Positive electrode plate, secondary battery, battery module, battery pack and electrical device

By setting a conductive coating on the current collector of a lithium-ion battery and controlling the amount of conductive agent and binder, the problem of positive electrode active material layer delamination is solved, thereby improving the cycle performance and safety performance of the lithium-ion battery.

CN123120624APending Publication Date: 2026-11-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611215172.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the positive electrode active material layer is prone to delamination, leading to a decline in cycle performance and safety performance.

Method used

A conductive coating containing 20% ​​to 50% conductive agent and 50% to 80% binder is applied to the current collector. The positive electrode active layer is applied to the surface of the conductive coating away from the current collector. The amount of conductive agent and binder is controlled by using conductive binder or insulating binder to enhance the peel strength between the current collector and the conductive coating.

Benefits of technology

It effectively prevents the positive electrode active layer from peeling off, improves the cycle performance and cycle stability of the secondary battery, enhances the tensile strength of the electrode sheet at break, and improves the high-temperature safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120624A_ABST
    Figure CN123120624A_ABST
Patent Text Reader

Abstract

This application provides a positive electrode sheet, a secondary battery, a battery module, a battery pack, and an electrical device. The positive electrode sheet includes a current collector, a conductive coating, and a positive active layer. The conductive coating is disposed on at least one surface of the current collector and includes 20%–50% by mass of a conductive agent and 50%–80% by mass of a binder. The positive active layer is disposed on the surface of the conductive coating away from the current collector. The positive active material in the positive active layer is at least one of lithium manganese oxide-based positive electrode materials, ternary positive electrode materials, and quaternary positive electrode materials. The conductive coating effectively avoids the problem of electrode breakage caused by oxidation. Furthermore, by controlling the amount of conductive agent and binder, the stability of electron conduction between the current collector and the positive active material is ensured, and the peel strength between the current collector and the conductive coating is enhanced, effectively improving the cycle performance and cycle stability of the secondary battery with this positive electrode sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application based on the invention with application number 202280013062.9, application date April 29, 2022, applicant CATL, and invention title "positive electrode sheet, secondary battery, battery module, battery pack and power supply device". Technical Field This application relates to the field of battery technology, and in particular to a positive electrode sheet, a secondary battery, a battery module, a battery pack, and an electrical device. Background Technology

[0002] Currently, lithium-ion batteries are widely used in all aspects of daily life, such as cameras, laptops, and electric vehicles. With the significant advancements in lithium-ion battery technology, higher demands are being placed on their safety performance, cycle life, and overall lifespan. Particularly in the electric vehicle sector, ensuring that lithium-ion batteries possess both high safety performance and long cycle life has become a pressing technical challenge. Summary of the Invention

[0003] This application provides a positive electrode sheet, a secondary battery, a battery module, a battery pack, and an electrical device. This addresses the problem in the prior art where the conductive coating applied to the positive electrode current collector causes the positive electrode active material layer to easily detach.

[0004] The first aspect of this application provides a positive electrode sheet, comprising: a current collector, a conductive coating, and a positive electrode active layer. The conductive coating is disposed on at least one side surface of the current collector, and the conductive coating comprises a conductive agent with a mass content of 20% to 50% and a binder with a mass content of 50% to 80%. The positive electrode active layer is disposed on the surface of the conductive coating away from the current collector, and the positive electrode active material in the positive electrode active layer is at least one of lithium manganese oxide-based positive electrode material, ternary positive electrode material, and quaternary positive electrode material.

[0005] The conductive coating on the positive electrode sheet of this application mitigates the damage to the oxide layer on the aluminum foil surface caused by the positive electrode active particles during cold pressing, while simultaneously improving the tensile strength at break of the electrode sheet and effectively avoiding the problem of electrode breakage caused by oxidation. Specifically, by utilizing a conductive agent to facilitate electron conduction between the current collector and the positive electrode active material, and by controlling the dosage of the conductive agent and binder, the stability of electron conduction between the current collector and the positive electrode active material is ensured, and the peel strength between the current collector and the conductive coating is enhanced. This effectively solves the problem of positive electrode active layer delamination and significantly improves the cycle performance and cycle stability of the secondary battery with this positive electrode sheet.

[0006] In any embodiment of this application, the adhesive is a conductive adhesive, and the volume resistivity of the conductive adhesive is ≤10. -3Ω•cm; Optionally, the conductive coating comprises 20%~30% by mass of a conductive agent and 70%~80% by mass of a conductive binder. In the above embodiments, using a conductive binder as the binder allows for a further reduction in the amount of conductive agent while maintaining the same electronic conductivity, thereby relatively increasing the amount of binder and achieving the goal of further improving the peel strength between the current collector and the conductive coating.

[0007] In any embodiment, the conductive binder is selected from any one or more of the group consisting of epoxy resin conductive adhesive, silicone resin conductive adhesive, polyimide resin conductive adhesive, phenolic resin conductive adhesive, and polyurethane conductive adhesive. The conductive binders described above exhibit high chemical and thermal stability, thus meeting the requirements for long-cycle use of secondary batteries.

[0008] In any embodiment, the adhesive is an insulating adhesive with a volume resistivity ≥ 10⁻⁶. 10 Ω•cm; Optionally, the conductive coating comprises 30% to 45% by mass of a conductive agent and 55% to 70% by mass of an insulating binder. In this embodiment, the binder used is an insulating material, thus requiring a corresponding increase in the amount of conductive agent. The aforementioned mass content ensures simultaneous optimization of both the electronic conduction and adhesion effects of the conductive coating.

[0009] In any embodiment, optionally, the insulating adhesive is selected from any one or more of the group consisting of PVDF, polyacrylonitrile, styrene-butadiene rubber, polyvinyl alcohol, gum arabic, xanthan gum, and polyacrylate. The above-mentioned adhesives exhibit high bonding strength, good compatibility with conductive agents, and ideal chemical and thermal stability, thus meeting the requirements for long-cycle use of secondary batteries.

[0010] In any embodiment, the conductive agent comprises any one or more selected from the group consisting of acetylene black (AB), carbon fiber, conductive carbon black, conductive graphite, single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene nanosheets, graphene oxide nanosheets, and micronized graphite. All of the above-mentioned conductive agents are commonly used in the art and possess high conductivity. Based on the above-mentioned dosage, the conductive coating is guaranteed to have good conductivity.

[0011] In any embodiment, the thickness of the conductive coating is 0.5 micrometers to 5 micrometers, and optionally, the thickness of the conductive coating is 0.8 micrometers to 3 micrometers. The conductive coating with the thickness within the above range effectively bonds the conductive coating and the current collector, effectively mitigating the damage to the aluminum foil surface oxide layer caused by the positive electrode active particles during cold pressing, and constructing an effective electron conduction channel to ensure that the secondary battery with the positive electrode has a sufficiently high volumetric energy density.

[0012] In any embodiment, the current collector described above is an aluminum foil, optionally, the thickness of the aluminum foil is 8 micrometers to 20 micrometers; and / or, the tensile strength of the current collector in the longitudinal direction and the transverse direction is ≥ 175 MPa, so as to provide better mechanical strength and better meet the long-term cycle use of the secondary battery.

[0013] In any embodiment, the positive electrode active material includes at least one of Formulas (I) to (III): Li a1 Ni x1 Co y1 M1 z1 M2 1-x1-y1-z1 O 2-b1 Formula (I) Li a2 Mn 2-y2 M3 y2 O 4-b2 Formula (II) cLi₂MnO₃·(1-c)Liₐ₃M₄ x3 O 2-b3 Formula (III) In Formula (I), M1 is Mn and / or Al, M2 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti, 0.8≤a1<1.2, 0≤x1<1, 0≤y1≤1, 0≤z1≤1, x1+y1+z1≤1, -0.2≤b1≤0.2. In Formula (II), 0.8≤a2<1.2, 0.6≤y2≤1, -0.2≤b2≤0.2, M3 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti. In Formula (III), 0<c<1, 0<x3<1, 0.8<a3<1.2, -0.2≤b3≤0.2, M4 is any one selected from Ni, Co, Mn, and any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti. The above positive electrode active materials are mainly selected from lithium manganate-based positive electrode materials, ternary positive electrode materials, and quaternary positive electrode materials, wherein the lithium manganate-based positive electrode material shown in Formula (II) is a doped lithium manganate-based positive electrode material, so on the basis of ensuring high rate performance, the dissolution of manganese is relatively reduced, thereby ensuring higher cycle performance.

[0014] The second aspect of this application provides a secondary battery, including a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the positive electrode is any of the positive electrode types described in the first aspect. Because the conductive coating on the positive electrode of this application mitigates the damage to the oxide layer on the aluminum foil surface caused by the positive electrode active particles during cold pressing, and simultaneously improves the tensile strength at break of the electrode, it effectively avoids the problem of electrode breakage caused by oxidation. Furthermore, by controlling the amount of conductive agent and binder, it ensures the stability of electronic conduction between the current collector and the positive electrode active material, and enhances the peel strength between the current collector and the conductive coating, thereby effectively solving the problem of positive electrode active layer delamination, and simultaneously effectively improving the cycle performance and cycle stability of the secondary battery with this positive electrode.

[0015] In any embodiment of the second aspect, the electrolyte comprises a lithium salt, which includes lithium fluorosulfonylimide and lithium hexafluorophosphate. Optionally, the lithium fluorosulfonylimide is any one or more of the group consisting of lithium bis(trifluoromethyl)fluorosulfonylimide, lithium (fluorosulfonyl)(trifluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(pentafluoroethylsulfonyl)imide, lithium (trifluoromethylsulfonyl)(difluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(perfluorobutylsulfonyl)imide, and lithium bis(pentafluoroethylsulfonyl)imide. The application of the aforementioned lithium fluorosulfonylimide in the electrolyte improves the high-temperature safety performance of the secondary battery having this electrolyte.

[0016] In any embodiment of the second aspect, optionally, the total concentration of lithium salt in the electrolyte is 0.6 mol / L to 2 mol / L. Optionally, the concentration C1 of lithium hexafluorophosphate in the electrolyte is 0.1 mol / L to 1 mol / L, and the concentration C2 of lithium fluorosulfonylimide is 0.5 mol / L to 1.5 mol / L. Optionally, 1 ≤ C2 / C1 ≤ 5. Within the above concentration range, lithium fluorosulfonylimide can sufficiently improve the conductivity of the electrolyte. Further controlling the concentration ratio of the two within the above range allows for the improvement of electrolyte conductivity using lithium fluorosulfonylimide; simultaneously, it allows the formation of an aluminum trifluoride film on the positive electrode current collector during the first charge-discharge process of lithium hexafluorophosphate, which, together with the conductive coating, mitigates the corrosion of the current collector by lithium fluorosulfonylimide, thereby further improving the high-temperature cycle performance of the secondary battery.

[0017] In any embodiment of the second aspect, the thickness d of the conductive coating of the positive electrode, the concentration C1 of lithium hexafluorophosphate, and the concentration C2 of lithium fluorosulfonylimide satisfy the following relationship: C2 / (5×C1)≤d≤lg(C2 / C1)+4, where C1 and C2 are in mol / L and d is in μm. By controlling the thickness of the conductive coating, the concentration of lithium hexafluorophosphate, and the concentration of lithium fluorosulfonylimide through the above relationship, the high-temperature cycle performance, energy density, and corrosion resistance of the secondary battery are better improved through their combined effect.

[0018] In any embodiment of the second aspect, the electrolyte further includes an organic solvent and additives. The organic solvent is selected from any one or more of the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butene carbonate, ethyl propyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, methyl propionate, and tetrahydrofuran. The organic solvents mentioned above are all commonly used organic solvents in the art, and lithium salts exhibit good dispersion performance therein.

[0019] In any embodiment of the second aspect, the organic solvent has a mass content of 65% to 85% in the electrolyte.

[0020] In any embodiment of the second aspect, the additive is selected from at least one group consisting of vinylene carbonate, vinyl sulfate, lithium difluorooxalate borate, lithium difluorophosphate, lithium tetrafluoroborate, 1,3-propanesulfonate lactone, lithium trifluoromethanesulfonate, and lithium diacetate borate. Those skilled in the art can select to add the above additives according to the specific performance requirements of the secondary battery. For example, 1,3-propanesulfonate lactone can mitigate the oxidation and gas generation of lithium fluorosulfonylimide under high voltage by oxidizing it earlier at the positive electrode, thereby better mitigating the corrosion of the current collector by lithium fluorosulfonylimide.

[0021] In any embodiment of the second aspect, the total mass content of the above-mentioned additives in the electrolyte is 0.5% to 7%. This ensures that the effects of the additives are fully utilized without affecting the effects of the lithium salts.

[0022] In any embodiment of the second aspect, the negative electrode active material of the aforementioned negative electrode includes natural graphite, artificial graphite, mesophase microcarbon, hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O. 12Any one or more of the following groups: and Li-Al alloys. The above-mentioned negative electrodes are commonly used negative electrodes in the field of secondary electrodes, and those skilled in the art can select suitable negative electrode materials from the above categories according to the performance requirements of the secondary battery.

[0023] A third aspect of this application provides a battery module including a secondary battery, which is any of the secondary batteries described in the second aspect.

[0024] The fourth aspect of this application provides a battery pack including a battery module, which is any of the battery modules described in the third aspect.

[0025] The fifth aspect of this application provides an electrical device, including a secondary battery, a battery module, or a battery pack, wherein the secondary battery is any type of secondary battery according to the second aspect, the battery module is any type of battery module according to the third aspect, and the battery pack is any type of battery pack according to the fourth aspect.

[0026] Because the positive electrode sheet of this application is corrosion resistant and the positive electrode active layer adheres stably to the current collector, the secondary battery, battery module, battery pack and power device having it have the advantages of good high temperature stability and good cycle performance. Attached Figure Description

[0027] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.

[0028] Figure 1 This is a side view of the positive electrode sheet according to one embodiment of this application.

[0029] Figure 2 This is a schematic diagram of a secondary battery according to one embodiment of this application.

[0030] Figure 3 yes Figure 2 An exploded view of a secondary battery according to one embodiment of this application is shown.

[0031] Figure 4 This is a schematic diagram of a battery module according to one embodiment of this application.

[0032] Figure 5 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0033] Figure 6 yes Figure 5 An exploded view of a battery pack according to one embodiment of this application is shown.

[0034] Figure 7 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.

[0035] Explanation of reference numerals in the attached figures: 11 Current collector; 12 Conductive coating; 13 Positive electrode active layer; 1 Battery pack; 2 Upper casing; 3 Lower casing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Top cover assembly.

[0036] The accompanying drawings are not drawn to scale. Detailed Implementation

[0037] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.

[0038] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the positive electrode, secondary battery, battery module, battery pack, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0039] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0040] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0041] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0042] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0043] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0044] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0045] Safety is the minimum requirement for lithium-ion batteries, and improving their safety has always been a relentless pursuit for researchers. From the perspective of electrolytes, lithium fluorosulfonylimide has a higher thermal decomposition temperature and is less sensitive to water, which can improve battery safety to some extent. However, electrolytes containing this type of lithium salt pose a risk of corrosion to the aluminum foil, potentially leading to electrode breakage and seriously threatening the safety and lifespan of the rechargeable battery.

[0046] Specifically, the positive electrode substrate is currently usually aluminum foil. When aluminum foil is exposed to air, its surface oxidizes, forming a uniform oxide film. During the cold pressing process of the active material, some active material particles are pressed into the aluminum foil, damaging this oxide film. When the electrolyte contains fluorosulfonylimide lithium salt, this lithium salt oxidizes at the positive electrode. The oxidation products combine with aluminum, and the combined products further dissolve into the electrolyte, creating corrosion pits. This can lead to electrode breakage, seriously threatening the safety performance and lifespan of the secondary battery.

[0047] Patent application CN 13851724 A discloses a method that combines fluorosulfonylimide lithium salt with a conductive coating. The introduction of the conductive coating reduces the contact resistance between the current collector and the active material, and also reduces the corrosion risk caused by the contact between the fluorosulfonylimide lithium salt and the current collector to a certain extent. This can improve the high-rate cycling performance of the electrochemical device and reduce the temperature rise of the electrochemical device, while also mitigating the corrosive effect of the fluorosulfonylimide lithium salt on the positive electrode current collector, thus improving the long-term stability of the electrochemical device.

[0048] However, conductive coatings can easily cause the positive electrode active material layer to detach from the current collector, thus affecting the cycle performance of lithium-ion batteries.

[0049] As described above, although conductive coatings can mitigate the corrosive effects of lithium fluorosulfonylimide salts on the positive electrode current collector and improve the long-term stability of electrochemical devices, in practical applications, the conductive coating can easily cause the positive electrode active material layer to detach from the current collector, thereby affecting the cycle performance of lithium-ion batteries. To address this issue, this application provides a positive electrode sheet, a secondary battery, a battery module, a battery pack, and an electrical device.

[0050] [Positive electrode plate] The first aspect of this application provides a positive electrode sheet, such as... Figure 1 As shown, the positive electrode includes: a current collector 11, a conductive coating 12, and a positive electrode active layer 13. The conductive coating 12 is disposed on at least one side surface of the current collector 11, and the conductive coating 12 includes a conductive agent with a mass content of 20% to 50% and a binder with a mass content of 50% to 80%. The positive electrode active layer 13 is disposed on the surface of the conductive coating 12 away from the current collector 11, and the positive electrode active material in the positive electrode active layer 13 is at least one of lithium manganese oxide positive electrode material, ternary positive electrode material, and quaternary positive electrode material.

[0051] In this application, lithium manganese oxide cathode materials refer to LiMn2O4 cathode materials with a spinel structure, whether doped or undoped. Ternary cathode materials refer to lithium transition metal oxides with a layered structure and transition metal sites containing at least Ni, Co, and Mn or Ni, Co, and Al. Quaternary cathode materials refer to lithium transition metal oxides with a layered structure and transition metal sites containing at least Ni, Co, Mn, and Al.

[0052] The conductive coating 12 of the positive electrode sheet in this application mitigates the damage to the oxide layer on the current collector surface caused by the positive electrode active particles during cold pressing, while improving the tensile strength at break of the electrode sheet and effectively avoiding the problem of electrode breakage caused by oxidation. By utilizing a conductive agent to facilitate electron conduction between the current collector and the positive electrode active material, and by controlling the dosage of the conductive agent and binder, the stability of electron conduction between the current collector and the positive electrode active material is ensured, and the peel strength between the current collector 11 and the conductive coating 12 is enhanced. This effectively solves the problem of positive electrode active layer 13 delamination, and simultaneously improves the cycle performance and cycle stability of the secondary battery with this positive electrode sheet.

[0053] The mass content of the conductive agent and the mass content of the binder in the above conductive coating can be any value within the above range. For example, the mass content of the conductive agent can be 20%, 25%, 30%, 35%, 40%, 45% or 50%; and the mass content of the binder can be 50%, 55%, 60%, 65%, 70%, 75% or 80%.

[0054] As mentioned above, the conductive coating of this application must provide sufficient conductivity while also enhancing adhesion to the positive electrode active layer. Based on this, the inventors of this application discovered, by adjusting the ratio of the conductive agent and the binder, that when the volume resistivity of the binder has a significant difference, the ratio can be further adjusted to further improve both conductivity and adhesion.

[0055] In any embodiment of the first aspect described above, the adhesive is a conductive adhesive, and the volume resistivity of the conductive adhesive is ≤10. -3 Ω•cm; Optionally, the conductive coating comprises 20%~30% by mass of a conductive agent and 70%~80% by mass of a conductive binder. In the above embodiments, using a conductive binder as the binder allows for a further reduction in the amount of conductive agent while maintaining the same electronic conductivity, thereby relatively increasing the amount of binder and achieving the goal of further improving the peel strength between the current collector and the conductive coating.

[0056] The conductive binder used in the secondary battery can be selected from commonly used conductive binders in the prior art. Considering that the better the dispersion of the conductive agent, the stronger the conductivity, in some embodiments, to further ensure the full utilization of the conductive agent's conductivity, the conductive binder is selected from any one or more of the group consisting of epoxy resin conductive adhesive, silicone resin conductive adhesive, polyimide resin conductive adhesive, phenolic resin conductive adhesive, and polyurethane conductive adhesive. The above-mentioned conductive binders have high chemical and thermal stability; moreover, they have high dispersibility for inorganic conductive agents, thus ensuring uniform dispersion of the conductive agent and meeting the requirements for long-cycle, high-performance cyclic use of the secondary battery.

[0057] In some embodiments, the adhesive is an insulating adhesive with a volume resistivity ≥10. 10 Ω•cm; Optionally, the conductive coating comprises 30%~45% by mass of a conductive agent and 55%~70% by mass of an insulating binder. In this embodiment, the binder used has a high volume resistivity, thus requiring a corresponding increase in the amount of conductive agent. The aforementioned mass content ensures simultaneous optimization of both the electronic conduction and adhesion effects of the conductive coating.

[0058] When the volume resistivity of the adhesive is high, in addition to increasing the amount of conductive agent, in some embodiments, the insulating adhesive may be further selected from any one or more of the group consisting of PVDF, polyacrylonitrile, styrene-butadiene rubber, polyvinyl alcohol, gum arabic, xanthan gum, and polyacrylate. The above-mentioned adhesives have high bonding strength, good compatibility with the conductive agent, and ideal chemical and thermal stability, thus ensuring that the conductive agent dispersed therein can fully exert its conductive effect.

[0059] The conductive agent used in this application can be selected from conductive agents commonly used in secondary batteries. In some embodiments, the conductive agent comprises any one or more selected from the group consisting of acetylene black (AB), carbon fiber, conductive carbon black, conductive graphite, single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene nanosheets, graphene oxide nanosheets, and micronized graphite. All of the above-mentioned conductive agents are commonly used in the art for high conductivity, and the above-mentioned dosage ensures that the conductive coating has good conductivity.

[0060] In some embodiments, the thickness of the conductive coating is 0.5 micrometers to 5 micrometers. The thickness of the conductive coating can be any two of the following values: 0.5 micrometers, 0.8 micrometers, 1.0 micrometers, 1.5 micrometers, 1.8 micrometers, 2.0 micrometers, 2.2 micrometers, 2.5 micrometers, 3.0 micrometers, 3.5 micrometers, 4.0 micrometers, 4.5 micrometers, or 5.0 micrometers. Optionally, the thickness of the conductive coating is 0.8 micrometers to 3 micrometers. A conductive coating with a thickness within the above range effectively bonds the conductive coating and the current collector, effectively mitigating the damage to the aluminum foil oxide layer caused by the positive electrode active particles during cold pressing, and constructing an effective electron conduction channel to ensure that the secondary battery with the positive electrode has a sufficiently high volumetric energy density. In some embodiments, the corresponding binder is a conductive binder with a volume resistivity ≤ 10. -3 In the Ω•cm scheme, the thickness of the conductive coating can optionally be 2.2 micrometers to 3 micrometers; in some embodiments, the corresponding adhesive is an insulating adhesive with a volume resistivity ≥10. 10In the Ω•cm technical solution, the thickness of the conductive coating can optionally be 1.2 micrometers to 1.8 micrometers.

[0061] As an example, the current collector has two surfaces opposite each other in its own thickness direction, and the conductive coating 12 and the positive electrode active layer 13 are sequentially disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0062] In some embodiments, the current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.). Further optionally, the current collector is aluminum foil, and optionally, the thickness of the current collector is 8 micrometers to 20 micrometers (e.g., 8 micrometers, 9 micrometers, 10 micrometers, 12 micrometers, 14 micrometers, 16 micrometers, 18 micrometers or 20 micrometers). Optionally, the longitudinal and transverse tensile strength of the current collector is ≥175 MPa to provide better mechanical strength and better meet the requirements of long-term cycle use of secondary batteries.

[0063] The transverse tensile strength of the current collector in this application can be tested using methods known in the art. As an example, the test can be performed as follows: Take a sample with a length of 50 mm, a width of 20 mm, and a thickness of 15 μm. Fix both ends of the sample in the length or width direction to the fixture of an Instron 3365 high-speed rail tensile testing machine. Pull at a speed of 10 mm / min until the sample breaks to complete the test. Obtain the width direction tensile force F (N) according to the instrument's built-in software. The transverse tensile strength can be calculated using R = F / (width of aluminum foil × thickness of aluminum foil).

[0064] The positive electrode active material of this application is at least one of lithium manganese oxide-based positive electrode materials, ternary positive electrode materials, and quaternary positive electrode materials. In some embodiments, the positive electrode active material includes at least one of formulas (I) to (III): Li a1 Ni x1 Co y1 M1 z1 M2 1-x1-y1-z1 O 2-b1 Formula (I) Li a2 Mn 2-y2 M3 y2 O4-b2 Formula (II) cLi2MnO3·(1-c)Lia3M4 x3 O 2-b3 Formula (III) In formula (I), M1 is Mn and / or Al, M2 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti, 0.8≤a1<1.2, 0≤x1<1, 0≤y1≤1, 0≤z1≤1, x1+y1+z1≤1, -0.2≤b1≤0.2. In formula (II), 0.8≤a2<1.2, 0.6≤y2≤1, -0.2≤b2≤0.2, M3 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti. In formula (III), 0<c<1, 0<x3<1, 0.8<a3<1.2, -0.2≤b3≤0.2, M4 is any one selected from Ni, Co and Mn, as well as any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti. The above positive electrode active materials are mainly selected from lithium manganate-based positive electrode materials, ternary positive electrode materials, and quaternary positive electrode materials, wherein the lithium manganate-based positive electrode material shown in formula (II) is a doped lithium manganate-based positive electrode material, so on the basis of ensuring high rate performance, the dissolution of manganese is relatively reduced, thereby ensuring relatively high cycle performance.

[0065] A second aspect of the present application provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, an electrolyte and a separator, wherein the positive electrode plate is any one of the positive electrode plates according to the first aspect.

[0066] A secondary battery, also referred to as a rechargeable battery or an accumulator, refers to a battery that can be continuously used by activating the active material through charging after the battery is discharged.

[0067] Normally, a secondary battery includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte. During the charging and discharging process of the battery, active ions (such as lithium ions) intercalate and deintercalate back and forth between the positive electrode plate and the negative electrode plate. The separator is arranged between the positive electrode plate and the negative electrode plate, which mainly functions to prevent short circuit between the positive electrode and the negative electrode, and at the same time allows active ions to pass through. The electrolyte is located between the positive electrode plate and the negative electrode plate, which mainly functions to conduct active ions.

[0068] Because the conductive coating of the positive electrode sheet in this application mitigates the damage to the oxide layer on the aluminum foil surface caused by the positive electrode active particles during cold pressing, and simultaneously improves the tensile strength at break of the electrode sheet, it effectively avoids the problem of electrode sheet breakage caused by oxidation. Furthermore, by controlling the amount of conductive agent and binder, it ensures the stability of electronic conduction between the current collector and the positive electrode active material, and enhances the peel strength between the current collector and the conductive coating, thereby effectively solving the problem of positive electrode active layer delamination, and simultaneously improving the cycle performance and cycle stability of the secondary battery with this positive electrode sheet.

[0069] In some embodiments of the second aspect, the electrolyte comprises a lithium salt, which includes lithium fluorosulfonyl imide and lithium hexafluorophosphate. Optionally, the lithium fluorosulfonyl imide is any one or more of the group consisting of lithium bis(trifluoromethyl)fluorosulfonyl imide, lithium (fluorosulfonyl)(trifluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(pentafluoroethylsulfonyl)imide, lithium (trifluoromethylsulfonyl)(difluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(perfluorobutylsulfonyl)imide, and lithium bis(pentafluoroethylsulfonyl)imide. During the initial charge and discharge process, lithium hexafluorophosphate (LiPF6) undergoes oxidative decomposition at the anode, and the oxidation product aluminum trifluoride is deposited on the current collector surface, which to some extent alleviates the corrosion of aluminum foil by lithium fluorosulfonylimide. Lithium fluorosulfonylimide has a high degree of dissociation in non-aqueous organic solvents, resulting in high electrolyte conductivity. Furthermore, this type of lithium salt has good thermal stability and fewer side reactions at high temperatures. Therefore, secondary batteries containing this type of lithium salt electrolyte exhibit superior high-temperature cycle performance.

[0070] In any embodiment of the second aspect, optionally, the total concentration of lithium salt in the electrolyte is 0.6 mol / L to 2 mol / L (e.g., 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L or 2.0 mol / L). Optionally, in the electrolyte, the concentration C1 of lithium hexafluorophosphate is 0.1 mol / L to 1 mol / L (e.g., 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, or 1 mol / L), and the concentration C2 of lithium fluorosulfonylimide is 0.5 mol / L to 1.5 mol / L (e.g., 0.5 mol / L, 0.7 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.4 mol / L, or 1.5 mol / L). Further optionally, 1 ≤ C2 / C1 ≤ 5 (e.g., 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5). Within the above concentration range, lithium fluorosulfonylimide can significantly improve the conductivity of the electrolyte. By further controlling the concentration ratio of the two within the above range, lithium fluorosulfonylimide can be used to improve the conductivity of the electrolyte, while lithium hexafluorophosphate and the conductive coating can be fully utilized to alleviate the corrosion of the current collector by lithium fluorosulfonylimide, thereby further improving the high-temperature cycle performance of the secondary battery.

[0071] In any embodiment of the second aspect, the thickness d of the conductive coating of the positive electrode, the concentration C1 of lithium hexafluorophosphate, and the concentration C2 of lithium fluorosulfonylimide satisfy the following relationship: C2 / (5×C1)≤d≤lg(C2 / C1)+4, where C1 and C2 are in mol / L and d is in μm. By controlling the thickness of the conductive coating, the concentration of lithium hexafluorophosphate, and the concentration of lithium fluorosulfonylimide through the above relationship, the high-temperature cycle performance, energy density, and corrosion resistance of the secondary battery are better improved through their combined effect.

[0072] In any embodiment of the second aspect, the electrolyte further includes an organic solvent and additives. The organic solvent is selected from any one or more of the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butene carbonate, ethyl propyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, methyl propionate, and tetrahydrofuran. The organic solvents mentioned above are all commonly used organic solvents in the art, and lithium salts exhibit good dispersion performance therein.

[0073] In any embodiment of the second aspect, the organic solvent has a mass content of 65% to 85% in the electrolyte. Typically, but not limitingly, the mass content is 65%, 70%, 75%, 80%, or 85%.

[0074] In any embodiment of the second aspect, the additive is selected from at least one group consisting of vinylene carbonate, vinyl sulfate, lithium difluorooxalate borate, lithium difluorophosphate, lithium tetrafluoroborate, 1,3-propanesulfonate lactone, lithium trifluoromethanesulfonate, and lithium diacetate borate. Those skilled in the art can select to add the above additives according to the specific performance requirements of the secondary battery. For example, 1,3-propanesulfonate lactone can mitigate the oxidation and gas generation of lithium fluorosulfonylimide under high voltage by oxidizing it earlier at the positive electrode, thereby better mitigating the corrosion of the current collector by lithium fluorosulfonylimide.

[0075] In any embodiment of the second aspect, the total mass content of the above-mentioned additives in the electrolyte is 0.5% to 7% (e.g., 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, or 7%). This is to fully utilize the function of the respective additives without affecting the function of the lithium salts.

[0076] [Negative electrode plate] In the secondary battery of this application, the negative electrode sheet may include a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector and including a negative electrode active material. The negative electrode material layer may be disposed on one of the surfaces of the negative electrode current collector or on both surfaces of the negative electrode current collector.

[0077] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0078] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: graphite (e.g., artificial graphite, natural graphite), soft carbon, hard carbon, mesophase carbon microspheres, carbon fibers, carbon nanotubes, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0079] In some embodiments of the second aspect, the negative electrode active material of the aforementioned negative electrode includes natural graphite, artificial graphite, mesophase microcarbon, hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O. 12 Any one or more of the group consisting of Li-Al alloys.

[0080] In some embodiments, the negative electrode film layer may optionally include an adhesive. The adhesive may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0081] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0082] In some implementations, the negative electrode material layer comprises the negative electrode active material artificial graphite, the conductive agent acetylene black, and the binder styrene-butadiene rubber (SBR).

[0083] In some embodiments, the negative electrode material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0084] In some embodiments, the negative electrode sheet can be prepared by dispersing the above-mentioned components for preparing the negative electrode sheet, such as negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0085] [Isolation membrane] In the secondary battery of this application, a separator is disposed between the positive electrode and the negative electrode to provide isolation. The type of separator is not specifically limited; any known porous separator with good chemical and mechanical stability can be selected. In some embodiments, the separator material can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0086] The secondary battery in this application can be a lithium-ion battery.

[0087] The secondary battery of this application can be prepared using conventional methods. In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process. Exemplary preparation methods include: Step 1: Stack the positive electrode, separator, and negative electrode in sequence, with the separator between the positive and negative electrodes, and then wind them to obtain the electrode assembly; Step 2: Place the electrode assembly in the secondary battery casing, dry it, inject electrolyte, and then process it through formation and settling to obtain the secondary battery.

[0088] In some embodiments, the secondary battery of this application may include an outer packaging. The outer packaging may be used to encapsulate the aforementioned electrode assembly and electrolyte.

[0089] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0090] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2 This is an example of a square-structured secondary battery 5.

[0091] In some implementations, refer to Figure 3The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 using a winding or stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.

[0092] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.

[0093] Figure 4 This is battery module 4, used as an example. (See reference...) Figure 4 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.

[0094] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.

[0095] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0096] Figure 5 and Figure 6 This is battery pack 1 as an example. (See reference...) Figure 5 and Figure 6 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0097] In addition, this application also provides an electrical device, which includes a secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device can be selected from mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited to these. The secondary battery, battery module, or battery pack can be selected as the electrical device according to its usage requirements.

[0098] Figure 7 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.

[0099] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0100] Because the positive electrode sheet of this application is corrosion resistant and the positive electrode active layer adheres stably to the current collector, the secondary battery, battery module, battery pack and power device having it have the advantages of good high temperature stability and good cycle performance.

[0101] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0102] Table 1 below describes the source and properties of some of the materials used in the examples.

[0103] Table 1

[0104] (1) Preparation of electrolyte In an argon-filled glove box (water content <10 ppm, oxygen content <1 ppm), 2% vinylene carbonate was added to an organic solvent (EC:EMC=3:7 wt% / wt%). After mixing thoroughly, an appropriate amount of lithium salt (LiPF6 and lithium fluorosulfonylimide content are shown in the table below) was slowly added to the non-aqueous organic solvent. After the lithium salt was completely dissolved, the target electrolyte was obtained, which is the electrolyte.

[0105] The ratios of solvents and additives used in the examples and comparative examples are shown in Table 2. The ratios of solvents and additives in Table 2 are calculated as mass percentages based on the total mass of the electrolyte. In addition, unless otherwise specified, the solvents in the electrolytes of each example and comparative example are ethylene carbonate: methyl ethyl carbonate (3:7 wt% / wt%), and the additives are vinylene carbonate with a mass content of 2%.

[0106] Table 2

[0107] (2) Preparation of the positive electrode (adding a base coating): First, an aqueous solution containing a conductive agent and a binder was coated onto an aluminum foil substrate (15 μm aluminum foil with a transverse tensile strength of 180 MPa), and then dried in an oven at 85°C to form a corresponding conductive coating on the aluminum foil substrate for later use. The electrolyte composition in Examples 6-33 and Comparative Examples 1 to 5 in Table 3 is consistent with that in Example 3.

[0108] The composition of the conductive coatings in each embodiment and comparative example is recorded in Table 3.

[0109] Table 3

[0110] A positive electrode slurry was prepared by mixing positive electrode active material, conductive agent Super P, and binder polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP). The solid content of the positive electrode slurry was 50 wt%, and the mass ratio of positive electrode active material, Super P, and PVDF in the solid components was 8:1:1. The positive electrode slurry was coated onto a pre-coated current collector aluminum foil, dried at 85°C, and then cold-pressed. After edge trimming, cutting, and slitting, it was dried under vacuum at 85°C for 4 hours to form a positive electrode sheet. The positive electrode active material in Examples 1 to 33 was Li[Ni] 0.8 Co 0.1 Mn 0.1 O2, the positive electrode active material in Example 34 is Li[Ni 0.5 Co 0.2 Mn 0.3 O2, the positive electrode active material in Example 35 is Li[Ni0.6 Co 0.2 Mn 0.2 O2.

[0111] (2) Preparation of the positive electrode (without primer): LiNi, the positive electrode active material 0.8 Co 0.1 Mn 0.1 A positive electrode slurry is prepared in N-methylpyrrolidone (NMP) using O2, conductive agent Super P, and binder polyvinylidene fluoride (PVDF). The solid content of the positive electrode slurry is 50 wt%, and the solid component is LiNi. 0.8 Co 0.1 Mn 0.1 The mass ratio of O2, Super P, and PVDF is 8:1:1. The positive electrode slurry is coated onto the current collector aluminum foil and dried at 85°C. After cold pressing, the foil is trimmed, cut, and slit. Then, it is dried under vacuum at 85°C for 4 hours to produce the positive electrode sheet.

[0112] (3) Preparation of negative electrode: Graphite, used as the negative electrode active material, was mixed evenly with conductive agent Super P, thickener CMC, and binder styrene-butadiene rubber (SBR) in deionized water to prepare a negative electrode slurry. The solid content of the negative electrode slurry was 30 wt%, and the mass ratio of graphite, Super P, CMC, and binder styrene-butadiene rubber (SBR) in the solid components was 80:15:3:2. The negative electrode slurry was coated onto a current collector copper foil (8 μm thick) and dried at 85 °C. Then, it was cold-pressed, trimmed, cut into sheets, and slit. Finally, it was dried under vacuum at 120 °C for 12 h to prepare the negative electrode sheet.

[0113] (4) Preparation of lithium-ion batteries: A 16μm polyethylene film (PE) is used as the separator. The prepared positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to isolate them. The cells are then wound to obtain a bare cell, tabs are welded on, and the bare cell is placed in an outer package. The electrolyte prepared above is injected into the dried casing. The process includes encapsulation, settling, formation, shaping, and capacity testing to complete the preparation of the lithium-ion battery (the thickness of the soft-pack lithium-ion battery is 4.0mm, the width is 60mm, and the length is 140mm).

[0114] The testing process for lithium-ion batteries will be explained next.

[0115] (1) Cyclic performance test of lithium-ion batteries A lithium-ion battery is charged at 25°C with a constant current of 1C to 4.2V, then charged at a constant voltage of 4.2V to a current of 0.05C, and finally discharged at a constant current of 1C to 2.8V. This constitutes one charge-discharge cycle. Using the initial discharge capacity as 100%, calculate the capacity retention rate of the lithium-ion battery after 500 cycles. Capacity retention rate (%) after 500 cycles = (Discharge capacity of the 500th cycle / Initial discharge capacity) × 100%.

[0116] (2) Thermal runaway performance test of lithium-ion batteries The ambient temperature was adjusted to 25℃. The lithium-ion battery was charged at 1C to 4.2V, followed by constant voltage charging to 0.05C. The lithium-ion battery was then placed in a heating furnace, which was heated at a rate of 10℃ / min and held at that temperature for 10 minutes until thermal runaway occurred in the lithium-ion battery, at which point the process was terminated. The furnace temperature was recorded at the point of thermal runaway. Electrode transverse tensile strength test As an example, the following method can be used for testing: After 500 cycles, the two ends of the positive electrode sheet (50 mm in length and 20 mm in width) are fixed on the clamps of the Instron 3365 high-speed rail tensile testing machine, and pulled at a speed of 10 mm / min until the sample is broken to complete the test. The tensile force values ​​F (N) in the length and width directions are obtained according to the instrument's built-in software. The transverse tensile strength can be obtained by R = F / (width of aluminum foil × thickness of aluminum foil).

[0117] Electrode peel strength test As an example, the following test method can be used: Fix one side of the positive electrode sheet (which has undergone 500 cycles) to a steel plate (double-sided tape can be used). Gently peel the membrane, allowing approximately 2cm of the membrane to detach from the substrate. Fix one end of the steel plate to the tensile testing machine clamp, and fix the detached membrane to the clamp at the top of the tensile testing machine. Use an Instron 3365 high-speed rail tensile testing machine at a speed of 60mm / min. The membrane will slowly peel off from the substrate. The computer will display the tensile force value when the tension stabilizes, which is the peel strength value of the membrane. During peeling, the base coating layer and the active material layer are a single unit, peeling off from the substrate.

[0118] Positive electrode resistance test Place the initial positive electrode into the Yuaneng Technology BER2100 multi-functional electrode resistance meter and wait 10 seconds between the upper and lower contact surfaces. After the data appears on the computer monitor, proceed to the next position for testing. Test 10 different positions and take the average value.

[0119] (5) 45℃ capacity retention test A lithium-ion battery is charged at 45℃ with a constant current of 1C to 4.2V, then charged at a constant voltage of 4.2V to a current of 0.05C, and finally discharged at a constant current of 1C to 2.8V. This constitutes one charge-discharge cycle. Using the initial discharge capacity as 100%, calculate the capacity retention rate of the lithium-ion battery after 200 cycles. Capacity retention rate (%) after 200 cycles = (Discharge capacity of the 200th cycle / Initial discharge capacity) × 100%.

[0120] (6) Lithium-ion battery charging temperature rise test The lithium-ion battery was placed in a 25°C constant temperature chamber and left to stand for 30 minutes to allow it to reach a constant temperature. The battery was then charged at a constant current of 1.0C to a voltage of 4.2V, followed by constant voltage charging at 4.2V to a current of 0.05C. Next, it was discharged at a constant current of 1.0C to 2.8V. The charging process was monitored using a multi-channel temperature sensor to track the surface temperature rise of the battery. The test results are recorded in Table 4.

[0121] Table 4

[0122] The test results in Table 4 show that the overall performance of Examples 1-35 is improved compared to Comparative Examples 1-5. This indicates that the composition of the conductive coating in this application effectively ensures a balance between adhesion and conductivity. Comparative Example 1 lacks a primer, failing to suppress the corrosion of the aluminum foil by lithium fluorosulfonylimide, potentially leading to electrode breakage and internal short circuits during use, resulting in the worst cycle performance and safety performance. Comparative Examples 2 and 4, although containing primers, have excessively high binder content, severely affecting the conductivity of the primer, increasing electrode impedance, increasing secondary battery polarization, and deteriorating secondary battery performance and safety. Comparative Examples 3 and 5 have insufficient binder content, failing to effectively bond the membrane. During cycling, electrode adhesion weakens, resulting in poor electrical contact between the current collector and the active material, causing extremely high contact resistance, thus leading to poor overall secondary battery performance.

[0123] Furthermore, a comparison of the results of Example 27 and the other examples shows that when the binder / conductive agent in the primer meets the above range and the primer thickness satisfies C2 / (5×C1)≤d≤lg(C2 / C1)+4, a battery with better performance can be obtained.

[0124] Although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A secondary battery, comprising a positive electrode and an electrolyte, wherein, The positive electrode sheet comprises: a current collector; a conductive coating, disposed on at least one surface of the current collector, wherein the conductive coating comprises a conductive agent with a mass content of 20% to 50% and a binder with a mass content of 50% to 80%; a positive electrode active layer, disposed on the surface of the conductive coating facing away from the current collector; The electrolyte comprises a lithium salt, and the lithium salt comprises lithium fluorosulfonylimide and lithium hexafluorophosphate; The total concentration of the lithium salt in the electrolyte is 0.6 mol / L to 2 mol / L; The concentration C2 of the lithium fluorosulfonylimide is 0.5 mol / L to 1.5 mol / L.

2. The secondary battery according to claim 1, wherein, The adhesive is a conductive adhesive, and the volume resistivity of the conductive adhesive is ≤10. -3 Ω•cm.

3. The secondary battery according to claim 1, wherein, The conductive coating comprises a conductive agent with a mass content of 20% to 30% and a conductive binder with a mass content of 70% to 80%.

4. The secondary battery according to claim 1, wherein, The conductive binder is selected from any one or more of the group consisting of epoxy resin conductive adhesives, silicone resin conductive adhesives, polyimide resin conductive adhesives, phenolic resin conductive adhesives, and polyurethane conductive adhesives.

5. The secondary battery according to claim 1, wherein, The adhesive is an insulating adhesive, and the volume resistivity of the insulating adhesive is ≥10. 10 Ω•cm.

6. The secondary battery according to claim 1, wherein, The conductive coating comprises a conductive agent with a mass content of 30% to 45% and an insulating binder with a mass content of 55% to 70%.

7. The secondary battery according to claim 1, wherein, The insulating binder is selected from any one or more of the group consisting of PVDF, polyacrylonitrile, styrene-butadiene rubber, polyvinyl alcohol, gum arabic, xanthan gum, and polyacrylate.

8. The secondary battery according to claim 1, wherein, The conductive agent comprises any one or more selected from the group consisting of acetylene black, carbon fibers, conductive carbon black, conductive graphite, single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene nanosheets, graphene oxide nanosheets, and fine powdered graphite.

9. The secondary battery according to claim 1, wherein, The thickness of the conductive coating is 0.5 micrometers to 5 micrometers.

10. The secondary battery according to claim 9, wherein, The thickness of the conductive coating is 0.8 micrometers to 3 micrometers.

11. The secondary battery according to claim 1, wherein, The current collector is an aluminum foil.

12. The secondary battery according to claim 1, wherein, The thickness of the aluminum foil is 8 micrometers to 20 micrometers, and / or the tensile strength in the longitudinal direction and the transverse direction of the current collector is ≥ 175 MPa.

13. The secondary battery according to claim 1, wherein, The positive electrode active material comprises at least one of Formulas (I) to (III): Li a1 Ni x1 Co y1 M1 z1 M2 1-x1-y1-z1 O 2-b1 Formula (I) Li a2 Mn 2-y2 M3 y2 O 4-b2 Formula (II) cLi₂MnO₃·(1-c)Li a3 M4 x3 O 2-b3 Formula (III) In Formula (I), M1 is Mn and / or Al, M2 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti, 0.8≤a1<1.2, 0≤x1<1, 0≤y1≤1, 0≤z1≤1, x1+y1+z1≤1, -0.2≤b1≤0.2; In Formula (II), 0.8≤a2<1.2, 0.6≤y2≤1, -0.2≤b2≤0.2, M3 is any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti; In Formula (III), 0<c<1, 0<x3<1, 0.8<a3<1.2, -0.2≤b3≤0.2, M4 is any one of Ni, Co and Mn, as well as any one or more selected from the group consisting of Mg, Cu, Zn, Al, Sn, B, Ga, Zr, Cr, Sr, V and Ti.

14. The secondary battery according to claim 1, wherein, The electrolyte further satisfies at least one of the following conditions: (1) The fluorinated sulfonyl imide lithium is any one or more of the group consisting of lithium bis(trifluoromethyl)fluorosulfonyl imide, lithium (fluorosulfonyl)(trifluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(pentafluoroethylsulfonyl)imide, lithium (trifluoromethylsulfonyl)(difluoromethylsulfonyl)imide, lithium (fluorosulfonyl)(perfluorobutylsulfonyl)imide, and lithium bis(pentafluoroethylsulfonyl)imide; (2) In the electrolyte, the concentration C1 of lithium hexafluorophosphate and the concentration C2 of lithium fluorine sulfonyl imide satisfy: 1≤C2 / C1≤5.

15. The secondary battery according to claim 14, wherein, The thickness d of the conductive coating of the positive electrode, the concentration C1 of lithium hexafluorophosphate, and the concentration C2 of lithium fluorine sulfonyl imide satisfy the following relationship: C2 / (5×C1)≤d≤lg(C2 / C1)+4, Where C1 and C2 are in units of mol / L, and d is in units of μm.

16. The secondary battery according to claim 14 or 15, wherein, The electrolyte further includes an organic solvent and additives, wherein the organic solvent is selected from any one or more of the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, ethyl propyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and tetrahydrofuran; and / or, The organic solvent has a mass content of 65%–85% in the electrolyte; and / or, The additive is selected from at least one of the following groups: vinylene carbonate, vinyl sulfate, lithium difluorooxalate borate, lithium difluorophosphate, lithium tetrafluoroborate, 1,3-propanesulfonate lactone, lithium trifluoromethanesulfonate, and lithium diacetate borate; and / or, The total mass content of the additive in the electrolyte is 0.5% to 7%.

17. The secondary battery according to claim 1, wherein, The negative electrode active materials of the negative electrode sheet include natural graphite, artificial graphite, mesophase micro carbon, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O. 12 Any one or more of the group consisting of Li-Al alloys.

18. A battery module comprising a secondary battery, wherein, The secondary battery is any one of claims 1 to 17.

19. A battery pack comprising a battery module, wherein the battery module is the battery module of claim 18.

20. An electrical device comprising a secondary battery, a battery module, or a battery pack, wherein, The secondary battery is selected from any one of the secondary batteries of claims 1 to 17, the battery module is the battery module of claim 18, or the battery pack is the battery pack of claim 19.