Negative electrode, battery and electrical device
By introducing porous carbon materials and lithiophilic substances into the negative electrode material layer of lithium-ion batteries and controlling their content ratio, the problem of simultaneously improving the energy density and cycle life of lithium-ion batteries was solved. This achieved uniform lithium deposition and improved adhesion, thereby improving the safety and stability of the battery.
Patent Information
- Application Number
- CN202611223710.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion batteries are facing technical bottlenecks in simultaneously improving energy density and cycle life. The problem of lithium dendrite growth seriously affects battery safety and cycle stability.
Porous carbon materials and lithiophilic substances are introduced into the negative electrode material layer. By controlling the mass percentage of lithiophilic substances and element M within a suitable range, lithium is induced to deposit uniformly, reducing surface enrichment and improving conductivity and adhesion.
It improves the energy density and cycle life of the battery, reduces the risk of lithium dendrite growth, ensures the adhesion between the negative electrode material layer and the current collector, and extends the battery's lifespan.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to negative electrode sheets, batteries and electrical devices. Background Technology
[0002] Lithium-ion batteries are batteries that primarily function by the repeated insertion and extraction of lithium ions between the positive and negative electrodes. With their comprehensive advantages, including high energy density, excellent fast-charging performance, long cycle life, good safety and stability, and environmental friendliness, they have become the mainstream energy storage and power source. However, at present, lithium-ion batteries are facing technical bottlenecks in simultaneously improving energy density and cycle life. The industry generally adopts an electrode structure design that thins the negative electrode material layer and thickens the positive electrode material layer to increase battery energy density. However, this optimization method makes it difficult to achieve uniform deposition of lithium ions during nucleation on the negative electrode surface due to factors such as local electric field distortion and electrode surface defects. This can induce lithium dendrite growth, severely restricting battery safety and cycle stability. Summary of the Invention
[0003] The purpose of this application is to overcome the shortcomings of the prior art and provide a negative electrode, a battery and an electrical device. The battery using the negative electrode of this application can simultaneously have good energy density and cycle life, balancing the dual requirements of increasing battery capacity and long cycle life.
[0004] To achieve the above objectives, in a first aspect, this application provides a negative electrode sheet, including a negative electrode material layer, the negative electrode material layer including a negative electrode material, the negative electrode material including a porous carbon material and a lithium-loving substance, wherein the porous carbon material contains element M, and element M is selected from at least one of N, B, P and S; Based on the total mass of the negative electrode material layer, the mass percentage of the lithiophilic substance is a%, and the mass percentage of element M is b%. The condition a and b satisfy: 1.5 ≤ a × b ≤ 120.
[0005] Secondly, this application provides a battery, including a positive electrode, a negative electrode, and an electrolyte.
[0006] Thirdly, this application provides an electrical device including the battery.
[0007] Compared with the prior art, the beneficial effects of this application include: by introducing porous carbon materials containing a specific element M and lithiophilic substances into the negative electrode material layer, and by comprehensively controlling the mass percentage content a% of the lithiophilic substances and the mass percentage content b% of element M in the negative electrode material layer, so that a×b is within a suitable range, the energy density and cycle life of the battery can be comprehensively improved. Detailed Implementation
[0008] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0009] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0010] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0011] In this application, there are no particular restrictions on the specific dispersion and mixing methods.
[0012] Unless otherwise specified, all reagents or instruments used in this application are commercially available products.
[0013] According to a first aspect of this application, a negative electrode sheet is provided, comprising a negative electrode material layer, the negative electrode material layer comprising a negative electrode material, the negative electrode material comprising a porous carbon material and a lithium-loving substance, wherein the porous carbon material contains element M, the element M being selected from at least one of N, B, P, and S; Based on the total mass of the negative electrode material layer, the mass percentage of the lithiophilic substance is a%, and the mass percentage of element M is b%. The condition a and b satisfy: 1.5 ≤ a × b ≤ 120.
[0014] The inventors discovered that introducing element M into porous carbon materials allows it to replace carbon atoms or form surface functional groups that directly integrate into the carbon lattice, altering the electronic structure of carbon and serving as a lithiophilic active site. However, the introduction of element M also increases surface defects in the porous carbon material. This application involves setting a negative electrode material layer on the surface of the negative electrode current collector and introducing porous carbon material containing element M and lithiophilic substances into the negative electrode material layer. This induces uniform lithium deposition within the negative electrode material layer, reduces the enrichment of lithium ions on the surface of the negative electrode material layer, and reduces or avoids lithium deposition on the negative electrode surface. By increasing the mass percentage (a%) of the lithiophilic substances in the negative electrode material layer, more lithium storage sites can be provided, promoting uniform lithium deposition within the negative electrode material layer and thus improving the battery's energy density. However, if 'a' is too large, the excessive content of lithium-affinity substances in the negative electrode material layer will lead to excessive accumulation of lithium ions on the negative electrode surface. This will cause severe volume expansion during charge and discharge, resulting in increased mechanical stress on the electrode sheet, failure of the bond between the negative electrode material coating and the negative electrode current collector, and ultimately cracking and / or detachment of the negative electrode material layer, thus reducing the battery's cycle life. In this case, reducing the mass percentage (b%) of element M in the negative electrode material layer can reduce surface defects in the porous carbon material and reduce side reactions between the porous carbon material and the electrolyte, thereby improving the battery's cycle life.
[0015] Therefore, this application, by comprehensively controlling the mass percentage of lithiophilic material a% and the mass percentage of element M b% in the negative electrode material layer, within a suitable range, can synergistically improve the proportion of lithiophilic active sites and surface defects of porous carbon material in the negative electrode material. This induces a greater amount of lithium to be uniformly deposited inside the negative electrode material layer, reducing the degree of lithium ion enrichment on the surface of the negative electrode material layer. At the same time, it ensures good conductivity of the porous carbon material, high current density uniformity, and suppresses "hot spot" lithium deposition, which is beneficial to improving the energy density of the battery. The reduced enrichment of lithium ions on the surface of the negative electrode material layer helps to reduce the degree of lithium deposition on the surface of the negative electrode sheet. Meanwhile, there are fewer side reactions between the porous carbon material and the electrolyte, thereby suppressing the volume expansion of the negative electrode sheet during charging and discharging, reducing the mechanical stress inside the negative electrode sheet, ensuring high adhesion between the negative electrode material layer and the negative electrode current collector, making the negative electrode material layer less prone to detachment, improving the cycle life of the battery, and thus enabling the battery to have both good energy density and cycle life.
[0016] For example, a×b is an interval range formed by any two values of 1.5, 2, 4, 6, 8, 10, 12, 15, 18, 20, 22, 25, 28, 30, 32, 35, 38, 40, 42, 45, 48, 50, 52, 55, 58, 60, 62, 65, 68, 70, 72, 75, 78, 80, 82, 85, 88, 90, 82, 85, 98, 100, 102, 105, 108, 110, 112, 115, 118, 120 or more.
[0017] In some implementations, a and b satisfy the condition: 12 ≤ a × b ≤ 65, resulting in a better overall improvement in battery energy density and cycle life.
[0018] In some embodiments, the range of a% is 1.00% to 15.00%, such as a% being an interval formed by any two values of 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00%. In some embodiments, the range of a% is 5.00% to 10.00%.
[0019] When the a% is in the range of 1.00% to 15.00%, especially in the range of 5.00% to 10.00%, the content of lithium-affinity substances in the negative electrode material layer is more suitable. This can promote more uniform deposition of lithium in the internal structure of the negative electrode material layer, reduce the degree of lithium plating on the negative electrode surface, suppress the volume expansion of the negative electrode sheet during charging and discharging, reduce the mechanical stress inside the negative electrode sheet, improve the adhesion between the negative electrode material layer and the negative electrode current collector, reduce the risk of the negative electrode material layer falling off, and thus improve the energy density and cycle life of the battery.
[0020] The value of a% can be controlled by at least one of the following conventional process conditions: (1) the ratio of lithiophilic material to porous carbon material, and (2) the total amount of lithiophilic material and porous carbon material when preparing the negative electrode slurry.
[0021] This application does not limit the detection method for the value of a%, and it can be obtained using methods conventional in the art. For example, ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometry) can be used for determination, as detailed below: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the negative electrode sheet was obtained. The negative electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was then taken out and dried at room temperature in a humidity ≤15%. The negative electrode material layer on the surface of the current collector was scraped off to obtain powder. Weigh a certain amount of the obtained powder (e.g., 2g), disperse it in 20mL of water, add 10mL of nitric acid (concentration 65wt%~68wt%), heat it after dispersion, and after the powder dissolves, dilute it to 100mL with water to obtain the test solution. Use ICP-OES to perform elemental detection on the test solution, and read the concentration data of characteristic elements of the lithiophilic material through instrument analysis software. Further calculate the mass percentage of the lithiophilic material in the negative electrode material layer.
[0022] Before performing ICP-OES testing on the sample, a series of standard working solutions (typically with concentration gradients of 0 mg / L, 1 mg / L, 2 mg / L, and 3 mg / L) were prepared by serially diluting a 1000 mg / L standard solution with deionized water. ICP-OES detection was performed under the same instrument testing conditions as the sample, and a standard working curve was plotted, ensuring a linear correlation coefficient of no less than 0.999. The ICP-OES instrument testing parameters were set as follows: gas flow rate 0.5 L / min, power 1150 W, and the measurement wavelength was selected based on the characteristic elements of the lithiophilic substance (e.g., Zn 213.856 nm, Ti 336.121 nm, Al 396.153 nm).
[0023] In some embodiments, the range of b% is 1.00% to 10.00%, such as b% being an interval formed by any two values of 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.50%, 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, or higher. In some embodiments, the range of b% is 2.00% to 8.00%.
[0024] When b% is in the range of 1.00% to 10.00%, especially in the range of 2.00% to 8.00%, the surface defect ratio of porous carbon materials is more suitable. This can not only improve the conductivity of porous carbon materials, enhance the uniformity of current density, suppress lithium plating at "hot spots", and improve the energy density of the battery, but also reduce the side reactions between porous carbon materials and electrolytes, suppress the volume expansion of the negative electrode during charging and discharging, reduce the mechanical stress inside the negative electrode, improve the adhesion between the negative electrode material layer and the negative electrode current collector, reduce the risk of the negative electrode material layer falling off, and improve the cycle life of the battery.
[0025] The value of b% can be controlled by at least one of the following conventional process conditions: (1) the type of biomass raw material, (2) the mass ratio of biomass raw material to dopant (i.e. element M source) during the preparation of porous carbon material, and (3) the amount of porous carbon material used when preparing negative electrode slurry.
[0026] This application does not limit the detection method for the value of b%, and it can be obtained by conventional methods in the art. For example, ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometry) can be used for determination, as follows: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the negative electrode sheet was obtained. The negative electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was taken out and dried at room temperature in a humidity ≤15%. The material on the surface of the negative electrode current collector was scraped off and then dried at 105℃ to obtain material powder. Detection of elements B and P: Weigh a certain amount of the obtained material powder (e.g., 2g), disperse it in 20mL of water, add 10mL of nitric acid (concentration 65wt%~68wt%), and heat after dispersion. After the negative electrode material powder dissolves, dilute with water to 100mL to prepare the test solution. Use ICP-OES to detect the elements in the test solution. Read the concentration data of elements B and / or P through instrument analysis software, and further calculate the mass percentage content of elements B and / or P in the negative electrode material layer. Before the ICP-OES test of the sample, dilute the 1000mg / L standard solution stepwise with deionized water to prepare a series of standard working solutions (generally with concentration gradients of 0 mg / L, 1 mg / L, 2 mg / L, and 3 mg / L). Perform ICP-OES detection under instrument test conditions completely identical to those of the test solution, plot the standard working curve, and ensure that the linear correlation coefficient is not less than 0.999. The ICP-OES instrument test parameters are set as follows: gas flow rate 0.5 L / min, power 1150 W, and the measurement wavelength is selected according to the element to be measured (e.g., B 249.773 nm, P 213.618 nm). Detection of elements N and S: After grinding the obtained material powder, 10 mg was weighed and tested using a sulfur-nitrogen analyzer. The furnace temperature was set to 1000℃ and the oxygen partial pressure to 0.2 MPa. The concentration data of elements N and / or S were read by the instrument analysis software to obtain the mass percentage content of N and / or S in the negative electrode material. Before testing the sample, a standard curve was plotted using N and / or S standards (such as thiophene and pyridine) to ensure that the linear correlation coefficient was not less than 0.999. Based on the above data, the mass percentage of element M in the negative electrode material layer is calculated and denoted as b.
[0027] In some embodiments, the porous carbon material includes biomass porous carbon material, wherein biomass includes at least one of straw (such as wheat straw), rice husks, corn cobs, sugarcane bagasse, wood, fruit peels (such as grapefruit peel), and fruit shells (such as coconut shells and / or nut shells). Biomass-based porous carbon materials offer the following advantages: abundant and renewable resources, low cost, and naturally possessing nitrogen-containing functional groups and porous structures.
[0028] In some embodiments, the morphology of the porous carbon material satisfies the following: a porous material rich in pore structures of different sizes (micropores, mesopores, and macropores).
[0029] This application does not limit the method for detecting the morphology of porous carbon materials; conventional methods in the art can be used. For example, SEM (scanning electron microscopy) can be used for measurement.
[0030] In some embodiments, the negative electrode material layer has mesopores with a pore size of 2-50 nm. When the negative electrode material layer has mesopores, such as when its pore size is within the range formed by any two of the following values: 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, it can not only provide better lithium storage space, which is beneficial for inducing lithium deposits inside the negative electrode material layer and thus improving the battery energy density, but also ensure that the negative electrode material layer has good mechanical stability, suppressing structural collapse during charge-discharge cycles and improving the cycle life of the battery. In some embodiments, the volume ratio of mesopores in the negative electrode material layer is 20%-60%. When the volume ratio of the interstitial pores in the negative electrode material layer is within this range, such as 20%, 30%, 40%, 50%, 60%, or any two values forming a range, it can increase the lithium storage space, promote the deposition of lithium deposits inside the negative electrode material layer, and optimize the battery energy density. On the other hand, it can enhance the mechanical stability of the negative electrode material layer, suppress the problem of structural collapse during charging and discharging, and extend the cycle life of the battery.
[0031] In some embodiments, the negative electrode material layer also has micropores and macropores, wherein the micropores have a diameter of less than 2 nm and the macropores have a diameter of greater than 50 nm. The inventors have discovered that forming a pore structure with multiple pore sizes (micropores, macropores, and mesopores) in the negative electrode material layer, including macropores (diameter greater than 50 nm) and mesopores (diameter of 2-50 nm), can ensure the ion transport rate in the negative electrode material layer, improve the effective utilization rate of the active material in the negative electrode sheet, provide suitable lithium storage space for the negative electrode material layer, and also provide buffer space for volume expansion on the negative electrode side during cyclic charging and discharging, preventing cracking and / or detachment of the negative electrode material layer during battery charging and discharging, thereby comprehensively improving the battery's energy density and cycle life.
[0032] This application does not limit the detection methods for the pore size and volume ratio of the intermediate pores in the negative electrode material layer, as well as the pore size of the micropores and macropores; conventional methods in the art can be used for detection. For example, the BET method can be used, as detailed below: The battery was discharged at 0.33C to its lower limit voltage (2.5V for lithium iron phosphate LFP batteries, nickel-cobalt-manganese ternary NCM batteries, and lithium manganese iron phosphate LMFP batteries; 3.5V for lithium nickel manganese oxide batteries). The negative electrode was then disassembled and immersed in DMC (dimethyl carbonate) at room temperature (25℃) for 60 minutes. It was then removed and air-dried at room temperature with humidity ≤15%. The material on the surface of the negative electrode current collector was scraped off to obtain material powder. The pore size distribution of the material powder was tested using a BET specific surface area analyzer. The BET specific surface area analyzer is an instrument used to measure the specific surface area of materials. Based on the Brunauer-Emmett-Teller (BET) theory, it is determined by gas adsorption (usually using nitrogen). During the test, the total amount of nitrogen adsorbed when the relative pressure P / P0 is close to 1 (e.g., P / P0 is 0.99) is usually taken and converted into liquid nitrogen volume. This liquid nitrogen volume represents the total pore volume of the material. For the 2~50 nm mesoporous range, the cumulative desorption pore volume and pore size distribution curves of this range can be directly obtained by using the BJH model, or the mesoporous pore volume in this range can be calculated by integrating the DFT model. Based on the above data, the pore diameter and volume percentage of mesopores, the pore diameter of micropores, and the pore diameter of macropores can be calculated.
[0033] In some embodiments, the lithiophilic material is selected from metal oxides, including at least one of ZnO, TiO2, and Al2O3.
[0034] The inventors discovered that introducing metal oxides as lithiophilic substances into the negative electrode material layer exhibits excellent adsorption capacity for lithium ions, which can promote the uniform deposition of lithium inside the negative electrode material layer, thereby improving the energy density of the battery.
[0035] In some embodiments, the average particle size of the lithiophilic material is 1-20 nm. When the average particle size of the lithiophilic material is within this range, such as 1 nm, 3 nm, 5 nm, 8 nm, 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, or any two of these values, its specific surface area is more suitable. This not only results in more lithiophilic active sites, which can induce more lithium to be uniformly deposited inside the negative electrode material layer, improving the energy density of the battery, but also reduces side reactions with the electrolyte, which is beneficial for extending the cycle life of the battery.
[0036] This application does not limit the method for detecting the average particle size of the lithiophilic material; it can be obtained using methods conventional in the art. For example, the following method can be used: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the negative electrode sheet was obtained. The negative electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was taken out and dried in a room temperature environment with humidity ≤15%. The material on the surface of the negative electrode current collector was scraped off to obtain material powder. The obtained material powder was tested by TEM (transmission electron microscopy). The lithiophilic material was identified by mapping (elemental surface distribution imaging). The size data of the lithiophilic material was obtained by adding a scale and the average value was taken to obtain the average particle size.
[0037] The porous carbon material of this application can be prepared using conventional methods. In some embodiments, the preparation method of the porous carbon material includes the following steps: Pretreatment: Take biomass raw materials, clean, dry, crush, and acid or alkali wash to dissolve inorganic impurities to obtain pretreated biomass raw materials; Carbonization: Under the protection of inert gas, the pretreated biomass raw materials are carbonized to obtain carbonized semi-finished products; Activation and pore formation: The carbonized semi-finished product is activated and pore-formed using chemical reagents, pore-forming agents, or gases to obtain the porous carbon material.
[0038] In the above-mentioned method for preparing porous carbon materials, the inert gas includes at least one of nitrogen and argon, the carbonization temperature is 500~800℃, and the carbonization time is 4~8h.
[0039] In the above-mentioned method for preparing porous carbon materials, the chemical reagent pore-forming agent includes at least one of KOH and KHCO3, and the gas includes water vapor; when the chemical reagent pore-forming agent is used for activation and pore-forming treatment, the mass ratio of the chemical reagent pore-forming agent to the carbonized semi-finished product is (0.5~4):1.
[0040] In the above-mentioned method for preparing porous carbon materials, the carbonization treatment is carried out at a temperature of 600~800℃ for 1~2 hours. Activating and pore-forming treatment of the carbonized semi-finished product at a high temperature of 600~800℃ can create dense pores on the carbon skeleton and increase its specific surface area.
[0041] In the above-mentioned method for preparing porous carbon materials, if the content of element M in the biomass raw material itself is low and it is necessary to introduce element M additionally, the following step can be included before the carbonization step: mixing the pretreated biomass raw material with a dopant (i.e., element M source) solution and performing hydrothermal treatment. For example, the dopant includes at least one of urea, melamine, thiourea, phytic acid, phosphoric acid, and boric acid; the mass percentage of the dopant in the dopant solution is 5-10%; the mass of element M in the dopant solution is 0.9-12% of the mass of the pretreated biomass raw material; the hydrothermal treatment temperature can be selected from 180-250℃; the hydrothermal treatment pressure can be selected from 2-3.5 MPa; and the hydrothermal treatment time can be selected from 4-12 h.
[0042] In some embodiments, the thickness of the negative electrode material layer is 0.1~10µm. When the thickness of the negative electrode material layer is within this range, such as 0.1µm, 0.55µm, 1µm, 1.5µm, 2.0µm, 2.5µm, 3.0µm, 3.5µm, 4.0µm, 4.5µm, 5.0µm, 5.5µm, 6.0µm, 6.5µm, 7.0µm, 7.5µm, 8.0µm, 8.5µm, 9.0µm, 9.5µm, 10.0µm or any two of the above values, it can provide a larger lithium storage space, promote more uniform deposition of lithium inside the negative electrode material layer, inhibit the enrichment and lithium deposition of lithium ions on the surface of the negative electrode sheet, and improve the cycle life of the battery; at the same time, it ensures that the transport path of lithium ions in the negative electrode material layer is short, enhances the utilization rate of active materials, and thus improves the energy density of the battery.
[0043] This application does not limit the method for detecting the thickness of the negative electrode material layer; it can be detected using methods conventional in the art. For example, the following method can be used: Discharge the battery at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), disassemble to obtain the negative electrode sheet, place the negative electrode sheet in DMC (dimethyl carbonate) and immerse it in room temperature (25℃, the same below) for 60 minutes, take it out, and air dry it in a room temperature environment with humidity ≤15%; Use a micrometer to measure the thickness of the negative electrode material layer. If the current collector has a negative electrode material layer on both sides, take the arithmetic mean of the thicknesses of the negative electrode material layers on both sides as the thickness of the negative electrode material layer. If the current collector has a negative electrode material layer on only one side, take the thickness of the negative electrode material layer on that side directly.
[0044] In some embodiments, the total mass percentage of the porous carbon material and the lithiophilic substance is 90% to 98%, based on the total mass of the negative electrode material layer, such as 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or any two values forming a range.
[0045] The inventors discovered through research that by controlling the sum of the mass percentages of porous carbon materials and lithium-loving substances in the negative electrode material layer to the above-mentioned range, it is possible to ensure that the negative electrode material layer can hold more lithium ions at the same weight, while avoiding the negative electrode material layer becoming too dense and lacking elastic buffer space due to excessive inactive materials (such as binders), thereby reducing the risk of cracking and / or detachment of the negative electrode material layer, thus comprehensively balancing the energy density and cycle life of the battery.
[0046] In some embodiments, the negative electrode material layer further includes a negative electrode binder and a negative electrode dispersant.
[0047] The negative electrode binder in the negative electrode material layer is used to improve the adhesion between negative electrode material particles and the adhesion between the negative electrode material and the negative electrode current collector. Any binder can be used without particular limitation, as long as it has a suitable binder and does not significantly cause adverse chemical changes in the battery. For example, the negative electrode binder includes at least one of styrene-butadiene latex (SBR), aqueous acrylic resin, polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and sodium carboxymethyl cellulose (CMC). The aqueous acrylic resin may include at least one of polyacrylic acid (PAA), polymethacrylic acid (PMAA), and sodium polyacrylate (PAAS).
[0048] In some embodiments, the negative electrode binder in the negative electrode material layer has a mass percentage content of 1.5% to 5%, such as 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5% or more, or any two values forming a range.
[0049] The negative electrode dispersant in the negative electrode material layer is used to improve the dispersibility of the negative electrode material. Any dispersant can be used without particular limitation, as long as it has suitable dispersibility and does not significantly cause adverse chemical changes in the battery. For example, the negative electrode dispersant includes at least one of acrylics, acrylates, polyether esters, phosphate esters, small molecule alkanolamines, polyurethanes, modified styrene / maleic anhydride, nitrile rubber (HNBR), and polyvinylpyrrolidone (PVP).
[0050] In some embodiments, the mass percentage of the negative electrode dispersant in the negative electrode material layer is 0.3% to 1.5%, such as 0.3%, 0.5%, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, or any two of the above values forming a range.
[0051] In some embodiments, the negative electrode material layer further includes a negative electrode conductive agent. The negative electrode conductive agent in the negative electrode material layer is used to provide conductivity, and any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity and does not significantly cause adverse chemical changes in the battery. Exemplarily, the negative electrode conductive agent includes, but is not limited to, at least one of carbon nanotubes, carbon black, graphite, carbon fibers, activated carbon, mesoporous carbon, and fullerenes, wherein carbon fibers are, for example, carbon nanofibers; and carbon black is, for example, SP (Super P), acetylene black, Ketjen black, etc.
[0052] In some embodiments, the mass percentage of the negative electrode conductive agent in the negative electrode material layer is 0-5%, such as 0, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, or any two values within the range formed by these values.
[0053] In some embodiments, the compaction density of the negative electrode sheet is 0.3~0.8 g / cm³. 3 .
[0054] The inventors discovered through research that by controlling the compaction density of the negative electrode sheet to the above-mentioned range, the negative electrode material layer can retain sufficient porosity while ensuring the energy density of the battery. This is beneficial for the electrolyte to fully wet the negative electrode sheet, reduce local polarization, and prevent lithium ions from preferentially depositing on the surface to form dendrites due to obstructed transport, thereby improving the cycle life of the battery.
[0055] In some embodiments, the negative electrode includes a negative current collector. This application does not impose any particular limitation on the negative current collector, as long as it is conductive and will not cause adverse chemical changes in the battery, and at least one of, for example, copper, chromium, nickel, and titanium can be used.
[0056] The negative electrode material layer can be located on one side of the negative electrode current collector or on both sides of the negative electrode current collector.
[0057] The negative electrode sheet can be prepared according to conventional methods in the art. For example, the preparation method of the negative electrode sheet includes the following steps: mixing and dispersing a porous carbon material with a lithiophilic substance, then mixing and dispersing it with other components of the negative electrode material layer and a solvent to obtain a negative electrode slurry; coating the negative electrode slurry onto at least one side of a negative electrode current collector, drying, rolling, and slitting to obtain a negative electrode sheet; in the preparation method of the negative electrode sheet, water can be selected as the solvent.
[0058] According to a second aspect of this application, a battery is provided, including a positive electrode, a negative electrode, and an electrolyte.
[0059] In some embodiments, the positive electrode includes a positive electrode material layer, and the ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer is 100 to 1000. When the ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer is within this range, such as 100, 200, 400, 600, 800, 1000, or any two of these values, not only does the negative electrode have a larger lithium storage space, which can suppress lithium deposition on the surface of the negative electrode and improve the energy density of the battery, but the positive electrode can also load more positive electrode material, increase the supply of lithium ions, optimize the insertion and extraction behavior of lithium ions in the negative electrode, and extend the cycle life of the battery.
[0060] This application does not limit the method for detecting the ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer; it can be obtained using methods conventional in the art. For example, the following method can be preferentially used: Discharge the battery at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese lithium battery is 3.5V), disassemble to obtain positive and negative electrode sheets, place the negative and positive electrode sheets in DMC (dimethyl carbonate) and immerse them at room temperature (25℃, the same below) for 60 minutes, take them out and air dry them at room temperature in an environment with humidity ≤15%; Use a micrometer to measure the thickness of the positive electrode material layer. If the positive current collector has a positive electrode material layer on both sides, take the arithmetic mean of the thicknesses of the positive electrode material layers on both sides as the thickness of the positive electrode material layer. If the positive current collector has a positive electrode material layer on only one side, take the thickness of the positive electrode material layer on that side directly. The calculated ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer.
[0061] In some embodiments, the thickness change rate of the negative electrode material layer is 50% to 100% relative to the initial state of 0% SOC when the battery is at 80% SOC. When the thickness change rate of the negative electrode material layer is within this range, such as 50%, 60%, 70%, 80%, 100%, or any two of these values, the lithium intercalation amount in the negative electrode is more suitable. This not only helps to improve the energy density of the battery but also suppresses lithium plating on the surface of the negative electrode, reduces the mechanical stress inside the negative electrode, improves the adhesion between the negative electrode material layer and the negative electrode current collector, reduces the risk of negative electrode material layer detachment, and improves the cycle life of the battery.
[0062] This application does not limit the method for detecting the rate of change in the thickness of the negative electrode material layer of the battery at 80% SOC relative to the initial state of 0% SOC; conventional methods in the art can be used for detection. For example, the following method can be used: Take a fresh battery (the criteria for judging a fresh battery: the battery capacity has not shown significant decay, and the actual discharge capacity is not less than 95% of the nominal discharge capacity, which can be judged as a fresh battery), disassemble it to obtain the battery cell, discharge the battery cell to 0% SOC at 0.33C, select one electrode sheet from the inner ring, middle and outer ring of the negative electrode of the battery cell, and measure the thickness of the negative electrode material layer at no less than 7 different points on each electrode sheet. Calculate the average value of each group of test data and record it as the initial thickness H0; Disassemble the fresh battery to obtain the battery cell, charge the battery cell to 80% SOC at 0.33C, select one electrode sheet from the inner ring, middle and outer ring of the negative electrode of the battery cell, and measure the thickness of the negative electrode material layer at no less than 7 different points on each electrode sheet. Calculate the average value of each group of test data and record it as H1. Calculate the thickness change rate of the negative electrode material layer when the battery is at 80% SOC, relative to the initial state of 0% SOC = (H1-H0) / H0×100%.
[0063] In some embodiments, the positive electrode sheet includes a positive electrode material layer, the positive electrode material layer includes a positive electrode material, and the positive electrode material includes at least one of lithium iron phosphate and nickel-cobalt-manganese ternary materials.
[0064] When the cathode material is lithium iron phosphate, the overall performance of the battery is better.
[0065] In some embodiments, when the positive electrode material is lithium iron phosphate, the compaction density of the positive electrode sheet is 2.3~2.7 g / cm³. 3 When the compaction density of the positive electrode is within this range, such as 2.3 g / cm³, ... 3 2.4 g / cm 3 2.5 g / cm3 2.6 g / cm 3 2.7 g / cm 3 When the range is within the range formed by any two of the above values, it is beneficial for the electrolyte to wet the positive electrode, optimize the transport of lithium ions, improve the battery's reactivity, and extend the battery's cycle life. It can also ensure that the positive electrode has a high positive electrode material loading, thereby improving the battery's energy density.
[0066] In some embodiments, when the positive electrode material is selected from nickel-cobalt-manganese ternary materials, the compaction density of the positive electrode sheet is 3.2~3.8 g / cm³. 3 When the compaction density of the positive electrode is within this range, such as 3.2 g / cm³, ... 3 3.3 g / cm 3 3.4 g / cm 3 3.5g / cm 3 3.6 g / cm 3 3.7 g / cm 3 3.8g / cm 3 When the range is within the range formed by any two of the above values, it is beneficial for the electrolyte to wet the positive electrode, optimize the transport of lithium ions, improve the battery's reactivity, and extend the battery's cycle life. It can also ensure that the positive electrode has a high positive electrode material loading, thereby improving the battery's energy density.
[0067] This application does not limit the method for detecting the compaction density of the positive and negative electrode sheets; conventional methods in the art can be used. For example, the following method can be used: ① Pretreatment: Discharge the battery at 0.33C to the lower limit voltage (depending on the specific system, the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese lithium battery is 3.5V), disassemble the electrode sheets, soak the electrode sheets in dimethyl carbonate (DMC) solution for 4 hours and then air dry; ② Use a punching machine to punch the pretreated electrode sheet into circular pieces of a fixed area, denoted as S0. Take three circular pieces as parallel samples, and weigh each of the three circular pieces using an electronic balance. Take the average value and record it as M1. Use a micrometer to measure the thickness of the material layer in each of the three circular pieces (i.e., the total thickness of the electrode sheet minus the current collector), and take the average value and record it as H. Finally, add an appropriate amount of deionized water to each of the three circular pieces, gently wipe off the coating on the circular pieces with lint-free paper to expose the foil, and let it stand at room temperature (or dry) for 10 minutes. After the foil is dry, weigh each of the three foil pieces, take the average value and record it as M0. Calculate the compaction density of the electrode sheet using the following formula: A = (M1 - M0) / (H × S0), where A is in g / cm³. 3M1 and M0 are in g, H is in cm, and S0 is in cm. 2 .
[0068] In some embodiments, the particle size Dv50 of the cathode material ranges from 1.0 to 6.0 μm. When the particle size Dv50 of the cathode material is within this range, such as 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, or any two of these values, the lithium-ion diffusion path can be shortened, the battery's reactivity can be improved, and the battery's energy density can be enhanced. Simultaneously, the specific surface area of the cathode material can be reduced, side reactions between the cathode and the electrolyte can be decreased, and the battery's cycle life can be extended.
[0069] This application does not limit the method for detecting the particle size Dv50 of the cathode material; it can be obtained using methods conventional in the art. For example, it can be measured using the following method: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the positive electrode sheet was obtained by disassembly. The positive electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was then taken out and dried at room temperature in a humidity of ≤15%. The material on the surface of the positive electrode current collector was scraped off to obtain material powder. Take 1g of the obtained material powder and use a laser particle size distribution measuring instrument (Mastersizer 3000) to measure the particle size distribution according to the particle size distribution laser diffraction method (specific steps refer to GB / T19077-2016). The particle size corresponding to the cumulative particle size distribution percentage reaching 50% is the particle size Dv50.
[0070] In some embodiments, the positive electrode material layer includes a dopant element selected from at least one of Ti, V, Nb, Mg, Zn, Zr, Ni, and Al; the mass percentage of the dopant element in the positive electrode material layer is 0.5% to 5.0%. When the mass percentage of the specific dopant element in the positive electrode material layer is within this range, the stability of the crystal structure of the positive electrode material can be improved, side reactions between the positive electrode material and the electrolyte can be reduced, the cycle life of the battery can be optimized, and at the same time, it can also ensure that there is more active material in the positive electrode material layer, thereby improving the energy density of the battery. For example, the mass percentage of the dopant element in the positive electrode material layer is within the range formed by any two values of 0.5%, 1%, 2%, 3%, 4%, 5%, or higher.
[0071] This application does not limit the method for detecting the mass percentage content of doped elements in the cathode material layer; conventional methods in the art can be used. For example, the following method can be used: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the positive electrode sheet was obtained by disassembly. The positive electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was then taken out and dried at room temperature in a humidity of ≤15%. The material on the surface of the positive electrode current collector was scraped off to obtain material powder. Accurately weigh a certain amount (e.g., 0.5g) of the obtained material powder, disperse it in 20mL of water, add 10mL of nitric acid, mix well, and then heat it until the material powder dissolves. Then, dilute the material with water to 100mL to obtain the test solution. Perform ICP testing on the test solution. Before the test, a standard solution must be prepared. The linear correlation coefficient of the standard concentration must be above 0.999 to be used as a normal standard. The 1000 mg / L standard solution was diluted with deionized water to different concentrations (generally 0, 1 mg / 100mL, 2 mg / 100mL, 3 mg / 100mL), and the element detection wavelength was selected. Experimental conditions were set: based on the sample characteristics and the element to be detected, appropriate ICP instrument operating conditions were set: gas flow rate 0.5 L / min, power 1150 W, and the element detection wavelength was selected (e.g., Ti 336.121 nm, V 292.402 nm, Nb 316.340 nm, Mg 279.553 nm, Zn 213.856 nm, Zr 343.823 nm, Ni 231.604 nm, Al 396.153 nm). The element content in the sample can be read using the self-service analysis function of the ICP testing software, depending on the element being tested.
[0072] In some embodiments, the surface of the positive electrode material is provided with a coating layer, the average thickness of which is 1-10 nm. When the average thickness of the coating layer is within this range, such as 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any two of these values, the coating layer can better protect the positive electrode material, reduce side reactions between the positive electrode material and the electrolyte, optimize the cycle life of the battery, and at the same time, reduce the lithium ion transport path, improve the reactivity of the positive electrode, and increase the energy density of the battery.
[0073] This application does not limit the method for detecting the average thickness of the coating layer; it can be obtained using methods conventional in the art. For example, the following method can be used: The battery was discharged at 0.33C to the lower limit voltage (the lower limit voltage of lithium iron phosphate LFP battery, nickel cobalt manganese ternary material NCM battery and lithium manganese iron phosphate LMFP battery is 2.5V; the lower limit voltage of nickel manganese oxide battery is 3.5V), and the positive electrode sheet was obtained by disassembly. The positive electrode sheet was placed in DMC (dimethyl carbonate) and immersed in it at room temperature (25℃, the same below) for 60 minutes. It was then taken out and dried at room temperature in a humidity of ≤15%. The material on the surface of the positive electrode current collector was scraped off to obtain material powder. The obtained powder was ultrasonically dispersed in ethanol. The liquid containing the powder was then drawn up with a pipette and dropped onto a copper grid covered with a carbon support film and dried. The grid was then placed in the TEM scanning area for scanning. Based on the TEM image, the coating thickness was measured with a ruler. The coating thickness of 200 cathode material particles was tested and the average value was taken.
[0074] Optionally, the material of the coating layer is selected from at least one of carbon, tungsten oxide, boron oxide, and aluminum oxide.
[0075] In some embodiments, the mass percentage of the positive electrode material in the positive electrode material layer is 94% to 99.4%, such as the range formed by any two values of 94%, 95%, 96%, 97%, 98%, 99%, 99.4% or above.
[0076] Specifically, in this application, lithium iron phosphate may or may not contain doping elements, and the application does not limit the types of doping elements in lithium iron phosphate. In some embodiments, the doping elements in lithium iron phosphate include at least one selected from Ti, V, Nb, Mg, Zn, Zr, Ni, and Al. In some embodiments, when the lithium iron phosphate does not contain doping elements, the chemical formula of the lithium iron phosphate is Li. e FePO4, where 0.9≤e≤1.1 (e is 0.9, 1, 1.1 or any two of the above values forming a range).
[0077] In this application, the nickel-cobalt-manganese ternary material may or may not contain doping elements, and the type of doping element in the nickel-cobalt-manganese ternary material is not limited. In some embodiments, the doping element in the nickel-cobalt-manganese ternary material includes at least one of Ti, V, Nb, Mg, Zn, Zr, Ni, and Al. In some embodiments, when the nickel-cobalt-manganese ternary material does not contain doping elements, the chemical formula of the nickel-cobalt-manganese ternary material is Li. a Ni x Co y Mn 1-x-yO2, wherein a is in the range of 0.9-1.1, 0<x<1; 0<y<1; x+y<1. For example, a is 0.9, 1, 1.1 or an interval range formed by any two of the above values; x is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.95 or an interval range formed by any two of the above values; y is 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.12, 0.14, 0.16, 0.18, 0.2, 0.22, 0.24, 0.26, 0.28, 0.3, 0.32, 0.35 or an interval range formed by any two of the above values; x+y is 0.15, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.95 or an interval range formed by any two of the above values.
[0078] In some of the embodiments, the positive electrode material layer further comprises a positive electrode conductive agent. The positive electrode conductive agent in the positive electrode material layer is used to provide electrical conductivity, and any conductive agent may be used without particular limitation, as long as it has appropriate electronic conductivity and does not apparently cause adverse chemical changes in the battery. Exemplarily, the positive electrode conductive agent includes, but is not limited to, at least one of carbon nanotubes, carbon black, graphite, activated carbon, carbon fibers, mesoporous carbon, and fullerenes, where the carbon fibers are, for example, carbon nanofibers and the like; the carbon black is, for example, acetylene black, SP, Ketjen black and the like. Alternatively, in the positive electrode material layer, the mass percentage content of the positive electrode conductive agent is 0.3% to 3%, such as 0.3%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.5%, 2%, 2.5%, 3% or an interval range formed by any two of the above values.
[0079] In some of the embodiments, the positive electrode material layer further comprises a positive electrode binder. The positive electrode binder in the positive electrode material layer is used to improve the adhesion between positive electrode material particles and the adhesion between the positive electrode material and the positive electrode current collector, and any binder may be used without particular limitation, as long as it has appropriate adhesive properties and does not apparently cause adverse chemical changes in the battery. Exemplarily, the positive electrode binder includes, but is not limited to, fluorine-containing polyolefin-based binders, and the fluorine-containing polyolefin-based binders include, but are not limited to, polyvinylidene fluoride (PVDF), vinylidene fluoride copolymers, or modified (e.g., modified with carboxylic acid, acrylic acid, acrylonitrile, etc.) derivatives thereof and the like. Alternatively, in the positive electrode material layer, the mass percentage content of the positive electrode binder is 0.5% to 3%, such as 0.5%, 0.7%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 2%, 2.5%, 3% or an interval range formed by any two of the above values.
[0080] In some embodiments, the positive electrode includes a positive current collector. This application does not impose any particular limitation on the positive current collector, as long as it is conductive and will not cause adverse chemical changes in the battery, and materials such as aluminum, nickel, titanium, stainless steel, sintered carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc., can be used.
[0081] The positive electrode material layer can be located on one side of the positive electrode current collector or on both sides of the positive electrode current collector.
[0082] The positive electrode sheet can be prepared according to conventional methods in the art. For example, the preparation method of the positive electrode sheet includes the following steps: mixing a positive electrode active material, a conductive agent, a binder, and a solvent to obtain a positive electrode slurry; coating the positive electrode slurry onto at least one side of a positive electrode current collector, drying, cold pressing, and slitting to obtain the positive electrode sheet. The solvent may be N-methylpyrrolidone.
[0083] In some embodiments, the viscosity of the electrolyte at 25°C is 1~1.5 mPa·s. When the viscosity of the electrolyte at 25°C is within this range, such as 1 mPa·s, 1.1 mPa·s, 1.2 mPa·s, 1.3 mPa·s, 1.4 mPa·s, 1.5 mPa·s, or any two of the above values, it can improve the fluidity of the electrolyte, improve the lithium-ion transport efficiency, optimize the cycle life of the battery, avoid poor wetting of local areas of the negative electrode, help form a dense and stable SEI film, reduce the consumption of active lithium, and improve the energy density of the battery.
[0084] This application does not limit the method for detecting the viscosity of the electrolyte at 25°C. Conventional methods in the art can be used for detection. For example, the following method can be used: 1) Collecting the electrolyte: Discharge the battery at 0.33C to the lower limit voltage of 2.5V. Disassemble the battery and collect the electrolyte in a glove box (H2O≤0.1ppm, O2≤0.1ppm). There are three methods for collecting the electrolyte: After opening the battery cover... ① If there is free electrolyte, collect the electrolyte into a 5mL sample tube with a pipette and seal it with sealing tape to prevent electrolyte leakage; ② If there is no free electrolyte, a hydraulic press (FY-30 hydraulic press of Beijing Heng'ao Technology Co., Ltd.) can be used to continuously pressurize until free electrolyte appears. Collect the electrolyte into the sample tube and seal it. ③ Add an appropriate amount of dichloromethane extractant to the battery and record the dichloromethane content. After adding dichloromethane, put the battery into an aluminum-plastic bag and seal it with a heat sealer. Transfer it to an ultrasonic oscillator and oscillate for 12 hours to allow the electrolyte in the electrode to mix thoroughly with the dichloromethane. Then, use a pipette to draw the mixture of dichloromethane and electrolyte into a 5mL sample tube and seal the sample tube with sealing glue. 2) Remove the electrolyte and test it using a Cambridge viscometer. The Cambridge viscometer is designed based on electromagnetic oscillation viscosity detection technology and uses a magnetically levitated probe for viscosity measurement. Specifically, place the electrolyte in a beaker and control the sample temperature at 25°C for testing. Read the value after the display value stabilizes.
[0085] In some embodiments, the electrolyte comprises a lithium salt. Exemplary examples include, but are not limited to, at least one of lithium hexafluorophosphate (LiPF6), lithium difluorooxalate borate (LiODFB), lithium difluorophosphate (LiPO2F2), and lithium bis(fluorosulfonyl)imide (LiFSI).
[0086] In some embodiments, the lithium salt is selected from LiPF6, and the concentration of the lithium salt in the electrolyte is 0.8~1.5 mol / L. When the concentration of the lithium salt in the electrolyte is within this range, the number of free lithium ions in the electrolyte can be increased, thereby improving the battery energy density; at the same time, the lithium ion transport efficiency can be improved, and the cycle life of the battery can be extended.
[0087] This application does not limit the method for detecting the concentration of lithium salt in the electrolyte; conventional methods in the art can be used for detection. For example, the following method can be used for detection: 1) Electrolyte Collection: Discharge the battery at 0.33C to the lower limit voltage (2.5V for lithium iron phosphate (LFP) batteries, nickel-cobalt-manganese (NCM) batteries, and lithium manganese iron phosphate (LMFP) batteries; 3.5V for nickel-manganese lithium batteries). Disassemble the battery and collect the electrolyte in a glove box (H2O≤0.1ppm, O2≤0.1ppm). There are three methods for collecting the electrolyte. After opening the battery cover... ① If there is free electrolyte, collect the electrolyte into a 5mL sample tube with a pipette and seal it with sealing tape to prevent electrolyte leakage; ② If there is no free electrolyte, a hydraulic press (FY-30 hydraulic press of Beijing Heng'ao Technology Co., Ltd.) can be used to continuously pressurize until free electrolyte appears. Collect the electrolyte into the sample tube and seal it. ③ Add an appropriate amount of dichloromethane extractant to the battery and record the dichloromethane content. After adding dichloromethane, put the battery into an aluminum-plastic bag and seal it with a heat sealer. Transfer it to an ultrasonic oscillator and oscillate for 12 hours to allow the electrolyte in the electrode to mix thoroughly with the dichloromethane. Then, use a pipette to draw the mixture of dichloromethane and electrolyte into a 5mL sample tube and seal the sample tube with sealing glue. 2) After filtering out solid suspended matter from the collected electrolyte sample, transfer 0.2g to a centrifuge tube containing 19.8g of ultrapure water. Shake to allow the lithium salt (e.g., LiPF6) to react fully with the water, dissociating the anion to be tested (e.g., F⁻). Filter the sample solution using an aqueous syringe filter (0.22 or 0.45 μm pore size), place it in an IC-specific sample vial, and perform IC testing to obtain an IC spectrum. Compare the obtained IC spectrum with standard spectra in the IC database (the IC database contains spectra of all ionic substances) to confirm the type of lithium salt (the standard curve and the sample electrolyte curve match ≥98%). Then, determine the corresponding lithium salt content based on the peak area of the anion to be tested in the electrolyte, thereby calculating the lithium salt concentration. In some embodiments, the electrolyte includes additives. For example, the additive may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery high-temperature performance, battery overcharge performance, and battery low-temperature performance. For instance, the additives include, but are not limited to, at least one of the following: vinylene carbonate (VC), 1,3-propanesulfonate lactone (PS), vinyl sulfate (DTD), methylene disulfonate, fluoroethylene carbonate, propylene sulfonate lactone, tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, and hexamethylene diisocyanate.
[0088] In some embodiments, the additive includes vinylene carbonate, and the mass percentage of vinylene carbonate in the electrolyte is 1% to 5%. When the mass percentage of vinylene carbonate in the electrolyte is within this range, it can better participate in the formation of the SEI film, improve the stability of the SEI film, reduce the consumption of active lithium, and extend the cycle life of the battery. At the same time, it can prevent the SEI film from being too thick, reduce the electrode interface impedance, promote lithium-ion transport, and thus improve the energy density.
[0089] Controlling the mass percentage of VC in the electrolyte within this range not only allows it to better participate in the formation of the SEI film, resulting in a more stable SEI film and reduced consumption of active lithium, thus improving cycle life, but also prevents excessive growth and thickening of the SEI film, reduces electrode interface impedance, promotes lithium-ion transport, and increases the energy density of the battery.
[0090] This application does not limit the method for detecting the mass percentage of vitamin C in the electrolyte; conventional methods in the art can be used for detection. For example, the following detection method can be used: 1) Electrolyte Collection: Discharge the battery at 0.33C to the lower limit voltage (2.5V for lithium iron phosphate (LFP) batteries, nickel-cobalt-manganese (NCM) batteries, and lithium manganese iron phosphate (LMFP) batteries; 3.5V for nickel-manganese lithium batteries). Disassemble the battery and collect the electrolyte in a glove box (H2O≤0.1ppm, O2≤0.1ppm). There are three methods for collecting the electrolyte. After opening the battery cover... ① If there is free electrolyte, collect the electrolyte into a 5mL sample tube with a pipette and seal it with sealing tape to prevent electrolyte leakage; ② If there is no free electrolyte, a hydraulic press (Beijing Heng'ao Technology Co., Ltd. FY-30 hydraulic press) can be used to continuously pressurize until free electrolyte appears. Collect the electrolyte into the sample tube and seal it. ③ Add an appropriate amount of dichloromethane extractant to the battery and record the dichloromethane content. After adding dichloromethane, put the battery into an aluminum-plastic bag and seal it with a heat sealer. Transfer it to an ultrasonic oscillator and oscillate for 12 hours to allow the electrolyte in the electrode to mix thoroughly with the dichloromethane. Then, use a pipette to draw the mixture of dichloromethane and electrolyte into a 5mL sample tube and seal the sample tube with sealing glue. 2) After filtering the collected electrolyte sample, inject it into an Agilent Intuvo 9000 gas chromatograph-mass spectrometer using a microsyringe to obtain GC-MS chromatograms. Dissolve vitamin C in EMC solvent to prepare solutions of different concentrations, and inject each solution into the Agilent Intuvo 9000 gas chromatograph-mass spectrometer to obtain standard GC-MS chromatograms. Compare the GC-MS chromatogram of the electrolyte to be tested with the standard GC-MS chromatogram to confirm the presence of vitamin C. Then, determine the content of vitamin C based on the peak area of the vitamin C in the electrolyte to be tested.
[0091] In some embodiments, the electrolyte further includes a solvent. For example, the solvent includes at least one of carbonate solvents, carboxylic acid ester solvents, ether solvents, sulfone solvents, nitrile solvents, and phosphate ester solvents.
[0092] Exemplary examples include, but are not limited to, at least one of propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC); carboxylic acid ester solvents include, but are not limited to, at least one of ethyl acetate, methyl formate, and 1,4-butyrolactone; ether solvents include, at least one of dimethyltetrahydrofuran, tetrahydrofuran, and 1,2-dimethoxyethane; sulfone solvents include, at least one of methyl sulfone and dimethyl sulfoxide; nitrile solvents include, at least one of propionitrile, butyronitrile, 1-(2-cyanoethyl)pyrrole, and 1,3,6-hexanetrionitrile; and phosphate ester solvents include, at least one of trimethyl triphosphate and triethyl phosphate.
[0093] The battery may further include a separator located between the positive and negative electrode plates to separate them and prevent short circuits. The separator can be any suitable battery separator material in the art. Exemplarily, the separator includes, but is not limited to, at least one of polypropylene and polyethylene.
[0094] In some embodiments, the battery includes a separator with a permeability of 200-400 s / 100 mL. When the permeability of the separator is within this range, such as 200 s / 100 mL, 220 s / 100 mL, 240 s / 100 mL, 260 s / 100 mL, 280 s / 100 mL, 300 s / 100 mL, 320 s / 100 mL, 340 s / 100 mL, 360 s / 100 mL, 380 s / 100 mL, 400 s / 100 mL, or any two of the above values, it is beneficial for lithium ions to penetrate the separator, optimizing energy density. At the same time, it can also prevent excessive electrolyte from wetting the positive and negative electrode plates through the separator, reducing side reactions between the electrolyte and the positive and negative electrodes, and improving the cycle life of the battery.
[0095] According to a third aspect of this application, an electrical device is provided, including the battery. The battery serves as the power supply for the electrical device. The electrical device refers to any device that can utilize electrical energy and convert it into mechanical energy, thermal energy, light energy, or one or more other energy forms, such as an electric motor, electric heater, or electric light source. Specifically, it can include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Mobile devices can be mobile phones, laptops, drones, robot vacuum cleaners, e-cigarettes, etc.; electric vehicles can be pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.
[0096] The present application is further illustrated below with specific embodiments: Examples 1-22 and Comparative Examples 1-4 Each battery is provided, and the specific manufacturing method is as follows: S1. Preparation of porous carbon materials S11. After washing the biomass raw materials (see Table 1 for types), dry them, crush them into powder, and then wash them with hydrochloric acid (HCl mass fraction of 5%) to dissolve inorganic impurities, so as to obtain the pretreated biomass raw materials. S12. The pretreated raw material is mixed with the dopant (i.e., element M source) solution and subjected to hydrothermal treatment at 200℃ and 2.5MPa for 6 hours. After filtration and drying, a doped semi-finished product is obtained. The dopant solution is composed of phosphoric acid, boric acid, urea, thiourea and water. The mass ratio (N:B:P:S) between N element in urea, B element in boric acid, P element in phosphoric acid and S element in thiourea is shown in Table 1. The sum of the masses of elements N, B, P and S in the dopant is the percentage of the mass of the pretreated biomass raw material, denoted as w, as shown in Table 1. S13. Under nitrogen protection, the doped semi-finished product is treated at a high temperature of 600°C for 6 hours to obtain the carbonized semi-finished product; S14. The carbonized semi-finished product is mixed with a pore-forming agent (KOH) at a mass ratio of 2.45 to 2.45. The mixture is activated at 700℃ for 1.5 hours to obtain a porous carbon material.
[0097] S2, Preparation of the negative electrode The obtained porous carbon material was mixed and dispersed with a lithiophilic substance to obtain the negative electrode material. The types and average particle size of the lithiophilic substance, as well as the mass percentage of the lithiophilic substance in the negative electrode material, are shown in Table 1. The negative electrode material, conductive agent acetylene black, binder SBR, and dispersant CMC are mixed in the mass ratio shown in Table 1. Deionized water is added, and the mixture is stirred in a vacuum mixer to obtain a negative electrode slurry. The obtained negative electrode slurry is coated on both sides of the negative electrode current collector copper foil, dried, rolled, and cut to obtain a negative electrode sheet. The thickness of each negative electrode material layer in the negative electrode sheet is adjusted by controlling the coating thickness of the negative electrode slurry as shown in Table 1.
[0098] S3, Preparation of the positive electrode The positive electrode material (the types of which are shown in Table 1), the conductive agent acetylene black and the binder PVDF are mixed at a mass ratio of 96:2:2, and the solvent N-methylpyrrolidone (NMP) is added. The mixture is stirred in a vacuum mixer to obtain the positive electrode slurry. The obtained positive electrode slurry was coated on both sides of the positive electrode current collector aluminum foil, dried, cold-pressed, and slit to obtain the positive electrode sheet. Due to the change in the thickness of the negative electrode material layer, the ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer changed accordingly, as shown in Table 1. The compaction density of the positive electrode sheet of the nickel-cobalt-manganese ternary material battery is 3.5 g / cm³.3 The compaction density of the positive electrode sheet in the LFP battery is 2.5 g / cm³. 3 .
[0099] S4. Preparation of Electrolyte Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4 to obtain an organic solvent. Dry lithium salt (lithium hexafluorophosphate) and vitamin C were dissolved in the obtained organic solvent to prepare an electrolyte with a lithium salt concentration of 1.0 mol / L and a vitamin C mass percentage of 2%.
[0100] S5, Preparation of Lithium-ion Batteries The positive electrode, separator (PE film), and negative electrode are stacked in sequence, with the separator acting as an isolation between the positive and negative electrode sheets. The bare cell is obtained through the stacking process. The bare battery cell is placed in an outer packaging shell (made of aluminum-plastic film), dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping processes, a lithium-ion battery is obtained.
[0101] If the cathode material is a nickel-cobalt-manganese ternary material, the formation process is as follows: ① Place the battery in a 25℃ constant temperature chamber, connect the charging and discharging device, set the protection voltage to 4.0V, and let it stand for 2 hours to reach thermal equilibrium; ② Charge the battery at a constant current of 0.02C to 3.40V; let it stand for 10 minutes; ③ Charge the battery at a constant current of 0.05C to 3.75V, and let it stand for 10 minutes. If the cathode material is lithium iron phosphate, the formation procedure is as follows: ① Place the battery in a 45℃ constant temperature chamber, connect the charging and discharging device, set the protection voltage to 4.0V, and let it stand for 2 hours to reach thermal equilibrium; ② Charge at a constant current of 0.05C for 120 minutes; let it stand for 10 minutes; ③ Charge at a constant current of 0.3C for 120 minutes, and let it stand for 10 minutes.
[0102] Table 1 In accordance with the aforementioned exemplary method, this application tested the values of a and b, and the volume percentage of the intermediate pores (pore diameter in the range of 2~50nm) in the negative electrode material layer for each embodiment and comparative example. The results are shown in Table 2.
[0103] This application tested the energy density and cycle life of the batteries in various embodiments and comparative examples. The test results are shown in Table 2, and the test methods are as follows: (1) Energy density Weigh the battery and record the weight as m (unit: g); place the battery in a fixture, apply a force of 3000 N, charge it to the upper limit voltage with a constant current of 0.33 C, let it rest for 30 min, discharge it to the lower limit voltage with a constant current of 0.33 C, let it rest for 30 min, and repeat this cycle 3 times; calculate the battery discharge capacity (unit: Ah), and record the average discharge energy of the 3 cycles as E; calculate the discharge energy density using the formula: Discharge energy density = E / m, where the unit of discharge energy density is Wh / kg.
[0104] (2) Test method for cycle life At 25°C, the battery was cycle-tested according to the following procedure: 1) Charge at a constant current rate of 0.33C to the upper limit voltage, and then charge at a constant voltage until the current drops to 0.05C; 2) Let it stand for 10 minutes; 3) Discharge at a rate of 0.33C to the lower limit voltage; 4) Let it stand for 10 minutes; Perform cycle tests according to steps 1)-4) until the discharge capacity of the lithium-ion battery is less than 80% of the initial discharge capacity (i.e., the discharge capacity of the first cycle), and record the number of cycles.
[0105] In the above testing method, if the cathode material is a nickel-cobalt-manganese ternary material, the upper limit voltage is 4.25V and the lower limit voltage is 2.50V; if the cathode material is lithium iron phosphate, the upper limit voltage is 3.65V and the lower limit voltage is 2.50V.
[0106] Table 2 As can be seen from Tables 1 and 2, the embodiments of this application, by comprehensively controlling the mass percentage (a%) of the lithiophilic material in the negative electrode material layer and the mass percentage (b%) of element M in the negative electrode material layer, can comprehensively improve the energy density and cycle life of the battery, achieving an energy density of over 200 Wh / kg and a cycle life of over 300 cycles. When a% is 5.00%~10.00%, b% is 2.00%~8.00%, and 12≤a×b≤65, it is more conducive to balancing the battery's energy density and cycle life.
[0107] Compared with the embodiments, in Comparative Examples 1 and 2, even if the values of a and b are within a suitable range, the energy density and / or cycle life of the battery deteriorate when the value of a×b is not within the range of 1.4 to 120. In Comparative Example 3, a is too small and a×b is too small, resulting in a significant decrease in cycle performance and energy density, even lower than Comparative Example 1. In Comparative Example 4, b is too large and a×b is too large, resulting in a significant decrease in cycle performance and energy density, even lower than Comparative Example 2.
[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this article and are not intended to limit the scope of protection of this article. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this article without departing from the essence and scope of the technical solutions of this article.
Claims
1. A negative electrode sheet, characterized in that, The anode material includes a negative electrode material layer, the negative electrode material layer includes a negative electrode material, the negative electrode material includes a porous carbon material and a lithium-loving substance, wherein the porous carbon material contains element M, and element M is selected from at least one of N, B, P and S; Based on the total mass of the negative electrode material layer, the mass percentage of the lithiophilic substance is a%, and the mass percentage of element M is b%. The condition a and b satisfy: 1.5 ≤ a × b ≤ 120.
2. The negative electrode sheet as described in claim 1, characterized in that, The condition a and b satisfy the following condition: 12 ≤ a × b ≤ 65.
3. The negative electrode sheet as described in claim 1, characterized in that, The range of a% is 1.00% to 15.00%; And / or, the range of b% is 1.00% to 10.00%.
4. The negative electrode sheet as described in claim 1, characterized in that, The porous carbon material includes biomass porous carbon material.
5. The negative electrode sheet as described in claim 1, characterized in that, The negative electrode material layer has mesopores with a pore size of 2~50nm.
6. The negative electrode sheet as described in claim 5, characterized in that, In the negative electrode material layer, the volume ratio of mesopores is 20% to 60%.
7. The negative electrode sheet as described in claim 1, characterized in that, The lithiophilic material is selected from metal oxides.
8. The negative electrode sheet as described in claim 7, characterized in that, The metal oxide includes at least one of ZnO, TiO2, and Al2O3.
9. The negative electrode sheet as described in claim 1, characterized in that, The average particle size of the lithiophilic material is 1~20 nm.
10. The negative electrode sheet as described in claim 1, characterized in that, The thickness of the negative electrode material layer is 0.1~10µm.
11. The negative electrode sheet as described in claim 1, characterized in that, Based on the total mass of the negative electrode material layer, the sum of the mass percentages of the porous carbon material and the lithiophilic substance is 90% to 98%.
12. A battery, characterized in that, It includes a positive electrode, a negative electrode as described in any one of claims 1 to 11, and an electrolyte.
13. The battery as claimed in claim 12, characterized in that, The positive electrode includes a positive electrode material layer, and the ratio of the thickness of the positive electrode material layer to the thickness of the negative electrode material layer is 100 to 1000.
14. The battery as claimed in claim 12, characterized in that, When the battery is at 80% SOC, the thickness of the negative electrode material layer changes by 50% to 100% compared to the initial state of 0% SOC.
15. The battery as claimed in claim 12, characterized in that, The positive electrode sheet includes a positive electrode material layer, the positive electrode material layer includes a positive electrode material, and the positive electrode material includes at least one of lithium iron phosphate and nickel-cobalt-manganese ternary materials.
16. The battery as claimed in claim 15, characterized in that, When the positive electrode material is selected from nickel-cobalt-manganese ternary materials, the compaction density of the positive electrode sheet is 3.2~3.8 g / cm³. 3 ; Alternatively, when the positive electrode material is selected from lithium iron phosphate, the compaction density of the positive electrode sheet is 2.3~2.7 g / cm³. 3 .
17. The battery as claimed in claim 15, characterized in that, The particle size Dv50 of the cathode material ranges from 1.0 to 6.0 μm.
18. The battery as claimed in claim 13 or 15, characterized in that, The cathode material layer includes doped elements, wherein the doped elements include at least one of Ti, V, Nb, Mg, Zn, Zr, Ni, and Al; the mass percentage of the doped elements in the cathode material layer is 0.5% to 5.0%.
19. The battery as claimed in claim 15, characterized in that, The surface of the positive electrode material is provided with a coating layer, and the average thickness of the coating layer is 1~10nm.
20. The battery as claimed in claim 12, characterized in that, The electrolyte has a viscosity of 1~1.5 mPa·s at 25°C.
21. The battery as claimed in claim 12, characterized in that, The electrolyte includes a lithium salt selected from LiPF6, and the concentration of the lithium salt in the electrolyte is 0.8~1.5 mol / L.
22. The battery as claimed in claim 12, characterized in that, The electrolyte includes additives, including vinylene carbonate, and the mass percentage of vinylene carbonate in the electrolyte is 1% to 5%.
23. The battery as claimed in claim 12, characterized in that, The battery includes a separator with an air permeability of 200~400s / 100mL.
24. An electrical appliance, characterized in that, Includes the battery as described in any one of claims 12 to 23.