A multilayer negative electrode and a lithium-ion battery
By optimizing the multi-layer negative electrode structure and the kinetic balance index, the balance problem between high energy density and fast charging performance of lithium-ion batteries has been solved, thus improving the overall performance of the battery.
Patent Information
- Application Number
- CN202611314432.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion batteries face challenges in balancing high energy density and fast charging performance, and the design of traditional anode materials has failed to effectively balance the relationship between the two.
A multi-layer negative electrode structure is adopted. By optimizing the proportion of primary particles, rebound rate and binder content of the negative electrode active material, the parameters are optimized using the kinetic balance index Y=2.5(0.4×a+0.6×c)+e2/(b+d+0.05) to construct a gradient pore structure adapted to lithium-ion intercalation and deintercalation.
It achieves a balance between high energy density and fast charging performance, improves the overall electrochemical performance of the battery, enhances the diffusion and transport efficiency of lithium ions in the negative electrode active material, and reduces the risk of lithium plating.
Smart Images

Figure CN123120629A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical technology, and more specifically, relates to a multilayer negative electrode and a lithium-ion battery. Background Technology
[0002] The fast charging and energy density of lithium-ion batteries directly affect the charging time and driving range of electric vehicles. Therefore, faster charging and longer driving range have become the top concerns for users.
[0003] Currently, the mainstream power battery cells on the market have an energy density of 170-180Wh / kg and a fast charging capability of 1.6-2.6C. As demand increases, the energy density is moving towards 185-190Wh / kg, and the fast charging capability is developing towards 4C or even 6C, which means that both energy density and fast charging need to be taken into account.
[0004] High energy density means more active lithium ions; fast charging performance means that active lithium ions are extracted and reach the negative electrode in a short time, which requires the negative electrode material to have rapid lithium intercalation capability. Double-layer coating of the negative electrode sheet is an effective solution. Among them, the selection of negative electrode active material has a significant impact on the performance of double-layer negative electrode sheets. The physicochemical properties of the negative electrode active material, such as specific surface area, particle size, compaction density, physical rebound, and the ratio of primary and secondary particles, all affect fast charging and energy density. CN113875037A, CN113875046A, and CN113875047A, etc., achieve the secondary battery with good kinetic performance and long cycle life while maintaining high energy density by focusing on the force rebound rate of the negative electrode active material, powder resistivity, and the ratio of primary particles. However, they do not comprehensively consider the combined effects of the ratio of secondary particles, force rebound rate, and the content of binder in the electrode sheet on fast charging and energy density.
[0005] To address the industry pain point of traditional liquid lithium batteries, which struggle to simultaneously achieve high energy density, dynamic performance, cycle life, and safety, this invention provides a multilayer negative electrode and a lithium-ion battery. Summary of the Invention
[0006] The purpose of this invention is to address the shortcomings of existing technologies by proposing a multilayer negative electrode sheet and a lithium-ion battery. This invention achieves both high energy density and fast-charging performance by optimizing the proportion of primary particles, rebound rate, and binder content in the negative electrode active material, thus meeting the higher performance requirements of electric vehicles.
[0007] To achieve the above objectives, the present invention provides a multilayer negative electrode sheet, wherein the multilayer negative electrode sheet includes a current collector, a first negative electrode active material layer, and a second negative electrode active material layer; The first negative electrode active material layer is coated on the surface of the current collector, and the second negative electrode active material layer is coated on the surface of the first negative electrode active material layer; The multilayer negative electrode sheet satisfies the following relationship: Y = 2.5(0.4 × a + 0.6 × c) + e 2 / (b+d+0.05); in: Y is the kinetic balance index characterizing the performance of the multilayer negative electrode sheet, where 0 < Y ≤ 7; a and c represent the mass percentages of primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer, respectively, where a is 30-100% and c is 30-100%, and a≥c. b and d represent the rebound rates of the first and second negative electrode active material layers under full charge, respectively. b is 10-40% and d is 10-30%, and b ≥ d. e is the ratio of the mass content of the binder in the first negative electrode active material layer to the mass content of the binder in the second negative electrode active material layer, and e is 0.5-1.5.
[0008] In this invention, the relation Y = 2.5(0.4×a + 0.6×c) + e 2 / (b+d+0.05) is an empirical formula derived from regression fitting of multiple sets of experimental data, not a rigorous derivation from first principles. The specific process is as follows: (1) First, through orthogonal experimental design, the five parameters a, c, e, b, and d were varied in a system, and more than 15 sets of experimental data were obtained (including comparative examples 1-2 and examples 1-13 recorded in this invention). (2) Subsequently, a multivariate nonlinear regression analysis was performed on the above data; in terms of model selection, various candidate forms such as linear summation model and product interaction model were tried, and finally, the double summation structure of "nonlinear weighted average particle scaling factor + diffusion impedance modulation term" (i.e., K1(w1·a+w2·c)+e) was found to be adopted. α The general form of / (b+d+β) yields the best fit. Based on this, the regression determined the values of each coefficient: K1=2.5, w l =0.4, w2=0.6, α=2, β=0.05.
[0009] (3) The empirical formula of this invention has a significantly better fit to experimental data than a simple linear or exponential relationship model between a single parameter and performance. Specifically: Structural level: This invention adopts a double-layer structure of a first negative electrode active material layer and a second negative electrode active material layer, and constructs a gradient pore structure adapted to the fast charging process through differentiated design of the upper and lower layers in three dimensions: primary particle ratio, rebound rate and binder content ratio. This is the structural basis for achieving both high energy density and fast charging capability. At the quantitative screening level: Based on the structural design, this invention discovered a nonlinear synergistic relationship among the above-mentioned parameters (primary particle ratio, rebound rate, and binder content ratio), and for the first time expressed this relationship in the form of a quantitative formula (kinetic balance index Y), which elevates the performance optimization of the bilayer negative electrode from empirical screening to a calculable and predictable quantitative design method.
[0010] Furthermore, in this invention, for the relation Y = 2.5(0.4 × a + 0.6 × c) + e 2 / (b+d+0.05), where: 1) 2.5 (0.4×a+0.6×c) is a nonlinear weighted average particle proportion factor, representing the balance between solid-phase diffusion and lithium intercalation expansion. The "primary particle proportions a and c" of the negative electrode active material directly determine the length of the solid-phase lithium-ion diffusion path and the material's lithium intercalation volume expansion rate. That is, a high primary particle proportion results in a large specific surface area and a short diffusion path, which is beneficial for fast charging (kinetics), but also leads to large volume expansion, which is detrimental to energy density maintenance and cycle life. Conversely, a high secondary particle proportion results in the opposite. This is an inherent material property throughout the charge and discharge process. The coefficients 0.4 and 0.6 reflect the difference in the weight of the contribution of the first negative electrode active material layer (bottom layer) and the second negative electrode active material layer (top layer) to this term. Since lithium ions first arrive at and intercalate into the top layer (second negative electrode active material layer) during charging, the particle morphology of the top layer has a more direct and significant impact on the initial lithium-ion intercalation rate and concentration polarization formation. Therefore, c, representing the top layer, is given a higher weight of 0.6, while a, representing the bottom layer, is given a weight of 0.4.
[0011] 2) e 2 / (b+d+0.05) represents the diffusion impedance modulation term, characterizing the liquid-phase transport equilibrium of the electrolyte within the electrode's porous structure. During the slurry drying process, the binder SBR tends to migrate and accumulate towards the surface layer (the second negative electrode active material layer), leading to excessive blockage of the surface pores and increasing the tortuosity of lithium-ion liquid-phase transport within the pores. This transport resistance caused by the uneven distribution of the binder SBR exhibits a non-linear relationship with its distribution deviation; even small uneven distributions can lead to a significant increase in transport impedance. Therefore, e is used... 2 This is used to characterize the "additional" ion transport impedance caused by the uneven distribution of the binder SBR.
[0012] 3) b+d+0.05 represents the rebound rate of the first and second negative electrode active material layers in the fully charged state, and the contribution of the superimposed electrode to the baseline porosity in the initial state before lithium insertion and rebound. The rebound rate is positively correlated with the final porosity of the electrode. A high rebound rate means more abundant lithium-ion liquid phase transport channels, which can effectively reduce transport resistance. Here, "0.05" is essentially an empirical constant determined during the regression fitting process. Its main function in the formula is mathematical adjustment: to prevent the denominator from becoming invalid when the sum of the rebound rates (b+d) of the first and second negative electrode active material layers in the fully charged state approaches zero, thus ensuring the mathematical stability of the formula. From a numerical perspective, the working ranges of b and d are 10-40% and 10-30%, respectively, meaning that b+d is usually between 0.20 and 0.70. 0.05 accounts for only a small proportion of this and will not have a substantial impact on the overall trend and ranking of the Y-value calculation results. In terms of physical magnitude, 0.05 is exactly on the same order of magnitude as the initial residual porosity that the electrode may have in the un-lithiated, un-rebound state. Therefore, the expression "baseline porosity contribution" is used in this invention. However, this positioning is auxiliary. Strictly speaking, 0.05 should be understood as an empirical constant determined by regression, rather than a physical quantity with independent measurement basis.
[0013] 4) When the Y value is too low (e.g., Y→0), it means that the weighted particle ratio tends to be all large particles, or the SBR binder is severely unevenly distributed, resulting in excessively high diffusion resistance. At this time, the lithium-ion solid-phase diffusion path is long, the liquid-phase transport resistance is high, and the fast charging rate of the cell is low. When the Y value is too high (e.g., Y>7), it means that the weighted particle ratio tends to be all small particles, or the electrode rebounds excessively in pursuit of low impedance. Although the kinetics are excellent, the violent volume expansion of small particles and the excessive porosity will sacrifice the compaction density of the active material and the mechanical stability of the electrode, resulting in a sharp drop in energy density and the risk of lithium plating during long cycles. In this invention, the Y value quantitatively balances the competitive relationship between solid-phase diffusion kinetics and liquid-phase transport impedance (the fast-charging performance of a battery is not determined by a single factor, but is jointly constrained by the "diffusion rate of lithium ions within the negative electrode active material" (solid-phase diffusion kinetics) and the "migration rate of lithium ions in the pores of the negative electrode sheet" (liquid-phase transport impedance). These two processes are in competition, and the ingenuity of this invention lies in its use of a comprehensive index Y to quantify and balance this inverse relationship, thereby finding the optimal balance between fast charging and energy density). This invention controls the Y value to 0 < Y ≤ 7, preferably 2 ≤ Y ≤ 7, and more preferably 4 ≤ Y ≤ 6. By controlling the "primary particle ratio, rebound rate, and binder content ratio" within specific ranges, the multilayer negative electrode sheet of this invention can form a gradient pore structure adapted to the lithium ion insertion / extraction rate, significantly improving the overall electrochemical performance of the battery.
[0014] According to the present invention, preferably, 2≤Y≤7, more preferably 4≤Y≤6.
[0015] According to the present invention, preferably, a is 30-70% and c is 30-50%.
[0016] According to the present invention, preferably, b is 14-35% and d is 10-25%, more preferably, b is 20-30% and d is 12-25%.
[0017] In this invention, the rebound rate of the first and second negative electrode active material layers under full charge refers to the phenomenon where, when the battery cell is fully charged (lithium ions are fully embedded in the negative electrode), the thickness of the negative electrode sheet temporarily increases due to the volume expansion of the graphite negative electrode active material after lithium embedding. This is an "electrochemically induced rebound" that occurs during the battery cell's use / cycling stage. After the battery is charged to full charge after capacity testing, it is disassembled and the thickness of the negative electrode sheet at different locations is measured. The average value is recorded as h2, and the negative electrode rebound rate R is calculated as follows: R = (h2 - h1) × 100% / (h1 - h2) × 100% / (h2 ... Cu ),in: h1: Average thickness of negative electrode sheet immediately after rolling (μm). h2: The average thickness (μm) of the negative electrode sheet at different locations after the battery has been charged to a fully charged state following capacity testing and disassembly. h Cu Copper foil thickness (μm).
[0018] According to the present invention, preferably, e is 0.5-1.4, more preferably, e is 0.8-1.3.
[0019] In this invention, the binder in the first negative electrode active material layer and the second negative electrode active material layer is styrene-butadiene rubber (SBR) independently.
[0020] In this invention, primary particles and secondary particles refer to whether the morphology of the graphite anode active material is primary or secondary particles. This difference is mainly due to the different granulation processes in the most critical step of graphite anode material production. The granulation process directly affects the particle size, distribution, and morphology of the anode material, thereby affecting battery rate performance, cycle life, and compaction density, as detailed below: Primary granulation mainly involves pulverizing the pretreated raw coke into fine powder using an air jet mill, and then forming primary particles (with particle sizes typically ranging from nanometers to micrometers, such as 0.1-1μm) through simple mixing. The purpose of primary granulation is to reduce the volume of negative electrode particles, shorten the lithium-ion diffusion path, and focus on high-rate performance and fast charge and discharge. Secondary granulation involves using asphalt as a binder under specific temperature and pressure conditions. Based on the target particle size, primary particles are bonded into larger particles (typically in the micrometer to millimeter range, such as 5-30 μm) through a high-temperature pyrolysis process in a reactor. The purpose of secondary granulation is to bond small particles into larger particles, thereby improving mechanical stability and cycle life through agglomeration structure, while also increasing compaction density. However, it is necessary to optimize electrical conductivity and diffusion efficiency. Regarding rate capability, smaller negative electrode particles shorten the lithium-ion migration path, which is more conducive to lithium-ion movement. Conversely, larger negative electrode particles result in higher compaction density and increased space utilization of the active particles, which is more beneficial for lithium storage. Secondary particles prepared through granulation combine the advantages of large particles (high compaction density and large capacity), while primary particles offer advantages such as large specific surface area and numerous lithium-ion insertion / extraction channels. Therefore, there is no specific range of types for primary and secondary particles; they can be prepared based on a comprehensive consideration of fast-charging capability, compaction density, and cost, serving as the preferred option. The particle size of the primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer is independently 0.1-1 μm; The particle size of the secondary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer are each independently 5-30 μm.
[0021] According to the present invention, preferably, the active materials of the first negative electrode active material layer and the second negative electrode active material layer are each independently at least one of artificial graphite, natural graphite and hard carbon.
[0022] According to the present invention, preferably, the particle size of the primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer is independently 0.1-1 μm; The particle size of the secondary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer are each independently 5-30 μm.
[0023] According to the present invention, preferably, the first negative electrode active material layer and the second negative electrode active material layer each independently include a thickener and a conductive agent; Based on the total mass of the first negative electrode active material layer, the content of active material is 96.3-97.1 wt%, the content of binder is 2.1-3.0 wt%, the content of thickener is 0.5-1.5 wt%, and the content of conductive agent is 0-0.5 wt%. Based on the total mass of the second negative electrode active material layer, the content of active material is 96.3-97.1 wt%, the content of binder is 2.1-3.0 wt%, the content of thickener is 0.5-1.5 wt%, and the content of conductive agent is 0-0.5 wt%.
[0024] According to the present invention, preferably, the thickness of the multilayer negative electrode sheet is 120-155 μm.
[0025] Another aspect of the present invention provides a lithium-ion battery, the battery comprising a positive electrode, a separator, a negative electrode, and an electrolyte; The negative electrode sheet is the aforementioned multilayer negative electrode sheet.
[0026] The beneficial effects of the technical solution of the present invention are as follows: The proposed dual-layer anode structure facilitates the construction of a well-defined gradient pore structure, achieving a balance between power and energy density while overcoming the challenges of single-layer electrode structures. This invention, through the rational design of upper and lower anode active materials with different primary particle ratios (a≥c), combined with the rebound rate and binder (e.g., SBR) content ratio, achieves a reasonable match between the active sites in the upper and lower layers (between the first and second anode active material layers). This promotes the formation of a gradient pore distribution, effectively regulating the diffusion path of active ions and facilitating their rapid diffusion within the electrode. The liquid-phase transport resistance of active ions extracted from the positive electrode on the surface of the anode active material layer is reduced, preventing lithium plating problems caused by accumulation on the surface layer (second anode active material layer). Simultaneously, the uniform diffusion of active ions within the anode active material layer helps reduce polarization, further improving kinetic performance. Specifically: First, in this invention, the proportion of primary particles in the negative electrode active material directly affects the lithium-ion diffusion rate and the relative volume expansion of the graphite negative electrode material, thus affecting the fast-charging capability and energy density of the battery cell. Specifically: when the proportion of primary particles is high, the lithium-ion diffusion path within the graphite negative electrode material is shorter, the lithium-ion diffusion resistance is lower, and the fast-charging performance is better. However, small-diameter graphite negative electrode materials lead to a larger relative volume expansion due to lithium intercalation, making the graphite negative electrode material more susceptible to damage during cycling, resulting in deteriorated cycle performance. When the proportion of primary particles is low, the relative volume expansion due to lithium intercalation in the graphite negative electrode material is smaller, the graphite structure is more stable during cycling, and the cycle performance is better. However, large-diameter graphite negative electrode materials prolong the lithium-ion diffusion path within the graphite negative electrode material, leading to increased lithium-ion diffusion resistance and deteriorated fast-charging performance. The graphite negative electrode material provided by this invention has a moderate primary and secondary particle ratio, achieving both superior fast-charging and cycle performance.
[0027] Secondly, due to the issue of SBR binder floating during electrode baking, when the SBR content of the first negative electrode active material layer is greater than that of the second negative electrode active material layer, the SBR content of the upper and lower layers can be better matched. This results in a better match between the negative electrode active material and the conductive agent in the negative electrode active material layer, which is well matched with the concentration gradient distribution of active ions during battery charging and discharging. This effectively regulates the diffusion rate of active ions at different positions on the electrode, thus effectively improving the battery's fast charging performance. Furthermore, within the given range, the SBR content of the upper and lower layers is beneficial for increasing the compaction density of the negative electrode film, thereby further improving the battery's energy density.
[0028] Third, the rebound rate of the electrode affects its porosity, ultimately impacting wettability and fast charging capability. When the rebound rate of the first negative electrode active material layer is greater than that of the second negative electrode active material layer, the overall porosity of the electrode increases. However, the differentiated rebound rates of the two layers create a gradient pore structure, which is more conducive to improving fast charging and energy density.
[0029] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0030] The above and other objects, features and advantages of the present invention will become more apparent from the more detailed description of exemplary embodiments of the invention in conjunction with the accompanying drawings.
[0031] Figure 1 A schematic diagram of a multilayer negative electrode sheet provided in Embodiment 1 of the present invention is shown. Detailed Implementation
[0032] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0033] Example 1
[0034] This embodiment provides a multilayer negative electrode sheet, which includes a current collector, a first negative electrode active material layer, and a second negative electrode active material layer. like Figure 1 As shown, the first negative electrode active material layer is coated on the surface of the current collector, and the second negative electrode active material layer is coated on the surface of the first negative electrode active material layer.
[0035] The multilayer negative electrode sheet satisfies the following relationship: Y = 2.5(0.4 × a + 0.6 × c) + e2 / (b+d+0.05); in: Y is the kinetic balance index characterizing the performance of the multilayer negative electrode sheet, which is 2.660; 'a' represents the mass percentage of primary particles in the active material of the first negative electrode active material layer, which accounts for the total mass of primary and secondary particles; a is 67%. c represents the mass percentage of primary particles in the active material of the second negative electrode active material layer, which is 43% of the total mass of primary and secondary particles. b represents the rebound rate of the first negative electrode active material layer in the fully charged state, which is 26.5%. d represents the rebound rate of the second negative electrode active material layer in the fully charged state, and d is 13.8%; e is the ratio of the mass content of the binder in the first negative electrode active material layer to the mass content of the binder in the second negative electrode active material layer, and e is 1.28.
[0036] The binder in the first negative electrode active material layer and the second negative electrode active material layer is styrene-butadiene rubber (SBR) independently.
[0037] The active materials of the first negative electrode active material layer and the second negative electrode active material layer are each independently artificial graphite; The particle size of the primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer is 0.5 μm, respectively. The particle size of the secondary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer is 13 μm, respectively.
[0038] The first negative electrode active material layer and the second negative electrode active material layer each independently include a thickener and a conductive agent; Based on the total mass of the first negative electrode active material layer, the content of the active material artificial graphite is 96.3 wt%, the content of the binder styrene-butadiene rubber (SBR) is 2.2 wt%, the content of the thickener carboxymethyl cellulose is 1.0 wt%, and the content of the conductive agent conductive carbon black is 0.5 wt%. Based on the total mass of the second negative electrode active material layer, the content of the active material artificial graphite is 97.1 wt%, the content of the binder styrene-butadiene rubber (SBR) is 1.9 wt%, the content of the thickener carboxymethyl cellulose is 0.5 wt%, and the content of the conductive agent conductive carbon black is 0.5 wt%.
[0039] The overall thickness of the multilayer negative electrode sheet is 120 μm.
[0040] The preparation method of the multilayer negative electrode sheet in this embodiment is as follows: (1) Preparation of the slurry for the first negative electrode active material layer Artificial graphite, binder SBR, thickener carboxymethyl cellulose, conductive carbon black and deionized water are added to a mixing tank in sequence and mixed to prepare a stable and uniform first negative electrode active material layer slurry. (2) Preparation of the slurry for the second negative electrode active material layer Artificial graphite, binder SBR, thickener carboxymethyl cellulose, conductive carbon black and deionized water are added to a mixing tank in sequence and mixed to prepare a stable and uniform second negative electrode active material slurry. (3) Preparation of multilayer negative electrode sheets A 4.5µm copper foil is used as the negative electrode current collector. A first negative electrode active material layer slurry is uniformly coated on the surface of the copper foil, and a second negative electrode active material layer slurry is uniformly coated on the surface of the first negative electrode active material layer. After drying, the material is cold-pressed into a multilayer negative electrode sheet.
[0041] This embodiment also provides a lithium-ion battery, characterized in that the battery includes a positive electrode, a separator, a negative electrode, and an electrolyte; wherein: The negative electrode sheet is the multilayer negative electrode sheet described in this embodiment; Preparation of the positive electrode sheet: A 12µm aluminum foil was used as the positive electrode current collector. A positive electrode active slurry was uniformly coated on the surface of the aluminum foil, and then cold-pressed to obtain the positive electrode sheet. The positive electrode active slurry consisted of 96.7wt% lithium iron phosphate, 0.8wt% conductive carbon black, 0.7wt% carbon nanotubes, and 1.8wt% polyvinylidene fluoride. The overall thickness of the positive electrode sheet was 172µm. Preparation of lithium-ion batteries: The above-mentioned positive electrode sheet, coated separator (base film material: polypropylene) and negative electrode sheet are stacked in a Z-shape to obtain stacked units. Then, the stacked units are thermally composited, followed by processes such as casing, baking, electrolyte injection (electrolyte is injected according to the injection coefficient of 3.0g / Ah), formation, high-temperature storage, capacity testing, high-temperature aging, and room-temperature aging, and finally a 135Ah lithium-ion battery is obtained.
[0042] Table 1
[0043] Test case
[0044] This test case examines the energy density and fast charging rate of the batteries obtained in the above embodiments and comparative examples.
[0045] Battery energy density test: After the battery is left to stand in an environment of 25℃±2℃ for 30 minutes, it is charged to 3.65V with a constant current of 1C (135A), and then charged to 0.05C (6.75A) with a constant voltage until the current is cut off; it is left to rest for 30 minutes; then it is discharged to 2.5V with a constant current of 1C (135A); the cycle is repeated for 3 times. The test can be stopped if the energy difference between the 3 cycles does not exceed 3%. The discharge energy of the cell in the last cycle is recorded as E (Wh); the weight of the cell is weighed with an electronic balance and recorded as G (kg). The energy density ED (Wh / kg) = E / G is calculated.
[0046] Battery fast charging capability test: The battery is made into a three-electrode configuration, and then the equivalent fast charging capability from 0% to 80% SOC at 25℃±2℃ is tested.
[0047] The results are shown in Table 1.
[0048] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A multilayer negative electrode sheet, characterized in that, The multilayer negative electrode sheet includes a current collector, a first negative electrode active material layer, and a second negative electrode active material layer; The first negative electrode active material layer is coated on the surface of the current collector, and the second negative electrode active material layer is coated on the surface of the first negative electrode active material layer; The multilayer negative electrode sheet satisfies the following relationship: Y=2.5(0.4×a+0.6×c)+e 2 / (b+d+0.05); in: Y is the kinetic balance index characterizing the performance of the multilayer negative electrode sheet, where 0 < Y ≤ 7; a and c represent the mass percentages of primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer, respectively, where a is 30-100% and c is 30-100%, and a≥c. b and d represent the rebound rates of the first and second negative electrode active material layers under full charge, respectively. b is 10-40% and d is 10-30%, and b ≥ d. e is the ratio of the mass content of the binder in the first negative electrode active material layer to the mass content of the binder in the second negative electrode active material layer, and e is 0.5-1.
5.
2. The multilayer negative electrode sheet according to claim 1, wherein, 2≤Y≤7, preferably 4≤Y≤6.
3. The multilayer negative electrode sheet according to claim 1, wherein, a is 30-70%, and c is 30-50%.
4. The multilayer negative electrode sheet according to claim 1, wherein, b is 14-35% and d is 10-25%, preferably b is 20-30% and d is 12-25%.
5. The multilayer negative electrode sheet according to claim 1, wherein, e is 0.5-1.4, preferably e is 0.8-1.
3.
6. The multilayer negative electrode sheet according to claim 1, wherein, The active materials of the first negative electrode active material layer and the second negative electrode active material layer are each independently at least one of artificial graphite, natural graphite and hard carbon.
7. The multilayer negative electrode sheet according to claim 6, wherein, The particle size of the primary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer is independently 0.1-1 μm; The particle size of the secondary particles in the active materials of the first negative electrode active material layer and the active materials of the second negative electrode active material layer are each independently 5-30 μm.
8. The multilayer negative electrode sheet according to claim 1, wherein, The first negative electrode active material layer and the second negative electrode active material layer each independently include a thickener and a conductive agent; Based on the total mass of the first negative electrode active material layer, the content of active material is 96.3-97.1 wt%, the content of binder is 2.1-3.0 wt%, the content of thickener is 0.5-1.5 wt%, and the content of conductive agent is 0-0.5 wt%. Based on the total mass of the second negative electrode active material layer, the content of active material is 96.3-97.1 wt%, the content of binder is 2.1-3.0 wt%, the content of thickener is 0.5-1.5 wt%, and the content of conductive agent is 0-0.5 wt%.
9. The multilayer negative electrode sheet according to claim 1, wherein, The thickness of the multilayer negative electrode sheet is 120-155 μm.
10. A lithium-ion battery, characterized in that, The battery includes a positive electrode, a separator, a negative electrode, and an electrolyte; The negative electrode sheet is a multilayer negative electrode sheet as described in any one of claims 1-9.
Citation Information
Patent Citations
Secondary battery, preparation method therefor, and apparatus comprising secondary battery
CN113875037A
Secondary battery, preparation method therefor and device comprising the secondary battery
CN113875046A
Secondary battery and method for preparing same, and device including secondary battery
CN113875047A