excess metal layer outside the trench, exposing the metal layer with the top groove;

[0023] A current layer of photoresist is formed on the planarized wafer surface, and the current layer of photoresist is exposed and developed to form an alignment mark window;

[0024] The overlay marking area is illuminated using an optical measurement device;

[0025] Based on the reflected signal, calculate the center coordinates of the top groove in the bottom layer and the center coordinates of the alignment mark window in the current layer, and obtain the offset between the two as the overlay deviation measurement value;

[0026] The optical effective detection depth of the optical measuring device is less than the depth of the groove, so that the collected reflection signal mainly reflects the symmetrical edge of the top groove.

[0027] In some embodiments of the present invention, the material of the metal layer is tungsten, aluminum or copper.

[0028] The present invention also provides a semiconductor device, characterized in that the semiconductor device includes the overlay marking structure.

[0029] The technical solution of this invention forms a marker layer by directly stacking a first dielectric layer and a second dielectric layer. A high aspect ratio trench is formed in the marker layer, and the high aspect ratio trench is used to form a closed cavity by pre-sealing effect during the metal deposition process. Combined with the physical characteristic that the effective optical detection depth is much smaller than the trench depth, the measurement signal and the bottom asymmetric topography are decoupled at a depth. This can effectively reduce the overlay measurement error caused by shadow effect and center offset, and improve the measurement accuracy of the overlay mark. Attached Figure Description

[0030] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0031] Figure 1 This is a schematic diagram of the overlay marking structure of the present invention;

[0032] Figure 2 This invention relates to a method for preparing the overlay marking structure;

[0033] Figure 3 This invention relates to a method for measuring the overlay marking structure;

[0034] Figure 4 This is an electron microscope image of a section of the trench-deposited metal of the present invention;

[0035] Figure 5 Electron micrograph of a section of metal deposited using existing techniques. Attached Figure Description

[0036] 100, Marker layer; 110, First dielectric layer; 120, Second dielectric layer; 200, Trench;

[0037] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0038] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0039] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative positional relationship and movement of each component in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indication will also change accordingly.

[0040] Furthermore, the use of terms such as "first" and "second" in this invention is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of that feature. Additionally, the technical solutions of the various embodiments can be combined with each other, but only on the basis of being achievable by those skilled in the art. When the combination of technical solutions is contradictory or impossible to implement, the user should consider such a combination of technical solutions to be non-existent and not within the scope of protection claimed by this invention.

[0041] See appendix Figure 1 This embodiment provides an overlay marking structure for overlay alignment measurement in integrated circuit photolithography, and aims to solve the measurement distortion problem caused by shadow effect and center offset in traditional low aspect ratio marking structures.

[0042] This marking structure includes a marking layer 100, which has grooves 200. The depth of the grooves 200 is less than the thickness of the marking layer 100, and the depth-to-width ratio of the grooves is 0.4-0.5. Preferably, the width of the grooves 200 is 1.7μm~2.3μm, and the depth is 0.8μm~1.0μm.

[0043] Based on the aforementioned technical characteristics, during the deposition of a metal layer on the overlay marking structure, the high aspect ratio (0.4-0.5) trenches 200, due to their relatively small width and large depth, cause a premature sealing effect within the trenches 200 during the metal layer deposition process, forming closed isolation voids. These isolation voids serve as physical isolation, allowing the metal layer above the voids to grow vertically upwards.

[0044] Therefore, the asymmetrical topography caused by process fluctuations at the bottom cannot be transmitted upwards and is effectively diluted by the vertically grown metal layer above. Ultimately, the top groove exposed after planarization has more symmetrical left and right edges than traditional edges, thereby improving the accuracy of optical measurement equipment in extracting center coordinates.

[0045] In traditional processes, the critical dimension of the overlay precision (OVL) mark is 3μm, the alignment mark is 4μm, and an etching stop layer is set at the bottom of the mark. The etching depth is about 0.7μm, and the aspect ratio is about 0.2. In its low aspect ratio trench, because the opening is wide enough, metal atoms can uniformly fill to the bottom without prematurely sealing the top, thus avoiding this effect.

[0046] Furthermore, during the overlay offset measurement process, the measuring equipment calculates the geometric center of the metal mark using image processing algorithms. Since the volume of the top metal layer is much larger than the volume of the asymmetrical region on the bottom sidewall, the bottom asymmetry signal does not affect the final center of gravity position when the algorithm calculates it. Optical measurements primarily reflect the symmetry of the top.

[0047] Specifically, the effective optical detection depth L of the optical measurement equipment d It is approximately 5nm, while the trench depth H is typically greater than 500nm, L d << H. Therefore, the penetration depth of the measurement beam in the metal is extremely short, and it cannot reach the bottom of the trench 200. The reflected signal almost entirely originates from the metal layer at the top of the trench 200, and the topographic information of the bottom of the trench 200 is physically shielded.

[0048] By implementing pre-sealing at the manufacturing end to suppress the influence of bottom defects, and by using probe depth decoupling to shield bottom interference signals at the measurement end, the measurement signal and the bottom asymmetric topography were successfully decoupled, thus improving the accuracy of overlay deviation measurement.

[0049] The following section further explains the fabrication of the depth decoupling machine of this invention, based on a theoretical model.

[0050] In physical vapor deposition (PVD), asymmetric deposition occurs on the sidewalls of the trench due to the non-perpendicular incident sputtered atoms. Let the alignment mark width be W and the depth be H. The sidewall thickness difference decreases exponentially along the trench depth direction, satisfying:

[0051]

[0052] Where z is the height coordinate measured from the bottom of trench 200 (z=0 is the bottom, z=H is the top). λ represents the initial thickness difference at the bottom (determined by the physical vapor deposition process, typically 5nm~15nm), and λ is the attenuation coefficient (typically 2μm). -1~4μm -1 (This is related to process pressure and target distance). The sidewall thickness difference function shows that the asymmetry is most severe at the bottom of trench 200, decreasing exponentially upwards.

[0053] Furthermore, the equivalent center X of the alignment system measurement meas The deviation δ from the true bottom center X0 is determined by the weighted average of the sidewall thickness differences:

[0054]

[0055] in This is the optical detection weighting function.

[0056] For reflective alignment systems:

[0057]

[0058] Where L d The effective optical detection depth is determined by both the skin depth of the metal and the numerical aperture of the optical system.

[0059]

[0060] When deposited as a metallic Al film, σ≈3.5×10 7 S / m, wavelength λ=663nm, L d ≈5nm. Due to L d << H (in this embodiment, H≈800nm~1000nm) means that the optical system can only detect a very thin layer (about 5nm) at the top of the mark, and the bottom asymmetry does not contribute to the measurement signal.

[0061] Furthermore, Substituting w(z) into the integral, we get:

[0062]

[0063] For typical parameter values: α = 3μm -1 L d =5μm, =10nm; using parameter calculations, the width of trench 200 is 2μm, and the analysis results are shown in Table 1:

[0064] Table 1

[0065] As shown in Table 1, with an aspect ratio of 0.15 as the baseline, when the aspect ratio increases from 0.15 to 0.40, the OVL shift decreases from 8.2 nm to 1.8 nm, representing an improvement of 78%. When the aspect ratio is further increased to 0.75, the OVL shift is reduced to only 0.2 nm, representing an improvement of 98%. The above theoretical calculation results indicate that high aspect ratio trench structures can significantly suppress OVL shift caused by asymmetric sidewall deposition, and the improvement effect increases with increasing aspect ratio.

[0066] Furthermore, an overlay marking structure is formed in the marking layer 100. The marking layer 100 can be a single-layer dielectric layer structure or a multi-layer dielectric layer stacked structure. The material of the marking layer 100 can be selected from any one or more combinations of silicon oxide, silicon oxynitride, or silicon nitride.

[0067] In this embodiment, the marking layer 100 includes a first dielectric layer 110 and a second dielectric layer 120 stacked sequentially from bottom to top. The first dielectric layer 110 is an interlayer dielectric (ILD), and its material is preferably undoped silicon dioxide; the second dielectric layer 120 is an intermetallic dielectric (IMD), and its material is preferably a low dielectric constant material (such as carbon-doped silicon oxide).

[0068] In this technical solution, there is no metal interconnect layer between the first dielectric layer 110 and the second dielectric layer 120. The trench 200 penetrates the second dielectric layer 120, and the bottom of the trench 200 is located inside the first dielectric layer 110. That is, after the trench 200 penetrates the second dielectric layer 120, it continues to extend downward to a portion of the thickness of the first dielectric layer 110 and stops, without penetrating the first dielectric layer 110.

[0069] Specifically, since there is no metal interconnect layer between the first dielectric layer 110 and the second dielectric layer 120, the etching process can penetrate both dielectric layers in one go. The depth of the trench 200 is formed by the combined thickness of the two dielectric layers. Compared with the traditional structure, which can only form the trench 200 within a single dielectric layer, the trench 200 depth of this solution can be significantly increased, thereby achieving a higher aspect ratio with the same trench 200 width. At the same time, in the traditional structure, because there is a metal interconnect layer between the first dielectric layer 110 and the second dielectric layer 120, the etching process must be stopped at the surface of the metal interconnect layer, which places high demands on the etching selectivity and endpoint detection. However, this invention removes the metal interconnect layer between the two dielectric layers, and a trench 200 penetrating both dielectric layers with its bottom located inside the first dielectric layer 110 can be formed in one etching process, further reducing the difficulty of controlling the etching process and improving process stability and repeatability.

[0070] This invention achieves the fabrication of a high aspect ratio trench 200 by directly stacking the first dielectric layer 110 and the second dielectric layer 120 without increasing the additional layout area. This does not require occupying the effective area inside the chip. While realizing the high aspect ratio trench 200, it simplifies the process, reduces the difficulty of etching control, and provides a reliable structural basis for the pre-sealing effect and optical detection depth decoupling in the subsequent metal deposition process.

[0071] like Figure 2 As shown, this embodiment also provides a method for preparing an overlay marking structure, including the following steps:

[0072] Step S100: Provide a marker layer 100, which includes a first dielectric layer 110 and a second dielectric layer 120 stacked sequentially from bottom to top;

[0073] The deposition method for the first dielectric layer 110 and the second dielectric layer 120 can be chemical vapor deposition, plasma-enhanced chemical vapor deposition, or other suitable thin film deposition processes. No metal interconnect layer is formed between the first dielectric layer 110 and the second dielectric layer 120.

[0074] Step S120: A photoresist layer is formed on the marking layer 100, and the trench 200 pattern is defined by exposure and development;

[0075] Specifically, a photoresist layer 400 is coated on the upper surface of the second dielectric layer 120, and patterned openings corresponding to the trench 200 are formed in the photoresist layer 400 through exposure and development processes.

[0076] The thickness and exposure dose of the photoresist layer 400 can be optimized according to the target size of the trench 200 to ensure the sharpness of the pattern edges and dimensional accuracy.

[0077] S130: Using the photoresist layer as a mask, the second dielectric layer 120 is etched, and the first dielectric layer 110 of a certain thickness is further etched to form a trench 200, so that the bottom of the trench 200 is located inside the first dielectric layer 120.

[0078] Plasma etching is the preferred etching process, and the etching gas is preferably a fluorocarbon-based gas, such as a mixture of carbon tetrafluoride and trifluoromethane. By adjusting process parameters such as the flow rate ratio of the etching gas, RF power, and chamber pressure, the etching rate and etching morphology can be precisely controlled.

[0079] Specifically, the etching process first penetrates the second dielectric layer 120. When the etching reaches the upper surface of the first dielectric layer 110, if there is a material difference between the first dielectric layer 110 and the second dielectric layer 120, the interface can be identified using endpoint detection technology (such as optical emission spectroscopy endpoint detection). Subsequently, etching continues to a portion of the thickness of the first dielectric layer 110 until the bottom of the trench 200 reaches a predetermined depth within the first dielectric layer 110. By controlling the etching time or using endpoint detection, the final depth of the trench 200 can be precisely controlled.

[0080] Through the above etching process, the formed trench 200 penetrates the second dielectric layer 120 and its bottom is located inside the first dielectric layer 110. The aspect ratio of the trench 200 is controlled between 0.4 and 0.5.

[0081] Preferably, the trench 200 has a width of 1.7 μm to 2.3 μm and a depth of 0.8 μm to 1.0 μm. After etching, the photoresist layer 400 is removed. In this embodiment, the trench 200 has a depth of 0.9 μm and a width of 2 μm.

[0082] This fabrication method does not introduce any additional or special process equipment or materials. It achieves the fabrication of high aspect ratio overlay marks solely through the synergistic optimization of etching time (i.e., etching depth control) and photolithographic pattern size (i.e., trench width control) in existing etching processes. This significantly reduces the cost of technology upgrades and facilitates rapid implementation and application on existing production lines.

[0083] like Figure 3 As shown, this embodiment also provides an overlay measurement method, including the following steps:

[0084] Step S210: Provide an overlay marking structure;

[0085] Specifically, the overlay marking structure provided in any of the above embodiments includes a groove 200 in the marking layer 100, wherein the aspect ratio of the groove 200 is 0.4-0.5. Preferably, the marking layer 100 includes a first dielectric layer 110 and a second dielectric layer 120, wherein the groove 200 penetrates the second dielectric layer 120 and extends into the interior of the first dielectric layer 110.

[0086] Step S220: Deposit a metal layer in trench 200;

[0087] The material of the metal layer can be selected from tungsten, aluminum, or copper. In this embodiment, a physical vapor deposition (PVD) metal deposition process is used.

[0088] Step S230: Planarize the wafer with the deposited metal layer, remove excess metal layer outside the trench 200, and expose the metal layer with the top groove.

[0089] The wafer with the deposited metal layer is planarized to remove excess metal layer outside the trench 200, making the upper surface of the metal layer in the top region of the trench 200 flush with the upper surface of the marking layer 100. Chemical mechanical polishing is preferably used for planarization.

[0090] Step S240: Form the current layer photoresist layer on the planarized wafer surface, and expose and develop the current layer photoresist layer to form alignment mark windows;

[0091] A current layer photoresist layer 600 is coated on the planarized wafer surface, and the current layer photoresist layer 600 is exposed and developed to form an alignment mark window 610. The size of the alignment mark window 610 may be different from the size of the trench 200 so that the measurement equipment can distinguish between the bottom layer mark and the current layer mark during image processing.

[0092] Step S250: Illuminate the overlay marking area using an optical measurement device;

[0093] The overprinted marking area is illuminated using optical measurement equipment, and the reflected signals are collected.

[0094] In this embodiment, since the depth H of the trench 200 is 800nm~1000nm, and the effective optical detection depth L... d The difference is only 3nm to 10nm, more than two orders of magnitude. According to optical principles, for common metals such as tungsten, aluminum, and copper, their penetration depth in the visible light band is only a few nanometers. The measurement beam cannot actually penetrate the metal layer several nanometers thick at the top of the trench 200 to reach the bottom of the trench. The reflected signal almost entirely originates from the metal layer in the top region of the trench.

[0095] Based on the reflected signal, calculate the center coordinates of the metal layer in the top region of the trench 200 and the center coordinates of the current layer alignment mark window 610, and obtain the offset between the two as the overlay deviation measurement value.

[0096] This measurement method directly addresses the relationship between overlay measurement error and trench depth. By leveraging the pre-sealing effect of high aspect ratio trenches and the physical limitations of the effective optical detection depth, it achieves depth decoupling between the measurement signal and the asymmetric topography at the bottom. Based on the fundamental principles of overlay measurement error, when the measurement signal primarily originates from the symmetrical region at the top of the trench, the contribution of the asymmetric topography at the bottom, caused by the shading effect, to the measurement results is reduced, thereby improving the accuracy of overlay measurement.

[0097] In actual process development, it is also necessary to consider that the etching depth is limited by the etching menu—the actual etching depth of trenches 200 with different critical dimensions will vary under the same etching conditions. Therefore, this application will remove the etching stop layer at the bottom of the marker and select multiple groups of different trench widths for group verification.

[0098] Specifically, experiments were conducted using 1.5μm, 1.7μm, 2.0μm, 2.3μm, and 3.0μm as the design values ​​for the trench width, respectively. The morphology, etching depth, and recognition performance of the measurement equipment for each size mark were evaluated under the same etching menu.

[0099] When the width is 1.5μm, although the depth-to-width ratio is high, the narrow bottom width of the trench makes it difficult to fill the metal, and there is a risk of premature over-sealing or incomplete filling.

[0100] When the width is 1.7 μm, the trench morphology is good and the metal filling performance is better than that at 1.5 μm;

[0101] When the width is 2.0 μm, the trench morphology is good, the etching depth reaches the expected value, the metal filling is uniform, and the image contrast and edge sharpness meet the OVL measurement requirements.

[0102] When the width is 2.3μm or more, the etching depth decreases under the same etching time due to the increased trench width, the aspect ratio decreases, and the improvement effect is weakened.

[0103] When the width is 3.0μm, the aspect ratio drops to about 0.2~0.25, which is close to the level of traditional structures, and the improvement effect is not obvious.

[0104] See appendix Figure 4 A width of 2.0 μm and a depth of 900 nm were selected as the dimensions for the overlay marking mechanism. (See appendix.) Figure 5 Compared with the traditional structure (overlay mark critical size 3.0μm, alignment mark 4.0μm, etch stop layer between IMD and ILD, etch depth 0.7μm, aspect ratio 0.2), the overlay offset of edge grains was reduced from 580nm to 210nm, an improvement rate of 63.8%.

[0105] The above experimental verification shows that the high aspect ratio overlay marking structure of the present invention can achieve significant improvement in OVL offset under actual production line conditions, and has good industrial applicability.

[0106] The present invention also provides a semiconductor device, which may be a chip, wafer or intermediate structure thereof that has completed some or all of the manufacturing processes.

[0107] Specifically, it includes the overlay marking structure of any of the above embodiments. By utilizing the high aspect ratio trench 200 to form a closed cavity during the metal deposition process through pre-sealing, and combined with the physical characteristic that the effective optical detection depth is much smaller than the depth of the trench 200, depth decoupling between the measurement signal and the asymmetrical topography at the bottom is achieved. This effectively reduces overlay measurement errors caused by shadowing effects and center offset, fundamentally improving the measurement accuracy of the overlay marking. Furthermore, it requires no major modifications to existing production lines, demonstrating good industrial applicability and promotional value.

[0108] It is understood that although the present invention has been disclosed above with reference to preferred embodiments, these embodiments are not intended to limit the present invention. For any person skilled in the art, many possible variations and modifications can be made to the technical solutions of the present invention based on the disclosed technical content, or equivalent embodiments can be modified accordingly, without departing from the scope of the present invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the present invention shall still fall within the protection scope of the present invention.

[0109] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

Claims

1. A lithography mark structure, comprising: The overlay marking structure includes a marking layer, the marking layer is provided with grooves, and the marking layer includes a first dielectric layer and a second dielectric layer stacked from bottom to top; The trench penetrates the second dielectric layer, and the bottom of the trench is located inside the first dielectric layer.

2. The overlay mark structure of claim 1, wherein, The depth-to-width ratio of the trench is 0.4-0.

5.

3. The overlay mark structure of claim 2, wherein, The width of the groove is 1.7μm-2.3μm.

4. The overlay marking structure as described in claim 2 or 3, characterized in that, The depth of the trench is 0.8μm - 1.0μm.

5. The overlay marking structure as described in claim 1, characterized in that, The material of the marking layer is silicon oxide, silicon oxynitride, or silicon nitride.

6. A method of manufacturing an overlay mark structure, the method comprising: The preparation method includes: A marking layer is provided, the marking layer comprising a first dielectric layer and a second dielectric layer stacked sequentially from bottom to top; A photoresist layer is formed on the marking layer, and the trench pattern is defined by exposure and development. Using the photoresist layer as a mask, the second dielectric layer is etched, and a portion of the thickness of the first dielectric layer is further etched to form a trench, such that the bottom of the trench is located inside the first dielectric layer.

7. The method of claim 6, wherein the overlay mark structure is formed by a process comprising: The depth-to-width ratio of the trench is 0.4-0.

5.

8. A method of overlay measurement, the method comprising: The overlay measurement method includes: Provides an overlay marking structure as described in any one of claims 1 to 5; A metal layer is deposited within the trench; The wafer with the deposited metal layer is planarized to remove excess metal layer outside the trench, exposing the metal layer with the top groove; A current layer of photoresist is formed on the planarized wafer surface, and the current layer of photoresist is exposed and developed to form an alignment mark window; The overlay marking area is illuminated using an optical measurement device; Based on the reflected signal, calculate the center coordinates of the top groove in the bottom layer and the center coordinates of the alignment mark window in the current layer, and obtain the offset between the two as the overlay deviation measurement value; The optical effective detection depth of the optical measuring device is less than the depth of the groove, so that the collected reflection signal mainly reflects the symmetrical edge of the top groove.

9. The overlay measurement method of claim 8, wherein, The metal layer is made of tungsten, aluminum, or copper.

10. A semiconductor device, characterized by comprising: The semiconductor device includes the overlay marking structure as described in any one of claims 1-5.