A positive electrode and a battery
By introducing metal oxides and thermally conductive materials with particle sizes smaller than the cathode material into the positive electrode active layer, a multi-scale structure is formed, which solves the problems of interface stability and heat dissipation requirements of the cathode sheet under high energy density, and improves thermal stability and safety.
Patent Information
- Application Number
- CN202611523926.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cathode materials struggle to simultaneously achieve interface stability and heat dissipation requirements at high energy densities, leading to increased internal resistance and decreased compaction density, which in turn affects the battery's thermal stability and electrochemical performance.
Metal oxides and thermally conductive materials with particle sizes smaller than the cathode material are introduced into the positive electrode active layer to form a multi-scale structure. The metal oxides are responsible for interface barrier, and the thermally conductive materials are responsible for heat conduction, which synergistically improves interfacial side reactions and thermal diffusion.
It improves the thermal stability and safety of the positive electrode, reduces the side reaction rate under high-temperature cycling conditions, and enhances the cycle stability and safety performance of the battery.
Smart Images

Figure CN123120636A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemical technology, and in particular to a positive electrode and a battery. Background Technology
[0002] Lithium-ion batteries, due to their high energy density and other characteristics, have become a core energy solution in electric vehicles, energy storage systems, and consumer electronics. However, with the continuous improvement of battery energy density, structural damage to cathode materials under abuse conditions, release of reactive oxygen species, and violent reactions in the electrolyte have become critical issues that urgently need to be addressed.
[0003] Existing cathode sheets often fail to simultaneously meet the requirements of interface stability and heat dissipation in practical applications. They are prone to problems such as insufficient compatibility with cathode materials, uneven dispersion, and increased interfacial side reactions. This may lead to increased internal resistance and decreased compaction density, thereby affecting the thermal stability and electrochemical performance of the battery.
[0004] Therefore, developing a cathode technology that can significantly improve safety while maintaining high battery energy density is of great significance for promoting the application of lithium-ion batteries in the aforementioned key areas. Summary of the Invention
[0005] This application provides a positive electrode and a battery. When the positive electrode is applied to a battery, it can improve the battery's safety performance and high-temperature cycle performance.
[0006] This application provides a positive electrode sheet, wherein the positive electrode sheet includes a positive current collector and a positive active layer located on at least one side surface of the positive current collector, and the positive active layer includes additives and a positive electrode material;
[0007] The cathode material includes Li e Ni a Co b Mn c M d O2, wherein 0≤a≤1, 0≤b≤1, 0≤c≤1, 0≤d≤1, 0<e≤1.2, at least one of a, b, and c is not 0, and M includes at least one of Mg, Al, Ti, Zr, Nb, W, V, Zn, Sc, Y, Mo, In, Sb, Ta, Cr, and La;
[0008] The additives include metal oxides and thermally conductive materials, wherein the thermally conductive materials include at least one of silicon carbide, silicon nitride, aluminum nitride, boron nitride, titanium nitride, titanium carbide, and beryllium oxide;
[0009] The Dv50 of the metal oxide is less than the Dmin of the positive electrode material, and the Dv50 of the metal oxide is less than the Dv50 of the thermally conductive material.
[0010] The positive electrode as described above, wherein the thermal conductivity of the thermally conductive material is >25 W / (m·K);
[0011] And / or, the metal oxide includes at least one of titanium dioxide, barium titanate, barium strontium titanate, aluminum oxide, magnesium oxide, zinc oxide, zirconium dioxide, tungsten trioxide, copper oxide, molybdenum trioxide, barium oxide, tantalum pentoxide, niobium pentoxide, cobalt oxide, and nickel oxide.
[0012] In the positive electrode sheet described above, the percentage of the additive by mass in the positive electrode material is 0.3%-5%.
[0013] And / or, the mass ratio of the metal oxide to the thermally conductive material is (2-8):(2-8); preferably, the mass ratio of the metal oxide to the thermally conductive material is (4-6):(4-6).
[0014] In the positive electrode sheet described above, the ratio of Dmin of the positive electrode material to Dv50 of the metal oxide is 2-40;
[0015] And / or, the ratio of Dmin of the positive electrode material to Dv50 of the thermally conductive material is 1.5-8.
[0016] In the positive electrode sheet as described above, the Dv50 of the metal oxide is 0.1 μm-0.5 μm; and / or, the Dv50 of the thermally conductive material is 0.5 μm-1.5 μm; and / or, the Dmin of the positive electrode material is 1 μm-4 μm.
[0017] The positive electrode sheet as described above, wherein the positive electrode material further includes materials located in the Li e Ni a Co b Mn c M d The particles coating at least part of the surface of O2, wherein the Dv50 of the metal oxide is greater than the Dv50 of the coating particles;
[0018] Preferably, the coated particles include at least one of aluminum oxide, magnesium oxide, titanium dioxide, zirconium dioxide, lanthanum oxide, yttrium oxide, and boron oxide; and / or, the Dv50 of the coated particles is 10-50 nm.
[0019] The positive electrode as described above, wherein the exothermic peak temperature of the differential scanning calorimetry test curve of the positive electrode is ≥235℃.
[0020] The positive electrode as described above has a resistivity of 0.5 kΩ·cm to 4 kΩ·cm.
[0021] This application also provides a battery, wherein a positive electrode plate as described above is included.
[0022] This application improves the dispersion state of the additives in the positive electrode active layer and their interfacial compatibility with the positive electrode material by setting a specific positive electrode material in the positive electrode active layer on at least one side surface of the positive electrode current collector, and by combining it with an additive containing a metal oxide and a thermally conductive material, and by limiting the Dv50 of the metal oxide to be less than the Dmin of the positive electrode material and less than the Dv50 of the thermally conductive material. This improves the thermal conductivity of the electrode and reduces the risk of interfacial side reactions, thereby improving the thermal stability and safety of the positive electrode, and thus improving the high-temperature cycle performance and safety performance of the battery. Attached Figure Description
[0023] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0024] Figure 1 Here is a surface SEM image of the positive electrode active layer in Example 1;
[0025] Figure 2 This is a distribution diagram of Co elements on the surface of the positive electrode active layer in Example 1;
[0026] Figure 3 This is a distribution diagram of C element on the surface of the positive electrode active layer in Example 1;
[0027] Figure 4 This is a distribution diagram of Ti elements on the surface of the positive electrode active layer in Example 1;
[0028] Figure 5 This is a distribution diagram of Al elements on the surface of the positive electrode active layer in Example 1;
[0029] Figure 6 This is a cross-sectional SEM image of the positive electrode active layer in Example 1;
[0030] Figure 7 This is a cross-sectional EDS image of the positive electrode active layer in Example 1;
[0031] Figure 8 The image shows the distribution of Ti elements in the cross-section of the positive electrode active layer in Example 1.
[0032] Figure 9 This is a cross-sectional SEM image of the positive electrode active layer of Comparative Example 3;
[0033] Figure 10 This is a cross-sectional EDS image of the positive electrode active layer in Comparative Example 3;
[0034] Figure 11 The image shows the differential scanning calorimetry curves of the positive electrode sheets of Example 1 and Comparative Example 1. Detailed Implementation
[0035] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.
[0036] Lithium-ion battery cathode technology is used in electric vehicle power batteries, energy storage batteries, and consumer electronics batteries. These batteries typically consist of a cathode, anode, separator, and electrolyte. The positive electrode active layer directly affects the battery's energy density, cycle performance, and thermal safety. Currently, damage to the positive electrode material structure in the active layer exacerbates the reaction between released active components and the electrolyte, making it difficult for localized heat to dissipate quickly. This can easily lead to hot spots and drive thermal runaway, limiting the safe application of high-energy-density batteries in power and energy storage applications.
[0037] To address the aforementioned technical challenges, a functionally differentiated additive system is introduced into the positive electrode active layer, integrating interfacial barrier and thermal conductivity within the same electrode structure. The metal oxide particle size is smaller than the minimum particle size of the positive electrode material and also smaller than the particle size of the thermally conductive material, allowing it to preferentially penetrate the interparticle gaps and surface areas of the positive electrode material. The thermally conductive material, distributed within the active layer, can then perform heat dissipation. Based on this, co-configuring the metal oxide and thermally conductive material within the positive electrode sheet, which includes the positive electrode current collector and the positive electrode active layer, and using it in conjunction with doped ternary positive electrode materials, can simultaneously improve the balance between interfacial side reactions, localized temperature rise, and electrode structural stability, thereby mitigating the adverse effects on electrochemical performance during safety enhancement.
[0038] This application provides a positive electrode sheet, which includes a positive current collector and a positive active layer located on at least one side surface of the positive current collector. The positive active layer includes additives and a positive electrode material.
[0039] Cathode materials include Li e Ni a Co b Mn c M d O2, wherein 0≤a≤1, 0≤b≤1, 0≤c≤1, 0≤d≤1, 0<e≤1.2, at least one of a, b, and c is not 0, and M includes at least one of Mg, Al, Ti, Zr, Nb, W, V, Zn, Sc, Y, Mo, In, Sb, Ta, Cr, and La;
[0040] The additives include metal oxides and thermally conductive materials, the thermally conductive materials including at least one of silicon carbide (SiC), silicon nitride, aluminum nitride (AlN), boron nitride, titanium nitride, titanium carbide and beryllium oxide (BeO);
[0041] The Dv50 of metal oxides is less than that of cathode materials, and the Dv50 of metal oxides is less than that of thermally conductive materials.
[0042] In this application, the positive electrode current collector can be aluminum foil, aluminum alloy foil, or an aluminum-based current collector with a conductive surface treatment. The thickness is exemplarily 8 μm to 20 μm. The positive electrode active layer is formed on one or both sides of the positive electrode current collector. In addition to the positive electrode material and additives, the positive electrode active layer may also contain a conductive agent and a binder. The conductive agent can be one or more of conductive carbon black, conductive graphite, carbon nanotubes, or graphene. The binder can be polyvinylidene fluoride, acrylic binders, or a styrene-butadiene rubber / carboxymethyl cellulose composite system. The positive electrode material uses Li... e Ni a Co b Mn c M d In the O2 layered oxide system, e represents the lithium content, and a, b, c, and d represent the molar coefficients corresponding to Ni, Co, Mn, and the dopant element M, respectively. M is a stabilizing element that enters the crystal lattice or is distributed in the near-surface region. Controlling e to be greater than 0 and not higher than 1.2 can cover stoichiometry and mildly lithium-rich designs. At least one of a, b, and c is not 0, indicating that the cathode material contains at least one of the main transition metal components of nickel, cobalt, and manganese, thereby maintaining the layered oxide as the electrochemical reaction framework for lithium storage. For example, the cathode material can be a cobalt-based or nickel-cobalt-manganese-based layered oxide conforming to the above general formula, or the dopant element can be introduced to form a doped layered cathode material. By partially replacing transition metal sites or forming a stabilizing structure on the surface, the dopant element can reduce the lattice oxygen activity under high delithiation conditions, suppress cation mixing and the tendency of layered structure collapse, and make the cathode material have higher structural retention under high voltage, high temperature, or overcharge conditions.
[0043] The additive in this application is composed of a metal oxide and a thermally conductive material. The metal oxide can be any metal oxide applicable in the art, and the thermally conductive material can be one or more of aluminum nitride, silicon carbide, silicon nitride, boron nitride, titanium nitride, titanium carbide, or beryllium oxide. Further, the Dv50 of the metal oxide is defined as being smaller than the Dmin of the cathode material, and the Dv50 of the metal oxide is smaller than the Dv50 of the thermally conductive material. Here, Dv50 represents the median particle size distribution, which can be in micrometers, meaning that the particle size of 50% of the volume of the sample is not greater than this value; Dmin represents the smallest particle size in the cathode material particle group, which can be obtained by laser particle size analyzer, image particle size analysis, or sieving combined with microscopic measurement. By controlling the Dv50 of the metal oxide to be smaller than the Dmin of the cathode material, fine-particle-size metal oxides can preferentially enter the spaces between cathode material particles, near the particle surface, and in the microporous region inside the cathode active layer, forming a more continuous interface distribution after drying and compaction. It can achieve local isolation of the area where the surface of the positive electrode material is in direct contact with the electrolyte, and adsorb, buffer, or block acidic or active byproducts formed during electrolyte decomposition. If the particle size of the metal oxide is too large, it is difficult to enter the interparticle gaps and exists only as isolated particles, weakening the interfacial protection effect and potentially disrupting compaction and stacking; if the particle size is too small and the surface energy is too high, agglomeration is likely to occur.
[0044] Furthermore, the Dv50 of the thermally conductive material is set to be larger than that of the metal oxide, so that it does not compete with the fine-particle metal oxide for surface coverage in the positive electrode active layer, but is instead distributed more in larger channels, particle contact gaps, or the bulk region of the active layer. Through this particle size division, the thermally conductive material can construct continuous or semi-continuous thermal diffusion paths, allowing local heat release to be dissipated within the plane and thickness direction of the active layer. Since the thermally conductive material performs the function of heat conduction rather than surface sealing, its particle size is appropriately larger than that of the metal oxide, which can reduce the excessive occupation of the effective reaction area and ion transport pores on the surface of the active particles. In the resulting multi-scale structure, the fine-particle metal oxide is responsible for interface barrier, while the larger particles or sheet-like thermally conductive material is responsible for heat diffusion. The two work synergistically with the doped layered positive electrode material, so that the improvement in safety does not depend on a single material to perform all functions, thus enabling the electrode to maintain a relatively stable interface and thermal field distribution under high pressure and high temperature environments.
[0045] The positive electrode sheet in this application can be prepared by mixing positive electrode material, metal oxide, thermally conductive material, conductive agent, and binder in a solvent to form a positive electrode slurry, which is then coated onto at least one side of the positive electrode current collector. After drying and rolling, a positive electrode sheet including a positive electrode active layer is obtained. To better achieve spatial division of labor corresponding to particle size distribution, in one possible embodiment, the metal oxide and positive electrode material can be premixed or wet-dispersed first, so that the metal oxide is preferentially adsorbed on the surface of the positive electrode material particles and near the gaps, and then the thermally conductive material, conductive agent, and binder are added. In another possible embodiment, the metal oxide and thermally conductive material can be pre-dispersed separately before being incorporated into the main slurry, thereby reducing heterogeneous agglomeration between powders with different surface properties. Slurry mixing can be carried out using a combination of high-speed dispersion, planetary stirring, wet ball milling, or vacuum degassing processes to control slurry viscosity, particle dispersion uniformity, and bubble content. During the drying process, a gradient heating method can be used to make solvent migration more gradual and reduce the tendency of fine particles to concentrate to the surface or coarse particles to settle. Through the above process control, metal oxides can be more stably distributed on the surface of active particles and in the microporous region, and thermally conductive materials are more likely to maintain a continuous or dispersed heat conduction path, so that the particle size distribution relationship in the design can still be reflected after the sheet is formed.
[0046] In the positive electrode of this application, Li e Ni a Co b Mn c M d The O2 cathode material first provides a lithium storage host with high structural stability. Smaller metal oxides enter and occupy a finer interface region around the cathode material, reducing the direct contact intensity between the active surface and the electrolyte during charging and discharging, especially under high voltage conditions, and buffering the interfacial side reaction products. Larger thermally conductive materials are dispersed in the bulk phase of the cathode active layer to form a thermal diffusion framework. When local areas release heat due to side reactions, polarization, or structural evolution, the heat can be dissipated to the surrounding areas along the thermally conductive material and particle contact network. Through the synergistic principle of interfacial barrier and thermal conduction, the formation rate of local hot spots is suppressed, the degree of heat accumulation is reduced, and the tendency of the cathode material to further release active components under heating conditions is weakened, thus delaying the thermal runaway evolution chain. At the same time, the limitation that the Dv50 of the metal oxide is smaller than that of the cathode material and smaller than that of the thermally conductive material prevents the two types of additives from functionally overlapping on the same spatial scale, reducing pore damage and transport blockage caused by the filling of a single large particle or the agglomeration of a single ultrafine particle, thereby maintaining good integrity of the compacted structure, ion diffusion channels, and electron conduction network.
[0047] Therefore, this application establishes a composite system with interface stability, thermal diffusion, and structural support within the same positive electrode active layer through the synergistic matching of doped positive electrode materials, fine-particle-size metal oxides, and larger-particle-size thermally conductive materials. Consequently, under high temperature, high pressure, or overcharge conditions, the degree of side reactions on the surface of the positive electrode material is reduced, the local temperature rise distribution within the electrode is more uniform, and the ability of the positive electrode active layer structure to maintain its structure during cycling is enhanced, thus reducing interference with capacity utilization, rate performance, and cycle stability during safety improvement. It should be understood that the above examples are merely illustrative and not limiting; the types of metal oxides, thermally conductive materials, dopant element combinations, and feeding sequences can all be adjusted without departing from the core concept of this application.
[0048] In this application, by employing a layered oxide cathode material containing specific doped elements and introducing metal oxides and thermally conductive materials that satisfy the particle size distribution relationship in the cathode active layer, the fine-particle-size metal oxides preferentially perform the interface barrier function, and the larger-particle-size thermally conductive materials preferentially perform the thermal diffusion function. Combined with the structural stabilization design of the cathode material body, a multi-scale synergistic structure is formed, thereby enabling the cathode sheet to achieve a more stable balance between safety, thermal management capability and electrochemical performance.
[0049] For example, 'a' can be any of 0, 0.1, 0.3, 0.5, 0.8, 1, or a range consisting of any two of them;
[0050] b can be any one of 0, 0.2, 0.4, 0.5, 0.7, 1, or any two of them;
[0051] c can be any of 0, 0.1, 0.3, 0.5, 0.8, 1, or any combination of two of them;
[0052] d can be any one of 0, 0.1, 0.3, 0.5, 0.8, 1, or any combination of two of them;
[0053] e can be any one of 0.1, 0.3, 0.6, 0.9, 1.0, 1.2 or any combination of two of them.
[0054] In some embodiments of this application, when the thermal conductivity of the thermally conductive material is >25 W / (m·K), it is possible to form a sufficiently defined thermal diffusion capability in the pores and particle contact area of the positive electrode sheet.
[0055] For example, the thermal conductivity can be in the range of any one or any two of 30 W / (m·K), 45 W / (m·K), 60 W / (m·K), 80 W / (m·K), 100 W / (m·K), and 150 W / (m·K). Further, the thermally conductive material includes at least one of AlN, SiC, and BeO.
[0056] In some embodiments of this application, the metal oxide includes at least one selected from titanium dioxide (TiO2), barium titanate (BaTiO3), barium strontium titanate, aluminum oxide, magnesium oxide, zinc oxide, zirconium dioxide, tungsten trioxide, copper oxide, molybdenum trioxide, barium oxide, tantalum pentoxide, niobium pentoxide, cobalt oxide, and nickel oxide (NiO). These metal oxides provide interfacial barrier and thermal stabilization functions. By preferentially distributing themselves in the interparticle gaps and surface regions of the cathode material, they reduce the direct contact between the electrolyte and the cathode material, and adsorb or passivate byproducts, thereby weakening interfacial side reactions under high voltage, high temperature, or overcharge conditions. Further, the metal oxide includes at least one selected from titanium dioxide (TiO2), barium titanate (BaTiO3), and nickel oxide (NiO). In some embodiments, the surface of the metal oxide can also be carbon-coated to further improve its conductivity. The carbon coating amount in the metal oxide can be 0.5-5 wt%, preferably 0.5-1.5 wt%. In some embodiments, the conductivity of the metal oxide is >10. -3 S / cm.
[0057] In some embodiments of this application, the presence of metal oxides and thermally conductive materials in the positive electrode active layer can be tested using SEM-EDS, and the Dv50 of the thermally conductive material and the Dv50 of the metal oxide in the positive electrode material can be determined. Specifically, the positive electrode active layer is scanned using EDS, and the metal oxides and thermally conductive materials are distinguished by elemental analysis. Then, the dimensions of the thermally conductive material and the metal oxide are marked using calipers in conjunction with SEM, thus obtaining the corresponding particle size. In some embodiments, the positive electrode active layer powder can be sintered at 500°C for 5 hours, and then the particle size distribution of the powder can be tested using a Malvern 5000 instrument to obtain the Dmin of the positive electrode material.
[0058] In some embodiments of this application, the additive accounts for 0.3%-5% of the mass of the cathode material. This allows for an effective distribution of the metal oxide and thermally conductive material within the electrode, while avoiding excessive addition that could lead to decreased compaction density, damaged pore structure, and weakened electron transport pathways. Within this range, lower addition amounts can amplify interfacial barrier and thermal conduction effects through high dispersion processes and particle size matching, while higher addition amounts prevent excessive dilution of the active material by limiting the total amount, thus balancing safety and capacity retention.
[0059] For example, the percentage of the additive in the mass of the cathode material can be any of 0.3%, 1%, 2%, 3.5%, 5%, or any combination thereof.
[0060] In some embodiments of this application, the mass ratio of metal oxide to thermally conductive material is (2-8):(2-8). The two can form a synergistic network on the surface of the positive electrode material and in the gaps between particles, so that the metal oxide preferentially undertakes the role of isolating electrolyte decomposition products and inhibiting side reactions, while the thermally conductive material is responsible for rapidly dissipating local heat.
[0061] For example, the mass ratio of metal oxide to thermally conductive material can be any of 2:8, 3:7, 5:5, 7:3, 8:2, or any combination thereof.
[0062] By optimizing the ratio to (4-6):(4-6), the interface barrier and thermal diffusion capacity can be further balanced, avoiding functional bias caused by excessive amounts of a certain component. This allows for more effective suppression of hot spot formation and reduction of thermal runaway risk under high voltage, high temperature, or overcharge conditions.
[0063] This application achieves precise control over the microstructure of the positive electrode active layer at limited addition levels, enabling the additive to cover key reaction interfaces within the active layer without significantly compromising its density and conductive continuity. Because the ratio of metal oxide to thermally conductive material is controlled within a synergistic range, the positive electrode maintains good rate performance and cycle stability while improving thermal safety, thus ensuring its applicability and safety in power batteries, energy storage batteries, and consumer electronics batteries.
[0064] Furthermore, the ratio of Dmin of the cathode material to Dv50 of the metal oxide is 2-40, which ensures that the particle size of the metal oxide is significantly smaller than the minimum particle size of the cathode material. This makes it easier for the metal oxide to enter the particle packing voids and stably adhere to the particle surface during the coating and compaction process, thus improving the isolation effect and avoiding insufficient surface coverage caused by excessively large particle size. For example, the ratio of Dmin of the cathode material to Dv50 of the metal oxide can be any of 2, 5, 15, 30, 40, or any combination thereof.
[0065] Furthermore, when the ratio of Dmin of the cathode material to Dv50 of the thermally conductive material is 1.5-8, the particle size of the thermally conductive material is relatively larger, making it more suitable for constructing heat conduction pathways in the pores inside the cathode active layer without excessively occupying the active sites on the cathode material surface. This achieves a division of labor and synergy between rapid heat diffusion and active interface protection. For example, the ratio of Dmin of the cathode material to Dv50 of the thermally conductive material can be any of 1.5, 4, 6, 8, or a range of any two of them.
[0066] When the above ratios are satisfied simultaneously, fine-grained metal oxides are responsible for interfacial barrier, while coarse-grained thermally conductive materials are responsible for heat dissipation. The two form a multi-scale distribution structure inside the positive electrode active layer, thereby reducing the side reaction rate and local temperature rise under high temperature, overcharge, or abuse conditions, thus ensuring a balance between electrode structure stability, thermal safety, and electrochemical performance.
[0067] In some embodiments of this application, the Dv50 of the metal oxide is 0.1 μm-0.5 μm, which allows the metal oxide to preferentially enter the interparticle spaces, surface defects, and pore wall regions of the cathode material in a finer particle form, thereby enhancing the coverage and isolation of electrolyte decomposition products and side reaction active sites. Exemplarily, the Dv50 of the metal oxide can be any of 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, or a combination of any two thereof.
[0068] In some embodiments of this application, the Dv50 of the thermally conductive material is 0.5 μm-1.5 μm, making its particle size larger than that of the metal oxide and forming a suitable gradation with the active material particles. This facilitates the construction of continuous or semi-continuous thermal conductive pathways within the positive electrode active layer, while avoiding excessive occupation of the positive electrode material surface and reduction of the active contact area. Exemplarily, the Dv50 of the thermally conductive material can be any of 0.5 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.5 μm, or a combination of any two of these ranges.
[0069] In some embodiments of this application, when the Dmin of the cathode material is 1μm-4μm, it can form a stable particle size gradient with the aforementioned two types of additives, thereby providing attachment and embedding space for the metal oxide and providing a structural basis for the distribution of the thermally conductive material in the pores. Exemplarily, the Dmin of the cathode material can be any of 1μm, 1.5μm, 2μm, 3μm, 4μm, or any combination thereof.
[0070] Once the positive electrode active layer forms a graded particle structure, fine metal oxides first fill the weak interfacial regions, inhibiting direct contact between the electrolyte and the highly active positive electrode surface. Larger-diameter thermally conductive materials are dispersed between the particles, playing a role in rapid heat diffusion and reducing localized hotspots. By controlling the particle size relationship between the metal oxides, thermally conductive materials, and positive electrode materials, interfacial barrier and thermal conduction can be achieved simultaneously, reducing pore structure collapse, increased internal resistance, and rate performance degradation caused by particle size mismatch. This enhances the interfacial stability and thermal safety between the positive electrode and the electrolyte while ensuring electrode compaction density and the integrity of electron and / or ion transport channels. This reduces the side reaction rate and thermal runaway risk under high voltage, overcharge, or high temperature conditions, thereby improving the battery's cycle life, rate performance, and overall safety and reliability.
[0071] In some embodiments of this application, the cathode material further includes materials located in Li e Ni a Co b Mn c M d For O2 particles that are at least partially coated on the surface, the Dv50 of the metal oxide is greater than that of the coated particles.
[0072] Li e Ni a Co b Mn c M d The surface of the O2 cathode material is further coated with particles to construct a nanoscale interfacial protective layer on the outer layer of the cathode material particles. The coated particles are located on at least part of the surface, preferentially covering active sites that are easily in contact with the electrolyte, thereby reducing surface side reactions and transition metal dissolution under high voltage. The Dv50 of the metal oxide is greater than that of the coated particles, allowing smaller-diameter coated particles to form a dense or semi-dense coating layer first, while larger-diameter metal oxide particles are mainly distributed on the outer side of the coating layer or in the interparticle gaps, forming a hierarchical structure from the inside out, thus achieving both interfacial passivation and spatial isolation.
[0073] Furthermore, the coated particles include at least one of lithium aluminum substituted phosphate metal salts, aluminum oxide, magnesium oxide, titanium dioxide, zirconium dioxide, lanthanum oxide, yttrium oxide, and boron oxide. These inorganic particles possess good chemical inertness, thermal stability, or acid-base regulation capabilities, which can inhibit electrolyte decomposition and slow down the release of lattice oxygen from the surface of the cathode material. Among these, lithium aluminum substituted phosphate metal salts can form a stable protective phase, aluminum oxide, magnesium oxide, titanium dioxide, and zirconium dioxide can enhance interfacial heat resistance, and lanthanum oxide, yttrium oxide, and boron oxide can further improve the surface chemical environment. In some embodiments, the molecules of the lithium aluminum substituted phosphate metal salt can be Li... 1+X Al X M' 2-X (PO4)3, 0≤X≤1, wherein M' includes at least one of Ti, Li, Si, Ge, Zr and V.
[0074] Furthermore, the Dv50 of the coated particles is 10-50 nm, which allows the coated particles to be more uniformly spread on the surface of the cathode material, reducing local exposed areas and preventing excessively large particles from damaging the electrode pore structure or electron transport channels. For example, the Dv50 of the coated particles can be any of 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, or any combination thereof.
[0075] In this application, nano-coated particles first chemically passivate and physically isolate the surface of the cathode material, reducing direct electrolyte erosion. Simultaneously, in synergy with larger-diameter metal oxide particles, they further inhibit the diffusion of heat and side reactions between particles. This achieves a balance between interfacial stability, thermal stability, and structural integrity, enabling the cathode material to maintain a low side reaction rate and good cycle stability even under high voltage, high temperature, or overcharge conditions. This improves the safety of the cathode sheet and minimizes adverse effects on rate performance and compaction density.
[0076] In some embodiments of this application, SEM or TEM can be used to determine whether the surface of the cathode material has coated particles, and simultaneously confirm the particle size of the coated particles. In some embodiments, SEM can be used to image the cathode active layer, magnifying individual cathode material particles to 10k or 20k, adjusting the magnification according to the actual particle size. For smaller particles, the magnification can be increased to identify surface protrusions. The size of the protrusions can be marked using calipers, thus obtaining the particle size of the coated particles.
[0077] In some embodiments of this application, when the metal oxide includes alumina, and / or the coating particles include alumina, and / or the thermally conductive material includes aluminum nitride, the mass content of Al in the positive electrode active layer can be 500ppm-40000ppm; and / or, when the metal oxide includes at least one of titanium dioxide, barium titanate, and barium strontium titanate, the mass content of Ti in the positive electrode active layer can be 50ppm-80000ppm; and / or, when the metal oxide includes barium strontium titanate, the mass content of Sr in the positive electrode active layer can be 300ppm-4000ppm; and / or, when the metal oxide includes barium strontium titanate and / or barium oxide, the mass content of Ba in the positive electrode active layer can be 100ppm-2500ppm; and / or, when the metal oxide includes magnesium oxide, the mass content of Mg in the positive electrode active layer can be 500ppm-3000ppm; and / or, when the metal oxide includes zinc oxide, the mass content of Zn in the positive electrode active layer can be 300ppm-4000ppm. And / or, when the metal oxide includes zirconium dioxide, the Zr content in the positive electrode active layer can be 300ppm-4000ppm; and / or, when the metal oxide includes tungsten trioxide, the W content in the positive electrode active layer can be 600ppm-20000ppm; and / or, when the metal oxide includes copper oxide, the Cu content in the positive electrode active layer can be 300ppm-4000ppm; and / or, when the metal oxide includes molybdenum trioxide, the Mo content in the positive electrode active layer can be 300ppm-4000ppm; and / or, when the metal oxide includes tantalum pentoxide, the Ta content in the positive electrode active layer can be 600ppm-8000ppm; and / or, when the metal oxide includes niobium pentoxide, the Nb content in the positive electrode active layer can be 300ppm-3500ppm; and / or, when the thermally conductive material includes silicon carbide and / or silicon nitride, the Si content in the positive electrode active layer can be 300ppm-4000ppm.
[0078] Among these, when the Al content is between 500 ppm and 40000 ppm, it can enhance the lattice stability of the layered cathode material, reduce structural collapse and surface reconstruction under high lithium delithiation state, and thus suppress side reactions. When the Ti content is between 50 ppm and 80000 ppm, it can improve the framework strength by stabilizing MO bonds and reduce oxygen evolution at high temperatures. Sr and Ba can induce local lattice buffering through their larger ionic radii, Mg and Zn can improve charge compensation and interfacial acidity, Zr, W, Ta, and Nb can help improve thermal stability and resistance to phase transitions, and Cu, Mo, and Si can improve surface chemical stability and ion transport continuity, thereby reducing the rise in interfacial impedance. The lower limit of each element ensures that its stabilizing effect can be fully realized, while the upper limit avoids lattice distortion, phase separation, or capacity loss caused by excessive doping. Therefore, it is preferable to achieve a performance balance without destroying the main structure.
[0079] After these elements are incorporated into the cathode material through bulk solid solution, surface enrichment, or gradient distribution, they can jointly suppress oxygen release, reduce electrolyte erosion, and decrease surface acidity under conditions of delithiation, thermal shock, and high voltage, thereby stabilizing the cathode / electrolyte interface. This achieves a synergistic improvement in the structural stability, interface stability, and thermal stability of the cathode active layer. When the cathode active layer is combined with metal oxides and thermally conductive materials, it can maintain low side reaction activity and good electron and ion transport channels, thereby improving cycle life, rate performance, and safety, and mitigating the risk of thermal runaway under high temperature, overcharge, and abuse conditions.
[0080] For example, in the positive electrode active layer, the mass content of Al can be any one or a combination of any two of the following: 500 ppm, 5000 ppm, 6000 ppm, 8000 ppm, 9000 ppm, 10000 ppm, 15000 ppm, 40000 ppm; the mass content of Ti can be any one or a combination of any two of the following: 50 ppm, 300 ppm, 600 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 8000 ppm, 80000 ppm; and the mass content of Sr can be 300 ppm, 800 ppm, 1500 ppm, 2500 ppm, ... The mass content of Ba can be any of the following ranges, or any two of them: 100 ppm, 200 ppm, 500 ppm, 1000 ppm, 1800 ppm, 2500 ppm; the mass content of Mg can be any of the following ranges, or any two of them: 500 ppm, 1000 ppm, 1500 ppm, 2200 ppm, 3000 ppm; the mass content of Zn can be any of the following ranges, or any two of them: 300 ppm, 800 ppm, 1600 ppm, 2800 ppm, 4000 ppm; the mass content of Zr... The amount can be any one of 300ppm, 700ppm, 1400ppm, 2600ppm, 4000ppm, or any combination thereof; the mass content of W can be any one of 600ppm, 1500ppm, 3000ppm, 5500ppm, 8000ppm, 20000ppm, or any combination thereof; the mass content of Cu can be any one of 300ppm, 900ppm, 1700ppm, 2900ppm, 4000ppm, or any combination thereof; the mass content of Mo can be 300ppm, 850ppm, 1800ppm, 3100ppm, 4000ppm, or any combination thereof. The mass content of Ta can be any of 0 ppm, 4000 ppm, or any two of them; the mass content of Nb can be any of 300 ppm, 750 ppm, 1400 ppm, 2400 ppm, 3500 ppm, or any two of them; the mass content of Si can be any of 300 ppm, 800 ppm, 1300 ppm, 2100 ppm, 3000 ppm, 4000 ppm, or any two of them.
[0081] In some implementations, the content of each element in the positive electrode active layer can be tested by ICP-MS.
[0082] In some embodiments of this application, the exothermic peak temperature of the differential scanning calorimetry (DSC) curve of the positive electrode is ≥235°C, indicating that the positive electrode requires a higher temperature for the main exothermic reaction under heating conditions, demonstrating improved thermal stability and effectively delaying thermal runaway evolution under high voltage, overcharge, or abuse conditions. This process achieves a synergistic effect of interface suppression, thermal diffusion, and structural stability, thereby ensuring that the positive electrode maintains its electrochemical performance as much as possible while improving safety. For example, the exothermic peak temperature of the DSC curve of the positive electrode can be any one of 235°C, 255°C, 270°C, 290°C, or 310°C, or a range of any two thereof.
[0083] In some embodiments of this application, the resistivity of the positive electrode is 0.5 kΩ·cm to 4 kΩ·cm, which allows the positive electrode to maintain acceptable electron transport capacity after the introduction of metal oxides and thermally conductive materials, avoiding a significant increase in internal resistance due to excessive additives, uneven dispersion, or channel blockage. When the resistivity is close to 0.5 kΩ·cm, it indicates that the conductive network of the positive electrode is more unobstructed, suitable for higher charge-discharge rates; when the resistivity is close to 4 kΩ·cm, it indicates that the internal resistance of the positive electrode has increased slightly but is still within the usable window, providing stronger interface inhibition. The resistivity can be measured by the four-probe method or other conventional testing methods, and can be synergistically controlled by combining the proportion of conductive agent, additive particle size distribution, slurry dispersion state, and electrode compaction density. Exemplarily, the resistivity of the positive electrode can be any of 0.5 kΩ·cm, 1 kΩ·cm, 2 kΩ·cm, 3 kΩ·cm, 4 kΩ·cm, or any combination thereof.
[0084] By limiting the parameters mentioned above, this positive electrode can simultaneously suppress side reactions, mitigate local temperature rise, and maintain basic conductivity under high voltage, high temperature, or overcharge conditions, thereby reducing the risk of thermal runaway and ensuring compatibility between safety enhancement and electrochemical performance. This process integrates interface barrier and thermal diffusion functions into the same positive electrode structure, enabling the electrode to maintain good rate performance and cycle stability while enhancing safety.
[0085] This application also provides a battery including the above-described positive electrode.
[0086] With the aforementioned positive electrode, the metal oxide and thermally conductive material in the positive electrode active layer of this battery can work synergistically within the same electrode structure. The metal oxide can be distributed between the particles and on the surface of the positive electrode material, forming a more effective barrier at the interface between the active material and the electrolyte, thereby reducing the degree of side reactions under high voltage, high temperature, or overcharge conditions. The thermally conductive material facilitates the timely dissipation of heat within the active layer, making it less likely for local hot spots to form, thus suppressing heat accumulation and thermal runaway. Therefore, this battery improves thermal safety while also ensuring electrode structure stability, cycle performance, and rate performance, making it more suitable for applications such as power, energy storage, and consumer electronics where both safety and energy density are required.
[0087] In some embodiments, the electrolyte in the battery may include ethoxy(pentafluoro)cyclotriphosphazene, and the content of ethoxy(pentafluoro)cyclotriphosphazene in the electrolyte may be 5-20 wt%.
[0088] The solution of this application will be further described below with reference to specific embodiments.
[0089] Example 1
[0090] The battery in this embodiment is prepared by a method including the following steps:
[0091] 1) Preparation of positive electrode sheet
[0092] Lithium cobalt oxide (LiCoO2), TiO2, AlN, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone in a mass ratio of 97.2:0.5:0.5:1.0:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. The positive electrode slurry was coated on both sides of a 9 μm thick aluminum foil and dried to obtain a positive electrode sheet including a positive electrode active layer.
[0093] The lithium cobalt oxide has coated particles on its surface, including Y2O3.
[0094] 2) Preparation of negative electrode sheet
[0095] The negative electrode material (graphite and silicon carbide in a mass ratio of 9:1), conductive carbon black, and polyacrylic acid are mixed with water in a mass ratio of 97.2:1.45:1.35. The mixture is stirred to obtain a negative electrode slurry. The negative electrode slurry is coated on both sides of a copper foil and dried to obtain a negative electrode sheet including a negative electrode active layer.
[0096] 3) Battery manufacturing
[0097] After stacking positive electrode, separator and negative electrode, they are wound to form an electrode assembly. The electrode assembly is placed in an aluminum-plastic film and an electrolyte is injected into the aluminum-plastic film to obtain a lithium-ion battery.
[0098] The membrane comprises layers of PP, PE, and PP, with a thickness of 8μm and a porosity of 42%.
[0099] The electrolyte is made by dissolving 1 mol / L lithium hexafluorophosphate (LiPF6) in a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1.
[0100] Other battery parameters are shown in Table 1 and Table 2.
[0101] The preparation method of the battery in Example 2 is basically the same as that of the battery in Example 1, except that: 1) the positive electrode sheet
[0102] LiNiO2, BaTiO3, SiC, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone at a mass ratio of 97.9:0.06:0.24:1.0:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. The surface of LiNiO2 was coated with particles, including La2O3. The particle sizes of LiNiO2, BaTiO3, SiC, and La2O3 were adjusted simultaneously.
[0103] The preparation method of the battery in Example 3 is basically the same as that of the battery in Example 1, except that: 1) the positive electrode sheet
[0104] LiNi 0.8 Co 0.1 Mn 0.1 O2, WO3, BN, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone at a mass ratio of 93.2:4:1:1:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. LiNi 0.8 Co 0.1 Mn 0.1 The surface of O2 is coated with particles, including Al2O3; LiNi is simultaneously adjusted. 0.8 Co 0.1 Mn 0.1 Particle sizes of O2, WO3, BN, and Al2O3.
[0105] The preparation methods of the batteries in Examples 4-5 are basically the same as those of the battery in Example 1, except that different particle sizes of LiCoO2, TiO2 and AlN are selected to prepare the positive electrode sheets.
[0106] The preparation method of the battery in Example 6 is basically the same as that of the battery in Example 1, except that lithium cobalt oxide, TiO2, AlN, conductive carbon black, and polyvinylidene fluoride are mixed with N-methylpyrrolidone in a mass ratio of 98:0.1:0.1:1.0:0.8.
[0107] The preparation method of the battery in Example 7 is basically the same as that of the battery in Example 1, except that lithium cobalt oxide, TiO2, AlN, conductive carbon black, and polyvinylidene fluoride are mixed with N-methylpyrrolidone in a mass ratio of 92.8:2.7:2.7:1:0.8.
[0108] The preparation method of the battery in Example 8 is basically the same as that of the battery in Example 1, except that lithium cobalt oxide, TiO2, AlN, conductive carbon black, and polyvinylidene fluoride are mixed with N-methylpyrrolidone in a mass ratio of 92.8:0.1:0.9:1:0.8.
[0109] The preparation method of the battery in Example 9 is basically the same as that of the battery in Example 1, except that lithium cobalt oxide, TiO2, AlN, conductive carbon black, and polyvinylidene fluoride are mixed with N-methylpyrrolidone in a mass ratio of 92.8:0.9:0.1:1:0.8.
[0110] The preparation methods of the batteries in Examples 10-19 are basically the same as those of the battery in Example 1, except that: different particle sizes of titanium dioxide, cathode material and AlN are used respectively, and the ratio of Dmin of cathode material to Dv50 of titanium dioxide and the ratio of Dmin of cathode material to Dv50 of AlN are adjusted.
[0111] The preparation method of the battery in Example 20 is basically the same as that of the battery in Example 1, except that the surface of the positive electrode material is not coated with particles.
[0112] The preparation method of the battery in Example 21 is basically the same as that of the battery in Example 1, except that: positive electrode materials with different particle sizes of surface-coated particles are used.
[0113] Comparative Example 1
[0114] The preparation method of the battery in this comparative example is basically the same as that of the battery in Example 1, with the following differences:
[0115] 1) Preparation of positive electrode sheet
[0116] Lithium cobalt oxide, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone at a mass ratio of 98.2:1.0:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. The positive electrode slurry was coated on both sides of a 9 μm thick aluminum foil and dried to obtain a positive electrode sheet including a positive electrode active layer.
[0117] Comparative Example 2
[0118] The preparation method of the battery in this comparative example is basically the same as that of the battery in Example 1, with the following differences:
[0119] 1) Preparation of positive electrode sheet
[0120] Lithium cobalt oxide, TiO2, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone at a mass ratio of 97.2:1.0:1.0:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. The positive electrode slurry was coated on both sides of a 9 μm thick aluminum foil and dried to obtain a positive electrode sheet including a positive electrode active layer.
[0121] Comparative Example 3
[0122] The preparation method of the battery in this comparative example is basically the same as that of the battery in Example 1, with the following differences:
[0123] 1) Preparation of positive electrode sheet
[0124] Lithium cobalt oxide, AlN, conductive carbon black, and polyvinylidene fluoride were mixed with N-methylpyrrolidone at a mass ratio of 97.2:1.0:1.0:0.8. The mixture was stirred for 3 hours at a revolution speed of 30 rpm and a rotation speed of 3000 rpm to obtain a positive electrode slurry with a solid content of 75.5%. The positive electrode slurry was coated on both sides of a 9 μm thick aluminum foil and dried to obtain a positive electrode sheet including a positive electrode active layer.
[0125] The preparation methods of the batteries in Comparative Examples 4-5 are basically the same as those of the batteries in the Examples, except that different particle sizes of TiO2 and AlN are used respectively, with the two having the same particle size or the Dv50 of TiO2 being the same as the Dmin of the cathode material.
[0126] Performance testing
[0127] The positive electrode and battery of the examples and comparative examples were subjected to the following performance tests, and the results are shown in Table 1 and Table 2 respectively;
[0128] 1) SEM-EDS test
[0129] SEM-EDS tests were performed on the positive electrode sheets of the examples and comparative examples respectively, and the distribution state of each material in the positive electrode sheet was confirmed based on the SEM-EDS image of the positive electrode active layer.
[0130] Figure 1 Here is a surface SEM image of the positive electrode active layer in Example 1; Figure 2 This is a distribution diagram of Co elements on the surface of the positive electrode active layer in Example 1; Figure 3 This is a distribution diagram of C element on the surface of the positive electrode active layer in Example 1; Figure 4 This is a distribution diagram of Ti elements on the surface of the positive electrode active layer in Example 1; Figure 5 This is a distribution diagram of Al elements on the surface of the positive electrode active layer in Example 1; Figure 6 This is a cross-sectional SEM image of the positive electrode active layer in Example 1; Figure 7 This is a cross-sectional EDS image of the positive electrode active layer in Example 1; Figure 8 The image shows the distribution of Ti elements in the cross-section of the positive electrode active layer in Example 1. Figure 9 This is a cross-sectional SEM image of the positive electrode active layer of Comparative Example 3; Figure 10 This is a cross-sectional EDS image of the positive electrode active layer in Comparative Example 3. From... Figure 1-5 It can be seen that Ti and Al are uniformly distributed on the surface of the positive electrode active layer, because the lithium cobalt oxide material includes Al and Ti.
[0131] from Figure 6-10 It can be seen that, compared with Comparative Example 3, the cross-section of the positive electrode active layer in this application embodiment contains Ti element, corresponding to titanium dioxide, and from... Figure 7-8 It can be seen that in the cross-section of the positive electrode active layer, Ti is distributed in the pores between the positive electrode material particles, indicating that titanium dioxide is distributed around the positive electrode material; from Figure 7 and Figure 10 It can be seen that Al in Example 1 and Comparative Example 3 is not only distributed in the cathode material particles, but also in the gaps between the cathode material particles, indicating that the cathode material contains Al, and AlN is distributed around the cathode material.
[0132] Figure 7 Silicon is present in it. Figure 10 The reason why silicon is not present in the sample is that a silicon wafer is used as the sample support substrate during the test. If the positive electrode in some samples completely covers the support substrate, there will be no silicon signal. If it is not completely covered, there will be a silicon signal. Figure 10 The presence of fluorine is due to the presence of F in the binder. Because the F content in the positive electrode active layer is relatively low, the detection signal is weak. Some locally enriched areas in the positive electrode active layer may be detected, while some positive electrode sheets may not show any detectable fluorine. Figure 7 Not detected).
[0133] 2) Differential Scan Measurement (DCS) Test
[0134] After the batteries of the examples and comparative examples were fully charged, they were disassembled to obtain the positive electrode sheet. DCS tests were performed on the positive electrode sheet to obtain the DCS curve of the positive electrode sheet. The thermal decomposition temperature of the positive electrode sheet was obtained based on the DCS curve of the positive electrode sheet. Figure 11 This is a differential scanning calorimetry (DSC) curve of the positive electrode of Example 1 and Comparative Example 1. From... Figure 11 It can be seen that after the positive electrode of Example 1 is charged to 100% SOC, its peak temperature (representing thermal runaway temperature) and initial temperature are both higher than those of Comparative Example 1, and its peak area (representing heat generation) is smaller than that of Comparative Example 1, indicating that the thermal stability of the positive electrode prepared in Example 1 is significantly increased.
[0135] 3) Capacity testing
[0136] After letting the battery rest for 5 minutes, charge it to 4.53V at 0.5C with constant current and constant voltage, with a cutoff current of 0.025C. After letting it rest for 5 minutes, discharge it to 3V at 0.2C with constant current, and record the capacity Q1 at this point.
[0137] 4) 45℃ Cyclic Performance Test
[0138] Place the battery in an environment of (45±2)℃ and let it stand for 10 minutes. Charge the battery at a constant current and constant voltage of 1.2C to 4.53V, with a cutoff current of 0.05C. After the battery is fully charged, let it rest for 5 minutes, and then discharge it at a constant current of 0.5C to a cutoff voltage of 3.0V. Record the highest discharge capacity of the first 3 cycles as the initial capacity Q4. When the number of cycles reaches 600, record the discharge capacity Q5 of the last cycle. Cycle retention rate = Q5 / Q4*100%.
[0139] 5) Hot box test
[0140] ① Let stand for 10 minutes; ② Discharge at 0.2C to the lower limit voltage, let stand for 10 minutes; ③ Charge at 0.5C to the upper limit voltage, cut off at 0.05C, let stand for 10 minutes; ④ Place in a thermal shock test chamber and adjust to the corresponding temperature, raise the temperature to the set temperature at a rate of 5℃±2℃ / min, and maintain for 60 minutes, monitoring the voltage and body temperature rise. If the cell shows no smoke, no leakage, no explosion, and no fire after the test, it has passed the thermal shock test at that temperature.
[0141] Table 1
[0142]
[0143] In Table 1, A represents the percentage of the additive's mass in the cathode material's mass; B represents the mass ratio of the metal oxide to the thermally conductive material; C represents the ratio of the cathode material's Dmin to the metal oxide's Dv50; and D represents the ratio of the cathode material's Dmin to the thermally conductive material's Dv50.
[0144] Table 2
[0145]
[0146] As can be seen from Tables 1 and 2, when the positive electrode sheet of this application is applied to a battery, it can improve the battery's discharge capacity, high-temperature cycle performance, and thermal box temperature. This indicates that by adding metal oxides and thermally conductive materials to the positive electrode active layer and matching the particle sizes of the metal oxides, positive electrode materials, and thermally conductive materials, this application can improve the thermal conductivity and stability of the positive electrode sheet with almost no loss of its capacity, thereby improving the battery's high-temperature cycle performance and safety performance.
[0147] Furthermore, as can be seen from Examples 1 and 6-21, by further selecting the amount and particle size of the metal oxide, thermally conductive material, and cathode material, as well as the type of cathode material, the high-temperature cycle performance and safety performance of the battery can be further improved, resulting in a battery with superior capacity, high-temperature cycle performance, and safety performance.
[0148] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.
Claims
1. A positive electrode plate, characterized in that, The positive electrode sheet includes a positive current collector and a positive active layer located on at least one side of the surface of the positive current collector, the positive active layer including additives and positive electrode material; The cathode material includes Li e Ni a Co b Mn c M d O2, wherein 0≤a≤1, 0≤b≤1, 0≤c≤1, 0≤d≤1, 0<e≤1.2, at least one of a, b, and c is not 0, and M includes at least one of Mg, Al, Ti, Zr, Nb, W, V, Zn, Sc, Y, Mo, In, Sb, Ta, Cr, and La; The additives include metal oxides and thermally conductive materials, wherein the thermally conductive materials include at least one of silicon carbide, silicon nitride, aluminum nitride, boron nitride, titanium nitride, titanium carbide, and beryllium oxide; The Dv50 of the metal oxide is less than the Dmin of the positive electrode material, and the Dv50 of the metal oxide is less than the Dv50 of the thermally conductive material.
2. The positive electrode sheet according to claim 1, characterized in that, The thermal conductivity of the thermally conductive material is >25 W / (m·K); And / or, the metal oxide includes at least one of titanium dioxide, barium titanate, barium strontium titanate, aluminum oxide, magnesium oxide, zinc oxide, zirconium dioxide, tungsten trioxide, copper oxide, molybdenum trioxide, barium oxide, tantalum pentoxide, niobium pentoxide, cobalt oxide, and nickel oxide.
3. The positive electrode sheet according to claim 2, characterized in that, The mass percentage of the additive in the mass of the cathode material is 0.3%-5%.
4. The positive electrode sheet according to any one of claims 1-3, characterized in that, The mass ratio of the metal oxide to the thermally conductive material is (2-8):(2-8); preferably, the mass ratio of the metal oxide to the thermally conductive material is (4-6):(4-6).
5. The positive electrode sheet according to any one of claims 1-4, characterized in that, The ratio of Dmin of the cathode material to Dv50 of the metal oxide is 2-40; And / or, the ratio of Dmin of the positive electrode material to Dv50 of the thermally conductive material is 1.5-8.
6. The positive electrode sheet according to claim 5, characterized in that, The Dv50 of the metal oxide is 0.1 μm-0.5 μm; and / or the Dv50 of the thermally conductive material is 0.5 μm-1.5 μm; and / or the Dmin of the positive electrode material is 1 μm-4 μm.
7. The positive electrode sheet according to any one of claims 1-6, characterized in that, The positive electrode material also includes the Li e Ni a Co b Mn c M d The particles coating at least part of the surface of O2, wherein the Dv50 of the metal oxide is greater than the Dv50 of the coating particles; Preferably, the coated particles include at least one of aluminum oxide, magnesium oxide, titanium dioxide, zirconium dioxide, lanthanum oxide, yttrium oxide, and boron oxide; and / or, the Dv50 of the coated particles is 10-50 nm.
8. The positive electrode sheet according to any one of claims 1-7, characterized in that, The peak temperature of the exothermic curve of the positive electrode is ≥235℃.
9. The positive electrode sheet according to any one of claims 1-8, characterized in that, The resistivity of the positive electrode is 0.5 kΩ·cm - 4 kΩ·cm.
10. A battery, characterized in that, Includes the positive electrode sheet as described in any one of claims 1-9.