A secondary battery and an electrical device
By setting gradient distributions of conductive agent and active material particle sizes in the positive and negative electrode films of the secondary battery, combined with geometric structure design, the problems of lithium plating in the tab area and lifespan failure in the secondary battery during fast charging are solved, thereby improving the battery's fast charging performance and cycle performance.
Patent Information
- Application Number
- CN202611497595.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing rechargeable batteries suffer from severe lithium plating and lifespan failure in the tab area during fast charging. In particular, the current density in the tab area is higher than that in the main body area, resulting in excessively high activity in the positive electrode tab area. During charging, the local lithium-ion flux surges, while the negative electrode edge is in a low kinetic region. Uneven lithium-ion diffusion leads to severe lithium plating.
Different regions are set in the positive and negative electrode films of the secondary battery. The region near the tab has a higher proportion of conductive agent and a smaller particle size of active material. The geometric structure design ensures that the edge of the positive electrode film is completely covered by the negative electrode film, forming a gradient distribution and suppressing lithium ion flux concentration and lithium plating.
It effectively reduces the risk of lithium plating and life failure in the tab area, improves the fast charging performance and cycle performance of secondary batteries, ensures uniform distribution and rapid insertion of lithium ions, and reduces the risk of heat generation and cycle failure.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Technology
[0002] With the development of fast charging technology, the current density in the tab region of a secondary battery is significantly higher than that in the main electrode region. While existing technologies have proposed adding highly active materials or lithium replenishing agents to the tab region to improve performance, these methods suffer from two serious drawbacks. First, to reduce heat generation at the positive electrode tab, a common approach is to increase the conductive agent; however, this leads to excessively high activity in the positive electrode tab region, causing a surge in the localized flux of lithium ions "sprayed" to the negative electrode during charging. Second, if the negative electrode is simply widened (overhang), its edges are typically located in the main region (large particles, low kinetics region); when the high-flux ion current at the positive electrode diffuses due to the "edge effect," it falls into the low-kinetics region of the negative electrode, resulting in severe edge lithium plating. Summary of the Invention
[0003] The purpose of this application is to solve the technical problems of severe lithium plating in the tab area and life failure in the fast charging of secondary batteries, especially high-rate fast charging, in the prior art. It proposes a secondary battery and power device with less lithium plating under fast charging and excellent long-term cycle life.
[0004] To achieve the above objectives, a first aspect of this application provides a secondary battery, including a positive electrode and a negative electrode. The positive electrode includes a positive current collector, a positive electrode tab, and a positive electrode film layer disposed on at least one surface of the positive current collector. The negative electrode includes a negative current collector, a negative electrode tab, and a negative electrode film layer disposed on at least one surface of the negative current collector. The positive electrode film layer includes a positive active material and a positive conductive agent, and the negative electrode film layer includes a negative active material and a negative conductive agent. The secondary battery has a first orientation; The positive electrode film layer includes a first positive electrode film layer region close to the positive electrode tab and a second positive electrode film layer region away from the positive electrode tab along the first direction; The negative electrode film layer includes a first negative electrode film layer region close to the negative electrode tab and a second negative electrode film layer region away from the negative electrode tab along the first direction; The secondary battery satisfies (A) to (C): (A) The equivalent mass percentage C of the positive electrode conductive agent in the first positive electrode film region. p1 The equivalent mass percentage C of the positive electrode conductive agent in the second positive electrode film region is greater than that of the positive electrode conductive agent. p2 ; (B) The average particle size D of the negative electrode active material in the first negative electrode film layer region n1The average particle size D of the negative electrode active material in the second negative electrode film region is smaller than that of the negative electrode active material. n2 ; (C) The maximum dimension W of the first negative electrode film region along the first direction n1 The maximum dimension W along the first direction of the region of the first positive electrode film is greater than that of the first positive electrode film layer. p1 .
[0005] As some embodiments of this application, at least one of the following conditions is met: (A) 1.10≤C p1 / C p2 ≤5.5; (B) 1.05≤D n2 / D n1 ≤1.55; (C) 1.0mm≤W n1 -W p1 ≤12.0mm.
[0006] As some embodiments of this application W pt This refers to the maximum dimension of the positive electrode tab perpendicular to the first direction. W p This refers to the maximum dimension of the positive electrode film layer along the first direction; The secondary battery satisfies: 0.021 ≤ (W pt / W p )×(W p1 / W p )≤0.595.
[0007] As some embodiments of this application, the specific surface area S of the negative electrode active material in the first negative electrode film layer region is... n1 The specific surface area S of the negative electrode active material in the second negative electrode film region is greater than that of the negative electrode active material. n2 .
[0008] As some embodiments of this application, 1.05 ≤ S n1 / S n2 ≤1.60.
[0009] As some embodiments of this application, the secondary battery satisfies the following formula: k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c ≥0.01; in, f(C p ) is the compensation factor for the positive electrode electron conduction network, f(C)p )=C p1 / C p2 ; f(D n ) is the solid-state diffusion compensation factor for the negative electrode phase, f(D) n )=D n2 / D n1 ; f(W p ) represents the macroscopic current collection bottleneck leakage factor of the secondary battery, f(W) p )=(W pt / W p )×(W p1 / W p ); f(S n ) is the charge transfer activation factor at the negative electrode interface, f(S) n )=S n1 / S n2 ; k is an empirical parameter for system design, 0.2≤k≤0.8; N c The value of the charging rate parameter for the secondary battery.
[0010] As some embodiments of this application, the negative electrode film layer region further includes a lithium plating inhibitor, the lithium plating inhibitor having a lithium intercalation potential higher than that of the negative electrode active material.
[0011] In some embodiments of this application, the negative electrode film layer satisfies: M1 > M2. Wherein, M1 is the mass percentage of the lithium plating inhibitor in the first negative electrode film region. M2 is the mass percentage of the lithium plating inhibitor in the second negative electrode film region.
[0012] As some embodiments of this application, the lithium plating inhibitor includes silicon-carbon composite materials and silicon suboxide (SiO2). x It includes at least one of the following: pure silicon material, hard carbon, soft carbon, and lithium titanate.
[0013] As some embodiments of this application, the positive electrode film layer also includes lithium supplementation additives.
[0014] In some embodiments of this application, the positive electrode film layer satisfies: C1 > C2. Wherein, C1 is the mass percentage of the lithium-replenishing additive in the first positive electrode film region. C2 represents the mass percentage of the lithium-replenishing additive in the second positive electrode film region.
[0015] As some embodiments of this application, the lithium supplementing additive is selected from at least one of lithium-rich metal oxides, lithium-rich nitrides, lithium-rich sulfides, or lithium-containing organic compounds.
[0016] A second aspect of this application provides an electrical device comprising the secondary battery described in this application.
[0017] Compared with the prior art, the beneficial effects of this application are: The secondary battery provided in this application comprises a first positive electrode film layer region near the positive electrode tab and a second positive electrode film layer region away from the positive electrode tab in the positive electrode film layer, and a first negative electrode film layer region near the negative electrode tab and a second negative electrode film layer region away from the negative electrode tab in the negative electrode film layer; and further defines (1) the equivalent mass ratio C of the positive electrode conductive agent in the first positive electrode film layer region. p1 The equivalent mass percentage C of the positive electrode conductive agent in the region greater than the second positive electrode film layer p2 (2) The average particle size D of the negative electrode active material in the first negative electrode film layer region n1 The average particle size D of the negative electrode active material in the region smaller than that of the second negative electrode film layer is... n2 (3) The maximum dimension W of the first negative electrode film region along the first direction n1 The maximum dimension W along the first direction of the first positive electrode film region is greater than that of the first positive electrode film region. p1 This effectively reduces the risk of lithium plating in the tab area of the secondary battery and its lifespan failure, and improves the fast charging performance and cycle performance of the secondary battery. Attached Figure Description
[0018] Figure 1 Here are the plan view and partial cross-sectional view of the secondary battery prepared in Example 1: 1-Positive electrode plate, 2-Negative electrode plate, 4-Positive electrode tab, 7-Negative electrode tab; Figure 2 A cross-sectional view of the positive electrode sheet prepared in Example 1: 3-Positive current collector, 5-Positive electrode film, 51-First positive electrode film region, 52-Second positive electrode film region, W p1 The maximum dimension of the first positive electrode film region along the first direction, W p The maximum dimension of the positive electrode film layer along the first direction; Figure 3 A cross-sectional view of the negative electrode sheet prepared in Example 1: 6 - Negative electrode current collector, 8 - Negative electrode film layer, 81 - First negative electrode film layer region, 82 - Second negative electrode film layer region, W n1 The maximum dimension of the first negative electrode film layer region along the first direction; Figure 4This is a schematic diagram of the unfolded state of the positive electrode sheet prepared in Example 1; Figure 5 This is a schematic diagram of the unfolded state of the negative electrode sheet prepared in Example 1. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0020] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0021] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0022] In one embodiment of this application, a secondary battery is provided, comprising a positive electrode 1 and a negative electrode 2. The positive electrode 1 includes a positive current collector 3, a positive electrode tab 4, and a positive electrode film 5 disposed on at least one surface of the positive current collector 3. The negative electrode 2 includes a negative current collector 6, a negative electrode tab 7, and a negative electrode film 8 disposed on at least one surface of the negative current collector 6. The positive electrode film 5 includes a positive active material and a positive conductive agent, and the negative electrode film 8 includes a negative active material and a negative conductive agent. The secondary battery has a first orientation; The positive electrode film layer 5 includes a first positive electrode film layer region 51 close to the positive electrode tab 4 and a second positive electrode film layer region 52 away from the positive electrode tab 4 along the first direction; The negative electrode film layer 8 includes a first negative electrode film layer region 81 close to the negative electrode tab 7 and a second negative electrode film layer region 82 away from the negative electrode tab 7 along the first direction. The secondary battery satisfies (A) to (C): (A) The equivalent mass percentage C of the positive electrode conductive agent in the first positive electrode film region 51 p1The equivalent mass percentage C of the positive electrode conductive agent in the second positive electrode film region 52 is greater than that of the positive electrode conductive agent. p2 ; (B) The average particle size D of the negative electrode active material in the first negative electrode film region 81 n1 The average particle size D of the negative electrode active material in the second negative electrode film region 82 is smaller than that of the negative electrode active material. n2 ; (C) The maximum dimension W of the first negative electrode film region 81 along the first direction n1 The maximum dimension W along the first direction of the first positive electrode film region 51 is greater than that of the first positive electrode film region 51. p1 .
[0023] This application research found that the secondary battery provided in this application has a first positive electrode film layer region 51 near the positive electrode tab 4 and a second positive electrode film layer region 52 away from the positive electrode tab 4 in the positive electrode film layer 5, and a first negative electrode film layer region 81 near the negative electrode tab 7 and a second negative electrode film layer region 82 away from the negative electrode tab 7 in the negative electrode film layer 8; and further defines (A) the equivalent mass ratio C of the positive electrode conductive agent in the first positive electrode film layer region 51. p1 The equivalent mass percentage C of the positive electrode conductive agent in region 52 of the second positive electrode film layer is greater than that of the second positive electrode film layer. p2 (B) The average particle size D of the negative electrode active material in the first negative electrode film region 81 n1 The average particle size D of the negative electrode active material in region 82 of the second negative electrode film layer is smaller than that of the second negative electrode film layer. n2 (C) The maximum dimension W of the first negative electrode film region 82 along the first direction. n1 The maximum dimension W along the first direction of the first positive electrode film region 51 is greater than that of the first positive electrode film region 51. p1 It can effectively reduce lithium plating and lifespan failure in the electrode area of secondary batteries, and improve the fast charging performance and cycle performance of secondary batteries.
[0024] Specifically, in the first aspect, the equivalent mass percentage C of the positive electrode conductive agent in the first positive electrode film layer region 51 is defined. p1 The equivalent mass percentage C of the positive electrode conductive agent in region 52 of the second positive electrode film layer is greater than that of the second positive electrode film layer. p2 This allows for the formation of a highly conductive enhanced interface (equivalent to a lithium-ion "emitter") near the tab on the positive electrode side, resulting in a denser conductive network and reducing electron transport impedance and local polarization in that region. During fast charging, when lithium ions are extracted from the positive electrode, the highly conductive region provides a more uniform current distribution, reducing the concentration of lithium-ion flux caused by excessively high current density near the tab and thus reducing lithium deposition. Simultaneously, the relatively high conductivity of the first positive electrode film layer region 51 on the tab 4 side reduces heat generation in this region, minimizing local hot spots and reducing the risk of cycle failure.
[0025] Secondly, the average particle size D of the negative electrode active material in the first negative electrode film layer region 81 is defined. n1 The average particle size D of the negative electrode active material in region 82 of the second negative electrode film layer is smaller than that of the second negative electrode film layer. n2 This involves creating a particle size gradient distribution of the negative electrode active material along the width direction on the negative electrode side (i.e., kinetic gradient design). This allows for a shorter lithium-ion diffusion path near the tab region of the negative electrode, significantly improving the lithium-ion insertion kinetic rate in this region. Under fast charging conditions, lithium ions can rapidly insert into the small-particle-size active material after reaching the negative electrode surface, preventing lithium ion accumulation on the negative electrode surface and thus effectively suppressing lithium plating. Furthermore, the particle size gradient design of the negative electrode active material in the first negative electrode film region 81 and the second negative electrode film region 82 achieves kinetic gradient matching, synergizing with the actual transport path of lithium ions from the positive electrode to the negative electrode, further suppressing lithium plating. Moreover, the particle size gradient design of the negative electrode active material in the first negative electrode film region 81 and the second negative electrode film region 82 can also reduce side reactions while ensuring fast charging performance, and can also avoid uneven negative electrode volume expansion and stress concentration caused by localized lithium insertion oversaturation, thereby improving cycle performance.
[0026] Thirdly, the maximum dimension W along the first direction of the first negative electrode film layer region 81 is defined. n1 The maximum dimension W along the first direction of the first positive electrode film region 51 is greater than that of the first positive electrode film region 51. p1 This geometrical coating structure, in which the maximum dimension of the first negative electrode film region 81 along the first direction is greater than the maximum dimension of the first positive electrode film region 51 along the first direction, ensures that the edge region of the first positive electrode film region 51 is always completely covered by the first negative electrode film region 81. This helps all lithium ions extracted from the edge of the first positive electrode film region 51 fall into the first negative electrode film region 81, avoiding local lithium plating. In addition, this geometrical coating structure can also prevent lithium plating caused by alignment deviation or offset during the winding / stacking process between the edge of the first positive electrode film region 51 and the edge of the first negative electrode film region 81, resulting in kinetic mismatch or capacity design mismatch, thereby reducing the risk of cycle failure.
[0027] Fourthly, the secondary battery of this application simultaneously satisfies (A) to (C), with the three working together to provide a uniform lithium-ion "emission" interface on the positive electrode side to avoid flux concentration; to construct a kinetic gradient "receiving" layer on the negative electrode side to ensure that lithium ions can be quickly embedded after arrival; and to provide "coating" protection in terms of geometry to eliminate the edge lithium plating blind zone; that is, the combination of the three can effectively suppress the lithium-ion flux concentration and lithium plating risk in the edge region, and reduce the risk of cycle failure of the secondary battery; that is, it significantly improves the fast charging performance and cycle performance of the secondary battery.
[0028] It should be noted that the first positive electrode film region 51 and the second positive electrode film region 52 in the positive electrode film layer 5 are defined as follows: the secondary battery is disassembled to obtain the positive electrode plate 1. The cross-section of the positive electrode plate 1 is analyzed by elemental line scanning using an energy dispersive X-ray spectrometer (EDS) equipped with a field emission scanning electron microscope (SEM). The boundary between the first positive electrode film region 51 and the second positive electrode film region 52 is defined by the boundary line where the carbon element (positive electrode conductive agent) content changes abruptly or the boundary line where the type of positive electrode conductive agent changes abruptly.
[0029] It should be noted that the first negative electrode film region 81 and the second negative electrode film region 82 in the negative electrode film layer 8 are defined as follows: the secondary battery is disassembled to obtain the negative electrode sheet 2. The cross-section of the negative electrode sheet 2 is analyzed by backscattered electron imaging. The boundary line where the statistical distribution of the particle size of the negative electrode active material particles undergoes a step change is defined as the boundary line between the first negative electrode film region 81 and the second negative electrode film region 82.
[0030] It should be noted that the maximum dimension along the first direction refers to the vertical distance from the starting edge of the electrode film layer (near the tab side) to the corresponding dividing line mentioned above.
[0031] In some embodiments, 1.10 ≤ C p1 / C p2 ≤5.5.
[0032] For example, C p1 / C p2 It can be any point value or any two-point range value between 1.10 and 5.5, such as 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.0, 3.0, 4.0, 5.0, 5.5, etc.
[0033] This application study found that the equivalent mass percentage C of the positive electrode conductive agent in the first positive electrode film region 51 is... p1 The equivalent mass percentage C of the positive electrode conductive agent in the second positive electrode film region 52 p2 The ratio of the two will affect the conductivity enhancement effect of the first positive electrode film region 51, thus affecting the uniformity of current distribution on the positive electrode side and the concentration of lithium-ion flux during fast charging; at the same time, the ratio of their equivalent mass ratios will also affect the difference in reaction rates between the first positive electrode film region 51 and the second positive electrode film region 52, thus affecting the magnitude of interfacial stress; in addition, the ratio of their equivalent mass ratios will also affect the uniformity of ohmic heat generation and the degree of side reactions; when the equivalent mass ratio C of the positive electrode conductive agent in the first positive electrode film region 51 is further selected... p1 The equivalent mass percentage C of the positive electrode conductive agent in the second positive electrode film region 52 p2When the ratio is 1.20 to 5.0, the resulting secondary battery has a lower risk of lithium plating and better cycle performance.
[0034] It should be noted that the test method for the equivalent mass ratio of the positive electrode conductive agent in the first positive electrode film region 51 and the second positive electrode film region 52 is as follows: The secondary battery is disassembled to obtain the positive electrode sheet 1. The cross-section of the positive electrode sheet 1 is analyzed by elemental line scanning using an energy dispersive X-ray spectrometer (EDS) equipped with a field emission scanning electron microscope (SEM). The boundary line between the first positive electrode film region 51 and the second positive electrode film region 52 is defined by the boundary line where the carbon element (positive electrode conductive agent) content changes abruptly or the boundary line where the type of positive electrode conductive agent changes abruptly. Then, powder samples from the first positive electrode film region 51 and the second positive electrode film region 52 are scraped off respectively. Thermogravimetric analysis (TGA) is used to heat the sample to 750°C in an air atmosphere. The contents of the positive electrode active material, positive electrode binder and positive electrode conductive agent are distinguished according to the weight loss curve. Then, the mass ratio of the positive electrode conductive agent in the corresponding film region is calculated.
[0035] It should be noted that, due to the existence of conductive agents with different morphologies and properties in this field, such as zero-dimensional (e.g., conventional carbon black, SuperP), one-dimensional (e.g., carbon nanotubes, CNTs), and two-dimensional (e.g., graphene), their intrinsic conductivity and percolation threshold vary greatly. If only physical absolute weight is used for comparison (e.g., 0.5% CNTs are added to the first region, and 2% ordinary carbon black is added to the second region), since 0.5% < 2%, the surface size ratio will show a distorted and falsified reverse relationship. Therefore, the mass ratio C of the positive electrode conductive agent referred to in the claims of this application is... p1 With C p2 All are defined as equivalent mass percentages, and their conversion rule is as follows: all types of conductive agents applied are benchmarked according to their conductivity and aspect ratio performance, and converted into virtual mass percentages after conversion to conventional zero-dimensional conductive carbon black. For areas using highly efficient conductive agents such as carbon nanotubes or graphene, their actual mass percentage is calculated by substituting into C. p1 Or C p2When multiplying by the corresponding “conductivity efficiency equivalent coefficient K” (for example, the coefficient K=1 for conventional carbon black SuperP, and the K value range for mainstream multi-walled nanotubes is usually 3~8). It should be noted that the conductivity equivalence coefficient K is defined using the volume conductivity of the compacted film. Taking a 2% SuperP-based pressed film as the baseline, the film resistance (mainly composed of 95% NCM523 and 3% PVDF) is used to prepare CNTs with different contents (keeping the PVDF content at 2% and controlling the CNT content by adjusting the NCM523 content). The amount of CNTs added that equals the SuperP film resistance (considering testing error, the SuperP film resistance is defined as R1, and the CNT film resistance as R2; when R1(1-0.05)≤R2≤R1(1+0.05), the CNT film resistance is considered equal to the SuperP film resistance) is denoted as 'a'. The conductivity equivalence coefficient K is calculated using the ratio 2% / a. This rule ensures that regardless of the component mix used, the intrinsic physical matching relationship of the electrode is accurately reflected.
[0036] In one embodiment, the ratio of the compacted film volume conductivity of the first positive electrode film region 51 to the second positive electrode film region 52 is 1.2 to 5.0.
[0037] For example, the ratio of the compacted film volume conductivity of the first positive electrode film region 51 to the second positive electrode film region 52 can be any point value or any two points between 1.2 and 5.0, such as 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.0, 3.0, 4.0, 5.0, etc.
[0038] It should be noted that the test method for the ratio of the compacted film volume conductivity of the first positive electrode film region 51 to the second positive electrode film region 52 is as follows: The secondary battery is disassembled to obtain the positive electrode 1. Elemental line scanning analysis is performed on the cross-section of the positive electrode 1 using an energy-dispersive X-ray spectroscopy (EDS) instrument equipped with a field emission scanning electron microscope (SEM). The boundary between the first positive electrode film region 51 and the second positive electrode film region 52 is defined by the boundary line where the carbon element (positive electrode conductive agent) content or the type of positive electrode conductive agent undergoes a step change. Multiple points (≥5 points) are measured in both the first and second positive electrode film regions 51 using the four-probe method or a dedicated electrode film resistivity meter. The volume conductivity is calculated by combining the sheet resistance obtained from the test with the corresponding film thickness. Those skilled in the art will understand that by directly measuring the actual volume conductivity of the compacted membrane layer, regardless of the specific composition or type of conductive agent used internally, the most realistic verification of the significant enhancement of the conductive network in the first membrane layer region compared to the second membrane layer region can be achieved. Furthermore, this test method is mature, the evidence is clear, and it is unique.
[0039] In some embodiments, 1.05 ≤ D n2 / D n1 ≤1.55.
[0040] For example, D n2 / D n1 It can be any point value or any two-point range value between 1.05 and 1.55, such as 1.05, 1.10, 1.15, 1.20, 1.25, 1.30, 1.35, 1.40, 1.45, 1.50, 1.55, etc.
[0041] This application research found that the average particle size D of the negative electrode active material in the second negative electrode film layer region 82 is... n2 The average particle size D of the negative electrode active material in the first negative electrode film region 81 n1 The ratio of the average particle size to the average particle size of the first negative electrode film region 81 affects the degree of kinetic difference between the second negative electrode film region 82 and the first negative electrode film region 81, thus affecting the matching degree between the lithium insertion rate and lithium-ion flux in the first negative electrode film region 81 during fast charging; it also affects the ease with which lithium ions diffuse from the first negative electrode film region 81 to the second negative electrode film region 82 after lithium insertion; in addition, the ratio of the average particle size to the average particle size of the first negative electrode film region 82 also affects the degree of side reaction and the magnitude of internal resistance, thus affecting heat generation; when the average particle size D of the negative electrode active material in the second negative electrode film region 82 is further selected... n2 The average particle size D of the negative electrode active material in the first negative electrode film region 81 n1 When the ratio is 1.05 to 1.45, the resulting secondary battery has a lower risk of lithium plating and better cycle performance.
[0042] It should be noted that the average particle size D of the negative electrode active material in the second negative electrode film region 82 is... n2 The average particle size D of the negative electrode active material in the first negative electrode film region 81 n1 The testing method is as follows: the secondary battery is disassembled to obtain the negative electrode plate 2. The cross-section of the negative electrode plate 2 is analyzed by backscattered electron imaging. The boundary line where the statistical distribution of the particle size of the negative electrode active material particles changes abruptly is defined as the boundary line between the first negative electrode film layer region 81 and the second negative electrode film layer region 82. Subsequently, the cross-section of the corresponding film layer is photographed by scanning electron microscope (SEM). At least 50 negative electrode active material particles are randomly selected in the corresponding region, their diameters are measured and the average value is taken.
[0043] In some embodiments, 1.0 mm ≤ W n1 -W p1 ≤12.0mm.
[0044] For example, W n1 -W p1 It can be any point value or any two-point range value between 1.0mm and 12.0mm, such as 1.0mm, 3.0mm, 4.0mm, 5.0mm, 6.0mm, 7.0mm, 8.0mm, 9.0mm, 10.0mm, 12.0mm, etc.
[0045] This application research found that the width W of the first negative electrode film layer region 81 n1 The width W of the first positive electrode film region 51 p1 The difference affects the degree to which lithium ions extracted from the first positive electrode film region 51 are accepted by the negative electrode, thus affecting the lithium ion concentration in the edge region; when the width W of the first negative electrode film region 81 is further selected... n1 The width W of the first positive electrode film region 81 p1 When the difference is 2.0mm to 10.0mm, the resulting secondary battery has a lower risk of lithium plating and better cycle performance.
[0046] It should be noted that the width W of the first negative electrode film region 81 n1 The width W of the first positive electrode film region 51 p1 The testing method is as follows: The secondary battery is disassembled to obtain the positive electrode 1 and the negative electrode 2, respectively. Then, the average particle size D of the negative electrode active material in the first negative electrode film region 81 is used. n1 The average particle size D of the negative electrode active material in the second negative electrode film region 82 n2The test method distinguishes between the first negative electrode film region 81 and the second negative electrode film region 82; and uses a test method based on the equivalent mass ratio of the positive electrode conductive agent in the first positive electrode film region 51 and the second positive electrode film region 52 to distinguish between the first positive electrode film region 51 and the second positive electrode film region 52. Then, an optical measuring instrument is used to measure the vertical distance from the edge of the electrode film starting region (near the tab side) to the boundary line to obtain the width W of the first negative electrode film region 81. n1 (Specifically as follows) Figure 5 (As shown) and the width W of the first positive electrode film region 51 p1 (Specifically as follows) Figure 2 (As shown).
[0047] In some embodiments, W pt The maximum dimension of the positive electrode tab 4 perpendicular to the first direction. W p This refers to the maximum dimension of the positive electrode film layer 5 along the first direction; The secondary battery satisfies: 0.021 ≤ (W pt / W p )×(W p1 / W p )≤0.595.
[0048] For example, (W pt / W p )×(W p1 / W p It can be any point value or any two-point range value between 0.021 and 0.595, such as 0.021, 0.038, 0.050, 0.100, 0.150, 0.200, 0.250, 0.300, 0.400, 0.500, 0.568, 0.595, etc.
[0049] This application research found that the tab is a channel for current inflow / outflow. The difference between the width of the first positive electrode film region 51 and the width of the positive electrode tab 4 affects the symmetry of the current path in the film regions on both sides of the tab, thereby affecting the concentration of current at the junction of the tab and the film, and thus affecting the degree of lithium plating and heat concentration. When a secondary battery is selected that satisfies 0.021≤(W pt / W p )×(W p1 / W p When the current density is ≤0.595, the symmetry of the current path can be improved, the concentration of current between the tab and the film can be reduced, thereby reducing the risk of lithium plating and improving cycle performance.
[0050] It should be noted that the test method for the maximum dimension of the positive electrode tab 4 perpendicular to the first direction and the maximum dimension of the positive electrode film layer 5 along the first direction is as follows: the secondary battery is disassembled to expose the positive electrode tab 4, and then the vertical distance from the root of the free end extending from the current collector to the opposite edge is measured using an optical image measuring instrument to obtain the maximum dimension W of the positive electrode tab 4 perpendicular to the first direction. pt Next, an optical measuring instrument was used to measure the vertical distance from the edge of the starting region of the electrode film (near the tab side) to the end of the electrode, thus obtaining the maximum dimension W of the positive electrode film region along the first direction. p (Specifically as follows) Figure 2 (As shown).
[0051] In some embodiments, the specific surface area S of the negative electrode active material in the first negative electrode film region 81 is... n1 The specific surface area S of the negative electrode active material in the second negative electrode film region 82 is greater than that of the negative electrode active material. n2 .
[0052] In some embodiments, 1.05 ≤ S is satisfied. n1 / S n2 ≤1.60.
[0053] For example, S n1 / S n2 It can be any point value or any two-point range value between 1.05 and 1.60, such as 1.05, 1.15, 1.20, 1.25, 1.30, 1.35, 1.40, 1.45, 1.50, 1.55, 1.60, etc.
[0054] This study found that the ratio of the specific surface area of the negative electrode active material in the first negative electrode film region 81 to the specific surface area of the negative electrode active material in the second negative electrode film region 82 affects the charge transfer rate of lithium ions at the negative electrode interface in the first negative electrode film region 81, thereby affecting the lithium concentration in the first negative electrode film region 81; it also affects the degree of side reactions; when the specific surface area of the negative electrode active material in the first negative electrode film region 81 is further selected to be greater than that in the second negative electrode film region 82, and the ratio of the two is between 1.15 and 1.50, the resulting secondary battery has a lower risk of lithium plating and better cycle performance.
[0055] It should be noted that the test method for the specific surface area of the negative electrode active material in the first negative electrode film region 81 and the specific surface area of the negative electrode active material in the second negative electrode film region 82 is as follows: The secondary battery is disassembled, and the average particle size D of the negative electrode active material in the first negative electrode film region 81 is used. n1 The average particle size D of the negative electrode active material in the second negative electrode film region 82 n2The test method involves distinguishing between the first negative electrode film region 81 and the second negative electrode film region 82. Then, powder from the corresponding region is scraped, washed, dried, and sintered at 800°C. The powder is then sent to the BET nitrogen adsorption method to test its specific surface area, thereby obtaining the specific surface area of the negative electrode active material in the first negative electrode film region 81 and the specific surface area of the negative electrode active material in the second negative electrode film region 82.
[0056] In some embodiments, the secondary battery satisfies the following formula: k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c ≥0.01; in, f(C p ) is the compensation factor for the positive electrode electron conduction network, f(C) p )=C p1 / C p2 ; f(D n ) is the solid-state diffusion compensation factor for the negative electrode phase, f(D) n )=D n2 / D n1 ; f(W p ) represents the macroscopic current collection bottleneck leakage factor of the battery cell, f(W) p )=(W pt / W p )×(W p1 / W p ); f(S n ) is the charge transfer activation factor at the negative electrode interface, f(S) n )=S n1 / S n2 ; k is an empirical parameter for system design, 0.2≤k≤0.8; N c The value of the charging rate parameter for the secondary battery.
[0057] In some embodiments, the secondary battery satisfies the following formula: k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c ≥0.1.
[0058] This study found that during the process of achieving extreme fast charging (such as 3C~6C or even higher), the electric field distribution, ion concentration gradient, and thermal diffusion within the secondary battery electrode are highly nonlinear and non-uniform. Simply adjusting a single parameter in a single region (such as adjusting only the particle size or only the conductive agent) can easily trigger the deterioration of other physical quantities (such as electrode compaction density, total cell energy density, or electrode mechanical strength) due to the "weakest link" effect.
[0059] To address this, this application proposes a multi-dimensional adaptive compensation mechanism, which is summarized in the above formula. This formula demonstrates that a secondary battery can cope with extreme fast charging rates N. c When impacted, compensation and risk mitigation can be achieved through the synergistic effect of the product of four dimensions: positive electrode electronic conduction network, negative electrode solid-state diffusion, macroscopic electrode tab current collection, and negative electrode interface charge transfer.
[0060] Specifically, the physical and electrochemical meanings of each factor in the formula are explained below: I. Positive Electron Conductivity Network Compensation Factor f(C) p )=C p1 / C p2 : In the initial stage of fast charging, the huge current first impacts the first region near the current collector or the edge of the electrode (at this time, the local overcurrent is extremely large). C p1 Characterizing the electronic conductivity (or conductive agent content) of the first positive electrode film region 51, C p2 This represents the conductivity of the second positive electrode film region 52.
[0061] Design logic: By enabling C p1 Relative to C p2 Increase (i.e., f(C)) p (>1), which can establish an "electron flooding zone" on the positive electrode side, significantly reducing the ohmic polarization of the high-risk area and ensuring that the area will not induce side reactions due to overheating at high magnification.
[0062] II. Solid-state diffusion compensation factor f(D) in the negative electrode phase n )=D n2 / D n1 : D n1 and D n2 The solid-state diffusion resistance of lithium ions in the first negative electrode film region 81 (high current density region) and the second negative electrode film region 82 (main region) is characterized respectively (such as the Dv50 particle size or diffusion path length of the negative electrode active particles).
[0063] Design Logic: Solid-state diffusion of lithium ions within the negative electrode active material (such as graphite) / negative electrode is often the decisive step in fast charging. This formula uses D... n2 / D n1The form is intended to limit the diffusion resistance (i.e., D) in the high-risk region (the first negative electrode film layer region) to be reduced when it is challenged by concentration polarization. n1 Make the factor f(D) smaller. n (Magnification). For example, in the first negative electrode film region 81, a negative electrode material with a smaller particle size or highly developed pores with a shorter diffusion path is used to achieve local lithium ion "throughput acceleration".
[0064] III. Macroscopic current collection bottleneck leakage factor f(W) of secondary batteries p )=(W pt / W p )×(W p1 / W p ): This is a purely macroscopic geometric design factor. Where W... p W is the maximum dimension of the positive electrode film layer 5 along the first direction. pt W is the maximum dimension of the positive electrode tab 4 along the first direction. p1 It is the maximum dimension of the first positive electrode film region 51 along the first direction.
[0065] Design logic: It acts as a "bottleneck valve" between the heat source and current of the secondary battery. pt / W p The smoothness of current collection in the all-polare collector is determined by W. p1 / W p This determines the defensive depth of the non-uniform coating / processing functional area. Increasing the tab ratio and reasonably widening the specially designed edge area can accumulate heat at the geometric level, smoothing out the originally sharp local current peaks.
[0066] IV. Negative electrode interface charge transfer activation factor f(S) n )=S n1 / S n2 : S n1 and S n2 These represent the number of active sites (or charge transfer area) in the first negative electrode film region 81 and the second negative electrode film region 82 due to the specific surface area (BET) of the negative electrode active material or the pore formation of the structure.
[0067] Design logic: If solid-state diffusion (D) n If the limit has been reached, optimization must be performed on the interface phase (SEI / solid interface). This can be achieved by increasing S... n1 (make f(S) n (>1), which greatly increases the surface area for desolvation and charge transfer reactions, thereby effectively reducing the local interfacial activation potential and directly preventing lithium ions from queuing up and accumulating here to crystallize into dead lithium.
[0068] The most important contribution of this formula lies in revealing the compensatory relationship of the product among the four dimensions mentioned above. Due to the limitations of industrial mass production processes, designs in this field often cannot maximize any single parameter. For example, limited by the adhesion of the negative electrode sheet (powder shedding problem), it may not be possible to infinitely reduce the particle size (D) in the edge region. n1 (There exists a lower bound), at which point f(D) n The contribution of ) is hindered. However, according to the comprehensive discrimination formula of this application, it is entirely possible to increase the tab width W on the drawing. pt (i.e., raise f(W)) p Alternatively, more carbon nanotube conductive agents can be locally added to the edge of the positive electrode (to increase f(C)). p By utilizing this "cross-dimensional product compensation mechanism," the overall value is still maintained at ≥0.1×N. c The threshold of / k ensures that the secondary battery is in N c Safety at different magnification levels.
[0069] The empirical parameter k (0.2≤k≤0.8) in the formula is a system buffer coefficient set based on the thermodynamic differences between different chemical systems (such as lithium iron phosphate cathode material system and nickel cobalt manganese ternary cathode material system).
[0070] The secondary battery design using formulas eliminates the need for globally advanced materials and extreme monolithic thin-film designs. The system precisely targets all its defense resources at high-risk cross-sections across four dimensions: macroscopic geometric constraints, localized electron evacuation, bulk microscopic shortening, and interface area expansion. By dynamically adjusting the values of these four factors, k×[f(C] is achieved. p )×f(D n )×f(W p )×f(S n )] / N c The value of ≥0.01, especially making k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c The value of ≥0.1 satisfies the requirement of non-lithium deposition in the design system. For secondary battery designs, appropriately increasing the value can effectively extend cycle life. Therefore, this application mitigates the impact of high charging rates (N). c The localized lithium plating degradation caused by the short planks of the barrel further ensures that the secondary battery as a whole (main area) has extremely high compaction density, capacity and ultra-long service life.
[0071] It should be noted that in this application N c The extraction of numerical values follows a strict order of precedence (applicable in that order): First priority: Collect the dimensionless values of the "maximum continuous charging rate" or "maximum peak fast charging rate" specified or advertised in the publicly available specifications, factory labels, product launch materials, or third-party testing and certification reports corresponding to the target secondary battery, and directly use them as N. c (For example, if it claims to support 4C fast charging, then extract N) c =4; if it claims 5.5C fast charging, then it corresponds to N. c =5.5).
[0072] Second priority: When and only when the target secondary battery lacks clearly defined marketing parameters, or is configured in an electrical device (such as an electric vehicle, energy storage cabinet, consumer electronics, etc.) and there are calibration disputes, a reverse calculation method based on terminal operation is adopted: Under normal temperature conditions, using the highest power charging mode (fast charging mode or regular maximum permissible mode) supported by the electrical device, record the time t (in minutes) consumed by the environmental battery system to charge from 20% state of charge (SOC) to 70% SOC. The actual effective charging rate value at this time is determined as N. c = (0.7-0.2)×60÷t. This ranking method intuitively reflects the fast-charging chemical capabilities actually released and relied upon by the battery and its management system.
[0073] Third priority: When the test object is a bare cell that has not yet been assembled or cannot be subjected to the second priority test, an exhaustive physical limit test is adopted: Under an isothermal environment of 25°C, the brand-new test cell is charged to the rated voltage in steps at different constant current rates, and then dissected and observed after charging. The dimensionless value of the maximum safe charging rate at which no irreversible and visible lithium plating phenomenon appears on the negative electrode surface is used as the intrinsic performance proxy value N. c Perform verification calculations.
[0074] In some embodiments, the negative electrode film layer further includes a lithium plating inhibitor, wherein the lithium intercalation potential of the lithium plating inhibitor is higher than that of the negative electrode active material.
[0075] This study found that introducing lithium plating inhibitors into the negative electrode film can effectively improve the thermodynamic stability of the negative electrode film under extreme rate charging.
[0076] It should be noted that the test method for the lithium plating inhibitor and the lithium intercalation potential of the negative electrode active material is as follows: according to the definition method of the first negative electrode film region 81 and the second negative electrode film region 82 in the aforementioned negative electrode film layer, negative electrode region plates of different regions of the negative electrode are taken, with the negative electrode plate 2 as the working electrode and metallic lithium as the counter electrode. The potential corresponding to the reduction peak is the lithium intercalation potential of the corresponding test region by cyclic voltammetry.
[0077] For example, Y can be 0.01 to 0.6, such as 0.01, 0.02, 0.05, 0.08, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, 0.5, 0.52, 0.55, 0.58, 0.6, etc.
[0078] In some embodiments, the negative electrode film layer satisfies: M1>M2.
[0079] Wherein, M1 is the mass percentage of the lithium plating inhibitor in the first negative electrode film region 81, and M2 is the mass percentage of the lithium plating inhibitor in the second negative electrode film region 82.
[0080] In some embodiments, the lithium plating inhibitor includes silicon-carbon composite materials and silicon suboxide (SiO2). x It includes at least one of the following: pure silicon material, hard carbon, soft carbon, and lithium titanate.
[0081] Based on the above formula, this application further introduces a lithium plating inhibitor with a higher lithium intercalation potential platform compared to the negative electrode active material into the negative electrode film layer 8. This high potential characteristic artificially raises the lower limit of the negative electrode potential (thermodynamic defense) in the high current density region of the electrode tab. Even under extreme low temperature or excessively high current impact, the potential in the electrode tab region can be guaranteed to be no lower than 0V (vsLi / Li). + This reduces the deposition of metallic lithium.
[0082] It should be noted that the values of M1 and M2 mentioned in this application, for lithium plating inhibitors with characteristic elements (such as silicon-based materials and lithium titanate, etc.), can be determined by measuring the concentration of characteristic elements (e.g., silicon) in the lithium plating inhibitor in the electrode powder digestion solution using inductively coupled plasma optical emission spectrometry (ICP-OES) and calculating the mass percentage after returning to the characteristic material phase; for carbon-based lithium plating inhibitors (such as hard carbon, soft carbon, etc.), the type can be identified by Raman spectroscopy ID / IG method, and then combined with thermogravimetric-differential scanning calorimetry (TG-DSC) using an air atmosphere, setting the TG weight loss range according to the type of lithium plating inhibitor, and the corresponding weight loss measured is the amount of lithium plating inhibitor added.
[0083] In some embodiments, the positive electrode film 5 further includes a lithium supplementation additive.
[0084] In some embodiments, the positive electrode film 5 satisfies: C1 > C2. Wherein, C1 is the mass percentage of the lithium-replenishing additive in the first positive electrode film region 51. C2 is the mass percentage of the lithium-replenishing additive in the second positive electrode film region 52.
[0085] In some embodiments, the lithium supplementing additive is selected from at least one of lithium-rich metal oxides, lithium-rich nitrides, lithium-rich sulfides, or lithium-containing organic compounds.
[0086] In some embodiments, the lithium supplementing additive is selected from at least one of Li5FeO4, Li2NiO4, Li2O, Li2O2, and Li3N.
[0087] This study found that the decomposition products of the lithium-supplementing additives selected above can fill or improve the interfacial film performance of the positive electrode film in situ after formation, thereby better improving the overall performance of the secondary battery.
[0088] This application research found that edge lithium replenishment of the positive electrode can spatially and directionally replenish lithium to high-potential materials with low initial efficiency at the edge, making up for irreversible lithium loss in the high-risk area of the negative electrode and extending the cycle life of the edge region. The application of edge lithium replenishment technology also solves the problem of gas generation of the lithium replenishment agent. Through the hydrodynamic advantage of the natural proximity of this region to the exhaust channel, the gas is more easily discharged. At the same time, the lithium replenishment agent can also improve the interfacial film performance of the first negative electrode film layer region 81, resulting in a secondary battery with lower lithium plating risk and better cycle performance.
[0089] It should be noted that the concentrations C1 and C2 of the positive electrode lithium replenishment additive described in this invention can be defined by the mass ratio of the characteristic elements in the additive. The testing method is as follows: After charging and discharging, equal masses of positive electrode powder samples are taken from the first positive electrode film region 51 and the second positive electrode film region 52 of the secondary battery, respectively; these samples are digested, and the absolute content M of the characteristic elements in the samples is determined using inductively coupled plasma optical emission spectrometry (ICP-OES). trace And the total content M of the main ground-state elements in the positive electrode (such as Ni+Co+Mn in ternary materials). base ; via M trace and M base Calculate the types and amounts of additives.
[0090] This application does not have any special requirements for the selection of positive electrode active materials; conventionally available positive electrode active materials in the art can be used. For example, the positive electrode active materials include, but are not limited to, ternary positive electrode materials, lithium iron phosphate positive electrode materials, and lithium-rich manganese-based materials.
[0091] This application does not have any special requirements for the selection of the positive electrode conductive agent; any positive electrode conductive agent conventionally available in the art can be used. For example, the positive electrode conductive agent includes, but is not limited to, carbon black (SP), conductive graphite, carbon nanotubes (CNTs), graphene, carbon fiber, etc.
[0092] In some embodiments, the positive electrode film layer further includes a positive electrode binder.
[0093] This application does not have any special requirements for the selection of the positive electrode binder; any positive electrode binder conventionally available in the art can be used. Exemplarily, the positive electrode binder includes, but is not limited to, polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), and polyacrylonitrile (PAN).
[0094] This application does not have any special requirements for the selection of negative electrode active materials; commonly used negative electrode active materials in the art can be used. Exemplarily, the negative electrode active materials include, but are not limited to, graphite, hard carbon, silicon, silicon-carbon composites, silicon oxides, etc.
[0095] This application does not have any special requirements for the selection of the negative electrode conductive agent; any negative electrode conductive agent conventionally available in the art can be used. For example, the negative electrode conductive agent includes, but is not limited to, carbon black, conductive graphite, carbon nanotubes, graphene, carbon fibers, etc.
[0096] In some embodiments, the negative electrode film layer further includes a negative electrode binder.
[0097] This application does not have any special requirements for the selection of the negative electrode binder, and negative electrode binders conventionally available in the art can be used. Exemplary examples include, but are not limited to, styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN), sodium alginate, polyvinylidene fluoride (PVDF), polyimide (PI), polyvinyl alcohol (PVA), etc.
[0098] In some embodiments, the secondary battery further includes an electrolyte; the electrolyte includes an organic solvent and a lithium salt.
[0099] This application does not have any particular requirements for the selection of organic solvents; organic solvents conventionally used in the art can be used. For example, the organic solvent may be at least one of ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, and dimethyl carbonate.
[0100] This application does not have any particular requirements for the selection of lithium salt, and lithium salts conventionally available in the art can be used. For example, the lithium salt may be at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide.
[0101] In some embodiments, the secondary battery further includes a separator.
[0102] This application does not limit the choice of diaphragm; any diaphragm conventionally available in the art can be used. For example, the diaphragm may be a polyethylene film.
[0103] In one embodiment of this application, an electrical device is provided, which includes the secondary battery described in this application.
[0104] For example, the aforementioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0105] Example 1 This application provides a secondary battery, the preparation method of which includes the following steps: (1) Preparation of positive electrode sheet S1. Preparation of the slurry in the first positive electrode film layer region: The positive electrode active material (LiNi) is prepared... 0.6 Co 0.1 Mn 0.3 O2), positive electrode conductive agent (a mixture of SP and CNT in a mass ratio of 5:8.05, with the conductivity equivalent coefficient K=4 of the positive electrode conductive agent CNT), and positive electrode binder (PVDF) are mixed evenly in a mass ratio of 96.695:1.305:2 and uniformly dispersed in N-methylpyrrolidone (NMP) to form a slurry, thus obtaining the slurry for the first positive electrode film layer region; S2, Preparation of the slurry in the second positive electrode film region: The positive electrode active material (LiNi) is prepared... 0.6 Co 0.1 Mn 0.3 O2), positive electrode conductive agent (a mixture of SP and CNT in a mass ratio of 5:1.75, with the conductivity equivalent coefficient K=4 of the positive electrode conductive agent CNT), and positive electrode binder (PVDF) are mixed evenly in a mass ratio of 97.325:0.675:2 and uniformly dispersed in N-methylpyrrolidone (NMP) to form a slurry, thus obtaining the slurry for the second positive electrode film layer region; S3. Preparation of positive electrode sheet: The slurry of the first positive electrode film layer region and the slurry of the second positive electrode film layer region are coated on both sides of the aluminum foil to form a first positive electrode film layer region with a width (maximum dimension along the first direction) of 30 mm and a second positive electrode film layer region with a width (maximum dimension along the first direction) of 54 mm, respectively. After baking, rolling and cutting, the positive electrode sheet is obtained. The cross-sectional view of the positive electrode is as follows: Figure 2 As shown in the diagram, the unfolded state is as follows: Figure 4 As shown: 3 is the positive electrode current collector, 5 is the positive electrode film layer, 51 is the first positive electrode film layer region; 52 is the second positive electrode film layer region. The arrow indicates the first direction. p1The maximum dimension of the first positive electrode film region along the first direction, W p The maximum dimension of the positive electrode film layer along the first direction; wherein the C of the first positive electrode film layer region p1 3.72 (C) p1 =(((5 / (5+8.05))×1.305)+((8.05 / (5+8.05))×1.305×4)), C in the second positive electrode film region p2 It is 1.2.
[0106] (2) Preparation of negative electrode sheet S4. Preparation of the slurry for the first negative electrode film layer: The negative electrode active material (artificial graphite, with an average particle size of 10 μm and a specific surface area of 1.32 m²) is prepared. 2 Artificial graphite: conductive agent: CMC: SBR are mixed evenly in a mass ratio of 96:1:1.2:1.8 and uniformly dispersed in deionized water to form a slurry, thus obtaining the slurry for the first negative electrode film layer region. S5. Preparation of the slurry for the second negative electrode film layer: The negative electrode active material (artificial graphite, with an average particle size of 12.5 μm and a specific surface area of 0.99 m²) is prepared. 2 Artificial graphite: conductive agent: CMC: SBR are mixed evenly in a mass ratio of 96:1:1.2:1.8 and uniformly dispersed in deionized water to form a slurry, thus obtaining the slurry for the second negative electrode film layer region. S6. Preparation of negative electrode sheet: The slurry of the first negative electrode film layer region and the slurry of the second negative electrode film layer region are coated on both sides of the copper foil to form a first negative electrode film layer region with a width of 36mm and a second negative electrode film layer region with a width of 50.5mm, respectively. After baking, rolling and cutting, the negative electrode sheet is obtained. The cross-sectional view of the negative electrode 2 is as follows: Figure 3 As shown in the diagram, the unfolded state is as follows: Figure 5 As shown: 6 is the negative electrode current collector, 8 is the negative electrode film layer, 81 is the first negative electrode film layer region; 82 is the second negative electrode film layer region. The arrow indicates the first direction. n1 The maximum dimension of the first negative electrode film layer region along the first direction.
[0107] (2) Preparation of electrolyte The organic solvent is a mixture containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), wherein the volume ratio of EC, EMC, and DEC is 30:30:40. In an argon-atmosphere glove box with a water content of <10 ppm, thoroughly dried lithium hexafluorophosphate (LiPF6), lithium difluorosulfonyl imide (LiFSI) (mixed in a molar ratio of 1:1), and additives (fluoroethylene carbonate (FEC), tris(trimethylsilyl) phosphate (TMSP), and ethylene sulfate (DTD) mixed in a mass ratio of 1:1:1) are dissolved in the organic solvent and mixed thoroughly to obtain the electrolyte. In this embodiment, the concentration of lithium salt is 1.15 mol / L, and the concentration of additives is 3 wt%.
[0108] (5) Preparation of secondary batteries The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes. After winding, hot pressing, and shaping, the tabs are welded (the positive electrode tab width is 53mm; the negative electrode tab width is 53mm; during tab welding, the first positive electrode film layer is close to the positive electrode tab, and the first negative electrode film layer is close to the negative electrode tab) to obtain a bare battery. The bare battery is placed in an aluminum casing and baked in an oven at 85±10℃ for 24 hours. Electrolyte is injected into the dried battery, and the battery is allowed to stand, form, and undergo capacity testing to obtain the rated charge rate N. c For a secondary battery with a capacity of 5C, the empirical parameter k in the system design is 0.5; The resulting plan view and partial sectional view of the secondary battery are as follows: Figure 1 As shown.
[0109] Examples 2-4 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the dosage of the conductive agent to alter the equivalent mass ratio of the positive electrode conductive agent in the first positive electrode film region, thereby achieving C p1 / C p2 The change; where the amount of conductive agent added is balanced by the amount of positive electrode active material added; In Example 2, the first positive electrode film layer region contains 0.3% CNT conductive agent, 0.24% SP content, and C p1 It is 1.44; In Example 3, the first positive electrode film layer region contains 1.2% CNT conductive agent, 1.2% SP content, and C p1 It is 6; In Example 4, the first positive electrode film layer region contains 1.3% CNT conductive agent, 1.4% SP content, and C p1 It is 6.6.
[0110] Examples 5-7 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the selection of the negative electrode material to change the average particle size of the negative electrode active material in the first negative electrode film region, thereby achieving D n2 / D n1 The change; In Example 5, the average particle size of the negative electrode material in the first negative electrode film layer region is 11.905 μm; In Example 6, the average particle size of the negative electrode material in the first negative electrode film layer region is 8.621 μm; In Example 7, the average particle size of the negative electrode material in the first negative electrode film layer region is 8.065 μm.
[0111] Examples 8-11 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the size of the coating mold to change the width of the first negative electrode film region, thereby achieving W n1 -W p1 The change; In Example 8, the width of the first negative electrode film layer region is 32 mm; In Example 9, the width of the first negative electrode film layer region is 40 mm; In Example 10, the width of the first negative electrode film layer region is 31 mm; In Example 11, the width of the first negative electrode film layer region is 42 mm.
[0112] Examples 12-14 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the design of the positive electrode tab width and the width of the first positive electrode film layer to achieve the positive electrode tab width W. pt and the width W of the first positive electrode film region p1 The change synchronously alters the width of the first negative electrode film region, maintaining W. n1 -W p1 Keeping W unchanged and changing the width of the second positive electrode film region p Unchanged, thus achieving (W) pt / W p )×(W p1 / W p The change; In Example 12, the width of the positive electrode tab is 15 mm, and the width of the first positive electrode film layer region is 10 mm; In Example 13, the width of the positive electrode tab is 70 mm, and the width of the first positive electrode film layer region is 60 mm; In Example 14, the width of the positive electrode tab is 60 mm, and the width of the first positive electrode film layer region is 60 mm.
[0113] Examples 15-17 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the selection of the artificial graphite material for the negative electrode to change the specific surface area of the negative electrode active material in the first negative electrode film layer region, thereby achieving S n1 / S n2 The change; In Example 15, the specific surface area of the artificial graphite in the first negative electrode film layer region is 1.040 m². 2 / g; In Example 16, the specific surface area of the artificial graphite in the first negative electrode film layer region is 1.584 m². 2 / g; In Example 17, the specific surface area of the artificial graphite in the first negative electrode film layer region is 1.386 m². 2 / g.
[0114] Examples 18-20 This application provides a secondary battery, the preparation method of which differs from that of Example 1 in that the charging rate N is changed. c Value, thus achieving k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c The change; In Example 18, the charging rate N c The value is 1; In Example 19, the charging rate N c The value is 3; In Example 20, the charging rate N c The value is 6.
[0115] Examples 21-22 This application provides a secondary battery, the preparation method of which differs from that of Example 1 in that f(C) is changed. p ), f(D n ), f(W p ), f(S n ) is not within the initial setting range, but through comprehensive and coordinated adjustments of other parameters, k×[f(C) can be achieved. p )×f(D n )×f(W p )×f(S n )] / N c The change; In Example 21, f(C) p The value is 1.1 (achieved by adjusting the CNT conductive agent content in the first positive electrode film layer region to 0.205%). p1(1.32), f(D) n The value is 1.4 (by adjusting the average particle size D of the negative electrode material in the first negative electrode film layer region). n1 (8.929 μm), f(W) p The value is 0.451 (by adjusting W). p1 It is 60mm, W n1 It is 66mm, W p (84mm), f(S) n ) is 1.5 (by adjusting S) n1 It is 1.485m 2 / g); In Example 22, f(C) p The concentration was 3.5 (achieved by adjusting the CNT conductive agent content in the first positive electrode film layer region to 0.925%). p1 (4.2), f(D) n ) is 1.25, f(W p ) is 0.225, f(S) n The value is 1.05 (by adjusting S). n1 It is 1.040m 2 / g).
[0116] Examples 23-24 This application provides a secondary battery, the preparation method of which differs from that of Example 1 in that the LFP system is used to change the k value, and the f(C) value is adjusted. p ), f(D n ), f(W p ), f(S n ) parameters, thereby achieving k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c The change; In Example 23, f(Cp) is 3.1, f(D) n ) is 1.25, f(W p ) is 0.225, f(S) n The value is 1.33, and the k value is 0.4 (by using the positive electrode active material LiNi). 0.6 Co 0.1 Mn 0.3 (O2 was replaced with LiFePO4 to achieve a k value of 0.4). In Example 24, f(Cp) was 3.2 (achieved by adjusting the CNT conductive agent content in the first positive electrode film layer region to 0.835%). p1 (3.84), f(D) n ) is 1.25, f(W pThe value is 0.330 (by adjusting W). p1 It is 44mm, W n1 It is 50mm, W p (84mm), f(S) n The value of ) is 1.33, and the value of k is 0.4.
[0117] Examples 25-29 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 lies in the difference between the positive and negative electrode additives in the first film layer region, the amount of which is made up by positive electrode active material.
[0118] In Example 25, 3% silicon-carbon was added to the slurry in the first negative electrode film layer region as a lithium plating inhibitor. The silicon-carbon negative electrode used silicon-carbon composite particles with a particle size distribution of D. v50 It is 6μm; In Example 26, 3% silicon carbon was added to the slurry in the first negative electrode film layer region as a lithium plating inhibitor, while 1% Li2NiO2 was added to the first positive electrode film layer region as a lithium replenishing additive. In Example 27, 1% Li2NiO2 was added to the first positive electrode film layer region as a lithium supplement additive, and 0.4% Li2NiO2 was added to the second positive electrode film layer region as a lithium supplement additive. In Example 28, 3% silicon carbon was added to the slurry in the first negative electrode film layer region as a lithium plating inhibitor, and 1% silicon carbon was added to the second negative electrode film layer region as a lithium plating inhibitor. In Example 29, 3% silicon carbon was added to the slurry in the first negative electrode film layer region as a lithium plating inhibitor, and 1% silicon carbon was added to the second negative electrode film layer region as a lithium plating inhibitor. At the same time, 1% Li2NiO2 was added to the first positive electrode film layer region as a lithium replenishing additive, and 0.4% Li2NiO2 was added to the second positive electrode film layer region as a lithium replenishing additive.
[0119] Comparative Example 1 This application provides a secondary battery in comparison. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the dosage of the conductive agent to alter the equivalent mass ratio of the positive electrode conductive agent in the first positive electrode film layer region, thereby achieving C p1 / C p2 The changes; the amount of conductive agent added is balanced by the amount of SP and CNT added; In Comparative Example 1, the first positive electrode film layer region contained 0.175% CNT, 0.5% SP, and C p1 It is 1.2.
[0120] Comparative Example 2 This application provides a secondary battery in a comparative example. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the selection of the negative electrode material to change the average particle size of the negative electrode active material in the first negative electrode film layer region, thereby achieving D n2 / D n1 The change; In Comparative Example 2, the average particle size of the negative electrode material in the first negative electrode film layer region is 13.158 μm.
[0121] Comparative Example 3 This application provides a secondary battery in comparison. The difference between the preparation method of the secondary battery and that of Example 1 lies in changing the size of the coating mold to change the width of the first negative electrode film layer region, thereby achieving W n1 -W p1 The change; In Comparative Example 3, the width of the first negative electrode film layer region is 30 mm.
[0122] In the examples and comparative examples, C p1 / C p2 D n2 / D n1 W n1 -W p1 Q = (W) pt / W p )×(W p1 / W p )), S n1 / S n2 N c , k, Y = (k × [f(C) p )×f(D n )×f(W p )×f(S n )] / N c The additives are shown in Table 1-2; Table 1 Table 2 The secondary batteries prepared in the examples and comparative examples were subjected to performance tests, including the following aspects: 1. Lithium plating test: Charged at 10℃ using 1.2 times the set charging strategy. Specifically, charged from 0% SOC to 20% SOC at 0.5C; then charged from 20% SOC to 70% SOC at 1.2 × Nc rate; then charged from 70% SOC to 100% SOC at 0.5C; finally, charged at full capacity with constant voltage to 0.05C cutoff current, allowed to rest for 30 minutes, and discharged from 100% SOC to 0% SOC at 0.5C for 50 cycles. The secondary battery was disassembled, and the lithium plating area on the surface of the negative electrode in the disassembled study area (the entire negative electrode) was measured using the transparent graph paper method. The percentage value of the lithium plating area / the total area of the negative electrode in the disassembled study area (the entire negative electrode) was calculated, and the lithium plating situation was quantitatively determined by the percentage value. 2. 25℃ Cyclic Test: Charge using the set charging strategy, discharge at 0.5C, and cycle until the percentage of the discharge capacity to the first discharge capacity reaches 80%, then record the number of cycles. The results are shown in Table 2; Table 2 As can be seen from Table 2, when the technical solution provided in this application is adopted, the secondary battery has a low degree of lithium plating and excellent cycle performance. Specifically, in the lithium plating test, the lithium plating area ratio is less than 13%, and in the cycle performance test, the number of cycles is more than 860 when the percentage value of the discharge capacity to the first discharge capacity reaches 80%. As can be seen from Examples 1-29 and Comparative Examples 1-3, when the following conditions are met simultaneously: the equivalent mass ratio of the positive electrode conductive agent in the positive electrode film region of this application is greater than the equivalent mass ratio of the positive electrode conductive agent in the second positive electrode film region; the average particle size of the negative electrode active material in the first negative electrode film region is smaller than the average particle size of the negative electrode active material in the second negative electrode film region; and the maximum size of the first negative electrode film region along the first direction is greater than the maximum size of the first positive electrode film region along the first direction, significant effects can be achieved.
[0123] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of this application and not to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A secondary battery, comprising a positive electrode (1) and a negative electrode (2), wherein the positive electrode (1) comprises a positive current collector (3), a positive electrode tab (4), and a positive electrode film (5) disposed on at least one surface of the positive current collector (3); the negative electrode (2) comprises a negative current collector (6), a negative electrode tab (7), and a negative electrode film (8) disposed on at least one surface of the negative current collector (6); wherein the positive electrode film (5) comprises a positive active material and a positive conductive agent; and the negative electrode film (8) comprises a negative active material and a negative conductive agent, characterized in that... ; The secondary battery has a first orientation; The positive electrode film (5) includes a first positive electrode film region (51) close to the positive electrode tab (4) and a second positive electrode film region (52) away from the positive electrode tab (4) along the first direction. The negative electrode film layer (8) includes a first negative electrode film layer region (81) close to the negative electrode tab (7) and a second negative electrode film layer region (82) away from the negative electrode tab (7) along the first direction. The secondary battery satisfies (A) to (C): (A) The equivalent mass percentage C of the positive electrode conductive agent in the first positive electrode film region (51) p1 The equivalent mass percentage C of the positive electrode conductive agent in the second positive electrode film region (52) is greater than that of the positive electrode conductive agent. p2 ; (B) The average particle size D of the negative electrode active material in the first negative electrode film region (81) n1 The average particle size D of the negative electrode active material in the second negative electrode film region (82) is smaller than that of the negative electrode active material. n2 ; (C) The maximum dimension W of the first negative electrode film region (81) along the first direction n1 The maximum dimension W along the first direction of the first positive electrode film region (51) is greater than that of the first positive electrode film region (51). p1 .
2. The secondary battery according to claim 1, characterized in that, Satisfy at least one of the following: (A)1.10≤C p1 / C p2 ≤5.5; (B)1.05≤D n2 / D n1 ≤1.55; (C)1.0mm≤W n1 -W p1 ≤12.0mm。 3. The secondary battery according to claim 1, characterized in that, W pt The maximum dimension of the positive electrode tab (4) perpendicular to the first direction. W p The maximum dimension of the positive electrode film layer (5) along the first direction; The secondary battery satisfies: 0.021 ≤ (W pt / W p )×(W p1 / W p )≤0.
595.
4. The secondary battery according to claim 1, characterized in that, The specific surface area S of the negative electrode active material in the first negative electrode film region (81) n1 The specific surface area S of the negative electrode active material in the second negative electrode film region (82) is greater than that of the negative electrode active material. n2 .
5. The secondary battery according to claim 4, characterized in that, Satisfying 1.05≤S n1 / S n2 ≤1.
60.
6. The secondary battery according to any one of claims 1 to 5, characterized in that, The secondary battery satisfies the following formula: k×[f(C p )×f(D n )×f(W p )×f(S n )] / N c ≥0.01; in, f(C p ) is the compensation factor for the positive electrode electron conduction network, f(C) p )=C p1 / C p2 ; f(D n ) is the solid-state diffusion compensation factor for the negative electrode phase, f(D) n )=D n2 / D n1 ; f(W p ) represents the macroscopic current collection bottleneck leakage factor of the secondary battery, f(W) p )=(W pt / W p )×(W p1 / W p ); f(S n ) is the charge transfer activation factor at the negative electrode interface, f(S) n )=S n1 / S n2 ; k is an empirical parameter for system design, 0.2≤k≤0.8; N c The value of the charging rate parameter of the secondary battery, W pt W is the maximum dimension of the positive electrode tab (4) perpendicular to the first direction. p S is the maximum dimension of the positive electrode film layer (5) along the first direction. n1 S represents the specific surface area of the negative electrode active material in the first negative electrode film region (81). n2 The specific surface area of the negative electrode active material in the second negative electrode film region (82) is denoted as .
7. The secondary battery according to claim 1, characterized in that, The negative electrode film layer (8) also includes a lithium plating inhibitor, the lithium plating inhibitor having a lithium intercalation potential higher than that of the negative electrode active material.
8. The secondary battery according to claim 7, characterized in that, The negative electrode film layer satisfies: M1>M2, Wherein, M1 is the mass percentage of the lithium plating inhibitor in the first negative electrode film region (81); M2 is the mass percentage of the lithium plating inhibitor in the second negative electrode film region (82).
9. The secondary battery according to claim 7, characterized in that, The lithium plating inhibitor includes at least one of silicon-carbon composite materials, silicon suboxide, pure silicon materials, hard carbon, soft carbon, and lithium titanate.
10. The secondary battery according to claim 1, characterized in that, The positive electrode film (5) also includes lithium supplementation additives.
11. The secondary battery according to claim 10, characterized in that, The positive electrode film layer satisfies: C1>C2, Wherein, C1 is the mass percentage of the lithium-replenishing additive in the first positive electrode film region (51). C2 is the mass percentage of the lithium supplementation additive in the second positive electrode film region (52).
12. The secondary battery according to claim 10, characterized in that, The lithium supplement additive includes at least one of lithium-rich metal oxides, lithium-rich nitrides, lithium-rich sulfides, or lithium-containing organic compounds.
13. An electrical appliance, characterized in that, Includes the secondary battery as described in any one of claims 1 to 12.