negative electrode

By using composite active material particles containing Si or Sn elements in the negative electrode layer of a solid-state battery and subjecting them to magnetic field orientation treatment, the flatness ratio is controlled, which solves the problem of increased electrode expansion after pressing, improves Li ion conductivity, and enhances battery performance.

CN123120640APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610360836.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-03-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In solid-state batteries, the length of active material particles increases in the direction of the electrode surface after compression, resulting in increased electrode expansion and decreased Li ion conductivity.

Method used

By including composite active material particles containing Si or Sn elements in the negative electrode layer and using a magnetic field orientation process to orient the particles in the thickness direction, the negative electrode layer is prepared to control its flatness ratio to be above 0.30 and below 0.45, thereby suppressing the lateral flatness of the particles.

Benefits of technology

It effectively reduces the expansion of the negative electrode, improves the conductivity of Li ions, and enhances the performance stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120640A_ABST
    Figure CN123120640A_ABST
Patent Text Reader

Abstract

This invention relates to negative electrodes and solid-state batteries. The negative electrode includes a negative electrode layer containing composite active material particles and a negative electrode current collector. The composite active material particles contain a negative electrode active material containing at least one of Si and Sn elements, a binder, and a conductive carbon material. The flatness A1 of the composite active material particles contained in the negative electrode layer, calculated by a prescribed formula, is 0.30 or more and less than 0.45.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure pertains to the negative electrode. Background Technology

[0002] Various technologies have been proposed for the negative electrode disclosed in Japanese Patent Application Publication No. 2023-104840. Summary of the Invention

[0003] Compared to liquid batteries, in solid batteries manufactured by pressing the electrodes with high pressure, the length of the active material particles sometimes increases in the direction of the electrode surface after pressing. The active material particles that were spherical before pressing become flattened after pressing, resulting in increased electrode expansion and decreased Li ion conductivity of the electrode.

[0004] This disclosure was made in view of the above-mentioned actual situation, and its main purpose is to provide a negative electrode that can reduce the amount of expansion.

[0005] That is, this disclosure includes the following schemes.

[0006] <1> A negative electrode comprises: a negative electrode layer containing composite active material particles, and a negative electrode current collector, wherein the composite active material particles comprise: a negative electrode active material containing at least one of Si and Sn elements, a binder, and a conductive carbon material, and the flatness A1 of the composite active material particles contained in the negative electrode layer, calculated by the following formula, is 0.30 or more and less than 0.45.

[0007] Flatness ratio A1 = 1 - L1 / L2

[0008] L1: Length of the composite active material particles in the thickness direction of the negative electrode layer.

[0009] L2: The length of the composite active material particles in the width direction of the negative electrode layer.

[0010] <2> <1> The method for manufacturing the negative electrode includes:

[0011] The process of preparing the composite active substance particles;

[0012] The process of preparing a slurry for a negative electrode layer comprising the composite active material particles, the binder, the conductive material, and the solvent;

[0013] The process of coating the negative electrode layer slurry onto one surface of the negative electrode current collector;

[0014] The magnetic field alignment process involves applying a magnetic field perpendicular to the surface of the negative electrode current collector to the slurry used in the negative electrode layer, thereby aligning the composite active material particles in the thickness direction with their long sides aligned; and

[0015] In the drying process, after the magnetic field orientation process, the negative electrode layer is dried with a slurry to obtain the negative electrode layer.

[0016] <3> Solid-state batteries have <1> The aforementioned negative electrode.

[0017] According to this disclosure, a negative electrode capable of reducing expansion can be provided. Attached Figure Description

[0018] The features, advantages, technical and industrial significance of embodiments of the present invention are described with reference to the accompanying drawings, wherein like reference numerals denote like elements, wherein:

[0019] Figure 1 This is a schematic diagram illustrating an example of a conventional method for manufacturing a negative electrode;

[0020] Figure 2 A schematic diagram illustrating an example of a method for manufacturing the negative electrode according to this disclosure;

[0021] Figure 3 A flowchart illustrating an example of a method for manufacturing the negative electrode of this disclosure;

[0022] Figure 4 A cross-sectional schematic diagram illustrating an example of a solid-state battery of this disclosure; and

[0023] Figure 5 The graph shows the flatness A1 of each composite active material particle and the variation of the constraint pressure of each battery in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3. Detailed Implementation

[0024] The embodiments of this disclosure will now be described. Furthermore, the dimensional relationships (length, width, thickness, etc.) in the figures do not reflect actual dimensional relationships. Figure 1 , 2 The Y direction shown in Figure 4 is the planar direction or width direction of the negative electrode layer. Figure 1 , 2 The Z direction shown in Figure 4 is the stacking direction or thickness direction of the negative electrode layer.

[0025] Unless otherwise specified, elements described in the "singular form" may include plural forms. For example, "particle" sometimes also refers to multiple particles (a swarm of particles).

[0026] In this disclosure, an example of a method for calculating the average particle size is described below. First, in a transmission electron microscope (TEM) image or a scanning electron microscope (SEM) image at an appropriate magnification (e.g., 2,000 to 1,000,000 times), the particle size of a single particle is calculated if that particle is considered spherical. For 2 to 300 particles of the same type, such particle size calculations under TEM or SEM observations are performed, and the average of these particles is taken as the average particle size.

[0027] 1. Negative electrode

[0028] This disclosure provides a negative electrode comprising: a negative electrode layer containing composite active material particles, and a negative electrode current collector, wherein the composite active material particles contain a negative electrode active material containing at least one of Si and Sn elements, a binder, and a conductive carbon material, and the flatness A1 of the composite active material particles contained in the negative electrode layer, calculated by the following formula, is 0.30 or more and less than 0.45.

[0029] Flatness ratio A1 = 1 - L1 / L2

[0030] L1: Length of the composite active material particles in the thickness direction of the negative electrode layer

[0031] L2: Length of the composite active material particles in the width direction of the negative electrode layer

[0032] Figure 1 This is a schematic diagram illustrating an example of a conventional method for manufacturing a negative electrode.

[0033] In the prior art, by pressing the negative electrode layer 20, the composite active material particles 60 become horizontally elongated and flat (the length L2 of the composite active material particles 60 in the width direction Y of the negative electrode layer 20 is greater than the length L1 of the composite active material particles 60 in the thickness direction Z of the negative electrode layer 20).

[0034] Figure 2 A schematic diagram illustrating an example of a method for manufacturing the negative electrode of this disclosure.

[0035] In this disclosure, after coating the negative electrode layer 20 onto a negative electrode current collector (not shown), a magnetic field is applied to the negative electrode layer 20 to orient the composite active material particles 60 in a longitudinally elongated flat shape (the length L2 of the composite active material particles 60 in the width direction Y of the negative electrode layer 20 is smaller than the length L1 of the composite active material particles 60 in the thickness direction Z of the negative electrode layer 20). By pressing the negative electrode layer 20 in this state, the transverse flatness of the composite active material particles 60 can be suppressed compared to conventional methods.

[0036] The negative electrode disclosed herein has a negative electrode layer and a negative electrode current collector.

[0037] The negative electrode layer contains at least composite active material particles, and may include binders, conductive materials, and electrolytes as needed.

[0038] The composite active material particles include: a negative electrode active material containing at least one of the elements Si and Sn, a binder, and a conductive carbon material.

[0039] The proportion of composite active material particles in the negative electrode layer can be, for example, 40% or more by mass and less than 100% by mass.

[0040] The average particle size of the composite active material particles can be, for example, greater than 0.1 μm and less than 100 μm.

[0041] The negative electrode active material may be in particulate form. The average particle size of the negative electrode active material may be, for example, 0.05 μm or more and 30 μm or less.

[0042] The negative electrode active material only needs to contain at least one of the elements Si and Sn.

[0043] Examples of active Si-based materials containing Si include Si, SiO, and Si alloys.

[0044] Sn-based active materials containing the element Sn include, for example, Sn and Sn alloys.

[0045] The negative electrode layer may further include other negative electrode active materials besides Si-based and Sn-based active materials. Examples of other negative electrode active materials include at least one selected from carbon-based active materials, Li-based active materials, and lithium titanate.

[0046] Carbon-based active materials may include at least one selected from graphite, soft carbon, and hard carbon. "Graphite" is a general term for both natural and artificial graphite. Graphite can be a mixture of natural and artificial graphite.

[0047] Examples of Li-based active materials include Li, Li silicates, and Li alloys.

[0048] The proportion of negative electrode active material in the composite active material particles can be, for example, above 85% by mass and below 99.4% by mass.

[0049] Examples of adhesives include styrene-butadiene rubber (SBR), polyimide (PI), polyacrylic acid (PAA), acrylonitrile-butadiene rubber (NBR), butadiene rubber (BR), polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), styrene-isoprene-styrene block copolymer (SIS), and ethylene-propylene-diene copolymer (EPDM). The proportion of the adhesive in the composite active material particles can be, for example, 0.5% by mass or more and 15% by mass or less.

[0050] Examples of conductive carbon materials include graphite, soft carbon, hard carbon, fumed carbon fiber (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs). Conductive carbon materials can exhibit magnetic properties. The proportion of conductive carbon material in the composite active material particles can be, for example, 0.1% by mass or more and 5% by mass or less.

[0051] For the conductive materials and electrolytes used in the negative electrode layer, the same materials described in the positive electrode layer can be listed.

[0052] The proportion of conductive material in the negative electrode layer can be, for example, more than 0.1% by mass and less than 5% by mass.

[0053] The proportion of electrolyte in the negative electrode layer can be, for example, more than 0% by mass and less than 60% by mass.

[0054] There are no particular restrictions on the top view shape of the negative electrode layer; for example, it can be a quadrilateral shape or a rectangle.

[0055] The thickness of the negative electrode layer can be, for example, 0.1 μm or more and 1000 μm or less, 1 μm or more and 500 μm or less, or 30 μm or more and 100 μm or less.

[0056] The flatness A1 of the composite active material particles contained in the negative electrode layer, calculated by the following formula, is greater than 0.30 and less than 0.45.

[0057] Flatness ratio A1 = 1 - L1 / L2

[0058] L1: Length of the composite active material particles in the thickness direction of the negative electrode layer

[0059] L2: Length of the composite active material particles in the width direction of the negative electrode layer

[0060] The closer the flatness ratio A1 is to 0, the closer the cross-sectional shape of the composite active material particles is to a circle; the closer it is to 1, the greater the flatness of the transverse length of the composite active material particles oriented in the width direction of the negative electrode layer; if it is less than 0, the greater the flatness of the longitudinal length of the composite active material particles oriented in the thickness direction of the negative electrode layer.

[0061] Flatness A1 can be the average value of multiple composite active material particles.

[0062] The lengths L1 and L2 of the composite active material particles in the thickness direction of the negative electrode layer are calculated by observing the SEM cross-sectional image of the negative electrode layer.

[0063] A flatness ratio A1 of 0.30 or higher but less than 0.45 means that when L2 is set to 100, L1 should be between 55 and 70. A flatness ratio A1 of 0.30 or higher but less than 0.45 means that compared to a flatness ratio A1 of 0.45 or higher, the horizontal flatness of the composite active material particles is less. Although the composite active material particles have a horizontally flat shape, the degree of horizontal flatness is suppressed.

[0064] Examples of materials that can be used as negative electrode current collectors include SUS, aluminum, copper, nickel, iron, titanium, and carbon. Furthermore, the thickness of the negative electrode current collector can range from 1 μm to 50 μm. There are no particular limitations on the top-view shape of the negative electrode current collector; examples include circles, ellipses, rectangles, and arbitrary polygons. The negative electrode current collector can be configured with a buffer layer, an elastic layer, or a PTC (Positive Temperature Coefficient) thermistor layer disposed on its surface.

[0065] 2. Manufacturing method of negative electrode

[0066] In this disclosure, the method for manufacturing the negative electrode includes: a step of preparing the composite active material particles; a step of preparing a negative electrode layer slurry comprising the composite active material particles, the binder, the conductive material, and the solvent; a step of coating the negative electrode layer slurry on one surface of the negative electrode current collector; a magnetic field alignment step, wherein the composite active material particles are aligned such that the long side of the composite active material particles is aligned in the thickness direction by applying a magnetic field perpendicular to the surface of the negative electrode current collector to the negative electrode layer slurry; and a drying step, wherein after the magnetic field alignment step, the negative electrode layer slurry is dried to obtain the negative electrode layer.

[0067] The method for manufacturing the negative electrode disclosed herein includes (1) a composite active material particle preparation process, (2) a slurry preparation process for the negative electrode layer, (3) a coating process, (4) a magnetic field orientation process, (5) a drying process, and (6) a pressing process.

[0068] Figure 3 A flowchart illustrating an example of a method for manufacturing the negative electrode of this disclosure.

[0069] like Figure 3 As shown, the manufacturing method of the negative electrode disclosed herein can be implemented sequentially as follows: (1) preparation of composite active material particles, (2) preparation of slurry for negative electrode layer, (3) coating process, (4) magnetic field orientation process, (5) drying process, and (6) pressing process.

[0070] (1) Preparation process of composite active substance particles

[0071] The composite active substance particle preparation process is the process of preparing the composite active substance particles.

[0072] One method for preparing composite active material particles is to add a negative electrode active material and a conductive carbon material to an adhesive dispersion obtained by dispersing an adhesive in a solvent, and then composite the prepared composite active material with a slurry by spray drying at a specified spray pressure and a specified liquid delivery rate.

[0073] Examples of solvents include N-methylpyrrolidone (NMP), tetrahydronaphthalene, diisobutyl ketone, butyl butyrate, xylene, heptane, dibutyl ether, decane, dodecane, isodecane, and toluene, and may contain two or more of these components.

[0074] By adjusting at least one of the solid component concentration, spray pressure, and liquid delivery rate of the slurry used for composite active substances in the spray drying process, the flatness A0 of the composite active substance particles, calculated by the following formula, can be changed.

[0075] Flatness ratio A0 = 1 - (length a of the short side of the composite active material particle) / (length b of the long side of the composite active material particle)

[0076] The lengths 'a' of the short side and 'b' of the long side of the composite active material particles are calculated by observing the SEM cross-sectional images of the composite active material particles.

[0077] Flatness A0 is the flatness of the composite active material particles in the state before the formation of the negative electrode layer or before the negative electrode layer is pressed, which is different from the flatness A1 of the composite active material particles contained in the negative electrode layer after the negative electrode layer is pressed.

[0078] The composite active material particles prepared in the composite active material particle preparation process can be flat or spherical, but from the viewpoint of suppressing the flatness of the horizontal length of the composite active material particles contained in the negative electrode layer after the negative electrode layer is pressed, it can be flat.

[0079] There is no particular limitation on the flatness A0 of the composite active substance particles prepared in the composite active substance particle preparation process. For example, it can be above 0.17 and below 0.70.

[0080] (2) Preparation process of slurry for negative electrode layer

[0081] The negative electrode layer slurry preparation process is a process of preparing a negative electrode layer slurry containing the composite active material particles, the binder, the conductive material, and the solvent.

[0082] As an adhesive, the same adhesives described in the negative electrode layer can be cited as examples.

[0083] As conductive materials, the same conductive materials described in the positive electrode layer described later can be cited.

[0084] As solvents, the same solvents described in the slurry for composite active substances can be listed.

[0085] (3) Coating process

[0086] The coating process is a process of applying the slurry for the negative electrode layer to one surface of the negative electrode current collector.

[0087] There are no particular limitations on the coating method, and examples include doctor blade coating, metal mask printing, electrostatic coating, dip coating, spraying, roller coating, gravure coating, and screen printing.

[0088] (4) Magnetic field orientation process

[0089] The magnetic field orientation process is a process of orienting the composite active material particles in the thickness direction by applying a magnetic field perpendicular to the surface of the negative electrode current collector to the slurry of the negative electrode layer.

[0090] The angle θ between the straight line along the length direction of the composite active material particle, which represents the orientation degree of the composite active material particle, and the surface of the negative electrode current collector can be calculated using SEM, X-ray CT, or other images of the cross-section of the negative electrode.

[0091] In this disclosure, 30 to 100 composite active material particles are extracted from the field of view of the image of the cross-section of the negative electrode, and elliptical approximation is performed to extract their major and minor axes. The negative electrode current collector is defined as a horizontal plane, and the size of the minor angle (acute angle) at the intersection of the major axis of each composite active material particle and the horizontal plane is measured and taken as the tilt angle θ of the composite active material particle, thereby defining the orientation degree of each composite active material particle.

[0092] The orientation of the composite active material particles in the negative electrode layer can be controlled during the negative electrode manufacturing process by applying a negative electrode slurry to the negative electrode current collector and before the negative electrode slurry dries to become the negative electrode layer, by applying a predetermined time and a predetermined magnetic field to the negative electrode slurry.

[0093] The scheduled time can be, for example, 1 second to 1 hour, or 5 minutes to 30 minutes.

[0094] The predetermined magnetic field can be, for example, 0.1T~5T, or 1T~3T.

[0095] Regarding the orientation of the composite active material particles, as long as the tilt angle θ is greater than 45° and less than 90°, it can be greater than 60°, greater than 75°, or 90°.

[0096] (5) Drying process

[0097] The drying process is a process of drying the negative electrode layer with slurry after the magnetic field orientation process to obtain the negative electrode layer.

[0098] There are no particular limitations on the method of drying the slurry for the negative electrode layer; natural drying, reduced pressure drying, and vacuum drying are some examples.

[0099] (6) Pressing process

[0100] The pressing process is the process of pressing the negative electrode layer.

[0101] In the pressing process, pressing can be performed in the state of the negative electrode layer alone, in the state of the negative electrode, or in the state of a battery having a negative electrode, an electrolyte layer and a positive electrode in sequence.

[0102] There are no particular limitations on the method for pressing the negative electrode layer; examples include roller pressing and flatbed pressing. Alternatively, a constraint fixture can be used to apply constraint pressure along the thickness direction as a method for pressing the negative electrode layer.

[0103] 3. Solid-state batteries

[0104] The solid-state battery disclosed herein includes the negative electrode of this disclosure. The solid-state battery of this disclosure typically has a positive electrode, an electrolyte layer, and a negative electrode.

[0105] Figure 4 A cross-sectional schematic diagram illustrating an example of a solid-state battery of this disclosure.

[0106] like Figure 4 As shown, the solid-state battery 100 of this disclosure sequentially comprises a negative electrode current collector 10, a negative electrode layer 20, an electrolyte layer 30, a positive electrode layer 40, and a positive electrode current collector 50. The negative electrode layer 20 contains composite active material particles 60.

[0107] The negative electrode is the negative electrode of the present disclosure as described above.

[0108] The positive electrode has a positive electrode layer and a positive electrode current collector.

[0109] The positive electrode layer contains at least a positive electrode active material, and may contain at least one of an electrolyte, a conductive material, and a binder, as needed.

[0110] The positive electrode layer can be disposed on one surface of the positive electrode current collector or on both surfaces of the positive electrode current collector.

[0111] There are no particular restrictions on the top view shape of the positive electrode layer; for example, it can be a quadrilateral shape or a rectangle shape.

[0112] There are no particular limitations on the active material used as a positive electrode. Examples include rock salt layered active materials such as LiCoO2, LiMnO2, LiNiO2, LiVO2, Li(NiCoMn)O2, and Li(NiCoAl)O2; and LiMn2O4 and Li4Ti5O4. 12 , and Li(Ni 0.5 Mn 1.5 Spinel-type active materials such as Li(NiCoMn)O2; olivine-type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4. In "Li(NiCoMn)O2", "(NiCoMn)" and in "Li(NiCoAl)O2", "(NiCoAl)" indicate that the sum of the composition ratios within the parentheses is 1. As long as the sum is 1, the composition ratio of each element is arbitrary. For example, Li(NiCoMn)O2 can be Li(Ni... 1 / 3 Co 1 / 3Mn 1 / 3 O2, Li (Ni) 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, etc., Li(NiCoAl)O2 can be, for example, Li(Ni) 0.81 Co 0.15 Al 0.04 O2, etc.

[0113] A coating containing a Li-ion-conducting compound can be formed on the surface of the positive electrode active material. This is because it can suppress the reaction between the positive electrode active material and the solid electrolyte (especially a sulfide solid electrolyte). Examples of Li-ion-conducting compounds include B₂O₃, Li₂B₄O₇, LiBPO₄, Li₃PO₄, LiPO₃, and LiNbO₃. The coating thickness is, for example, 1 nm or more and 30 nm or less. The coverage of the positive electrode active material with the Li-ion-conducting compound is, for example, 70% or more, 90% or more, or 100%. There are no particular limitations on the coating method of the Li-ion-conducting compound, and conventionally known methods can be appropriately used.

[0114] The positive electrode active material is usually in the form of particles. The positive electrode active material can be a primary particle or a secondary particle formed by the aggregation of primary particles.

[0115] There is no particular limitation on the average particle size of the positive electrode active material particles. For example, it can be 0.01 μm or more and 50 μm or less, or 0.5 μm or more and 30 μm or less.

[0116] The proportion of positive electrode active material in the positive electrode layer is, for example, 20% by mass or more, 30% by mass or more, or 40% by mass or more. On the other hand, the proportion of positive electrode active material in the positive electrode layer is, for example, 95% by mass or less, 70% by mass or less, or 60% by mass or less.

[0117] As electrolytes, examples include solid electrolytes. Solid electrolytes can be inorganic solid electrolytes such as sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, and complex hydride solid electrolytes, or organic solid electrolytes such as gel electrolytes.

[0118] From the perspective of good processability, solid electrolytes can be in the form of particles.

[0119] In addition, there is no particular limitation on the average particle size of solid electrolyte particles, which can be 1 nm to 100 μm.

[0120] The proportion of solid electrolyte in the positive electrode layer can be, for example, more than 1% by mass and less than 60% by mass.

[0121] The positive electrode layer may contain conductive materials. By adding conductive materials, the electronic conductivity of the positive electrode layer is improved. Examples of conductive materials include carbon-based conductive materials, metal particles, and conductive polymers. Examples of carbon-based conductive materials include particulate materials such as acetylene black (AB) and Ketjen black (KB); and fibrous materials such as vapor-phase carbon fiber (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs).

[0122] The proportion of conductive material in the positive electrode layer can be, for example, more than 0.1% by mass and less than 5% by mass.

[0123] The positive electrode layer may contain an adhesive. Examples of adhesives include those described in the negative electrode layer.

[0124] The proportion of binder in the positive electrode layer can be, for example, more than 0.5% by mass and less than 15% by mass.

[0125] The thickness of the positive electrode layer is, for example, 0.1 μm or more and 1000 μm or less, 1 μm or more and 500 μm or less, or 30 μm or more and 100 μm or less.

[0126] There are no particular limitations on the manufacturing method of the positive electrode layer. For example, a method can be listed where a positive electrode active material, a conductive material, and a solvent are mixed to obtain a positive electrode slurry, which is then coated onto a positive electrode current collector and dried to form the positive electrode layer. During the formation of the positive electrode layer, a pressing process can be performed to press the positive electrode layer along its thickness direction. This pressing process is the same as the pressing process described in "2. Manufacturing Method of Negative Electrode" above.

[0127] The solvent may be the same as that described in "2. Method for manufacturing the negative electrode".

[0128] Materials used as positive current collectors include, for example, SUS, Cr, Au, Pt, Zn, aluminum, copper, nickel, iron, titanium, and carbon. The thickness of the positive current collector is, for example, 0.1 μm or more and 100 μm or less. There are no particular limitations on the top-view shape of the positive current collector; for example, circular, elliptical, rectangular, and arbitrary polygonal shapes are possible. The positive current collector can have a structure with a buffer layer, an elastic layer, or a PTC thermistor layer disposed on its surface.

[0129] The electrolyte layer is formed between the positive electrode layer and the negative electrode layer, and it contains at least an electrolyte. The electrolyte can be a liquid electrolyte or a solid electrolyte.

[0130] The electrolyte layer can be a solid electrolyte layer composed of solids.

[0131] In the case where the electrolyte layer is a solid electrolyte layer, the solid electrolyte layer contains a solid electrolyte and, if necessary, includes an adhesive, etc.

[0132] As a solid electrolyte, the same solid electrolyte as the solid electrolyte described in the above positive electrode layer can be listed.

[0133] Solid electrolytes can be used alone or in combination with two or more other solid electrolytes. Furthermore, when using two or more solid electrolytes, they can be mixed or formed into separate layers to create a multilayer structure.

[0134] There is no particular limitation on the proportion of solid electrolyte in the solid electrolyte layer. For example, it can be 50% or more by mass, or it can be 60% or more by mass but less than 100% by mass, or it can be 70% or more by mass but less than 100% by mass, or it can be 100% by mass. The solid electrolyte layer may contain less than 1% by mass of electrolyte relative to the total amount of solid electrolyte layer.

[0135] Examples of adhesives that can be contained in the positive electrode layer include the aforementioned adhesives.

[0136] The content of the binder in the solid electrolyte layer can be 0% to 10% by mass relative to the total amount of the solid electrolyte layer.

[0137] The thickness of the electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less, or 0.1 μm or more and 500 μm or less, or 0.1 μm or more and 100 μm or less.

[0138] There are no particular restrictions on the top view shape of the electrolyte layer; for example, it can be a quadrilateral or a rectangle.

[0139] The solid-state battery in this disclosure can be a lithium-ion battery. It can be a semi-solid-state battery or a fully solid-state battery. In this disclosure, a semi-solid-state battery is a battery in which the electrolyte layer has solid components such as an inorganic solid electrolyte and liquid components (e.g., solvents and electrolyte solutions). In this disclosure, a fully solid-state battery is a battery in which the electrolyte layer only has solid components such as an inorganic solid electrolyte as the electrolyte. Furthermore, the solid-state battery in this disclosure can be a primary battery or a secondary battery, wherein it can be a secondary battery. This is because it can be repeatedly charged and discharged, making it useful, for example, as a battery for automotive applications.

[0140] The solid-state battery disclosed herein can be either unipolar or bipolar.

[0141] The solid-state battery disclosed herein may further include a constraint clamp that applies a constraint pressure in the thickness direction relative to the positive electrode, the electrolyte layer, and the negative electrode. In particular, when the electrolyte layer is a solid electrolyte layer, a constraint pressure may be applied to form good ion conduction paths and electron conduction paths. The constraint pressure may be, for example, 0.1 MPa or more, 1 MPa or more, or 5 MPa or more. On the other hand, the constraint pressure may be, for example, 100 MPa or less, 50 MPa or less, or 20 MPa or less.

[0142] The solid-state battery disclosed herein may have an outer packaging.

[0143] The outer packaging contains the positive electrode, electrolyte layer, and negative electrode.

[0144] As for the material of the outer packaging, there are no special restrictions as long as it is stable to the electrolyte. Examples include metals such as Al and SUS, polypropylene, polyethylene, and resins such as acrylic resin.

[0145] There are no particular limitations on the shape of the outer packaging; for example, coin-shaped, flat, cylindrical, and laminated types can be listed.

[0146] There are no particular limitations on the top view shape of the outer packaging; for example, it can be a quadrilateral, a rectangle, a circle, or an oval.

[0147] Batteries are used in various applications, including as power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. Specifically, they can be used as a power source for driving hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or battery electric vehicles (BEVs). Furthermore, batteries can be used as a power source for mobile bodies other than vehicles (such as railways, ships, and aircraft), and also as a power source for electrical appliances such as information processing devices.

[0148] Example 1

[0149] Production of composite active substance particles

[0150] Si particles, which serve as the negative electrode active material, and graphite, which serves as the conductive carbon material, are added to a binder dispersion prepared by dispersing the binder in an organic solvent. The mixture is then compounded using a spray drying method with a specified spray pressure and liquid delivery rate to produce composite active material particles (composite active material particle preparation process).

[0151] Negative electrode fabrication

[0152] A binder, conductive material, solid electrolyte (SE), and the aforementioned composite active material particles are added to an organic solvent. Then, the mixture is kneaded using an ultrasonic homogenizer to obtain a slurry for the negative electrode layer (slurry preparation step for the negative electrode layer).

[0153] The obtained negative electrode layer is coated onto the Ni foil, which serves as the negative electrode current collector, using a slurry (coating process).

[0154] For the slurry used in the negative electrode layer, a magnetic field of 1T is applied for 5 minutes relative to the thickness direction of the negative electrode current collector (magnetic field orientation process).

[0155] The negative electrode layer is dried with slurry to form a negative electrode with a negative electrode layer on the negative electrode current collector (drying process).

[0156] Positive electrode production

[0157] Add binders, conductive materials, SE, and LiNi as the positive electrode active material to an organic solvent. 0.8 Co 0.15 Mn 0.05 O2. Then, the mixture is kneaded using an ultrasonic homogenizer to obtain a slurry for the positive electrode layer. The obtained slurry for the positive electrode layer is coated onto an Al foil serving as the positive electrode current collector, dried, and a positive electrode with a positive electrode layer on the positive electrode current collector is fabricated.

[0158] Fabrication of solid electrolyte layer

[0159] A binder and SE are added to an organic solvent. Then, the mixture is kneaded using an ultrasonic homogenizer to obtain a slurry for a solid electrolyte layer. The obtained solid electrolyte layer slurry is coated onto an Al foil as a substrate and dried to produce a solid electrolyte layer with an Al foil.

[0160] Battery manufacturing

[0161] The positive electrode layer of the positive electrode is bonded to a solid electrolyte layer containing an Al foil, and then rolled at 165°C and 50 kN / cm pressure to peel off the Al foil from the solid electrolyte layer, thereby transferring the first solid electrolyte to the positive electrode layer. Similarly, the negative electrode layer of the negative electrode is bonded to a solid electrolyte layer containing an Al foil, and then rolled at 25°C and 50 kN / cm pressure to peel off the Al foil from the solid electrolyte layer, thereby transferring the second solid electrolyte to the negative electrode layer. The negative electrode with the transferred second solid electrolyte layer is cut using a Φ13.00 mm die-cutting machine. The positive electrode with the transferred first solid electrolyte layer is cut using a Φ11.28 mm die-cutting machine. A third solid electrolyte layer is further transferred onto the second solid electrolyte layer of the negative electrode with the second solid electrolyte layer. The third solid electrolyte layer of the negative electrode with the transferred solid electrolyte layer is then aligned with the first solid electrolyte layer of the positive electrode with the transferred solid electrolyte layer, thus forming a battery. Finally, current is installed on the positive and negative electrodes to remove the tabs. The positive electrode, solid electrolyte layer and negative electrode are then sealed into the aluminum laminate using a vacuum lamination sealing machine and constrained with a pressure of 5MPa to produce the battery (pressing process).

[0162] Comparative Example 1

[0163] Except that the magnetic field orientation process was not performed in the above-mentioned "fabrication of the negative electrode", the battery was obtained in the same manner as in Example 1.

[0164] Observation of the negative electrode layer

[0165] The fabricated battery was disassembled, and the cross-section of the negative electrode layer after ion milling was analyzed using SEM. The SEM acceleration voltage was set to 2.0 kV, the magnification to 2000x, and five arbitrary locations were observed. After excluding images showing electrode cracking, the lengths L1 and L2 of the composite active material particles in the thickness direction and width direction of the negative electrode layer were measured within the field of view, and the flatness ratio A1 of the composite active material particles was calculated. The flatness ratio A1 of the composite active material particles was 0.45 in Comparative Example 1 and 0.30 in Example 1. A flatness ratio A1 of 0.45 means that when L2 is set to 100, L1 is 55. A flatness ratio A1 of 0.30 means that when L2 is set to 100, L1 is 70. Therefore, it can be seen that the composite active material particles of Example 1 are horizontally elongated and flat in the cross-section of the negative electrode layer, but compared with the composite active material particles of Comparative Example 1, the degree of horizontal elongation and flatness is suppressed (more spherical).

[0166] Constraint pressure variation measurement

[0167] Three batteries of Example 1 (Examples 1-1 to 1-3) and three batteries of Comparative Example 1 (Comparative Examples 1-1 to 1-3) were prepared. The constraint pressure of each prepared battery was measured using a load sensor, and the pressure change from the uncharged state of the battery to reaching 4.05V was taken as the constraint pressure change.

[0168] Figure 5 The graph shows the flatness A1 of each composite active material particle and the variation of the constraint pressure of each battery in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3.

[0169] It was confirmed that Example 1 was able to suppress the confinement pressure variation (i.e., the expansion amount of the negative electrode layer) compared to Comparative Example 1.

[0170] Based on the above results, it was confirmed that by making the flatness ratio A1 of the composite active material particles contained in the negative electrode layer greater than 0.30 and less than 0.45, the confinement voltage variation of the battery can be suppressed.

Claims

1. A negative electrode, which is a negative electrode comprising a negative electrode layer containing composite active material particles, and a negative electrode current collector, wherein The composite active material particles comprise: a negative electrode active material containing at least one of Si and Sn elements, a binder, and a conductive carbon material. The flatness A1 of the composite active material particles contained in the negative electrode layer, calculated by the following formula, is greater than 0.30 and less than 0.

45. Flatness ratio A1 = 1 - L1 / L2 L1: Length of the composite active material particles in the thickness direction of the negative electrode layer. L2: The length of the composite active material particles in the width direction of the negative electrode layer.

2. The method for manufacturing the negative electrode according to claim 1, comprising: The process of preparing the composite active substance particles; The process of preparing a slurry for a negative electrode layer comprising the composite active material particles, the binder, the conductive material, and the solvent; The process of coating the negative electrode layer slurry onto one surface of the negative electrode current collector; A magnetic field orientation process is performed by applying a magnetic field perpendicular to the surface of the negative electrode current collector to the slurry of the negative electrode layer, so that the long side of the composite active material particles is oriented in the thickness direction. A drying process is performed after the magnetic field orientation process to dry the negative electrode layer with a slurry to obtain the negative electrode layer. and The pressing process for pressing the negative electrode layer.

3. A solid-state battery having the negative electrode as described in claim 1.

Citation Information

Patent Citations

  • Anode for secondary battery, anode manufacturing method, and secondary battery including the anode

    JP2023104840A