Electrodes for lithium secondary batteries, methods for manufacturing the same, and lithium secondary batteries including the same.
By using a single-particle active material layer in the lithium secondary battery electrode and controlling its average diameter and most frequent particle size, the problem of unstable power and storage characteristics in the manufacturing process of lithium secondary battery electrodes is solved, and improved conductivity and high-temperature storage characteristics are achieved.
Patent Information
- Application Number
- CN202610670024.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
In the manufacturing process of existing lithium secondary batteries, it is difficult to achieve stable and balanced power and storage characteristics in the electrodes.
An active material layer containing single-particle active substances is used. The average diameter and most frequent particle size of the active substances are controlled to meet the requirements of Equation 1 (0.8≤DB-DA≤2.6) within a specific range, and the active material layer is formed by pressing with a roller press.
It improves the conductivity and power characteristics of lithium secondary batteries, reduces the capacity degradation rate, and enhances high-temperature storage characteristics.
Smart Images

Figure CN123120619A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an electrode for a lithium secondary battery, a method for manufacturing the electrode thereof, and a lithium secondary battery including the electrode thereof. Background Technology
[0002] Rechargeable batteries are batteries that can be recharged and discharged repeatedly. With the development of the information communication and display industries, rechargeable batteries are widely used as power sources for portable electronic communication devices such as portable cameras, mobile phones, and laptops. In addition, in recent years, battery packs that include rechargeable batteries have been developed for use as power sources for environmentally friendly vehicles such as electric vehicles and hybrid vehicles.
[0003] Examples of rechargeable batteries include lithium-ion batteries, nickel-cadmium batteries, and nickel-metal hydride batteries. Among them, lithium-ion batteries have high operating voltage and energy density per unit weight, and are advantageous for charging speed and lightweight design, thus they are being actively researched and developed.
[0004] With the expanding applications of lithium-ion rechargeable batteries, there is a growing demand for longer lifespans, higher capacity, and improved operational stability. Therefore, research and development of positive electrode active materials for lithium-ion rechargeable batteries is actively underway. Summary of the Invention
[0005] (a) Technical problems to be solved One technical problem of the present invention is to provide an electrode for lithium secondary batteries with improved power characteristics and storage characteristics.
[0006] One technical problem of the present invention is to provide a lithium secondary battery with improved power characteristics and storage characteristics.
[0007] One technical problem of the present invention is to provide a method for manufacturing an electrode for a lithium secondary battery with improved power characteristics and storage characteristics.
[0008] (II) Technical Solution An electrode for a lithium secondary battery according to an embodiment of the present invention may include an active material layer comprising an active material in the form of single particles, wherein the active material in the form of single particles may satisfy the following formula 1.
[0009] [Formula 1] 0.8≤D B -D A ≤2.6 In Equation 1, D A The average diameter is the average of the single-particle form of the active material measured from scanning electron microscope (SEM) images. This average diameter is the average of values greater than 0.5 μm among the maximum diameters passing through the center of the active material in the SEM images.B The most frequent particle size of the active material in single-particle form is measured from a particle size distribution (PSD) plot with the x-axis representing particle size and the y-axis representing volume percentage. The most frequent particle size is the particle size in which the maximum peak appears in the particle size range below 20 μm.
[0010] In one embodiment, in Equation 1, the average diameter (D) A ) and the most frequent particle size (D B The value can be based on the active material contained in the active material layer of the electrode for the lithium secondary battery manufactured by a pressing or rolling process.
[0011] In one implementation, the average diameter (D) A The most frequent particle size (D) can be measured from the SEM image of the cut surface after the active material layer is vertically cut. B The particle size distribution of the active substance can be determined from an organic solvent containing the active substance, obtained by immersing the active substance layer in an organic solvent, and then extracting and drying it.
[0012] In one embodiment, the average diameter (D) of the active material in single-particle form A The thickness can range from 1.2 μm to 2.4 μm.
[0013] In one embodiment, the most frequent particle size (D) of the active substance in single-particle form B The size can range from 2.2 μm to 4.2 μm.
[0014] In one embodiment, the active material contained in the active material layer may be composed of the active material in the form of single particles.
[0015] In one embodiment, the electrode density of the lithium secondary battery electrode can be from 3.0 g / cm³ (cc) to 3.9 g / cm³.
[0016] In one embodiment, the electrode density of the lithium secondary battery electrode can be from 3.5 g / cm³ to 3.7 g / cm³.
[0017] In one embodiment, the electrode for the lithium secondary battery may further include a current collector, and the active material layer may be located on one or both sides of the current collector.
[0018] In one embodiment, the thickness of the active material layer can be from 125 μm to 160 μm.
[0019] In one embodiment, the electrode for the lithium secondary battery can be a positive electrode.
[0020] A lithium secondary battery according to an embodiment of the present invention may include: a positive electrode; and a negative electrode, the negative electrode being disposed opposite to the positive electrode, wherein the positive electrode may be an electrode for a lithium secondary battery as described above.
[0021] A method for manufacturing an electrode for a lithium secondary battery according to an embodiment of the present invention may include: coating and drying an electrode active material slurry, and pressing the dried electrode active material slurry through a roller press to form an active material layer containing active material in the form of single particles, wherein the pressing gap between the upper and lower rollers of the roller press may be 130 μm to 160 μm, and the active material in the form of single particles contained in the active material layer may satisfy the following formula 1.
[0022] [Formula 1] 0.8≤D B -D A ≤2.6 In Equation 1, D A The average diameter is the average of the single-particle form of the active material as measured from scanning electron microscopy (SEM) images. This average diameter is the average of values greater than 0.5 μm among the maximum diameters passing through the center of the active material in the SEM images. B The most frequent particle size of the active substance in single-particle form is measured from a particle size distribution (PSD) plot with particle size on the x-axis and volume % on the y-axis. The most frequent particle size is the particle size in which the maximum peak appears in the particle size range below 20 μm.
[0023] In one embodiment, the electrode active material slurry can be prepared at 15 mg / cm³. 2 Up to 30 mg / cm 2 The loading amount is coated on one or both sides of the current collector and dried.
[0024] In one embodiment, the pressing gap between the upper and lower rollers of the roller press can be from 135 μm to 158 μm.
[0025] (III) Beneficial Effects The electrode for lithium secondary batteries according to embodiments of the present invention can achieve improved conductivity and reduced capacity degradation rate.
[0026] The lithium secondary battery according to the embodiments of the present invention can achieve improved power characteristics and high-temperature storage characteristics.
[0027] The method for manufacturing an electrode for a lithium secondary battery according to an embodiment of the present invention can provide an electrode for a lithium secondary battery as described above.
[0028] The lithium secondary battery electrode and the lithium secondary battery including the electrode of the present invention can be widely used in green technology fields such as electric vehicles, battery charging stations, and other battery-powered solar and wind power generation. The lithium secondary battery electrode and the lithium secondary battery including the electrode of the present invention can also be used in eco-friendly electric vehicles and hybrid vehicles that prevent climate change by suppressing air pollution and greenhouse gas emissions. Attached Figure Description
[0029] Figure 1 This is a SEM image of the cross-section of the active material layer of the electrode manufactured in Example 1.
[0030] Figure 2 This is a particle size distribution diagram of the active material contained in the active material layer of the electrode manufactured in Example 1.
[0031] Figure 3 This is a schematic plan view of a lithium secondary battery according to an exemplary embodiment.
[0032] Figure 4 This is a schematic cross-sectional view of a lithium secondary battery according to an exemplary embodiment.
[0033] Figure 5 This is a schematic process flow diagram of a method for manufacturing an electrode for a lithium secondary battery according to an exemplary embodiment. Detailed Implementation
[0034] Hereinafter, exemplary embodiments of the present invention will be described in detail with reference to the accompanying drawings, so that those skilled in the art can easily implement the invention.
[0035] <Electrodes for Lithium Secondary Batteries> An electrode for a lithium secondary battery according to an embodiment of the present invention includes an active material layer comprising an active material in the form of single particles, wherein the active material in the form of single particles satisfies the following formula 1.
[0036] [Formula 1] 0.8≤D B -D A ≤2.6 In Equation 1, D A The average diameter (D) of the active substance in single-particle form, as measured from scanning electron microscope (SEM) images. A The average diameter (D) A D is the average of the values greater than 0.5 μm of the maximum diameter passing through the center of the active substance in the SEM image. BThe most frequent particle size (D) of the active material in single-particle form, measured from a particle size distribution (PSD) plot with particle size on the x-axis and volume % on the y-axis. B The most frequent particle size (D) B () is the particle size in which the maximum peak appears in the particle size range below 20 μm.
[0037] The average diameter (D) A ) and the most frequent particle size (D B The values are based on those of the active material contained in the active material layer of an electrode manufactured by pressing or rolling processes.
[0038] That is, the average diameter (D) A ) and the most frequent particle size (D B This is not based on values measured for the active material contained in the electrode active material slurry used to form the active material layer.
[0039] The size or shape of the active material (hereinafter referred to as primary active material) contained in the electrode active material slurry may be deformed during the electrode manufacturing process due to processes such as pressing. Therefore, when only the size or shape of the primary active material is controlled, the manufactured electrode cannot stably and uniformly achieve the required power and storage characteristics.
[0040] In an electrode for a lithium secondary battery according to an exemplary embodiment of the present invention, by making the average diameter (D) of the active material contained in the active material layer in the manufactured electrode... A ) and most frequent particle size (D B Satisfying Equation 1 can result in improved power and storage characteristics, as well as enhanced reliability.
[0041] The average diameter (D) A It can be measured, for example, by the following method.
[0042] After the lithium secondary battery electrode is perpendicularly cut along its thickness direction, a scanning electron microscope (SEM) image of the cut surface of the active material layer can be captured at 5000x magnification. When capturing the SEM image, the total number of active materials contained therein can be 50 or more. The total number of active materials contained in the SEM image can be, for example, 50 to 150. Using image processing software (Image-J), the maximum diameter of the cross-section of all active materials present in the SEM image can be calculated. The maximum diameter is the length of the longest straight line extending from the center of each active material to its outermost edge. The average value of the obtained maximum diameters greater than 0.5 μm is defined as the average diameter (D). A ).
[0043] The most frequent particle size (D) B It can be measured, for example, by the following method.
[0044] The electrodes for the aforementioned lithium secondary batteries can be prepared into samples of predetermined sizes, such as samples with width (x), length (y), and thickness (z) of 1 mm × 1 mm × 150 μm. The samples can be immersed in an organic solvent, such as N-methyl-2-pyrrolidone (NMP), and subjected to sonication at room temperature. The solids of the active material layer can be separated from the sonicated sample. The separated solids are then immersed in an organic solvent, such as NMP, and subjected to sonication at room temperature to obtain a dispersion. The sonication is sufficient to disperse the active material in the dispersion; for example, the sonication can be performed for more than 2 hours, but is not limited thereto. The active material can be extracted from the dispersion by filtration and dried to obtain active material with removed moisture. The drying can be performed, for example, in a vacuum oven, and only needs to be carried out to remove moisture; for example, the drying can be performed for 24 hours. The obtained active material can be subjected to particle size analysis using a particle size analyzer to obtain a particle size distribution map. The particle size distribution map can be a particle size distribution curve with the x-axis representing particle size and the y-axis representing volume percentage. Based on the particle size distribution map, the particle size that exhibits the highest volume percentage (i.e., the largest peak) within the particle size range below 20 μm is defined as the most frequent particle size (D). B ).
[0045] In some embodiments, the active substance in single-particle form may satisfy the following formula 1-1.
[0046] [Equation 1-1] 1.9≤D B -D A ≤2.6 In Equation 1-1, the average diameter (D) A ) and the most frequent particle size (D B As described above.
[0047] The term "single particle" as used in this specification is used to exclude secondary particles, such as those formed by the aggregation of multiple primary particles. For example, in particles having a single particle form, secondary particle structures assembled or aggregated from primary particles (e.g., 20 or more, 30 or more, 40 or more, 50 or more, etc.) can be excluded.
[0048] The term "single particle" as used in this specification does not exclude a monolithic form, for example, observed as two or more but less than 20 or as a range of 2 to 10 single particles attached or closely adhered to each other (e.g., in scanning electron microscope (SEM) images).
[0049] That is, the single-particle form can refer to a particle that exists essentially as a single particle, and can include forms in which adjacent particles are in partial contact or tightly adhered during the manufacturing process. However, the single-particle form does not include secondary particle structures that are assembled or aggregated from multiple primary particles and behave like a single particle.
[0050] In some embodiments, the average diameter (D) of the active material in single-particle form A The micrometer can be, for example, 1.2 μm to 2.4 μm, 1.4 μm to 2.2 μm, or 1.7 μm to 1.9 μm.
[0051] When the average diameter (D) A When the above range is met, the power characteristics and high-temperature characteristics of the electrode can be improved simultaneously.
[0052] In some embodiments, the most frequent particle size (D) of the active substance in single-particle form B The micrometer can be, for example, 2.2 μm to 4.2 μm, 2.8 μm to 4.0 μm, or 3.4 μm to 3.8 μm.
[0053] When the most frequent particle size (D) B When the particle size is too large, it may cause particle cracks during rolling, which may lead to undesirable side reactions within the electrode, potentially reducing high-temperature performance. B If the particle size is too small, insufficient contact between particles may lead to a decrease in power characteristics.
[0054] In one embodiment, the active material in single-particle form may comprise a lithium metal oxide, which may be represented, for example, by the following chemical formula 1.
[0055] [Chemical Formula 1] Li x M1 a M2 b M3 c O y In the chemical formula 1, M1 can be Ni, M2 can be Co, and M3 can contain at least one of Mn and Al.
[0056] In the Chemical Formula 1, x, y, a, b and c may respectively satisfy 0<x≤1.1, 2≤y≤2.02, 0≤a≤1, 0≤b≤1, 0≤c≤1 and / or 0<a+b+c≤1.
[0057] The chemical structure represented by the Chemical Formula 1 denotes the bonding relationship included in the layered structure or crystal structure of the active material, and does not exclude the introduction of other additional elements.
[0058] For example, the active material in the form of a single particle may further include an auxiliary element for enhancing the chemical stability of the active material or the layered structure / crystal structure. The auxiliary element may be further incorporated into the layered structure / crystal structure and form a bond together with the main active element, and it should be understood that such a case is also included within the scope of the chemical structure represented by the Chemical Formula 1.
[0059] As a non-limiting example, the auxiliary element may be, for example, one or more metal elements selected from Mn, Na, Mg, Ca, Y, Ti, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Sr, Ba, Ra, P and Zr.
[0060] In one embodiment, the active material layer may further include at least one of a binder and a conductive material.
[0061] As non-limiting examples, the binder may include, for example, organic binders such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidenefluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and water-based binders such as styrene-butadiene rubber (SBR). These may be used alone or in combination of two or more. The binder may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0062] As non-limiting examples, the conductive material may include, for example, a linear conductive material, a point-type conductive material, or both. The linear conductive material may include, for example, carbon nanotubes (CNTs), and the carbon nanotubes (CNTs) may include single-walled CNT (SWCNT), double-walled CNT (DWCNT), multi-walled CNT (MWCNT), rope CNT, and the like.
[0063] The length of the linear conductive material can be, for example, from 15 μm to 65 μm.
[0064] The point-type conductive material may include, for example, carbon-based conductive materials such as graphite, carbon black, and graphene; metal-based conductive materials such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3; or combinations thereof.
[0065] The circularity of the dot-shaped conductive material can be, for example, 0.7 to 1, 0.8 to 1, or 0.9 to 1.
[0066] In some embodiments, the electrode may further include a current collector, and the active material layer may be located on one or both sides of the current collector.
[0067] In some embodiments, the active material layer may contain only the single-particle form of active material. That is, the active material in the active material layer may be composed of the single-particle form of active material. Therefore, the power characteristics and high-temperature stability of the electrode including the active material layer can be improved simultaneously.
[0068] In one embodiment, the content of the active substance in the active substance layer can be 90% to 98% by weight, 92% to 97% by weight, or 92% to 96% by weight, based on the total weight of the active substance layer.
[0069] In one embodiment, the adhesive content in the active material layer can be, for example, 0.5% to 4.0% by weight, 0.5% to 3.0% by weight, or 1.0% to 1.5% by weight, based on the total weight of the active material layer. When the adhesive content is within the above range, the adhesion of the active material layer to the current collector can be further improved.
[0070] In one embodiment, the content of the conductive material in the active material layer can be, for example, 0.5% to 7.0% by weight, 0.5% to 5.0% by weight, or 1.0% to 2.5% by weight, based on the total weight of the active material layer. When the content of the conductive material is within the above range, the conductivity of the active material layer can be further improved.
[0071] In some embodiments, the electrode density can be, for example, 3.0 g / cm³ to 3.9 g / cm³, 3.2 g / cm³ to 3.8 g / cm³, or 3.5 g / cm³ to 3.7 g / cm³. Electrode density can be defined as the mass per unit volume of the active material layer, and can be calculated by measuring the mass per unit area and the thickness of the active material layer. By having an electrode density within the aforementioned range, the storage characteristics of the electrode can be further improved.
[0072] In some implementations, the electrode can be a positive electrode.
[0073] In some embodiments, the thickness of the active material layer can be, for example, 125 μm to 160 μm or 130 μm to 140 μm.
[0074] As a non-limiting example, the current collector may include a metal foil, a metal plate, etc. The metal foil or the metal plate may include, for example, stainless steel, iron, aluminum, copper, germanium, nickel, titanium, magnesium, or alloys of two or more of these metals.
[0075] The thickness of the current collector can be, for example, 10 μm to 30 μm or 10 μm to 20 μm.
[0076] In some implementations, the current collector can be a positive current collector.
[0077] <Lithium secondary batteries> Figure 3 This is a schematic plan view of a lithium secondary battery according to an exemplary embodiment. Figure 4 This is a schematic cross-sectional view of a lithium secondary battery according to an exemplary embodiment. Figure 4 It is along Figure 3 A cross-sectional view taken along the thickness direction of the I-I' line.
[0078] A lithium secondary battery according to an exemplary embodiment includes a positive electrode 100 and a negative electrode 130 disposed opposite to the positive electrode 100. The positive electrode 100 is an electrode for a lithium secondary battery according to an exemplary embodiment, including an active material layer comprising the above-described active material in the form of single particles. The active material layer may be a positive electrode active material layer 110.
[0079] The negative electrode 130 may include a negative electrode current collector 125 and a negative electrode active material layer 120 located on one or both sides of the negative electrode current collector 125.
[0080] The negative current collector 125 may include, for example, copper foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper, a polymer substrate coated with a conductive metal, and the like. The thickness of the negative current collector 125 may be, for example, 10 μm to 50 μm.
[0081] The negative active material layer 120 may include a negative active material. The negative active material may include, for example, carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, and carbon fibers; lithium metal; lithium alloys; silicon (Si)-containing substances or tin (Sn)-containing substances, etc. These may be used alone or in combination of two or more.
[0082] The amorphous carbon may include hard carbon, soft carbon, coke, mesocarbon microbead (MCMB), mesophase pitch-based carbon fiber (MPCF), and the like.
[0083] The crystalline carbon may include graphite-based carbon such as natural graphite, artificial graphite, graphitized coke, graphitized mesocarbon microbead (MCMB), graphitized mesophase pitch-based carbon fiber (MPCF), and the like.
[0084] The lithium metal may include pure lithium metal and / or lithium metal formed with a protective layer for suppressing dendrite growth and the like.
[0085] Elements contained in the lithium alloy may include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, indium, and the like. These may be used alone or in combination of two or more.
[0086] The silicon-containing substance may include Si, SiO x (0<x<2), metal-doped SiO x (0<x<2), silicon-carbon composites, and the like.
[0087] The metal may include lithium and / or magnesium, and the metal-doped SiO x (0<x<2) may include metal silicate.
[0088] In an exemplary embodiment, a separator 140 may be disposed between the positive electrode 100 and the negative electrode 130. The separator 140 may be configured to prevent a short circuit between the positive electrode 100 and the negative electrode 130 and allow the flow of ions. For example, the thickness of the separator may be 10 μm to 20 μm.
[0089] For example, the separator 140 may include a porous polymer film or a porous non-woven fabric.
[0090] The porous polymer membrane may include polyolefin-based polymers such as ethylene polymers, propylene polymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers. These may be used alone or in combination of two or more.
[0091] The porous nonwoven fabric may include high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0092] The diaphragm 140 may also comprise a ceramic-based material. For example, inorganic particles may be coated on or dispersed in the polymer membrane to improve heat resistance.
[0093] The diaphragm 140 may have a single-layer or multi-layer structure comprising the aforementioned polymer membrane and / or nonwoven fabric.
[0094] According to an exemplary embodiment, the battery cell can be defined by a positive electrode 100, a negative electrode 130, and a separator 140, and an electrode assembly 150 can be formed, for example, in the form of a jelly roll, by stacking multiple battery cells. For example, the electrode assembly 150 can be formed by winding, stacking, z-folding, stack-folding, etc. of the separator 140.
[0095] The electrode assembly 150 can be housed together with the electrolyte within the housing 160, thereby defining a lithium secondary battery. According to an exemplary embodiment, the electrolyte can be a non-aqueous electrolyte.
[0096] Non-aqueous electrolytes may contain a lithium salt as the electrolyte and an organic solvent. For example, the lithium salt may be made from Li... + X - This is represented, for example, by the anion (X) of the lithium salt. - ), can be exemplified by F - Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - PF6 - (CF3)2PF4 - (CF3)3PF3 -, (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , (CF3CF2SO2)2N - , and the like.
[0097] The organic solvent may be, for example, propylene carbonate (PC), ethylene carbonate (EC), butene carbonate, diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, ethyl propyl carbonate, dipropyl carbonate, vinylene carbonate, methyl acetate (MA), ethyl acetate (EA), n-propylacetate (n-PA), 1,1-dimethylethyl acetate (DMEA), methyl propionate (MP), ethyl propionate (EP), ethyl fluoroacetate (FEA), ethyl difluoroacetate (DFEA), ethyl trifluoroacetate (TFEA), dibutyl ether, tetraethylene glycol dimethyl ether (TEGDME), and diethylene glycol dimethyl ether. These include ether (DEGDME), dimethoxyethane, tetrahydrofuran (THF), 2-methyltetrahydrofuran, ethyl alcohol, isopropyl alcohol, dimethyl sulfoxide, acetonitrile, diethoxyethane, sulfolane, γ-butyrolactone, propylene sulfite, etc. These can be used alone or in combination of two or more.
[0098] The non-aqueous electrolyte may further contain additives. These additives may include, for example, cyclic carbonate compounds, fluorinated carbonate compounds, sulfonyl lactone compounds, cyclic sulfate compounds, cyclic sulfite compounds, phosphate compounds, borate compounds, etc. These may be used alone or in combination of two or more.
[0099] The cyclic carbonate-based compound may include vinylene carbonate (VC), vinyl ethylene carbonate (VEC), etc.
[0100] The fluorine-substituted cyclic carbonate compounds may include fluoroethylene carbonate (FEC), etc.
[0101] The sulfonyl compounds may include 1,3-propane sultone, 1,3-propene sultone, 1,4-butane sultone, etc.
[0102] The cyclic sulfate-based compounds may include 1,2-ethylene sulfate, 1,2-propylene sulfate, etc.
[0103] The cyclic sulfite-based compounds may include ethylene sulfite, butylene sulfite, etc.
[0104] The phosphate-based compounds may include lithium difluorobis-oxalato phosphate, lithium difluorophosphate, etc.
[0105] The borate-based compounds may include lithium bis(oxalate) borate, etc.
[0106] In some embodiments, a solid electrolyte can be used instead of the non-aqueous electrolyte. In this case, the lithium secondary battery can be made into an all-solid-state battery. Furthermore, a solid electrolyte layer can be disposed between the positive electrode 100 and the negative electrode 130 instead of the separator 140.
[0107] The solid electrolyte may include a sulfide-based electrolyte. As a non-limiting example, the sulfide-based electrolyte may include Li₂S-P₂S₅, Li₂S-P₂S₅-LiCl, Li₂S-P₂S₅-LiBr, Li₂S-P₂S₅-LiCl-LiBr, Li₂S-P₂S₅-Li₂O, Li₂S-P₂S₅-Li₂O-LiI, Li₂S-SiS₂, Li₂S-SiS₂-LiI, Li₂S-SiS₂-LiBr, Li₂S-SiS₂-LiCl, Li₂S-SiS₂-B₂S₃-LiI, Li₂S-SiS₂-P₂S₅-LiI, Li₂S-B₂S₃, and Li₂S-P₂S₅-Z. m Sn (m and n are positive numbers, Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are positive numbers, M is P, Si, Ge, B, Al, Ga, or In), Li7-xPS6-xCl x (0≤x≤2), Li7-xPS6-xBr x (0≤x≤2), Li7-xPS6-xI x (0≤x≤2), etc. These can be used individually or in combination of two or more.
[0108] In one embodiment, the solid electrolyte may further include oxide-based amorphous solid electrolytes such as Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3, and Li2O-B2O3-ZnO.
[0109] like Figure 3 and Figure 4 As shown, the tabs (positive tab and negative tab) can protrude from the positive current collector 105 and negative current collector 125 belonging to each cell and extend to a side of the housing 160. The tabs can be fused to said side of the housing 160 to form electrode leads (positive lead 107 and negative lead 127) extending to or exposed outside the housing 160.
[0110] The lithium secondary battery can be manufactured in shapes such as cylindrical, prismatic, pouch, or coin, for example, using a can.
[0111] <Manufacturing Method of Electrodes for Lithium Secondary Batteries> Figure 5 This is a schematic process flow diagram illustrating a method for manufacturing an electrode for a lithium secondary battery according to an exemplary embodiment.
[0112] The manufacturing method includes: coating and drying an electrode active material slurry (S10); pressing the dried electrode active material slurry through a roller press to form an active material layer containing single-particle active materials (S20). The pressing gap between the upper and lower rollers of the roller press is 130 μm to 160 μm. In the manufacturing method, the active material layer can be formed such that the single-particle active materials satisfy the form of Formula 1 above.
[0113] In some embodiments, the pressing gap between the upper and lower rollers of the roller press can be, for example, 135 μm to 158 μm, 140 μm to 145 μm, or 141 μm to 143 μm.
[0114] The manufacturing method described above can be used to manufacture electrodes for lithium secondary batteries according to exemplary embodiments.
[0115] The roller press may include an upper roller and a lower roller, and the gap between the upper roller and the lower roller can be controlled.
[0116] The roller press can be, for example, a heated roller press, an electric vertical roller press, a hydraulic roller press, a manual vertical roller press, etc.
[0117] In some embodiments, the manufacturing method may further include preparing an electrode active material slurry.
[0118] The electrode active material slurry may contain primary active material, which is in the form of single particles.
[0119] In some embodiments, the primary active material may be in single-particle form, for example, with a specific surface area (BET) of 0.7 m². 2 / g to 1.0m 2 / g, for example, the average particle size (D50) can be 3.5μm to 4.0μm.
[0120] The electrode active material slurry may further comprise at least one selected from binders, conductive materials, and solvents. The primary active material may comprise lithium metal oxide, and the lithium metal oxide, the binder, and the conductive material are as described above in this specification. The electrode active material slurry may further comprise additives such as dispersants and thickeners.
[0121] The solvent may include, for example, N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, N,N-dimethylaminopropylamine, tetrahydrofuran, etc.
[0122] In one embodiment, the electrode active material slurry can be prepared by mixing a primary active material, a binder, a conductive material, and a solvent. The mixing can be carried out by milling methods such as a ball mill, bead mill, or basket mill.
[0123] For example, based on the total weight of solids in the electrode active material slurry, the content of the primary active material can be 90% to 98% by weight, 92% to 97% by weight, or 92% to 96% by weight.
[0124] For example, based on the total weight of solids in the electrode active material slurry, the content of the binder can be from 0.5% to 4.0% by weight, from 0.5% to 3.0% by weight, or from 1.0% to 1.5% by weight.
[0125] For example, based on the total weight of solids in the electrode active material slurry, the content of the conductive material can be from 0.5% to 7.0% by weight, from 0.5% to 5.0% by weight, or from 1.0% to 2.5% by weight.
[0126] In some embodiments, the solids content in the electrode active material slurry can be 70% to 80% by weight.
[0127] By ensuring that the content of each component in the prepared electrode active material slurry is within the above-mentioned range, the slurry can be pressed uniformly as a whole when pressed by a roller press.
[0128] As a non-limiting example, the coating of the electrode active material slurry can be performed using methods such as gravure coating, slot extrusion coating, multilayer simultaneous die coating, embossing, doctor blade coating, dip coating, bar coating, casting, etc.
[0129] In some embodiments, the electrode active material slurry can be prepared at a concentration of 15 mg / cm³. 2 Up to 30 mg / cm 2 The loading amount is coated on one or both sides of the current collector and dried.
[0130] In some embodiments, the electrode loading can be, for example, 15 mg / cm³. 2 Up to 30 mg / cm 2 20mg / cm 2 Up to 25 mg / cm 2 Or 22mg / cm 2 Up to 24 mg / cm 2 Loading capacity is a value representing the mass of active material per unit area of the active material layer. By giving the electrode a loading capacity within the above-mentioned range, the storage characteristics of the electrode at high temperatures can be further improved.
[0131] In one embodiment, the dried electrode active material slurry can be pressed, for example, at room temperature using a roller press.
[0132] In one embodiment, the pressing by the roller press can be performed once or more, for example, once, twice or three times.
[0133] In some embodiments, the dried electrode active material slurry may be pressed once or more using a roller press to achieve an electrode density of, for example, 3.0 g / cm³ to 3.9 g / cm³, 3.2 g / cm³ to 3.8 g / cm³, or 3.5 g / cm³ to 3.7 g / cm³. The pressing may be performed once or more using the roller press until the electrode density reaches the aforementioned range.
[0134] By forming the electrodes to have a density within the aforementioned range, further improved storage characteristics can be achieved.
[0135] By controlling the composition of the electrode active material slurry, the loading amount, the pressing gap between the upper and lower rollers of the roller press, the density, etc., an electrode for a lithium secondary battery that satisfies Formula 1 can be manufactured.
[0136] The embodiments of the present invention will be further described below with reference to specific experimental examples. The embodiments and comparative examples included in the experimental examples are only for illustrating the present invention and do not limit the scope of the claims.
[0137] Examples and Comparative Examples Preparation of electrode active material slurry In Examples 1 to 4 and Comparative Examples 1 to 4, LiNi was used as a primary active material in single-particle form. 0.8 Co 0.1 Mn 0.1 O2, the particle size and specific surface area of which are shown in Table 1 below. Table 1 also records information on the primary active material of a reference battery manufactured solely for the evaluation of power characteristics in Experimental Example 4 below.
[0138] D is recorded in Table 1 最小 (μm), D 最大 (μm), D 10 D 50 and D 90 It is based on the laser diffraction method, specifically, the particle size distribution measured by a Malvern Mastersizer 3000 laser diffraction particle size analyzer under the conditions of a refractive index of 1.741, an absorption coefficient of 1.0, and the use of distilled water as a solvent.
[0139] Among them, D 最小 D can represent the smallest particle size among the measured particles. 最大 D can represent the maximum particle size among the measured particles. 10 D can represent the particle size corresponding to a cumulative volume fraction of 10%.50 D can represent the particle size corresponding to a cumulative volume fraction of 50%. 90 It can represent the particle size corresponding to a cumulative volume fraction of 90%.
[0140] The specific surface areas listed in Table 1 were calculated using a TriStar 3020 analytical apparatus based on the amount of nitrogen adsorbed at liquid nitrogen temperature (77 K), and then measured according to the Brunauer-Emmett-Teller (BET) method.
[0141] [Table 1] The primary active material in single-particle form, carbon black as a conductive material, and polyvinylidene fluoride (PVDF) as a binder are mixed in a weight ratio of 92:5:3 to prepare positive electrode slurries.
[0142] Electrode manufacturing Using the positive electrode slurries according to the above embodiments and comparative examples, a positive electrode is manufactured in the following manner, and a lithium secondary battery including the positive electrode is manufactured.
[0143] The positive electrode slurry is uniformly coated onto the area excluding the protrusion of an aluminum foil (12 μm thick) with a protrusion (positive electrode tab) on one side and dried, and then calendered to obtain the positive electrode. At this time, the pressing gap between the upper and lower rollers of the calendering mill, the loading of the positive electrode active material layer in the calendered positive electrode, and the electrode density are shown in Table 2 below.
[0144] A negative electrode slurry is prepared by mixing a mixture of artificial graphite and natural graphite (by weight 7:3) as the negative electrode active material, styrene-butadiene rubber as the binder, and carboxymethyl cellulose as the thickener in a weight ratio of 97:1:2. The negative electrode slurry is then uniformly coated onto the area excluding the protrusion of a copper foil (15 μm thick) having a protrusion (negative electrode tab) on one side and dried. The coating is then calendered to 1.4 g / cm³ to obtain the negative electrode.
[0145] The positive and negative electrodes are cut into rectangular shapes including tab leads, and a polyethylene separator (20 μm thick) is placed between the positive and negative electrodes to form an electrode assembly. Next, the positive and negative leads are soldered to the positive and negative tabs, respectively. The electrode assembly is housed inside a soft case (shell), leaving portions of the positive and negative leads exposed, and sealing three sides except for the electrolyte injection surface. Electrolyte is injected, and the electrolyte injection surface is sealed, followed by immersion for 12 hours to obtain a secondary battery. The electrolyte used is prepared by adding 1% by weight of fluoroethylene carbonate (FEC), 0.3% by weight of vinylene carbonate (VC), 1.0% by weight of lithium difluorophosphate (LiPO2F2), 0.5% by weight of 1,3-propanesulfonyl lactone (PS), and 0.5% by weight of 1-propylene-1,3-sultone (PRS) based on the total weight of the electrolyte.
[0146] In addition, for the evaluation of the power characteristics in Experimental Example 4 below, a positive electrode for a reference battery and a lithium secondary battery including the positive electrode were manufactured using a positive electrode slurry containing the primary active material of the reference battery by the same method as described above.
[0147] Experimental Example Experimental Example 1: Average diameter (D) of active material A ) The positive electrodes of the above embodiments and comparative examples were cut perpendicularly along the thickness direction. For each active material layer, a cross-section with a width (x) and length (y) of 1 mm × 1 mm was captured using a scanning electron microscope (SEM) (Hitachi, S-4800) at 5000x magnification. The total number of active materials in the SEM cross-section image was 100.
[0148] Using image processing software (Image-J), the maximum diameter of the cross-section of all active substances present in the SEM cross-sectional image was calculated. The maximum diameter is the length of the longest straight line extending from the center of each active substance to its outermost edge, i.e., the diameter passing through the center of each active substance. The average value of the obtained maximum diameters greater than 0.5 μm was defined as the average diameter (D). A ).
[0149] The results are recorded in Table 2 below. Furthermore, Figure 1 The image shows a cross-sectional SEM image of the active material layer of the electrode manufactured in Example 1.
[0150] Experimental Example 2: Most Frequently Measured Particle Size (D) of Active Substances B ) The positive electrodes of the above examples and comparative examples were prepared as samples with dimensions of 1 mm × 1 mm × 150 μm in width (x), length (y), and thickness (z). The samples were completely immersed in N-methyl-2-pyrrolidone (NMP) and ultrasonically treated at room temperature for at least 2 hours. The solids of the active material layer were scraped and separated from the ultrasonically treated samples. The separated solids were completely immersed in NMP and ultrasonically treated at room temperature for at least 2 hours to obtain a dispersion. The active material was extracted from the dispersion by filtration and dried in a vacuum oven for 24 hours to obtain solvent-free active material. The obtained active material was measured using a laser diffraction particle size analyzer (Malvern Mastersizer 3000) with a refractive index of 1.741, an absorption coefficient of 1, and distilled water as the solvent, based on laser diffraction.
[0151] This yields a particle size distribution curve with the x-axis representing particle size and the y-axis representing volume percentage.
[0152] Based on the particle size distribution curve, the particle size that exhibits the highest volume percentage within the particle size range below 20 μm is defined as the most frequent particle size (D). B ).
[0153] Therefore, the most frequent particle size (D) can be calculated. B ) and the average diameter (D) A The difference (D) B -D A ).
[0154] The results are recorded in Table 2 below. Furthermore, Figure 2 The diagram shows the particle size distribution of the active material contained in the active material layer of the electrode manufactured in Example 1.
[0155] Experimental Example 3: Electrode Loading and Electrode Density For the positive electrode of the above embodiments and comparative examples, the mass of the active material layer per unit area is measured using an electronic balance, the thickness of the active material layer is measured using a micrometer, and then the mass per unit volume is calculated accordingly.
[0156] Experiment Example 4: Evaluation of Power Characteristics For the lithium secondary batteries according to the examples and comparative examples, they were charged and discharged three times at 25°C, within the range of 2.5V to 4.35V, under CC / CV (0.5C-0.05C) conditions, and the SOC was set to 50% based on the second discharge capacity. For the battery set to 50% SOC, the voltage before discharge (V0) and the voltage after discharge at 1C current for 10 seconds (V1) were measured, and the DC internal resistance (DCR) was calculated according to Equation 2 below.
[0157] [Equation 2] DCR=(V0-V1) / I In Equation 2, I represents the 1C discharge current (Ampere).
[0158] In addition, power characteristics can be evaluated based on the reciprocal of DCR. The lower the DCR, the better the power characteristics.
[0159] Specifically, the power characteristics of the embodiments and comparative examples are evaluated by relative values (%) according to Equation 3 below.
[0160] [Formula 3] Power characteristic (%) = (DCR of reference cell / DCR of individual cells) × 100 According to Equation 3, the higher the power characteristic, the better the power characteristic.
[0161] The results are recorded in Table 2 below.
[0162] Experiment Example 5: Evaluation of Storage Characteristics For the lithium secondary batteries according to the examples and comparative examples, at 25°C, within a voltage range of 2.5V to 4.35V, the charging and discharging were repeated 3 times under CC / CV (0.5C-0.05C) conditions, and then finally charged to 4.35V under the same conditions (CC / CV, 0.5C-0.05C).
[0163] The fully charged battery was discharged to 2.5V at 0.5C rate (C-rate) at 25℃, and the discharge capacity (C1) was measured.
[0164] The battery was then stored in a storage chamber at 60°C for 4 weeks. After storage, it was discharged to 2.5V at 25°C, and the discharge capacity (C2) was measured.
[0165] Storage characteristics are based on the discharge capacity before and after high-temperature storage and are calculated according to Equation 4 below.
[0166] [Formula 4] Storage characteristics (%) = (C2 / C1) × 100 The results are recorded in Table 2 below.
[0167] [Table 2] Referring to Table 2, in the lithium secondary battery according to the embodiment, the positive electrode active material in the positive electrode satisfies 0.8 ≤ D B -D A The concentration of active material is ≤2.6, which improves the network formation between individual active materials, thus enhancing power and storage characteristics. In the lithium secondary battery of Example 1, after the electrode pressing process, the individual active materials did not break or aggregate, thus maintaining their individual form more stably. Therefore, even though the positive electrode active material layer contains only individual active materials, the power and storage characteristics are significantly higher than 90%.
[0168] Although the lithium secondary battery according to the comparative example includes an electrode utilizing active material in the form of single particles, it is not controlled to satisfy 0.8≤D B -D A ≤2.6. That is, the positive electrode active material in the positive electrode of the lithium secondary battery according to the comparative example is not 0.8≤D. B -D A Within the numerical range of ≤2.6, it was confirmed that the size or shape of the active material contained in the electrode active material slurry was deformed during the electrode manufacturing process, including the pressing process.
[0169] Therefore, at least one of the power characteristics and storage characteristics of the comparative example lithium secondary battery is significantly degraded. Specifically, in the electrode of the comparative example using single-particle active material, when the electrode density is high, the reduced porosity within the electrode leads to decreased electrolyte permeability, resulting in a significant decrease in capacity retention during high-temperature storage. When the electrode density is low, the increased contact resistance between particles and the reduced reaction area lead to a decrease in power characteristics.
Claims
1. An electrode for a lithium secondary battery, comprising an active material layer containing active material in the form of single particles, in, The active substance in single-particle form satisfies the following formula 1. [Formula 1] 0.8≤D B -D A ≤2.6 In Equation 1, D A The average diameter is the average of the single-particle form of the active material as measured from scanning electron microscopy (SEM) images. This average diameter is the average of values greater than 0.5 μm among the maximum diameters passing through the center of the active material in the SEM images. B The most frequent particle size of the active material in single-particle form is measured from a particle size distribution (PSD) plot with particle size on the x-axis and volume % on the y-axis. The most frequent particle size is the particle size in which the maximum peak appears in the particle size range below 20 μm.
2. The electrode for a lithium secondary battery according to claim 1, wherein, In Equation 1, the average diameter D A and the most frequent particle size D B Based on values measured for the active material contained in the active material layer of the electrode for the lithium secondary battery manufactured by pressing or rolling processes.
3. The electrode for a lithium secondary battery according to claim 2, wherein, The average diameter D A The most frequent particle size D was measured from an SEM image of the cut surface after the active material layer was vertically cut. B It is measured from the particle size distribution map of the active substance obtained by immersing the active substance layer in an organic solvent to obtain an organic solvent in which the active substance is dispersed, and then extracting and drying it.
4. The electrode for a lithium secondary battery according to claim 1, wherein, The average diameter D of the active substance in single-particle form A The range is from 1.2 μm to 2.4 μm.
5. The electrode for a lithium secondary battery according to claim 1, wherein, The most frequent particle size D of the active substance in single-particle form B The range is from 2.2 μm to 4.2 μm.
6. The electrode for a lithium secondary battery according to claim 1, wherein, The active substances contained in the active substance layer are composed of active substances in the form of single particles.
7. The electrode for a lithium secondary battery according to claim 1, wherein, The electrode density of the electrode used in the lithium secondary battery is from 3.0 g / cm³ to 3.9 g / cm³.
8. The electrode for a lithium secondary battery according to claim 7, wherein, The electrode density of the electrode used in the lithium secondary battery is from 3.5 g / cm³ to 3.7 g / cm³.
9. The electrode for a lithium secondary battery according to claim 1, wherein, The electrode for the lithium secondary battery further includes a current collector, and the active material layer is located on one or both sides of the current collector.
10. The electrode for a lithium secondary battery according to claim 1, wherein, The thickness of the active material layer is 125 μm to 160 μm.
11. The electrode for a lithium secondary battery according to claim 1, wherein, The electrode used in the lithium secondary battery is the positive electrode.
12. A lithium secondary battery, comprising: positive electrode; as well as The negative electrode is positioned opposite to the positive electrode. The positive electrode is the lithium secondary battery electrode according to claim 1.
13. A method for manufacturing an electrode for a lithium secondary battery, comprising the following steps: The electrode active material slurry is coated and dried; as well as The dried electrode active material slurry is pressed using a roller press to form an active material layer containing single-particle active materials. The pressing gap between the upper and lower rollers of the roller press is 130μm to 160μm. The active substances in the active substance layer, in the form of single particles, satisfy the following formula 1. [Formula 1] 0.8≤D B -D A ≤2.6 In Equation 1, D A The average diameter is the average of the single-particle form of the active material as measured from scanning electron microscopy (SEM) images. This average diameter is the average of values greater than 0.5 μm among the maximum diameters passing through the center of the active material in the SEM images. B The most frequent particle size of the active material in single-particle form is measured from a particle size distribution (PSD) plot with particle size on the x-axis and volume % on the y-axis. The most frequent particle size is the particle size in which the maximum peak appears in the particle size range below 20 μm.
14. The method for manufacturing an electrode for a lithium secondary battery according to claim 13, wherein, The electrode active material slurry was prepared at 15 mg / cm³ 2 Up to 30 mg / cm 2 The loading amount is coated on one or both sides of the current collector and dried.
15. The method for manufacturing an electrode for a lithium secondary battery according to claim 13, wherein, The pressing gap between the upper and lower rollers of the roller press is 135μm to 158μm.