Positive electrode for lithium-ion secondary batteries

By using two lithium-nickel composite oxides in the cathode of lithium-ion secondary batteries and adjusting their nickel composition ratio and particle hardness relationship, the problem of insufficient capacity retention after cycling was solved, and a higher battery capacity retention rate was achieved.

CN123120633APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610592668.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-04-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

There is room for improvement in the post-cycle capacity retention of existing lithium-ion secondary battery cathodes, especially in mixtures of large and small particles, and particularly in mixtures of active materials with different compositions.

Method used

A mixed cathode using two lithium-nickel composite oxides is employed, wherein the nickel composition ratio of the first lithium-nickel composite oxide is higher than that of the second lithium-nickel composite oxide, and specific particle hardness, volume average diameter and mass ratio relationships are satisfied. Through pressing processing, the reactivity of the two active materials is well balanced.

Benefits of technology

By adjusting particle hardness and composition ratio, the capacity retention rate of lithium-ion secondary batteries was improved, resulting in better battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120633A_ABST
    Figure CN123120633A_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode for lithium ion secondary batteries. The positive electrode for lithium ion secondary batteries includes a first lithium-nickel composite oxide and a second lithium-nickel composite oxide. The nickel composition ratio of the first lithium-nickel composite oxide is higher than the nickel composition ratio of the second lithium-nickel composite oxide. The first lithium-nickel composite oxide includes first large particles and first small particles. The second lithium-nickel composite oxide includes second large particles and second small particles. The relationships of "H1<H2", "h1<h2", "H1<h1" and "H2<h2" are satisfied. "H1" represents the hardness of the first large particles. "h1" represents the hardness of the first small particles. "H2" represents the hardness of the second large particles. "h2" represents the hardness of the second small particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a positive electrode for lithium-ion secondary batteries. Background Art

[0002] Chinese Patent Application Publication No. 116565133 discloses a mixture of first positive electrode active material particles (LiNi 0.8 Co 0.1 Mn 0.1 O₂, 11.5 μm) and second positive electrode active material particles (LiNi 0.82 Co 0.135 Mn 0.045 O₂, 5.5 μm). Summary of the Invention

[0003] To increase the energy density of a positive electrode for lithium-ion secondary batteries (hereinafter may be abbreviated as "positive electrode"), mixtures of large particles and small particles, mixtures of two active materials having different compositions, and the like have been proposed. However, there remains room for improvement in the capacity retention rate after cycles.

[0004] An object of the present disclosure is to improve the capacity retention rate after cycles.

[0005] Hereinafter, the technical configuration of the present disclosure as well as its functions and effects will be described. Note that the mechanism of action includes speculation. The mechanism of action does not limit the technical scope of the present disclosure.

[0006] 1. A positive electrode for lithium-ion secondary batteries according to one aspect of the present disclosure includes a first lithium-nickel composite oxide and a second lithium-nickel composite oxide. The nickel composition ratio of the first lithium-nickel composite oxide is higher than the nickel composition ratio of the second lithium-nickel composite oxide. The first lithium-nickel composite oxide includes first large particles and first small particles. The second lithium-nickel composite oxide includes second large particles and second small particles. The relationships of "H1 < H2", "h1 < h2", "H1 < h1" and "H2 < h2" are satisfied. "H1" represents the hardness of the first large particles. "h1" represents the hardness of the first small particles. "H2" represents the hardness of the second large particles. "h2" represents the hardness of the second small particles.

[0007] Generally, the positive electrode is subjected to pressing. The positive electrode active material may be secondary particles. The softer the secondary particles are, the more easily particle cracking, pulverization and the like occur during the pressing process. It is considered that the finer the particles are pulverized, the larger the reaction area will be.

[0008] The positive electrode according to the present disclosure contains two types of active materials (lithium-nickel composite oxides) having different Ni composition ratios from each other. Since the two types of active materials have different Ni composition ratios, they are considered to also have different reactivities with Li. Each of the two types of active materials includes large particles and small particles. It is believed that the large particles and the small particles have different reactivities due to, for example, different specific surface areas.

[0009] According to the new findings in the present disclosure, improvement in capacity retention rate is expected when the combination of "large particles are more prone to cracking than small particles" and "the higher the Ni composition ratio, the more prone to cracking" is present. This is presumed to be because the particles tend to be densely packed in the pressed electrode, and the reactivities of the two types of active materials are well balanced.

[0010] 2. The positive electrode for lithium ion secondary batteries according to the above item "1" may include, for example, a configuration satisfying the relationship of "d1<d2<D1≤D2". "D1" represents the mean volume diameter of the first large particles. "d1" represents the mean volume diameter of the first small particles. "D2" represents the mean volume diameter of the second large particles. "d2" represents the mean volume diameter of the second small particles.

[0011] When the relationship of "d1<d2<D1≤D2" is satisfied, improvement in capacity retention rate is expected. This is considered to be because the reactivities of the two types of active materials are well balanced.

[0012] 3. The positive electrode for lithium ion secondary batteries according to the above item "1" or item "2" may include, for example, a configuration satisfying the relationship of "m1:m2=6:4 to 8:2". "m1" represents the mass ratio of the first lithium-nickel composite oxide. "m2" represents the mass ratio of the second lithium-nickel composite oxide.

[0013] When the relationship of "m1:m2=6:4 to 8:2" is satisfied, improvement in capacity retention rate is expected. This is considered to be because the reactivities of the two types of active materials are well balanced.

[0014] 4. The positive electrode for lithium ion secondary batteries according to any one of the above items "1" to "3" may include, for example, the following configuration. The first lithium-nickel composite oxide has a composition represented by the first composition formula "LiNi x Co y Mn z O2". The second lithium-nickel composite oxide has a composition represented by the second composition formula "LiNi u Co v Mn wO2" represents the composition. The relationships of "0.8≤x<1.0", "0<2y≤v", "0<3z≤w", "0.5≤u≤0.6", "0.1≤v≤0.2" and "0.2≤w≤0.3" are satisfied.

[0015] It is expected that the combination of the first composition formula and the second composition formula improves the balance of reactivity.

[0016] 5. A positive electrode for lithium-ion secondary batteries for a lithium-ion secondary battery according to one aspect of the present disclosure includes a first lithium-nickel composite oxide and a second lithium-nickel composite oxide. The first lithium-nickel composite oxide has a composition represented by the first composition formula "LiNi x Co y Mn z O2". The second lithium-nickel composite oxide has a composition represented by the second composition formula "LiNi u Co v Mn w O2". The relationships of "0.8≤x<1.0", "0<2y≤v", "0<3z≤w", "0.5≤u≤0.6", "0.1≤v≤0.2" and "0.2≤w≤0.3" are satisfied. The first lithium-nickel composite oxide includes first large particles and first small particles. The second lithium-nickel composite oxide includes second large particles and second small particles. The relationships of "H1<H2", "h1<h2", "H1<h1" and "H2<h2" are satisfied. "H1" represents the hardness of the first large particles. "h1" represents the hardness of the first small particles. "H2" represents the hardness of the second large particles. "h2" represents the hardness of the second small particles. The relationship of "d1<d2<D1≤D2" is satisfied. "D1" represents the volume average diameter of the first large particles. "d1" represents the volume average diameter of the first small particles. "D2" represents the volume average diameter of the second large particles. "d2" represents the volume average diameter of the second small particles. The relationship of "m1:m2=6:4 to 8:2" is satisfied. "m1" represents the mass ratio of the first lithium-nickel composite oxide. "m2" represents the mass ratio of the second lithium-nickel composite oxide.

[0017] Hereinafter, embodiments of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and examples of the present disclosure (hereinafter may be abbreviated as "the present example") will be described. However, it should be noted that the present embodiment and the present example do not limit the technical scope of the present disclosure. The present embodiment and the present example are illustrative in all respects. The present embodiment and the present example are non-restrictive. The technical scope of the present disclosure covers all modifications within the meaning and range equivalent to the description of the claims. For example, it is planned from the beginning to arbitrarily extract any configuration from the present embodiment and combine them arbitrarily. Brief Description of the Drawings

[0018] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will now be described with reference to the accompanying drawings, wherein like symbols denote like elements, and wherein: Figure 1 This is a conceptual diagram illustrating a method for measuring particle hardness in an embodiment; Figure 2 This is a conceptual diagram illustrating an example of a lithium-ion secondary battery according to an embodiment; and Figure 3 This is a table showing examples of experimental results according to the implementation method. Detailed Implementation

[0019] Terms and phrases

[0020] "Including," "containing," "having," and their variations are open-ended expressions. A configuration expressed as open-ended may further include additional elements beyond the required elements, or may not include them at all. The term "consisting of" is a closed-ended expression. However, even a configuration expressed as closed-ended may include the often-accompanying impurities and additional elements unrelated to the object technology. The term "substantially consisting of" is a semi-closed-ended expression. A configuration expressed as semi-closed-ended allows for the addition of elements that substantially do not affect the fundamental and novel characteristics of the object technology.

[0021] Geometric terms should not be interpreted in a strict sense. Examples of such terms include "parallel," "perpendicular," and "orthogonal." For example, directions, angles, and distances can vary relatively within a range to achieve essentially the same or similar functions. Geometric terms may include, for example, tolerances and errors related to design, operation, and manufacturing. There are instances where the dimensional relationships in the accompanying drawings do not match the actual dimensional relationships. There are instances where the dimensional relationships in the accompanying drawings have been altered for the reader's understanding. For example, there are instances where length, width, or thickness have been changed. There are instances where a portion of the configuration has been omitted.

[0022] Unless otherwise specified, numerical ranges such as "m to n%" are closed intervals including the upper and lower limit values thereof. That is, "m to n%" represents a numerical range of "m% or more and n% or less". Further, "m% or more and n% or less" includes "greater than m% and less than n". The phrases "or more" and "or less" are represented by the inequality signs "≥" and "≤" with an equal sign. The phrases "greater than" and "less than" are represented by the inequality signs ">" and "<" without an equal sign. A numerical value selected from a numerical range as needed can be set as a new upper limit value or a new lower limit value. For example, a new numerical range can be set by combining a numerical value within the numerical range with numerical values shown in other parts of the present specification, tables, drawings, and the like as needed. Regarding numerical ranges (intervals), for example, "a range formed by any one or two endpoints selected from the group a, b, c, and d" includes "a≤x", "x≤a", "b≤x", "x≤b", "c≤x", "x≤c", "d≤x", "x≤d", "a≤x≤b", "a≤x≤c", "a≤x≤d", "b≤x≤c", "b≤x≤d", and "c≤x≤d". Any range may or may not include the endpoints. That is, the above ranges include, for example, not only "a≤x" but also "a<x". The above ranges include, for example, not only "a≤x≤b" but also "a<x≤b", "a≤x<b", and "a<x<b".

[0023] Unless otherwise specified, singular terms are not limited to a single (one) element. Singular terms also include a plurality of elements.

[0024] "Volume average diameter" refers to the particle size at which the cumulative frequency reaches 50% in the volume-based particle size distribution (volume distribution). The volume average diameter of secondary particles can be measured using a laser diffraction particle size distribution measuring apparatus (for example, a product name "MT3000" manufactured by MicrotracBEL Corporation, etc.).

[0025] The particle size distribution of primary particles indicates the modal diameter of the particle size distribution measured by small-angle X-ray scattering (SAXS). For the measurement, a multipurpose X-ray diffractometer or a small-angle X-ray scattering apparatus, for example, a product name "SmartLab" (manufactured by Rigaku Corporation) or the like can be used.

[0026] Figure 1This is a conceptual diagram illustrating a method for measuring particle hardness according to an embodiment. The hardness of the particles is measured through the following steps: The volume average diameter of the particles to be measured (first largest particle, first smallest particle, second largest particle, or second smallest particle) is determined. Five particles whose maximum Ferete diameter is within ±10% of the volume average diameter are extracted from the particles (powder) to be measured. An indenter 11 is pressed into the particles 12 using a particle strength measuring instrument (e.g., a nanoindenter manufactured by Toyo Corporation), and the load-displacement curve of the particles 12 is measured. The indenter 11 is a triangular cone indenter (Berkovich indenter). The hardness "H" is determined by dividing the maximum load "Pmax" of the load-displacement curve by the contact projected area "A(hc)". The maximum and minimum values ​​are excluded from the five measurements, and the arithmetic mean of the three values ​​is used.

[0027] Lithium-ion secondary batteries

[0028] The lithium-ion secondary battery (hereinafter referred to as "battery") in this embodiment includes at least one electrolyte selected from the group consisting of liquid electrolytes, gel electrolytes, and solid electrolytes. The battery can be a liquid battery, polymer battery, solid-state battery, or all-solid-state battery. "Solid-state battery" refers to a battery containing a solid electrolyte. In addition to a solid electrolyte, a solid-state battery may also contain other electrolytes.

[0029] Figure 2 This is a conceptual diagram illustrating an example of a lithium-ion secondary battery according to this embodiment. The battery 1000 may include, for example, a power generation element 500 and a casing 600. The casing 600 stores the power generation element 500. The casing 600 may be, for example, a metal container, a bag made of aluminum laminate, etc. The power generation element 500 may include, for example, a positive electrode 100, a negative electrode 200, a separator 300, an electrolyte (omitted from the diagram), etc. The power generation element 500 may be, for example, a wound type or a laminated type. The power generation element 500 may have a unipolar structure or a bipolar structure. The separator 300 electrically isolates the negative electrode 200 from the positive electrode 100. The separator 300 may include, for example, a porous membrane made of resin. The electrolyte is a Li-ion conductor. The electrolyte may contain, for example, Li salts and organic solvents. For example, the separator 300 may be impregnated with the electrolyte. The separator 300 may contain a solid electrolyte. The electrolyte may contain, for example, a polymer electrolyte, a gel electrolyte, a solid electrolyte, etc. Solid electrolytes may include, for example, sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, etc. The negative electrode 200 includes a negative electrode active material. The negative electrode active material is, for example, at least one selected from the group consisting of natural graphite, artificial graphite, silicon, silicon oxides, silicon alloys, and Si-C. "Si-C" refers to composite particles containing at least one of silicon and silicon oxides and carbon. For example, Si can be supported on a carbon material.

[0030] positive electrode

[0031] The positive electrode 100 comprises a positive electrode active material. The positive electrode 100 may include, for example, a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer may be supported by the positive electrode current collector. The positive electrode active material layer may contain positive electrode active material. In addition to containing positive electrode active material, the positive electrode active material layer may also contain conductive material, binder, etc. The positive electrode active material layer may contain, for example, 0% to 10% conductive material and 1% to 10% binder by mass fraction, with the balance being positive electrode active material. The thickness range of the positive electrode active material layer may be, for example, formed by any one or two endpoints selected from the group consisting of 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 75 μm, 100 μm, 150 μm, 200 μm, 300 μm, 400 μm, 500 μm, 750 μm, and 1000 μm. The thickness of the positive electrode active material layer can range from, for example, "more than 10 μm", "less than 1000 μm", or "10 μm to 1000 μm". The density of the positive electrode active material layer can range from, for example, from 1.5 g / cm³. 3 2.0g / cm 3 2.5g / cm 3 3.0g / cm 3 3.5g / cm 3 4.0g / cm 3 and 4.5g / cm 3 The range formed by any one or both endpoints of the group. The density range of the positive electrode active material layer can be, for example, "1.5 g / cm³". 3 "Above", "4.5g / cm" 3 "below", "1.5g / cm" 3 Up to 4.5 g / cm 3 "wait.

[0032] The positive electrode active material comprises a first lithium nickel composite oxide and a second lithium nickel composite oxide. That is, the positive electrode 100 comprises a first lithium nickel composite oxide and a second lithium nickel composite oxide. The first lithium nickel composite oxide has a higher Ni composition ratio than the second lithium nickel composite oxide. The range of the Ni composition ratio of the first and second lithium nickel composite oxides is arbitrary, provided that the first lithium nickel composite oxide has a higher Ni composition ratio than the second lithium nickel composite oxide. The range of the Ni composition ratio can be, for example, a range formed by any one or two endpoints selected from the group consisting of 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, and 1.00. The range of the Ni composition can be, for example, "above 0.30", "below 1.00", or "0.30 to 1.00".

[0033] The first lithium-nickel composite oxide can be, for example, composed of the first formula "LiNi". x Co y Mn z "O2" indicates the composition. In the first composition formula, "x" represents the Ni composition ratio described above. For example, a relationship such as "0.700 ≤ x < 1.00" can be satisfied. In the first composition formula, the ranges of "y" and "z" can be, for example, ranges formed by any one or both endpoints of the group selected from 0.05, 0.10, 0.15, and 0.20. For example, a relationship such as "0 ≤ y ≤ 0.20" and "0 ≤ z ≤ 0.20" can be satisfied. The first lithium-nickel composite oxide may contain, for example, LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, etc.

[0034] The second lithium-nickel composite oxide can be, for example, composed of the second formula "LiNi". u Co v Mn w "O2" indicates the composition. In the second composition formula, "u" represents the Ni composition ratio described above. For example, a relationship such as "0.30 ≤ u ≤ 0.65" can be satisfied. In the second composition formula, the ranges of "v" and "w" can be, for example, ranges formed by any one or both endpoints of the group consisting of 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, and 0.35. For example, a relationship such as "0 ≤ v ≤ 0.35" and "0 ≤ w ≤ 0.35" can be satisfied. The second lithium-nickel composite oxide may contain, for example, LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.4 Co 0.3 Mn 0.3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.4 Mn 0.1 O2, LiNi 0.5 Co 0.1 Mn 0.4 O2, LiNi 0.6 Co 0.3 Mn 0.1 O2, LiNi 0.6 Co0.2 Mn 0.2 O2, LiNi 0.6 Co 0.1 Mn 0.3 O2, etc.

[0035] For example, the first and second compositional equations can satisfy relationships such as "0.8≤x<1.0", "0<2y≤v", "0<3z≤w", "0.5≤u≤0.6", "0.1≤v≤0.2", "0.2≤w≤0.3", etc. In the first and second compositional equations, some or all of Co and Mn can be substituted by, for example, Al.

[0036] The range of the ratio "m1:m2" of the mass ratio "m1" of the first lithium-nickel composite oxide to the mass ratio "m2" of the second lithium-nickel composite oxide can be, for example, a range formed by any two of the following: "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1". For example, relationships such as "m1:m2 = 6:4 to 8:2" can be satisfied.

[0037] The first lithium-nickel composite oxide comprises a first large particle and a first small particle. The second lithium-nickel composite oxide comprises a second large particle and a second small particle. Both the large and small particles can be secondary particles. A secondary particle comprises multiple primary particles. Each small particle can be a single particle. A single particle consists of fewer than 10 primary particles. A single particle can consist essentially of a single primary particle.

[0038] The average number of primary particles contained in each major particle can be, for example, a range formed by any one or both endpoints of a group selected from 50, 100, 500, 1000, 3000, 5000, and 10,000. The average number of primary particles contained in each major particle can be, for example, in the range of "more than 50", "less than 10,000", or "50 to 10,000".

[0039] Secondary particles can have any shape. They can be, for example, spherical, ellipsoidal, etc. The range of sphericity of secondary particles can be, for example, a range formed by any one or both endpoints of a group selected from 0.50, 0.60, 0.70, 0.80, 0.90, 0.95, and 1.00. The range of sphericity of secondary particles can be, for example, "above 0.50", "below 1.00", "0.50 to 1.00", etc.

[0040] The hardness "H1" of the first large particle and the hardness "H2" of the second large particle satisfy the relationship "H1<H2". The range of the ratio "H2 / H1" may be, for example, a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, 5.0 and 10. For example, a relationship such as "1.2≤H2 / H1≤10" or the like may be satisfied.

[0041] The hardness "h1" of the first small particle and the hardness "h2" of the second small particle satisfy the relationship "h1<h2". The range of the ratio "h2 / h1" may be, for example, a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, 5.0 and 10. For example, a relationship such as "1.2≤h2 / h1≤10" or the like may be satisfied.

[0042] The hardness "H1" of the first large particle and the hardness "h1" of the first small particle satisfy the relationship "H1<h1". The range of the ratio "h1 / H1" may be, for example, a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, 5.0 and 10. For example, a relationship such as "1.2≤h1 / H1≤10" or the like may be satisfied.

[0043] The hardness "H2" of the second large particle and the hardness "h2" of the second small particle satisfy the relationship "H2<h2". The range of the ratio "h2 / H2" may be, for example, a range formed by any one or two endpoints selected from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, 5.0 and 10. For example, a relationship such as "1.2≤h2 / H2≤10" or the like may be satisfied.

[0044] For example, the volume average diameter "D1" of the first large particle, the volume average diameter "d1" of the first small particle, the volume average diameter "D2" of the second large particle, and the volume average diameter "d2" of the second small particle satisfy the relationships "d1<D1" and "d2<D2". As long as these relationships are satisfied, the ranges of "D1", "d1", "D2" and "d2" may each independently be a range formed by any one or two endpoints selected from the group consisting of, for example, 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 9μm, 12μm, 15μm, 18μm, 21μm, 24μm, 27μm and 30μm. For example, relationships such as "d1<d2<D1≤D2", "d1<d2<D1<D2" and the like may be satisfied.

[0045] The range of the average primary particle size of the first large particles, first small particles, second large particles and second small particles may each independently be a range formed by any one or two endpoints selected from the group consisting of, for example, 0.01μm, 0.05μm, 0.1μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm and 3μm. The range of the average primary particle size of the first large particles, first small particles, second large particles and second small particles may each independently be, for example, "0.01μm or more", "3μm or less", or "0.01μm to 3μm", and the like.

[0046] For example, the average primary particle size "X1" of the first large particles, the average primary particle size "x1" of the first small particles, the average primary particle size "X2" of the second large particles, and the average primary particle size "x2" of the second small particles may satisfy a relationship such as "X1≤x1≤x2≤X2" or "X1<x1<x2<X2", and the like. By satisfying these relationships, it is expected that the balance of reactivity between the first lithium-nickel composite oxide and the second lithium-nickel composite oxide will be improved.

[0047] The range of the ratio of the mass ratio of the first large particles to the mass ratio of the first small particles "first large particles:first small particles" and the range of the ratio of the mass ratio of the second large particles to the mass ratio of the second small particles "second large particles:second small particles" may each independently be a range formed by a combination of any two of, for example, "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2" and "9:1". For example, a relationship such as "first large particles:first small particles=7:3 to 9:1" and the like may be satisfied. For example, a relationship such as "second large particles:second small particles=7:3 to 9:1" and the like may be satisfied.

[0048] The conductive material may contain, for example, at least one selected from the group consisting of carbon black (acetylene black, Ketjen Black "registered trademark"), flake graphite, vapor-grown carbon fibers, carbon nanotubes, and graphene flakes. The range of the volume average diameter of the conductive material may be, for example, a range formed by any one or two endpoints selected from the group consisting of 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm and 9μm. The range of the volume average diameter of the conductive material may be, for example, "0.5μm or more", "9μm or less", "0.5μm to 9μm", and the like. For example, the range of the volume average diameter of the flake graphite may be within the range between the volume average diameter of the first large particles and the volume average diameter of the second small particles. It is expected that since the flake graphite has a size between the large particles and the small particles, the balance of reactivity between the large particles and the small particles will be improved.

[0049] The adhesive may contain at least one of the following: selected from the group consisting of polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR).

[0050] No. 1

[0051] First lithium-nickel composite oxide (LiNi) 0.8 Co 0.1 Mn 0.1 Synthesis of O2.

[0052] A raw material aqueous solution is formed by dissolving NiSO4, CoSO4, and MnSO4 in ion-exchange water, such that the molar ratio is "Ni:Co:Mn = 8:1:1". The concentration of the raw material aqueous solution is 30% by mass fraction.

[0053] A predetermined amount of NH3 aqueous solution was placed in the reaction vessel. While stirring the NH3 aqueous solution with a stirrer, the atmosphere inside the reaction vessel was purged with nitrogen. A predetermined amount of NaOH was added to the reaction vessel to adjust the pH to alkaline. The raw material aqueous solution and the NH3 aqueous solution were added dropwise to the reaction vessel. The dripping rate of each aqueous solution was adjusted to maintain the pH of the reaction solution within a certain range. The precursor of the first large particle (transition metal hydroxide) was then allowed to precipitate for 6 hours. The precursor of the first small particle was allowed to precipitate for 3 hours. The precursor was recovered by filtration. The precursor was washed with water. That is, the precursor was dispersed in ion-exchanged water using a spoon or similar tool. The precursor was recovered again by filtration. The precursor was dried at 120°C for 16 hours.

[0054] The precursor and lithium compound (LiOH, Li₂CO₃, etc.) are mixed to prepare a mixture. The molar fraction of Li is adjusted to 100% to 110% relative to the total amount of transition metal contained in the precursor.

[0055] The mixture was calcined in a furnace at 700°C to 1100°C for 10 hours in an oxygen atmosphere to obtain a calcined product. The calcined product was then pulverized using a jet mill to adjust the particle size of the secondary particles. Thus, the first large particles and the first small particles of the first lithium-nickel composite oxide were prepared.

[0056] Second lithium-nickel composite oxide (LiNi) 0.5 Co 0.2 Mn 0.3 Synthesis of O2.

[0057] A raw material aqueous solution is formed by dissolving NiSO4, CoSO4, and MnSO4 in ion-exchange water, such that the molar ratio is "Ni:Co:Mn = 5:2:3". The concentration of the raw material aqueous solution is 30% by mass fraction.

[0058] A predetermined amount of NH3 aqueous solution was placed in the reaction vessel. While stirring the NH3 aqueous solution with a stirrer, the atmosphere inside the reaction vessel was purged with nitrogen. A predetermined amount of NaOH was added to the reaction vessel to adjust the pH to alkaline. The raw material aqueous solution and the NH3 aqueous solution were added dropwise to the reaction vessel. The dripping rate of each aqueous solution was adjusted to maintain the pH of the reaction solution within a certain range. The precursor of the second largest particle was allowed to precipitate for 6 hours. The precursor of the second smallest particle was allowed to precipitate for 1 hour. The precursor was recovered by filtration. The precursor was washed with water. That is, the precursor was dispersed in ion-exchanged water using a spoon or similar tool. The precursor was recovered again by filtration. The precursor was dried at 120°C for 16 hours.

[0059] The precursor and lithium compound (LiOH, Li₂CO₃, etc.) are mixed to prepare a mixture. The molar fraction of Li is adjusted to 100% to 110% relative to the total amount of transition metal contained in the precursor.

[0060] The mixture was calcined in a furnace at 700°C to 1100°C for 10 hours in an oxygen atmosphere to obtain a calcined product. The calcined product was then pulverized using a jet mill to adjust the particle size of the secondary particles. This process yielded the second large and second small particles of the second lithium-nickel composite oxide.

[0061] The first lithium-nickel composite oxide and the second lithium-nickel composite oxide are mixed at a mass ratio of "first lithium-nickel composite oxide: second lithium-nickel composite oxide = 7:3" to prepare the positive electrode active material.

[0062] No. 2

[0063] The positive electrode active material was prepared in the same way as No. 1, except that the hardness of each particle was changed by altering the amount of Li compound added and the firing temperature.

[0064] evaluate

[0065] Manufacturing a cylindrical lithium-ion secondary battery (evaluation single cell). This evaluation single cell has the following configuration.

[0066] Power generation element: wound type

[0067] Positive electrode: Positive electrode active material / AB / PVDF = 88 / 10 / 2 (mass ratio)

[0068] Negative electrode: Negative electrode active material (natural graphite), CMC, SBR

[0069] Electrolytes: LiPF6 (1 mol / L), EC / DMC / EMC = 3 / 4 / 3 (volume ratio)

[0070] The positive and negative electrodes are each manufactured by applying their respective slurries to the surface of a substrate (metal foil). An Allgood coating applicator (with film thickness control) is used as the coating device. After applying the slurry, the coating is dried at 80°C for 5 minutes.

[0071] Measure and evaluate the initial capacity of a single cell. After measuring the initial capacity, perform 100 charge-discharge cycles. Measure and evaluate the post-cycle capacity of the single cell. Calculate the capacity retention by dividing the post-cycle capacity by the initial capacity.

[0072] result

[0073] Figure 3 This is a table showing examples of experimental results according to the embodiments. Compared to No. 2, No. 1 has an improved capacity retention rate. In No. 1, the hardness of the first large particle, the first small particle, the second large particle, and the second small particle satisfies "H1".

Claims

1. A positive electrode for lithium-ion secondary batteries, comprising: a first lithium-nickel composite oxide and a second lithium-nickel composite oxide, wherein the nickel composition ratio of the first lithium-nickel composite oxide is higher than the nickel composition ratio of the second lithium-nickel composite oxide, the first lithium-nickel composite oxide comprises first large particles and first small particles, the second lithium-nickel composite oxide comprises second large particles and second small particles, the relationships of H1<H2, h1<h2, H1<h1 and H2<h2 are satisfied, wherein H1 represents the hardness of the first large particles, h1 represents the hardness of the first small particles, H2 represents the hardness of the second large particles, and h2 represents the hardness of the second small particles.

2. The positive electrode for lithium-ion secondary batteries according to claim 1, wherein the relationship of d1<d2<D1≤D2 is satisfied, wherein D1 represents the volume average diameter of the first large particles, d1 represents the volume average diameter of the first small particles, D2 represents the volume average diameter of the second large particles, and d2 represents the volume average diameter of the second small particles.

3. The positive electrode for lithium-ion secondary batteries according to claim 1 or 2, wherein the relationship of m1:m2=6:4 to 8:2 is satisfied, wherein m1 represents the mass ratio of the first lithium-nickel composite oxide, and m2 represents the mass ratio of the second lithium-nickel composite oxide.

4. The positive electrode for lithium-ion secondary batteries according to claim 1 or 2, wherein The first lithium nickel composite oxide has a composition represented by a first composition formula LiNi x Co y Mn z O2 indicates, and The second lithium nickel composite oxide has a composition represented by a second composition formula LiNi u Co v Mn w O2 represents, the relationships of 0.8≤x<1.0, 0<2y≤v, 0<3z≤w, 0.5≤u≤0.6, 0.1≤v≤0.2, and 0.2≤w≤0.3 are satisfied.

5. A positive electrode for lithium-ion secondary batteries, comprising: a first lithium-nickel composite oxide and a second lithium-nickel composite oxide, wherein The first lithium nickel composite oxide has a composition represented by a first composition formula LiNi x Co y Mn z O2 indicates, and The second lithium nickel composite oxide has a composition represented by a second composition formula LiNi u Co v Mn w O2 represents, the relationships of 0.8≤x<1.0, 0<2y≤v, 0<3z≤w, 0.5≤u≤0.6, 0.1≤v≤0.2, and 0.2≤w≤0.3 are satisfied, the first lithium-nickel composite oxide comprises first large particles and first small particles, the second lithium-nickel composite oxide comprises second large particles and second small particles, the relationships of H1<H2, h1<h2, H1<h1 and H2<h2 are satisfied, wherein H1 represents the hardness of the first large particles, h1 represents the hardness of the first small particles, H2 represents the hardness of the second large particles, h2 represents the hardness of the second small particles, the relationship of d1<d2<D1≤D2 is satisfied, wherein D1 represents the volume average diameter of the first large particles, d1 represents the volume average diameter of the first small particles, D2 represents the volume average diameter of the second large particles, d2 represents the volume average diameter of the second small particles, and the relationship of m1:m2=6:4 to 8:2 is satisfied, wherein m1 represents the mass ratio of the first lithium-nickel composite oxide, and m2 represents the mass ratio of the second lithium-nickel composite oxide.