Batteries and battery manufacturing methods

By using different distributions of the first and second composite particles in the negative electrode layer and adjusting the proportion and content of the binder, the problem of negative electrode layer peeling caused by volume change of Si-based active material was solved, thus improving the adhesion and energy density of the battery.

CN123120641APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610363593.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-03-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The large volume change of Si-based active materials during charging and discharging causes the negative electrode layer to peel off from adjacent components, and existing technologies are unable to effectively suppress this problem.

Method used

By employing the distribution of first and second composite particles in different regions of the negative electrode layer and adjusting the proportion and content of the adhesive, the adhesion between the negative electrode layer and adjacent components is ensured, and peeling is suppressed.

Benefits of technology

It effectively suppressed the peeling of the negative electrode layer, maintained the energy density of the battery, and improved adhesion, avoiding the reduction in energy density caused by large constraint components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120641A_ABST
    Figure CN123120641A_ABST
Patent Text Reader

Abstract

This invention relates to batteries and methods for manufacturing batteries. The negative electrode layer contains a first composite particle and a second composite particle, each containing a Si-based active material and a binder. The first composite particle has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. The second composite particle also has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. The negative electrode layer satisfies predetermined conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to batteries and methods for manufacturing batteries. Background Technology

[0002] In recent years, battery development has been booming. For example, in the automotive industry, development is underway for batteries used in battery electric vehicles (BEVs), plug-in hybrid electric vehicles (PHEVs), and hybrid electric vehicles (HEVs). Batteries typically have a positive electrode layer, a negative electrode layer, and an electrolyte layer disposed between the positive and negative electrode layers. Furthermore, active materials containing silicon (Si-based active materials) are known as electrode active materials.

[0003] For example, Japanese Patent Application Publication No. 2019-121557 discloses a negative electrode layer having a negative electrode active material and a sulfide solid electrolyte. The negative electrode active material is a composite particle having multiple particles containing Si or Sn elements and a binder, with a porosity of 15% or less. Furthermore, Japanese Patent Application Publication No. 2024-017879 discloses composite particles containing Si and resin. Summary of the Invention

[0004] Si-based active materials are high-capacity negative electrode active materials; however, they exhibit significant volume changes during charge and discharge. Large volume changes during charge and discharge can lead to the negative electrode layer peeling off from adjacent components such as the electrolyte layer and the negative electrode current collector. To address this, studies have been conducted on using a binder to absorb the expansion and contraction of the Si-based active material, thereby suppressing the volume change of the negative electrode layer. However, there is room for improvement in suppressing the peeling of the negative electrode layer.

[0005] The present invention was made in view of the above-mentioned actual situation, and provides a battery in which the peeling of the negative electrode layer is suppressed.

[0006] The battery of the first aspect of the present invention has a negative electrode current collector, a negative electrode layer, an electrolyte layer, a positive electrode layer, and a positive electrode current collector. In the thickness direction, the negative electrode current collector, the negative electrode layer, the electrolyte layer, the positive electrode layer, and the positive electrode current collector are stacked in the following order: negative electrode current collector, negative electrode layer, electrolyte layer, positive electrode layer, and positive electrode current collector. The negative electrode layer contains a first composite particle and a second composite particle. Each of the first and second composite particles contains a Si-based active material and a binder. The first composite particle has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. The second composite particle has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. When the proportion of the adhesive in the outer edge region of the first composite particle is set to X1, the proportion of the adhesive in the inner region of the first composite particle is set to X2, the proportion of the adhesive in the outer edge region of the second composite particle is set to Y1, and the proportion of the adhesive in the inner region of the second composite particle is set to Y2, X1 and X2 satisfy 1.2≤(X1 / X2), and Y1 and Y2 satisfy (Y1 / Y2)<1.2. When X1 and X2 satisfy 1.2 ≤ (X1 / X2), Y1 and Y2 satisfy (Y1 / Y2) < 1.2, and the thickness of the negative electrode layer is set to T, in the thickness direction, the region of the negative electrode layer at a distance of 0T or more and 0.2T or less from the end of the negative electrode current collector side of the negative electrode layer is designated as the first region, the region of the negative electrode layer at a distance of 0.4T or more and 0.6T or less from the end is designated as the second region, and the region of the negative electrode layer at a distance of 0.8T or more and 1.0T or less from the end is designated as the third region. In this case, the negative electrode layer satisfies any one of the first, second, and third conditions. The first condition is: in the first region, the content of the first composite particle is greater than the content of the second composite particle, and in the third region, the content of the second composite particle is greater than the content of the first composite particle. The second condition is: in the first region, the content of the second composite particle is greater than the content of the first composite particle; in the third region, the content of the first composite particle is greater than the content of the second composite particle. The third condition is: in the first region, the content of the first composite particle is greater than the content of the second composite particle; in the second region, the content of the second composite particle is greater than the content of the first composite particle; in the third region, the content of the first composite particle is greater than the content of the second composite particle. The content of the first composite particle is 0 or more. The content of the second composite particle is 0 or more.

[0007] In the battery of the first aspect of the present invention, X1 and X2 can satisfy (X1 / X2)≤3.6.

[0008] In the battery of the first aspect of the present invention, Y1 and Y2 can satisfy (Y1 / Y2)≤1.0.

[0009] In the battery described in the first aspect of the present invention, T can be 30 μm or more and 1000 μm or less.

[0010] In the battery described in the first aspect of the present invention, the electrolyte layer may contain a solid electrolyte.

[0011] In the battery of the first aspect of the present invention, the electrolyte layer may contain a sulfide solid electrolyte as the solid electrolyte.

[0012] In the battery described in the first aspect of the present invention, the Si-based active material may be porous particles.

[0013] In the battery described in the first aspect of the present invention, the battery may be a solid-state battery.

[0014] In the battery of the first aspect of the present invention, the content of the first composite particle can be 30% or more and 60% or less by weight, the content of the second composite particle can be 30% or more and 60% or less by weight, and the total content of the first composite particle and the second composite particle can be 60% or more and 90% or less by weight.

[0015] In the battery of the first aspect of the present invention, Y1 and Y2 can satisfy 0.6≤(Y1 / Y2).

[0016] The second aspect of the present invention describes a method for manufacturing the battery described above, which may include the following steps: preparing a first negative electrode composite material containing the first composite particles and a second negative electrode composite material containing the second composite particles; forming a first negative electrode layer using the first negative electrode composite material; and forming a second negative electrode layer on the first negative electrode layer using the second negative electrode composite material.

[0017] In the manufacturing method described above in the second aspect of the present invention, the following steps may be included: forming a third negative electrode layer on the second negative electrode layer using a third negative electrode composite material containing the first composite particles described above.

[0018] In this invention, the battery effect of suppressing the stripping of the negative electrode layer is achieved. Attached Figure Description

[0019] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will be described below with reference to the accompanying drawings, wherein the same symbols denote the same elements.

[0020] Figure 1 This is a schematic cross-sectional view illustrating the battery in this invention.

[0021] Figure 2A This is a schematic cross-sectional view illustrating the first and second composite particles in this invention.

[0022] Figure 2B yes Figure 2A A magnified view of a portion of the image.

[0023] Figure 3 This is a schematic cross-sectional view illustrating the negative electrode layer in this invention.

[0024] Figure 4 This is a schematic cross-sectional view of a battery in which the negative electrode layer satisfies condition (i).

[0025] Figure 5 This is a schematic cross-sectional view of a battery in which the negative electrode layer satisfies condition (ii).

[0026] Figure 6 This is a schematic cross-sectional view of a battery in which the negative electrode layer satisfies condition (iii).

[0027] Figure 7 This is a flowchart illustrating a method for manufacturing a battery according to the present invention.

[0028] Figure 8 This is a schematic cross-sectional view of the negative electrode layer fabricated in Comparative Example 1. Detailed Implementation

[0029] The battery and its manufacturing method according to the present invention will now be described in detail. It should be noted that the figures shown below are schematic illustrations, and the size and shape of the parts are appropriately exaggerated for ease of understanding.

[0030] A. Battery

[0031] Figure 1 This is a schematic cross-sectional view illustrating the battery in this invention. Figure 2A and Figure 2B This is a schematic cross-sectional view illustrating the first and second composite particles in this invention. It should be noted that... Figure 2B It is Figure 2A A magnified partial view of the right side. Additionally, Figure 3 This is a schematic cross-sectional view illustrating the negative electrode layer in this invention. Figure 1 As shown, the battery 10 has a thickness direction D TThe electrode comprises, in sequence, a negative current collector 1, a negative electrode layer 2, an electrolyte layer 3, a positive electrode layer 4, and a positive current collector 5. The negative electrode layer 2 contains a first composite particle and a second composite particle, each of which contains a Si-based active material and a binder.

[0032] In addition, such as Figure 2A and Figure 2B As shown, the first composite particle and the second composite particle each have an outer edge region α containing the outer edge E and an inner region β located inside the outer edge region α in their cross-sectional shape. That is, the first composite particle has an outer edge region α containing the outer edge E and an inner region β located inside the outer edge region α in its cross-sectional shape, and the second composite particle has an outer edge region α containing the outer edge E and an inner region β located inside the outer edge region α in its cross-sectional shape. In addition, when the proportion of the binder present in the outer edge region α of the first composite particle is set to X1, the proportion of the binder in the inner region β of the first composite particle is set to X2, the proportion of the binder present in the outer edge region α of the second composite particle is set to Y1, and the proportion of the binder in the inner region β of the second composite particle is set to Y2, X1 and X2 satisfy 1.2 ≤ (X1 / X2), and Y1 and Y2 satisfy (Y1 / Y2) < 1.2.

[0033] Furthermore, such as Figure 3 As shown, when the thickness of the negative electrode layer 2 is set to T, in the thickness direction D... T In this configuration, the region of the negative electrode layer 2 at a distance of 0T or more and 0.2T or less from the end P on the negative electrode current collector 1 side of the negative electrode layer 2 is designated as the first region 2a; the region of the negative electrode layer 2 at a distance of 0.4T or more and 0.6T or less from the end P on the negative electrode current collector 1 side of the negative electrode layer 2 is designated as the second region 2b; and the region of the negative electrode layer 2 at a distance of 0.8T or more and 1.0T or less from the end P on the negative electrode current collector 1 side of the negative electrode layer 2 is designated as the third region 2c. In this case, the negative electrode layer 2 satisfies any one of the following conditions (i), (ii), and (iii). Conditions (i), (ii), and (iii) can also be represented as the first condition, the second condition, and the third condition, respectively.

[0034] Condition(i)

[0035] In the first region 2a, the content of the first composite particle is greater than the content of the second composite particle (including 0), and in the third region 2c, the content of the second composite particle is greater than the content of the first composite particle (including 0).

[0036] Condition (ii)

[0037] In the first region 2a, the content of the second composite particle is greater than the content of the first composite particle (including 0), and in the third region 2c, the content of the first composite particle is greater than the content of the second composite particle (including 0).

[0038] Condition (iii)

[0039] In the first region 2a, the content of the first composite particle is greater than the content of the second composite particle (including 0); in the second region 2b, the content of the second composite particle is greater than the content of the first composite particle (including 0); and in the third region 2c, the content of the first composite particle is greater than the content of the second composite particle (including 0).

[0040] According to the present invention, the negative electrode layer contains a specified first composite particle and a second composite particle, and satisfies any one of the conditions (i) to (iii) above, thus becoming a battery in which the stripping of the negative electrode layer is suppressed. Furthermore, the content of the first composite particle and the content of the second composite particle can be 0 or more.

[0041] As detailed later, in the first composite particle, the binder is more concentrated near the outer edge compared to the second composite particle. Therefore, the first composite particle has better adhesion than the second composite particle. Furthermore, as detailed later, under any of the conditions (i) to (iii) above, such as... Figures 4-6 As shown, in the negative electrode layer, the first composite particles are present in greater quantity than the second composite particles on at least one side, either the negative electrode current collector side or the electrolyte layer side. Therefore, the adhesion between the negative electrode layer and adjacent components becomes good, and in the battery of the present invention, delamination of the negative electrode layer is suppressed.

[0042] Here, it is believed that the peeling of the negative electrode layer can be suppressed by increasing the strength and size of the constraint member. On the other hand, if the constraint member is enlarged, the energy density of the battery decreases. In contrast, in the battery of the present invention, by adjusting the configuration of the first composite particles with good adhesion, the peeling of the negative electrode layer can be suppressed, thus also having advantages in terms of energy density.

[0043] 1. Negative electrode layer

[0044] 1.1 Materials of the negative electrode layer

[0045] First composite particle and second composite particle

[0046] The negative electrode layer in this invention contains a first composite particle and a second composite particle. Both the first composite particle and the second composite particle function as negative electrode active materials in the negative electrode layer. Here, in this invention, when referred to only as "composite particles," it is considered that both the first composite particle and the second composite particle are mentioned.

[0047] like Figure 2A and Figure 2B As shown, the composite particle in this invention has an outer edge region α containing an outer edge E and an inner region β located inside the outer edge region α in its cross-sectional shape. In this invention, the outer edge region α is the portion of the composite particle within a length L from the outer edge E. Furthermore, the inner region β refers to the portion of the composite particle that is farther from the outer edge E than the length L.

[0048] Here, the average particle size (D) of the composite particles is... 50 Let L be the value of L. D In the case mentioned above, the length L satisfies L / L D =0.2. As mentioned above, the length L is based on the average particle size L of the composite particles. D Therefore, the specific value of the length L is not particularly limited, for example, it can be greater than 2 μm and less than 20 μm. Regarding the average particle size L of the composite particles... D (D 50 (This will be described later.)

[0049] Furthermore, in the first composite particle and the second composite particle, the proportion of the adhesive in the outer region and the proportion of the adhesive in the inner region each satisfy a specified relationship.

[0050] In the first composite particle, the proportion X1 of binder in the outer region and the proportion X2 of binder in the inner region satisfy 1.2 ≤ (X1 / X2). In the first composite particle, compared to the second composite particle (described later), the binder is more concentrated near the outer edge. (X1 / X2) can be 1.3 or higher, 1.5 or higher, 1.7 or higher, 2.0 or higher, 2.3 or higher, or 2.5 or higher. There is no particular upper limit for (X1 / X2), for example, it can be 4.8 or lower, 4.0 or lower, 3.8 or lower, 3.6 or lower, 3.3 or lower, 3.1 or lower, 2.8 or lower, or 2.5 or lower. If (X1 / X2) is too large, i.e., if the binder is excessively concentrated in the outer region, the binder may hinder the reaction of the Si-based active material within the first composite particle. In this case, the reaction concentrates in the second composite particle (described later), which deteriorates due to repeated charge-discharge cycles, potentially reducing the battery's capacity retention rate.

[0051] Furthermore, in the second composite particle, the ratio of binder Y1 in the outer region to the ratio of binder Y2 in the inner region satisfies (Y1 / Y2) < 1.2. (Y1 / Y2) can be 1.1 or less, or 1.0 or less. On the other hand, (Y1 / Y2) can be, for example, 0.6 or more, 0.8 or more, or 0.9 or more.

[0052] The proportion of the binder can be determined, for example, by cross-sectional observation of the negative electrode layer using a scanning electron microscope (SEM). First, the cross-section of the negative electrode layer is exposed by, for example, ion milling to obtain a cross-sectional image of the composite particle. EDX mapping analysis is performed on the obtained cross-sectional image to distinguish the Si-based active material portion and the binder portion. Then, the area of ​​the binder portion in each of the outer and inner regions is calculated, thereby determining the proportion of the binder. Alternatively, osmium oxide (OsO4) can be used to stain the binder in the cross-section of the composite particle, and the area of ​​the stained portion in each of the outer and inner regions can be calculated, thereby determining the proportion of the binder. Thus, the proportion of the binder in this invention can be understood as the area proportion of the binder. More specifically, X1 and Y1 can be understood as the proportion of the area of ​​the binder in the outer region relative to the area of ​​the outer region. Similarly, X2 and Y2 can be understood as the proportion of the area of ​​the binder in the inner region relative to the area of ​​the inner region.

[0053] For each particle in the first and second composite particles, the binder ratio is preferably the average value obtained by measuring multiple samples (particles). The number of samples can be, for example, 10 or more, 20 or more, 50 or more, or 100 or more. The field of view of the SEM image used to determine the binder ratio is preferably set to include the field of view of the aforementioned number or more composite particles. The field of view is, for example, 1000 μm. 2 Above and 50000μm 2 the following.

[0054] The composite particles in this invention contain Si-based active materials.

[0055] Examples of active materials based on Si include elemental Si, Si alloys, and Si oxides. Examples of Si alloys include Si-Al alloys, Si-Sn alloys, Si-In alloys, Si-Ag alloys, Si-Pb alloys, Si-Sb alloys, Si-Bi alloys, Si-Mg alloys, Si-Ca alloys, Si-Ge alloys, and Si-Pb alloys. Si alloys can be two-component alloys or multi-component alloys with three or more components. It should be noted that Si alloys preferably contain Si as the main component. Examples of Si oxides include SiO.

[0056] Si-based active materials can be primary particles or secondary particles formed by the aggregation of primary particles. Furthermore, Si-based active materials can be solid particles or porous particles (porous Si) with voids within, particularly within, the primary particles. The voids within the primary particles can be confirmed by SEM (scanning electron microscopy). The porosity of the primary particles is not particularly limited; for example, it can be 4% or more, or 10% or more. Additionally, the aforementioned porosity can be, for example, below 40%, or below 20%. The porosity can be calculated, for example, by the following steps: First, obtain a cross-sectional image of the Si-based active material using SEM. Use image analysis software to strictly distinguish between the silicon portion and the void portion from the obtained image and perform binarization. Calculate the area of ​​the silicon portion and the void portion, and then calculate the porosity (%) using the following formula.

[0057] Porosity (%) = 100 × (Area of ​​voids) / ((Area of ​​silicon) + (Area of ​​voids))

[0058] The average pore diameter in the primary particles (porous Si) is not particularly limited, but is, for example, 10 nm or more and 100 nm or less. In addition, the amount of voids with a pore diameter of 50 nm or less in the primary particles is, for example, 0.05 cc / g or more and 0.30 cc / g or less.

[0059] One method for producing porous Si is to prepare an alloy of Li and Si (LiSi alloy) and then remove Li from the LiSi alloy. The LiSi alloy is obtained, for example, by mixing Li and Si. Another method for removing Li from the LiSi alloy is to react the LiSi alloy with a Li extraction material. Examples of Li extraction materials include alcohols such as methanol and acids such as acetic acid.

[0060] Si-based active materials can be crystalline or amorphous. When crystalline, they typically possess a Si crystalline phase. One example of a Si crystalline phase is the diamond-type phase. Ordinary Si contains a diamond-type phase as its main Si crystalline phase. Si-based active materials can contain a diamond-type phase as the dominant Si crystalline phase.

[0061] Other examples of Si crystalline phases include silicon cladding phases. These silicon cladding phases can be either type I or type II. In a silicon cladding phase, multiple Si elements form a polyhedron (cage) containing pentagons or hexagons. This polyhedron has internal spaces capable of containing metal ions such as Li ions. By inserting metal ions into these spaces, volume changes caused by charging and discharging can be further suppressed. Si-based active materials can contain either type I or type II silicon cladding phases as the main Si crystalline phase.

[0062] The proportion (content) of Si-based active material in the first composite particle and the second composite particle is, for example, 70% by weight or more and 95% by weight or less.

[0063] The composite particles in this invention contain a binder.

[0064] There is no particular limitation on the type of binder in the composite particles. Examples of binders include rubber-based binders such as butadiene rubber (BR) and styrene-butadiene rubber (SBR), and fluoride-based binders such as polyvinylidene fluoride (PVdF). The composite particles may contain one type of binder or more than two types of binders. Furthermore, the types of binders may be the same or different in the first and second composite particles.

[0065] The content of binder in the composite particles is not particularly limited, for example, it is more than 1% by weight and less than 30% by weight.

[0066] The composite particles in this invention are particles formed by the aggregation of multiple of the aforementioned Si-based active materials with a binder. The number of Si-based active materials contained in the composite particles is, for example, 10 or more and 100 or less. The average particle size (D) of the composite particles... 50 There are no specific limitations; for example, it can be between 10 μm and 100 μm. Average particle size (D) 50 The average particle size refers to the particle size that accounts for 50% of the cumulative frequency in the particle size distribution. The average particle size can be a value determined by laser diffraction scattering particle size distribution measurement method, or a value determined by image analysis using software.

[0067] The total ratio of the first and second composite particles in the negative electrode layer (the content of composite particles) is not particularly limited, but is, for example, 60% by weight or more and 90% by weight or less. If the content of composite particles is too low, sufficient battery capacity may not be obtained. On the other hand, if the content of composite particles is too high, sufficient electronic and ionic conductivity may not be obtained. Furthermore, in the negative electrode layer, the content of the first composite particles is, for example, 30% by weight or more and 60% by weight or less, and the content of the second composite particles is, for example, 30% by weight or more and 60% by weight or less.

[0068] There are no particular limitations on the method for producing composite particles; spray drying is an example. Spray drying involves spraying a slurry containing the aforementioned Si-based active material, binder, and dispersion medium into hot air for drying. The proportions of the binder (X1, X2, Y1, and Y2) can be controlled by adjusting the NV value of the slurry, as well as the drying temperature and slurry feed rate, among other conditions of the spray drying method. For example, by increasing the NV value of the slurry, the concentration of the binder within the particles can be increased. Furthermore, by increasing the spray pressure, the concentration of the binder within the particles can be further increased. Additionally, by increasing the slurry feed rate, the concentration of the binder within the particles can be further increased.

[0069] The NV value of the slurry capable of producing the first composite particles is, for example, 15% or more and 30% or less. In this invention, NV value (Non-Volatile content) refers to the weight percentage of non-volatile components (solid components) contained in the slurry. Furthermore, the drying temperature capable of producing the first composite particles is, for example, 180°C or more and 200°C or less. Additionally, the slurry feed rate capable of producing the first composite particles is, for example, 100 g / hour or more and 200 g / hour or less.

[0070] The NV value of the slurry capable of producing the second composite particles is, for example, 5% or more and 15% or less. Furthermore, the drying temperature capable of producing the second composite particles is, for example, 120°C or more and 140°C or less. Additionally, the slurry feed rate capable of producing the second composite particles is, for example, 400 g / hour or more and 600 g / hour or less.

[0071] Other materials

[0072] In addition to the first and second composite particles mentioned above, the negative electrode layer may also contain at least one of conductive additives, binders, and electrolytes.

[0073] Examples of conductive additives include carbon materials, metal particles, and conductive polymers. Examples of carbon materials include particulate carbon materials such as acetylene black (AB) and Ketjen black (KB), as well as fibrous carbon materials such as carbon fibers, carbon nanotubes (CNTs), and carbon nanofibers (CNFs). The proportion of the conductive additive in the negative electrode layer is, for example, 0.1% by weight or more and 10% by weight or less.

[0074] As a type of binder, the same binder as the composite particles described above can be cited. The proportion of binder in the negative electrode layer (excluding the binder in the composite particles) is not particularly limited, for example, it is more than 1% by weight and less than 10% by weight.

[0075] The type of electrolyte is described in "3. Electrolyte Layer". The proportion of electrolyte in the negative electrode layer is, for example, 10% by weight or more and 60% by weight or less.

[0076] 1.2 Negative Electrode Layer Method

[0077] like Figure 3 As shown, when the thickness of the negative electrode layer 2 is set to T, in the thickness direction D... T In this designation, the region of the negative electrode layer 2 at a distance of 0T or more and 0.2T or less from its end P on the negative electrode current collector 1 side is designated as the first region 2a; the region of the negative electrode layer 2 at a distance of 0.4T or more and 0.6T or less from its end P on the negative electrode current collector 1 side is designated as the second region 2b; and the region of the negative electrode layer 2 at a distance of 0.8T or more and 1.0T or less from its end P on the negative electrode current collector 1 side is designated as the third region 2c. It should be noted that the position at a distance of 0T can be understood as the interface between the negative electrode current collector 1 and the negative electrode layer 2, and the position at a distance of 1.0T can be understood as the interface between the negative electrode layer 2 and the electrolyte layer 3.

[0078] The negative electrode layer in this invention can be broadly categorized into three types based on the relationship (conditions) between the content of the first composite particles and the content of the second composite particles in the aforementioned regions. Here, the content of the first composite particles can be by weight. Alternatively, the content of the first composite particles can be the area of ​​particles observed from cross-sectional SEM images of each region, or it can be the number of particles. The same applies to the content of the second composite particles.

[0079] The negative electrode layer in this invention can satisfy the following condition (i).

[0080] Condition(i)

[0081] In the first region, the content of the first composite particle is greater than the content of the second composite particle (including 0), and in the third region, the content of the second composite particle is greater than the content of the first composite particle (including 0).

[0082] In condition (i), the ratio of the content of the first composite particle in the first region to the total content of the first composite particle and the content of the second composite particle is typically 0.51 or more, but can be 0.60 or more, 0.70 or more, 0.80 or more, or 0.90 or more. Furthermore, the aforementioned ratio in the first region is typically 1 or less, but can be 0.99 or less, or 0.95 or less.

[0083] In condition (i), the ratio of the content of the second composite particle in the third region to the total content of the first composite particle and the second composite particle is typically 0.51 or more, and can be 0.60 or more, 0.70 or more, 0.80 or more, or 0.90 or more. Furthermore, the aforementioned ratio in the third region is typically 1 or less, and can be 0.99 or less, or 0.95 or less.

[0084] use Figure 4 An example of a battery in which the negative electrode layer satisfies condition (i) will be explained. Figure 4 The battery 10 shown has a thickness direction D T The electrode comprises, in sequence, a negative electrode current collector 1, a first negative electrode layer 2S containing only the aforementioned first composite particles as the negative electrode active material, a second negative electrode layer 2T containing only the aforementioned second composite particles as the negative electrode active material, and an electrolyte layer 3. The first negative electrode layer 2S and the second negative electrode layer 2T constitute the negative electrode layer 2. Furthermore, the thickness of both the first negative electrode layer 2S and the second negative electrode layer 2T is 0.5T. A first region (a region with a distance of 0T or more and 0.2T or less) is part of the first negative electrode layer 2S, and therefore does not contain second composite particles. That is, the ratio of the first composite particles in the first region to the total amount of the first and second composite particles is 1. Therefore, in the first region, the content of first composite particles is greater than the content of second composite particles. Similarly, a third region (a region with a distance of 0.8T or more and 1.0T or less) is part of the second negative electrode layer 2T, and therefore does not contain first composite particles. That is, the ratio of the second composite particles in the third region to the total amount of the first and second composite particles is 1. Therefore, in the third region, the content of second composite particles is greater than the content of first composite particles.

[0085] It should be noted that, in condition (i), the relationship between the content of the first composite particle and the content of the second composite particle in the second region (the region with a distance greater than 0.4T and less than 0.6T) is not particularly limited. For example, in Figure 4In the battery 10 shown, the second region includes a portion of the first negative electrode layer 2S and a portion of the second negative electrode layer 2T. In this case, if the content of composite particles in the first negative electrode layer 2S and the second negative electrode layer 2T is the same, then the content of the first composite particles in the second region is the same as the content of the second composite particles. On the other hand, in Figure 4 In the case where the thickness of the first negative electrode layer 2S is 0.3T and the thickness of the second negative electrode layer 2T is 0.7T, the second region is a part of the second negative electrode layer 2T. Therefore, in the second region, the content of the second composite particles is greater than the content of the first composite particles.

[0086] In addition, the negative electrode layer in this invention can satisfy the following condition (ii).

[0087] Condition (ii)

[0088] In the first region, the content of the second composite particle is greater than the content of the first composite particle (including 0), and in the third region, the content of the first composite particle is greater than the content of the second composite particle (including 0).

[0089] In condition (ii), the ratio of the content of the second composite particle in the first region to the total content of the first composite particle and the content of the second composite particle is typically 0.51 or more, and may be 0.60 or more, 0.70 or more, 0.80 or more, or 0.90 or more. Furthermore, the aforementioned ratio in the first region is typically 1 or less, and may be 0.99 or less, or 0.95 or less.

[0090] In condition (ii), the ratio of the content of the first composite particle in the third region to the total content of the first composite particle and the content of the second composite particle is typically 0.51 or higher, and may be 0.60 or higher, 0.70 or higher, 0.80 or higher, or 0.90 or higher. Furthermore, the aforementioned ratio in the third region is typically 1 or lower, and may be 0.99 or lower, or 0.95 or lower.

[0091] use Figure 5 An example of a battery in which the negative electrode layer satisfies condition (ii) will be described. Figure 5 The battery 10 shown has a thickness direction D T The structure comprises, in sequence, a negative electrode current collector 1, a second negative electrode layer 2T containing only the aforementioned second composite particles as the negative electrode active material, a first negative electrode layer 2S containing only the aforementioned first composite particles as the negative electrode active material, and an electrolyte layer 3. Figure 4Similarly, the first negative electrode layer 2S and the second negative electrode layer 2T constitute the negative electrode layer 2, both with a thickness of 0.5T. The first region (a region with a distance of 0T or more but less than 0.2T) is part of the second negative electrode layer 2T, and therefore does not contain first composite particles. Therefore, in the first region, the content of second composite particles is greater than the content of first composite particles. Furthermore, the third region (a region with a distance of 0.8T or more but less than 1.0T) is part of the first negative electrode layer 2S, and therefore does not contain second composite particles. Therefore, in the third region, the content of first composite particles is greater than the content of second composite particles.

[0092] Similar to condition (i) above, in condition (ii), there is no particular limitation on the relationship between the content of the first composite particle and the content of the second composite particle in the second region (the region with a distance of more than 0.4T and less than 0.6T).

[0093] In addition, the negative electrode layer in this invention can satisfy the following condition (iii).

[0094] Condition (iii)

[0095] In the first region, the content of the first composite particle is greater than the content of the second composite particle (including 0); in the second region, the content of the second composite particle is greater than the content of the first composite particle (including 0); and in the third region, the content of the first composite particle is greater than the content of the second composite particle (including 0).

[0096] In condition (iii), the relationship between the content of the first composite particle and the content of the second composite particle in the first and third regions is the same as that in the first region in condition (i). Furthermore, in condition (iii), the relationship between the content of the first composite particle and the content of the second composite particle in the second region is the same as that in the third region in condition (i).

[0097] use Figure 6 An example of a battery in which the negative electrode layer satisfies condition (iii) will be explained. Figure 6 The battery 10 shown has a thickness direction D TThe structure comprises, in sequence, a negative electrode current collector 1, a first negative electrode layer 2S containing only the aforementioned first composite particles as the negative electrode active material, a second negative electrode layer 2T containing only the aforementioned second composite particles as the negative electrode active material, a third negative electrode layer 2U containing only the aforementioned first composite particles as the negative electrode active material, and an electrolyte layer 3. The first negative electrode layer 2S, the second negative electrode layer 2T, and the third negative electrode layer 2U constitute the negative electrode layer 2. Furthermore, the thickness of the first negative electrode layer 2S, the second negative electrode layer 2T, and the third negative electrode layer 2U is 0.33T (1 / 3T). The first region (a region with a distance of 0T or more and 0.2T or less) is part of the first negative electrode layer 2S, and therefore does not contain the second composite particles. Therefore, in the first region, the content of the first composite particles is greater than the content of the second composite particles. The second region (a region with a distance of 0.4T or more and 0.6T or less) is part of the second negative electrode layer 2T, and therefore does not contain the first composite particles. Therefore, in the second region, the content of the second composite particles is greater than the content of the first composite particles. Furthermore, the third region (the region with a distance greater than 0.8T and less than 1.0T) is part of the third negative electrode layer 2U, and therefore does not contain second composite particles. Thus, in the third region, the content of first composite particles is greater than that of second composite particles.

[0098] In regions other than the first to third regions within the negative electrode layer, the relationship between the content of the first composite particles and the content of the second composite particles is not particularly limited. When a region at a distance greater than 0.2T and less than 0.4T from the end of the negative electrode current collector side of the negative electrode layer is designated as the fourth region, and a region at a distance greater than 0.6T and less than 0.8T from the end of the negative electrode current collector side of the negative electrode layer is designated as the fifth region, in each of the fourth and fifth regions, the content of the first composite particles compared to the content of the second composite particles can be less, the same, or more. The same content means that the absolute value of the difference between the two contents is less than 0.1. For example, in... Figure 4 In the fourth region of the negative electrode layer 2, the content of the first composite particles is greater than that of the second composite particles. Furthermore, in... Figure 4 In the fifth region of the negative electrode layer 2, the content of the second composite particles is greater than that of the first composite particles.

[0099] Here, the above Figures 4-6 The battery shown is an example of a multi-layered negative electrode layer, and the battery in this invention is not limited to these. For example, it may also be a so-called concentration gradient layer in which the negative electrode layer is a single layer and the contents of the first composite particles and the contents of the second composite particles change continuously in the thickness direction in such a way as to satisfy any of the conditions (i) to (iii) above.

[0100] The thickness (T) of the negative electrode layer is not particularly limited; for example, it can be 30 μm or more, 50 μm or more, or 100 μm or more. On the other hand, the thickness of the negative electrode layer can be, for example, 1000 μm or less, 800 μm or less, 500 μm or less, 300 μm or less, or 100 μm or less.

[0101] 2. Positive electrode layer

[0102] The positive electrode layer contains at least a positive electrode active material. In addition, the positive electrode layer may contain at least one of a conductive additive, a binder, and an electrolyte, as needed.

[0103] Examples of positive electrode active materials include oxide active materials. Examples of oxide active materials include LiCoO2 and LiNi. 1 / 3 CO 1 / 3 Mn 1 / 3 O2 and LiNi 0.8 Co 0.15 Al 0.05 O2 and other layered active substances in rock salt, LiMn2O4 and Li4Ti5O 12 Spinel-type active substances and olivine-type active substances such as LiFePO4.

[0104] A coating containing a Li-ion-conducting oxide can be formed on the surface of an oxide-active material. This is because it can inhibit the reaction between the oxide-active material and the solid electrolyte (especially a sulfide solid electrolyte). Examples of Li-ion-conducting oxides include LiNbO3 and Li4Ti5O3. 12 And Li3PO4.

[0105] The positive electrode active material has a shape, for example, particles. The average particle size D of the positive electrode active material... 50 For example, particles larger than 0.5 μm and smaller than 50 μm. Average particle size (D) 50 As described above.

[0106] Examples of conductive additives include carbon materials, metal particles, and conductive polymers. Examples of carbon materials include particulate carbon materials such as acetylene black (AB) and Ketjen black (KB), and fibrous carbon materials such as vapor-grown carbon fiber (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs). The information regarding binders and solid electrolytes is the same as described in "1. Negative Electrode Layer".

[0107] There is no particular limitation on the thickness of the positive electrode layer, for example, it can be above 1 μm and below 1000 μm.

[0108] 3. Electrolyte layer

[0109] The electrolyte layer is a layer disposed between the positive electrode layer and the negative electrode layer, and it contains at least an electrolyte. The electrolyte layer can contain a solid electrolyte or a liquid electrolyte (electrolyte), but the former is preferred. An electrolyte layer containing a solid electrolyte is called a solid electrolyte layer. Furthermore, generally speaking, a battery with a solid electrolyte layer is called a solid-state battery. Solid-state batteries can be semi-solid-state batteries or all-solid-state batteries. It should be noted that a battery with a solid electrolyte layer containing only an inorganic solid electrolyte is equivalent to an all-solid-state battery.

[0110] Examples of solid electrolytes include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, and complexed hydrides. Sulfide solid electrolytes are particularly preferred due to their high ionic conductivity. Sulfide solid electrolytes typically contain sulfur (S) as the main anionic element. Oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes typically contain oxygen (O), nitrogen (N), and halogen (X) as the main anionic elements, respectively.

[0111] Sulfide solid electrolytes preferably contain, for example, Li, X (X being at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, In), and S. Additionally, sulfide solid electrolytes may also contain at least one of O and a halogen.

[0112] Examples of sulfide solid electrolytes include Li₂S-P₂S₅, Li₂S-P₂S₅-LiI, Li₂S-P₂S₅-GeS₂, Li₂S-P₂S₅-Li₂O, Li₂S-P₂S₅-Li₂O-LiI, Li₂S-P₂S₅-LiBr, Li₂S-SiS₂, Li₂S-SiS₂-LiI, Li₂S-SiS₂-LiBr, Li₂S-SiS₂-LiCl, Li₂S-SiS₂-B₂S₃-LiI, Li₂S-SiS₂-P₂S₅-LiI, Li₂S-B₂S₃, and Li₂S-P₂S₅-Z. m S n (Where m and n are positive numbers, and Z is any one of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (Where x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In).

[0113] In addition, organic solid electrolytes such as polymer electrolytes and gel electrolytes can also be cited as examples of solid electrolytes.

[0114] Solid electrolytes can be glassy or have a crystalline phase. Examples of such crystalline phases include the Thio-Lisicon type, the argentite-germanium sulfide type, and the LGPS type. The shape of the solid electrolyte is, for example, particulate. The average particle size of the solid electrolyte is, for example, 0.01 μm or more and 10 μm or less. Furthermore, the ionic conductivity of the solid electrolyte at 25°C is, for example, 1 × 10⁻⁶. -4 For values ​​above S / cm, it can be 1×10 -3 S / cm or higher.

[0115] Additionally, the electrolyte layer may contain a binder as needed. Examples of binders include those described in "1. Negative Electrode Layer". The thickness of the electrolyte layer is not particularly limited, but may be, for example, 1 μm or more and 1000 μm or less.

[0116] 4. Negative current collector and positive current collector

[0117] A negative current collector is a component that collects electrons from a negative electrode layer, and a positive current collector is a component that collects electrons from a positive electrode layer. Examples of materials for a positive current collector include SUS, aluminum, nickel, iron, titanium, and carbon. Examples of materials for a negative current collector include SUS, copper, nickel, and carbon. A coating containing at least one of Ni, Cr, and C can be formed on the surface of both the positive and negative current collectors. The coating can be a plating or a vapor-deposited layer. Examples of shapes for the positive and negative current collectors include foil.

[0118] 5. Battery

[0119] The battery of the present invention may include an outer casing that houses the aforementioned components. Examples of such outer casings include laminated outer casings and shell-type outer casings. Furthermore, the battery of the present invention may include a constraint clamp that applies constraint pressure to the aforementioned components along the thickness direction. Known clamps may be used as the constraint clamp. The constraint pressure may be, for example, 0.1 MPa or more and 50 MPa or less, or 1 MPa or more and 20 MPa or less.

[0120] The battery in this invention is typically a lithium-ion secondary battery. Additionally, as mentioned above, the battery in this invention can be a solid-state battery with a solid electrolyte layer. Furthermore, the battery in this invention can be a semi-solid-state battery or a fully solid-state battery. Examples of applications for the battery include powering vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. Furthermore, the battery in this invention can be used as a power source for mobile bodies other than vehicles (e.g., railway vehicles, ships, and aircraft), and also as a power source for electrical products such as information processing devices.

[0121] B. Battery manufacturing method

[0122] Figure 7 This is a flowchart illustrating a method for manufacturing a battery according to the present invention. For example... Figure 7 As shown, in the battery manufacturing method of the present invention, firstly, a first negative electrode composite material containing the aforementioned first composite particles and a second negative electrode composite material containing the aforementioned second composite particles are prepared (preparation step). Next, a first negative electrode layer is formed using the aforementioned first negative electrode composite material (first negative electrode layer forming step). Then, a second negative electrode layer is formed on the aforementioned first negative electrode layer using the aforementioned second negative electrode composite material (second negative electrode layer forming step). Furthermore, as... Figure 7 As shown, the battery manufacturing method of the present invention may include a third negative electrode layer forming step of forming a third negative electrode layer on the second negative electrode layer using a third negative electrode composite material containing the first composite particles described above.

[0123] The method shown in this invention enables the manufacture of a battery in which the negative electrode layer satisfies any of the conditions (i) to (iii) described above.

[0124] 1. Preparation process

[0125] In the preparation process, a first negative electrode composite material containing the aforementioned first composite particles and a second negative electrode composite material containing the aforementioned second composite particles are prepared.

[0126] The first negative electrode composite material contains at least the aforementioned first composite particles, and may contain at least one of a binder, a conductive additive, and an electrolyte as needed. The contents of the first composite particles, binder, conductive additive, and electrolyte are the same as those described in "A. Battery".

[0127] The first negative electrode composite material may or may not contain the second composite particles. In the latter case, the weight proportion of the first composite particles in the first negative electrode composite material is greater than the weight proportion of the second composite particles.

[0128] In addition, the first negative electrode composite material may contain a dispersion medium such as a solvent. Examples of solvents include organic solvents such as butyl butyrate, dibutyl ether, heptane, and tetrahydrofuran. The first negative electrode composite material may be a slurry or a powder.

[0129] Regarding the second negative electrode composite material, the terms "first" and "second" can be interchanged in the above description of the first negative electrode composite material for clarification.

[0130] 2. First negative electrode layer formation process

[0131] The first negative electrode layer formation process is the process of forming the first negative electrode layer using the aforementioned first negative electrode composite material.

[0132] The first negative electrode layer can be formed on the negative electrode current collector or on the electrolyte layer. The first negative electrode layer can be formed by coating or pressing. It should be noted that the first negative electrode layer can be densified by pressing.

[0133] 3. Second negative electrode layer formation process

[0134] The second negative electrode layer formation process is a process of forming a second negative electrode layer on the first negative electrode layer using the aforementioned second negative electrode composite material.

[0135] The process for forming the second negative electrode layer is the same as the process for forming the first negative electrode layer, except that it uses a second negative electrode composite material and forms the second negative electrode layer on the first negative electrode layer.

[0136] 4. Third negative electrode layer formation process

[0137] The third negative electrode layer formation process is a process of forming a third negative electrode layer on the second negative electrode layer using a third negative electrode composite material containing the first composite particles mentioned above.

[0138] The process for forming the third negative electrode layer is the same as the process for forming the first negative electrode layer, except that it uses a third negative electrode composite material and forms the third negative electrode layer on the second negative electrode layer. It should be noted that the third negative electrode composite material can be the same composite material as the first negative electrode composite material described above, or it can be a different composite material.

[0139] 5. Other processes

[0140] The battery manufacturing method of the present invention generally includes a positive electrode layer forming process, an electrolyte layer forming process, and a lamination process to obtain a laminate having a negative electrode current collector, a negative electrode layer, an electrolyte layer, a positive electrode layer and a positive electrode current collector in sequence.

[0141] There are no particular limitations on the method for forming the positive electrode layer and the electrolyte layer; any previously known method can be used.

[0142] 6. Battery

[0143] Regarding the batteries manufactured through the above process, the content is the same as that described in "A. Battery", so the description here is omitted.

[0144] It should be noted that this invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any technical solution having a substantially the same structure and performing the same effect as the technical concept described in the claims of this invention is included within the technical scope of this invention.

[0145] Example 1

[0146] Production of the first and second composite particles

[0147] 0.65 g of Si particles (high-purity chemically prepared) and 0.60 g of Li metal (prepared by Honjo Metals) were mixed in an agate mortar under an Ar atmosphere to obtain a LiSi precursor. In a glass reactor under an Ar atmosphere, 1.0 g of the LiSi precursor and 125 ml of dispersion medium (1,3,5-trimethylbenzene, prepared by Nacalai Tesque) were mixed using an ultrasonic homogenizer (UH-50, prepared by SMT). The resulting LiSi precursor dispersion was cooled to 0°C, and 125 ml of ethanol (prepared by Nacalai Tesque) was added dropwise as the Li extraction solvent, reacting for 120 minutes. After the reaction, 50 ml of acetic acid (prepared by Nacalai Tesque) was further added dropwise, reacting for 60 minutes. After the reaction, the liquid and solid reactants were separated by vacuum filtration. The obtained solid reactants were vacuum dried at 120°C for 2 hours to recover the Si-based active material (porous Si) as porous particles.

[0148] Porous Si and styrene-butadiene rubber (SBR) were dispersed in dimethyl carbonate (made by Nacalai Tesque) to partially dissolve, resulting in a slurry. This slurry was then sprayed into a spray dryer under a nitrogen atmosphere at 140°C for drying (spray drying method). By adjusting the NV value of the slurry, the spray pressure in the spray drying method, and the slurry feed rate, first and second composite particles with the binder ratios shown in Table 1 were produced. The binder ratios in the first and second composite particles were confirmed using methods described later.

[0149] Negative electrode fabrication

[0150] Using an ultrasonic homogenizer (UH-50, SMT), 1.0g of the first composite particles, 0.04g of conductive additive (VGCF, Showa Denko), and sulfide solid electrolyte (LiI-LiBr-Li3PS4 series sulfide solid electrolyte, D...) were homogenized. 50 =0.776g of 0.2μm), 0.02g of binder (PVdF, manufactured by Kureha), and 1.7g of butyl butyrate (manufactured by Kishida Chemical) were mixed. A first negative electrode composite material (slurry) containing the first composite particles was thus prepared. Furthermore, a second negative electrode composite material (slurry) containing the second composite particles was prepared in the same manner as the first negative electrode composite material, except that the first composite particles were replaced with second composite particles. A first negative electrode layer containing the first composite particles was formed on a negative electrode current collector (Ni foil) using the coating method of the first negative electrode composite material described above. Furthermore, a second negative electrode layer containing the second composite particles was formed on the first negative electrode layer using the coating method of the second negative electrode composite material described above. Furthermore, a third negative electrode layer containing the first composite particles was formed on the second negative electrode layer using the coating method of the first negative electrode composite material described above. Thus, a third negative electrode layer containing the first composite particles was prepared. Figure 6 The negative electrode layer 2 shown has a first negative electrode layer 2S, a second negative electrode layer 2T and a third negative electrode layer 2U and satisfies condition (iii).

[0151] Positive electrode production

[0152] Add binder (PVDF), conductive additives, sulfide solid electrolyte, and positive electrode active material (NCM:LiNi) to an organic solvent. 0.8 Co 0.15 Mn 0.05 O2). After addition, the mixture is kneaded using an ultrasonic homogenizer to obtain a positive electrode slurry. The obtained positive electrode slurry is coated onto a positive electrode current collector (Al foil) and dried. Thus, a positive electrode with a positive electrode current collector and a positive electrode layer is obtained.

[0153] Evaluation of battery manufacturing

[0154] A binder (PVDF) and a sulfide solid electrolyte (Li₂S-P₂S₅ based sulfide solid electrolyte) are added to an organic solvent and mixed using an ultrasonic homogenizer. This yields a composite slurry. The composite slurry is then coated onto a substrate (Al foil) and dried. This results in a transfer component having a substrate and a solid electrolyte layer.

[0155] The fabricated positive electrode, negative electrode, and transfer component are each formed into a long strip. Next, the positive electrode layer and the transfer component are stacked with the solid electrolyte layer facing each other, and rolled at 165°C and 50 kN / cm. Then, the substrate is peeled off to obtain the positive electrode side component. Similarly, the negative electrode layer and the transfer component are stacked with the solid electrolyte layer facing each other, and rolled at 25°C and 50 kN / cm. Then, the substrate is peeled off to obtain the negative electrode side component. Next, the negative electrode side component is punched to Φ13.00 mm, and the positive electrode side component is punched to Φ11.28 mm. Powdered sulfide solid electrolyte is placed on the solid electrolyte layer of the punched negative electrode side component and uniaxially pressed. Next, the negative electrode side component and the positive electrode side component are stacked with the solid electrolyte layers facing each other, and tabs for current extraction are installed on the positive and negative electrodes. Then, they are sealed in an aluminum laminate using a vacuum lamination sealing machine and constrained at a pressure of 5 MPa. Therefore, an evaluation battery (all-solid-state battery) was manufactured.

[0156] Examples 2-7

[0157] By varying at least one of the NV value of the slurry, the spray pressure, and the slurry delivery rate, a first composite particle having the binder ratio shown in Table 1 was prepared. An evaluation battery was then prepared in the same manner as in Example 1, except that the first composite particle was used.

[0158] Comparative Example 1

[0159] like Figure 8 As shown, only the second negative electrode layer 2T containing the second composite particles is formed as the negative electrode layer 2. Otherwise, the evaluation battery is made in the same manner as in Example 1.

[0160] evaluate

[0161] Adhesive ratio

[0162] The first composite particles were pressed to form a molded body. The second composite particles were similarly molded. The resulting molded bodies underwent cross-sectional exposure processing, and the cross-sections were measured using SEM-EDX to determine the binder ratio in the first and second composite particles. The results are shown in Table 1.

[0163] Charge and discharge test

[0164] For the evaluation batteries produced, 80 charge-discharge cycles were performed at 25°C, 1 / 3C, and SOC of 5%–95%. The capacity retention rate (%) was calculated as the ratio of the capacity after 80 cycles to the capacity of the first cycle (initial capacity). The results are shown in Table 1.

[0165] stripping of the negative electrode layer

[0166] The presence or absence of negative electrode layer peeling was confirmed by cross-sectional images of the battery after the above charge-discharge tests. The results are shown in Table 1.

[0167] [Table 1]

[0168] As shown in Table 1, in the battery of the present invention, it was confirmed that the peeling of the negative electrode layer was suppressed. In Comparative Example 1, it was speculated that due to the peeling of the negative electrode layer, the electron conduction path or ion conduction path was interrupted, resulting in a decrease in capacity retention. Furthermore, in Examples 6 and 7, although the peeling of the negative electrode layer was suppressed, the capacity retention decreased. This is believed to be because the binder ratio (X1 / X2) of the first composite particles was too large, thus hindering the reaction of the first composite particles, causing the reaction to concentrate in the second composite particles, leading to the degradation of the second composite particles. This result suggests that by setting (X1 / X2) to 4.0 or less, particularly 3.6 or less, a battery with suppressed peeling of the negative electrode layer and good capacity retention can be obtained.

Claims

1. A battery comprising a negative current collector, a negative electrode layer, an electrolyte layer, a positive electrode layer, and a positive current collector, characterized in that, In the thickness direction, the negative electrode current collector, the negative electrode layer, the electrolyte layer, the positive electrode layer, and the positive electrode current collector are stacked in the following order: negative electrode current collector, negative electrode layer, electrolyte layer, positive electrode layer, and positive electrode current collector. The negative electrode layer contains a first composite particle and a second composite particle. The first composite particle and the second composite particle each contain a Si-based active material and a binder. The first composite particle has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. The second composite particle has an outer edge region including an outer edge and an inner region located inside the outer edge region in its cross-sectional shape. When the proportion of the binder in the outer edge region of the first composite particle is set to X1, the proportion of the binder in the inner region of the first composite particle is set to X2, the proportion of the binder in the outer edge region of the second composite particle is set to Y1, and the proportion of the binder in the inner region of the second composite particle is set to Y2, X1 and X2 satisfy 1.2 ≤ (X1 / X2), The Y1 and Y2 satisfy (Y1 / Y2) < 1.

2. When X1 and X2 satisfy 1.2 ≤ (X1 / X2), Y1 and Y2 satisfy (Y1 / Y2) < 1.2, and the thickness of the negative electrode layer is set to T, in the thickness direction, the region of the negative electrode layer at a distance of 0T or more and 0.2T or less from the end of the negative electrode current collector side of the negative electrode layer is designated as the first region, the region of the negative electrode layer at a distance of 0.4T or more and 0.6T or less from the end is designated as the second region, and the region of the negative electrode layer at a distance of 0.8T or more and 1.0T or less from the end is designated as the third region. In this case, The negative electrode layer satisfies any one of the first, second, and third conditions. The first condition is that in the first region, the content of the first composite particle is greater than the content of the second composite particle, and in the third region, the content of the second composite particle is greater than the content of the first composite particle. The second condition is that in the first region, the content of the second composite particle is greater than the content of the first composite particle, and in the third region, the content of the first composite particle is greater than the content of the second composite particle. The third condition is: in the first region, the content of the first composite particle is greater than the content of the second composite particle; in the second region, the content of the second composite particle is greater than the content of the first composite particle; and in the third region, the content of the first composite particle is greater than the content of the second composite particle. The content of the first composite particle is 0 or more. The content of the second composite particle is 0 or more.

2. The battery of claim 1, wherein, X1 and X2 satisfy (X1 / X2)≤3.

6.

3. The battery of claim 1, wherein, The Y1 and Y2 satisfy (Y1 / Y2)≤1.

0.

4. The battery of claim 1, wherein, The T is greater than 30 μm and less than 1000 μm.

5. The battery of claim 1, wherein, The electrolyte layer contains a solid electrolyte.

6. The battery of claim 5, wherein, The electrolyte layer contains a sulfide solid electrolyte as the solid electrolyte.

7. The battery of claim 1, wherein, The Si-based active material is a porous particle.

8. The battery of claim 1, wherein, The battery is a solid-state battery.

9. The battery according to claim 1, characterized in that, The content of the first composite particle is 30% by weight or more and 60% by weight or less. The content of the second composite particles is 30% by weight or more and 60% by weight or less. The total content of the first composite particle and the second composite particle is 60% by weight or more and 90% by weight or less.

10. The battery of claim 3, wherein, The condition Y1 and Y2 satisfy 0.6 ≤ (Y1 / Y2).

11. A method for manufacturing a battery, comprising a method for manufacturing the battery according to any one of claims 1 to 10, characterized in that, It has the following processes: Prepare a first negative electrode composite material containing the first composite particles and a second negative electrode composite material containing the second composite particles; The first negative electrode layer is formed using the first negative electrode composite material; and The second negative electrode layer is formed on the first negative electrode layer using the second negative electrode composite material.

12. The manufacturing method according to claim 11, characterized in that, It has the following processes: A third negative electrode layer is formed on the second negative electrode layer using a third negative electrode composite material containing the first composite particles.

Citation Information

Patent Citations

  • Negative electrode layer

    JP2019121557A

  • Active material composite particle, secondary battery, and method of manufacturing active material composite particle

    JP2024017879A