A method for preparing a silicon-based negative electrode sheet, a lithium-ion battery and the same method.
By employing a layered binder structure in the silicon-based anode sheet, with the flexible binder close to the current collector and the rigid binder on the outside, the structural instability caused by volume changes in silicon-based anode materials during charging and discharging is solved, thereby improving the cycle stability and interface stability of lithium-ion batteries.
Patent Information
- Application Number
- CN202611449361.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicon-based anode materials suffer from particle shedding and coating cracking due to volume changes during repeated charge and discharge processes, resulting in insufficient cycle stability. Traditional binders struggle to achieve a balance between flexibility and rigidity.
A layered adhesive structure is adopted, with a flexible adhesive (a mixture of sodium carboxymethyl cellulose and styrene-butadiene rubber) used on the side near the current collector and a rigid adhesive (polyacrylic acid) used on the outside. The layered structure is formed by high-temperature rolling, which improves the structural stability and interface stability of the electrode.
It improves the structural stability and interlayer bonding reliability of silicon-based anode sheets under repeated volume expansion and contraction, reduces the risk of particle pulverization and coating cracking, and enhances the cycle stability and interface stability of lithium-ion batteries.
Smart Images

Figure CN123120650A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery manufacturing technology, and in particular to a method for preparing a silicon-based negative electrode sheet, a lithium-ion battery, and the same method. Background Technology
[0002] With the expansion of lithium-ion battery applications, high-energy-density anodes have become a development trend, and silicon-based anode materials have attracted attention due to their high lithium storage capacity. The theoretical lithium storage capacity of elemental silicon is approximately 4200 mAh / g, significantly higher than the 372 mAh / g of graphite anodes. Its lithium insertion / extraction potential is close to that of metallic lithium, which is beneficial for improving the overall battery energy. Furthermore, it is less prone to lithium plating and has a lower tendency for lithium dendrite growth, resulting in better safety. However, silicon-based materials undergo significant volume changes during lithium insertion, expanding by approximately 300%. During repeated charge and discharge cycles, the particles are easily pulverized and detached from the conductive network, leading to cracking and material loss in the electrode coating, a rapid increase in electrode impedance, and a significant capacity decay. The surface layer continuously cracks during expansion and contraction, and the electrolyte continuously decomposes to form a solid electrolyte interface film, consuming electrolyte and active lithium. The first charge also consumes a significant amount of lithium, reducing the actual usable capacity. To alleviate these problems, current improvements mainly focus on binders and conductive agents. Traditional silicon-based anode binders primarily use water-based polyacrylic acid systems and styrene-butadiene rubber composite systems. Polyacrylic acid is a linear polymer with a large number of carboxyl groups distributed in its molecular chain. It forms strong hydrogen bonds or covalent bonds with the silicon surface through multi-point anchoring. It has high modulus and cohesive force, which can firmly bind silicon particles. The interfacial film is thin and stable with low impedance and is not easily swollen by electrolyte. The styrene-butadiene rubber composite system is mainly composed of flexible rubber segments. It relies on physical winding and local weak chemical bonds to elastically wrap the particles, and has good tensile and bending resistance.
[0003] In actual cycling, silicon particles repeatedly undergo significant volume expansion and contraction, demanding both flexible adaptation and rigid constraint from the bonding system. A single bonding system often struggles to achieve both. Styrene-butadiene rubber (SBR) composite systems have relatively weak adhesion, relying more on flexible encapsulation of particles. When faced with significant silicon expansion, they fail to provide strong constraint, leading to particle loosening and detachment after cycling, and gradual electrode structure collapse. While polyacrylic acid systems offer stronger binding capacity and more stable interfaces, their rigidity and brittleness make them prone to microcracks when bent or wound. They also have limitations in buffering volume changes and maintaining adhesion to the current collector. Although the characteristics of these two types of aqueous bonding systems are complementary, they struggle to function stably together in the same electrode. If the bonding scheme favors one over the other, it becomes difficult to achieve a balance between expansion constraint, interface stability, and flexible crack resistance. Therefore, existing silicon-based anode bonding schemes generally suffer from problems such as easy particle detachment, coating cracking and material loss, continuous regeneration of the interface film, and insufficient electrode cycling stability under repeated silicon expansion and contraction. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention discloses a method for preparing a silicon-based negative electrode sheet, applicable to lithium-ion batteries, comprising: Step S1: Prepare a first slurry containing a first binder and a second slurry containing a second binder, respectively; The first adhesive comprises a mixture of sodium carboxymethyl cellulose and styrene-butadiene rubber; The second adhesive comprises polyacrylic acid; Step S2: Apply the first slurry to the surface of the copper foil until the surface of the copper foil is dry to form the first electrode, and then proceed to step S3; Step S3: Apply the second slurry to the surface of the first electrode until the surface of the first electrode is dry to form the second electrode, and then proceed to step S4; Step S4: The second electrode sheet is rolled and stamped at 90~120℃ to obtain a silicon-based negative electrode sheet.
[0005] Preferably, the proportion of the first adhesive in the first slurry and the proportion of the second adhesive in the second slurry are equal.
[0006] Preferably, the coating density of the first slurry applied to the surface of the copper foil is equal to the coating density of the second slurry applied to the surface of the first electrode.
[0007] This invention discloses a method for preparing a lithium-ion battery. After preparing a silicon-based negative electrode sheet using the method described above, the following preparation method is performed: Step A1: Prepare the positive electrode sheet; Step A2: A separator is disposed between the silicon-based negative electrode and the positive electrode, and a third adhesive is applied to the side of the separator facing the silicon-based negative electrode. Step A3: Inject electrolyte into the cell formed by the silicon-based negative electrode, the separator, and the positive electrode to obtain an unactivated battery; The third adhesive includes polyvinylidene fluoride; Step A4: At 60~85℃, the unactivated battery is charged at a constant current rate until the voltage of the unactivated battery reaches the first voltage, then cooled to room temperature, and the subsequent steps are performed at room temperature. Step A5: Evacuate the gas in the unactivated battery to a vacuum, and then seal the unactivated battery. Step A6: The sealed unactivated battery is charged with a constant current at a second rate until the voltage of the unactivated battery reaches the second voltage. Step A7: The inactive battery is charged at a constant voltage under the second voltage until the current in the inactive battery drops to the third rate current. Step A8: The unactivated battery is discharged at a constant current rate using the second rate until the voltage in the unactivated battery reaches the third voltage, thus forming the lithium-ion battery. The second multiplier current is not less than the first multiplier current, and the first multiplier current is not less than the third multiplier current; The second voltage is greater than the first voltage, and the first voltage is greater than the third voltage.
[0008] Preferably, the thickness of the material layer formed after the third adhesive dries is 3~5μm.
[0009] Preferably, the first multiplier current ranges from 0.05 to 0.1C, the second multiplier current ranges from 0.1C to 0.2C, and the third multiplier current ranges from 0.01 to 0.05C. The first voltage ranges from 3.4 to 3.6V, the second voltage ranges from 4.2 to 4.45V, and the third voltage ranges from 2.5 to 2.75V.
[0010] This invention discloses a lithium-ion battery, including a silicon-based negative electrode sheet prepared using a lithium-ion battery preparation method.
[0011] This invention discloses a lithium-ion battery, which is prepared using a lithium-ion battery preparation method.
[0012] The following beneficial effects can be obtained by using the present invention: By layering two types of binders with different properties in the thickness direction of the electrode, the side near the current collector has flexible bonding and bending resistance, while the outer side has strong expansion constraint and interface stability. This improves the structural stability and interlayer bonding reliability of the silicon-based negative electrode under repeated volume expansion and contraction, reduces the risk of particle pulverization and coating cracking, and thus enhances the cycle stability of the lithium-ion battery. At the same time, it improves the anchoring and bonding effect of the binder on the silicon-based active material, improves the electrode interface stability, and is conducive to improving the battery cycle performance. Attached Figure Description
[0013] Figure 1 This is a schematic diagram of the preparation method in this invention; Figure 2 This is a schematic diagram of the process for manufacturing a lithium-ion battery in this invention. Detailed Implementation
[0014] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0015] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.
[0016] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the scope of the invention.
[0017] This invention discloses a method for preparing a silicon-based negative electrode sheet, applicable to lithium-ion batteries, such as... Figure 1 As shown, the preparation method includes: Step S1: Prepare a first slurry containing a first binder and a second slurry containing a second binder, respectively; The first adhesive comprises a mixture of sodium carboxymethyl cellulose and styrene-butadiene rubber; The second adhesive includes polyacrylic acid; Step S2: Apply the first slurry to the surface of the copper foil until the surface of the copper foil dries to form the first electrode, and then proceed to step S3; Step S3: Apply the second slurry to the surface of the first electrode until the surface of the first electrode is dry to form the second electrode, and then proceed to step S4; Step S4: The second electrode sheet is rolled and stamped at 90~120℃ to obtain a silicon-based negative electrode sheet.
[0018] Specifically, copper foil is used as the current collector for the silicon-based anode electrode. The copper foil serves as both a carrier for the collection and outward conduction of electrons from the anode and a substrate for coating the active material layer. The active materials used in preparing the first and second slurries include silicon-based anode materials and graphite. The silicon-based anode material provides the main lithium storage capacity, while graphite serves to store lithium, conduct electricity, and buffer volume changes.
[0019] Silicon-based anode materials are either silicon-carbon anode materials or silicon-oxygen anode materials. The basis of silicon-carbon anode materials is nanoscale elemental silicon particles (Si). In order to cope with the huge volume expansion of silicon during charging and discharging, it needs to be combined with carbon materials (such as graphite, graphene, carbon nanotubes) to form a buffer structure.
[0020] The first and second slurries also include a conductive agent. The conductive agent is used to construct an electronically conductive network between the active particles and can be one or more of carbon nanotubes, graphene, and conductive carbon black (Super P).
[0021] The first binder is a mixture of sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), which together form a flexible bonding system. Sodium carboxymethyl cellulose primarily acts as a thickener, dispersant, stabilizer, and binder, while SBR provides good tensile strength and bending resistance by elastically encapsulating the active particles. The second binder is polyacrylic acid (PAA), whose molecular chain contains a large number of carboxyl groups, enabling it to anchor silicon particles at multiple points. It exhibits strong rigidity and cohesion and is not easily swollen by the electrolyte, thus facilitating the maintenance of a stable interface on the outer side of the electrode.
[0022] Furthermore, the adhesive is applied in two stages. First, a first slurry is applied to the surface of the copper foil. After the copper foil surface dries, a first electrode is formed. This layer, containing a flexible first adhesive, is close to the current collector and can expand and contract with the silicon volume, maintaining adhesion to the copper foil. Then, a second slurry is applied to the surface of the first electrode. After the first electrode surface dries, a second electrode is formed. The second adhesive, containing polyacrylic acid, is located on the outer side and faces the electrolyte, used to constrain the expansion of silicon particles and maintain interface stability. This creates a layered structure along the electrode thickness direction, with the current collector, first adhesive layer, and second adhesive layer arranged sequentially, allowing flexible adaptation and rigid constraint to be undertaken by different layers.
[0023] The second electrode is then rolled and stamped to obtain a silicon-based negative electrode. A high-temperature rolling process is used to ensure good cross-linking of the adhesive at the contact surface between the inner and outer layers of the electrode, improving the adhesion at the electrode interface. The stamping process includes slitting and punching to obtain the negative electrode of the target size.
[0024] In a preferred embodiment of the present invention, the proportion of the first adhesive in the first slurry and the proportion of the second adhesive in the second slurry are equal.
[0025] Specifically, the first slurry and the second slurry are prepared separately. The first slurry is prepared by uniformly mixing the active material, the first binder, the conductive agent, and distilled water. The second slurry is prepared by uniformly mixing the active material, the second binder, the same conductive agent, and distilled water. The distilled water is an aqueous solvent that evaporates during the subsequent drying process and does not remain in the finished electrode sheet. The active material, binder, conductive agent, and distilled water are mixed in the same proportions in both slurries. The two slurries are prepared separately and are not pre-mixed, which avoids deep cross-linking of the two types of binders within the same slurry, thus preventing a weakening of the adhesion to the active material.
[0026] Furthermore, by using the same proportion of first binder and second binder to prepare the first slurry and the second slurry respectively, the solid composition ratio of the inner and outer layers is kept consistent. The two layers have similar lithium-ion intercalation degrees during charging and discharging, which is beneficial to maintain the overall uniformity of the electrode and suppress polarization caused by the inconsistent intercalation rates of the two layers.
[0027] In one embodiment, a first slurry is prepared using 93 wt% silicon-based anode material, 2 wt% conductive carbon black, 2.5 wt% sodium carboxymethyl cellulose and 2.5 wt% styrene-butadiene rubber, and a second slurry is prepared using 93 wt% silicon-based anode material, 2 wt% conductive carbon black and 5 wt% polyacrylic acid.
[0028] In a preferred embodiment of the present invention, in step S2, the coating density of the first slurry applied to the surface of the copper foil is equal to the coating density of the second slurry applied to the surface of the first electrode.
[0029] Specifically, coating density is the ratio of the mass of the solid coating remaining on the coated surface after the slurry dries to the area of the coated surface. Measurement is based on the dried coating and does not include evaporated distilled water. When applying coating to both sides, the area of a single side is used as the coating area.
[0030] Furthermore, by using the same coating density, the lithium-ion intercalation rate of the two layers is consistent and the electrode thickness is uniform.
[0031] In one embodiment, the coating density of the first slurry applied to the surface of the copper foil and the coating density of the second slurry applied to the surface of the first electrode are both 10 mg / cm². 2 .
[0032] In a preferred embodiment of the present invention, after preparing the silicon-based negative electrode sheet using the silicon-based negative electrode sheet preparation method, as follows: Figure 2 As shown, perform the following preparation method; Step A1: Prepare the positive electrode sheet; Step A2: A separator is placed between the silicon-based negative electrode and the positive electrode, and a third adhesive is applied to the side of the separator facing the silicon-based negative electrode. Step A3: Inject electrolyte into the cell formed by the silicon-based negative electrode, separator and positive electrode to obtain an unactivated battery; The third adhesive includes polyvinylidene fluoride; Step A4: At 60~85℃, charge the unactivated battery with a constant current at the first rate until the voltage of the unactivated battery reaches the first voltage, then cool it down to room temperature and perform the subsequent steps at room temperature. Step A5: Evacuate the gas in the unactivated battery to a vacuum, and then seal the unactivated battery. Step A6: Charge the sealed, unactivated battery with a constant current at a second rate until the voltage of the unactivated battery reaches the second voltage. Step A7: Perform constant voltage charging on the unactivated battery at the second voltage until the current in the unactivated battery drops to the third rate current. Step A8: The unactivated battery is discharged at a constant current rate of the second multiple until the voltage in the unactivated battery reaches the third voltage, thus forming a lithium-ion battery. The second-rate current is not less than the first-rate current, and the first-rate current is not less than the third-rate current. The second voltage is greater than the first voltage, and the first voltage is greater than the third voltage.
[0033] Specifically, the positive electrode sheet is prepared from a positive electrode material, a conductive agent, and a positive electrode binder. The positive electrode material is any one or more of lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, lithium manganese oxide, or lithium nickel oxide, and the positive electrode binder is polyvinylidene fluoride. In preparing the positive electrode sheet, the above solid components are stirred with a solvent to form a positive electrode slurry, which is then coated onto the surface of the positive electrode current collector aluminum foil. After drying, rolling, and slitting, the positive electrode sheet is obtained. The solvent used can be a commonly used positive electrode solvent in this field.
[0034] Furthermore, a separator is placed between the silicon-based negative electrode and the positive electrode. The separator is an insulating porous membrane that physically separates the positive and negative electrodes to prevent internal short circuits while allowing lithium ions to pass through. A third binder, made of polyvinylidene fluoride, is pre-coated on the side of the separator facing the silicon-based negative electrode. The separator, along with the positive and silicon-based negative electrodes, is then laminated or wound to form a battery cell. During the high-temperature pre-charge formation process, the third binder helps the separator adhere to the negative electrode, which is beneficial for maintaining interfacial contact during cycling. Electrolyte is then injected into the battery cell and allowed to stand, allowing the electrolyte to fully wet each layer, resulting in an unactivated battery.
[0035] In one embodiment, the battery cell is first packaged in an aluminum-plastic film and then vacuum-baked to remove moisture before being injected with electrolyte.
[0036] The unactivated batteries are then formed. At 60-85°C, the batteries are charged at a constant current rate until the battery voltage reaches the first voltage, completing the pre-charge. After reaching the first voltage, the batteries are cooled to room temperature, typically 25°C. During the pre-charge process, flat metal clamps are used to hold the batteries in place, ensuring close contact between the layers.
[0037] The first constant current charge will form a film on the negative electrode surface and produce gas. At room temperature, the gas in the battery is evacuated to a vacuum and discharged as gas. Then, the unactivated battery is sealed to ensure that there is no residual gas inside the battery and that it remains sealed. For aluminum-plastic film soft-pack batteries, the sealing is achieved by hot-pressing the aluminum-plastic film under vacuum conditions.
[0038] After sealing, further formation is performed, followed by constant current charging at a second-rate current until the voltage reaches a second voltage, and then constant voltage charging at the second voltage. During the constant voltage phase, the charging current gradually decreases, and charging stops when the current drops to a third-rate current. The second-rate current is not less than the first-rate current, and the first-rate current is not less than the third-rate current, so that the pre-charge current is small, the main charging current is large, and the constant voltage cutoff current is minimal, and the charging process gradually becomes more thorough.
[0039] Subsequently, a constant current discharge is applied at a second-highest current rate until the battery voltage reaches the third voltage, at which point the formation process ends. The voltages must satisfy the condition that the second voltage is greater than the first voltage, and the first voltage is greater than the third voltage. Through pre-charging, venting and sealing, constant current and constant voltage charging, and constant current discharging, the negative electrode interface SEI (Solid Electrolyte Interphase) gradually forms, the material is activated, and a lithium-ion battery is formed.
[0040] In a preferred embodiment of the present invention, the thickness of the material layer formed by the third adhesive is 3~5μm.
[0041] Specifically, the material layer is used to provide sufficient adhesion and bonding to the separator and silicon-based anode material after hot pressing, thereby reducing the lithium-ion transport path and lowering the lithium-ion transport resistance.
[0042] In a preferred embodiment of the present invention, the value range of the first multiplier current is 0.05~0.1C, the value range of the second multiplier current is 0.1C~0.2C, and the value range of the third multiplier current is 0.01~0.05C. The first voltage ranges from 3.4 to 3.6V, the second voltage ranges from 4.2 to 4.45V, and the third voltage ranges from 2.5 to 2.75V.
[0043] Specifically, C is the charge / discharge rate. 1C refers to the current required to fully charge or discharge the battery to its rated capacity within one hour. The actual current value is obtained by multiplying the charge / discharge rate value by the battery's rated capacity.
[0044] In one embodiment, the battery has a rated capacity of 3Ah, a first rate current of 0.05C corresponding to a first current of 0.15A, a second rate current of 0.2C corresponding to a second current of 0.6A, and a third rate current of 0.02C corresponding to a third current of 0.06A. The second rate current is not less than the first rate current, and the first rate current is not less than the third rate current.
[0045] This invention discloses a lithium-ion battery, comprising a silicon-based negative electrode sheet prepared by the above-described method for preparing a silicon-based negative electrode sheet.
[0046] The present invention also discloses a lithium-ion battery, which is prepared by the above-described method for preparing lithium-ion batteries.
[0047] A complete embodiment is now provided to enable those skilled in the art to better understand the preparation process of the present invention: The first slurry is prepared by mechanically mixing 93 wt% silicon-based anode material, 2 wt% conductive carbon black, 2.5 wt% sodium carboxymethyl cellulose, and 2.5 wt% styrene-butadiene rubber with deionized water. This slurry is coated onto copper foil with a single-sided areal density of 10 mg / cm². After double-sided coating and drying, the first electrode sheet is formed. The second slurry is prepared by mechanically mixing 93 wt% silicon-based anode material, 2 wt% conductive carbon black, and 5 wt% polyacrylic acid with deionized water. This slurry is coated onto the first electrode sheet with the same single-sided areal density of 10 mg / cm². After double-sided coating and drying, the second electrode sheet is formed. The second electrode sheet is rolled at 100°C, then slit and punched to produce silicon-based anode electrodes.
[0048] The positive electrode is composed of 92 wt% lithium nickel cobalt manganese oxide, 4 wt% conductive carbon black, and 4 wt% polyvinylidene fluoride. N-methylpyrrolidone is added and stirred to form a positive electrode slurry, which is then sprayed onto aluminum foil and dried, rolled, and slit. The positive electrode and silicon-based negative electrode are stacked alternately, separated by a porous polyethylene membrane. A 3-5 μm thick layer of polyvinylidene fluoride is coated onto the side of the membrane facing the silicon-based negative electrode as a third binder. The mixture is then packaged in aluminum-plastic film and baked in a vacuum oven to remove moisture. Electrolyte is injected into the cell and allowed to stand to allow for full electrolyte wetting, resulting in the battery.
[0049] The battery was then formed using a flat metal clamp. It was charged at 85°C with a constant current of 0.05C to 3.4V, with a first rate current of 0.05C (corresponding to a first current of 0.15A) and a first voltage of 3.4V. The temperature was then lowered from 85°C to room temperature, the battery was evacuated to a vacuum, and sealed. Subsequently, at its rated capacity of 3Ah, it was charged at a constant current of 0.2C (corresponding to a second current of 0.6A) to 4.2V, and then charged at a constant voltage of 4.2V until the current dropped to 0.02C (corresponding to a third current of 0.06A). Finally, it was discharged at a constant current of 0.2C (corresponding to a second current of 0.6A) to 2.5V, completing the formation process.
[0050] The lithium-ion battery prepared using the above method retains 91.7% of its capacity after 500 cycles.
[0051] The above description is merely a preferred embodiment of the present invention and does not limit the implementation and protection scope of the present invention. Those skilled in the art should realize that any equivalent substitutions and obvious changes made based on the description and illustrations of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a silicon-based negative electrode sheet, applied to lithium-ion batteries, characterized in that, include: Step S1: Prepare a first slurry containing a first binder and a second slurry containing a second binder, respectively; The first adhesive comprises a mixture of sodium carboxymethyl cellulose and styrene-butadiene rubber; The second adhesive comprises polyacrylic acid; Step S2: Apply the first slurry to the surface of the copper foil until the surface of the copper foil is dry to form the first electrode, and then proceed to step S3; Step S3: Apply the second slurry to the surface of the first electrode until the surface of the first electrode is dry to form the second electrode, and then proceed to step S4; Step S4: The second electrode sheet is rolled and stamped at 90~120℃ to obtain a silicon-based negative electrode sheet.
2. The preparation method according to claim 1, characterized in that, The proportion of the first adhesive in the first slurry is equal to the proportion of the second adhesive in the second slurry.
3. The preparation method according to claim 1, characterized in that, The coating density of the first slurry applied to the surface of the copper foil is equal to the coating density of the second slurry applied to the surface of the first electrode.
4. A method for preparing a lithium-ion battery, characterized in that, After obtaining the silicon-based negative electrode sheet using the preparation method described in any one of claims 1-3, the following preparation method is performed: Step A1: Prepare the positive electrode sheet; Step A2: A separator is disposed between the silicon-based negative electrode and the positive electrode, and a third adhesive is applied to the side of the separator facing the silicon-based negative electrode. Step A3: Inject electrolyte into the cell formed by the silicon-based negative electrode, the separator, and the positive electrode to obtain an unactivated battery; The third adhesive includes polyvinylidene fluoride; Step A4: At 60~85℃, the unactivated battery is charged at a constant current rate until the voltage of the unactivated battery reaches the first voltage, then cooled to room temperature, and the subsequent steps are performed at room temperature. Step A5: Evacuate the gas in the unactivated battery to a vacuum, and then seal the unactivated battery. Step A6: The sealed unactivated battery is charged with a constant current at a second rate until the voltage of the unactivated battery reaches the second voltage. Step A7: The inactive battery is charged at a constant voltage under the second voltage until the current in the inactive battery drops to the third rate current. Step A8: The unactivated battery is discharged at a constant current rate using the second rate until the voltage in the unactivated battery reaches the third voltage, thus forming the lithium-ion battery. The second multiplier current is not less than the first multiplier current, and the first multiplier current is not less than the third multiplier current; The second voltage is greater than the first voltage, and the first voltage is greater than the third voltage.
5. The preparation method according to claim 4, characterized in that, The thickness of the material layer formed after the third adhesive dries is 3~5μm.
6. The preparation method according to claim 4, characterized in that, The first multiplier current ranges from 0.05 to 0.1C, the second multiplier current ranges from 0.1C to 0.2C, and the third multiplier current ranges from 0.01 to 0.05C. The first voltage ranges from 3.4 to 3.6V, the second voltage ranges from 4.2 to 4.45V, and the third voltage ranges from 2.5 to 2.75V.
7. A lithium-ion battery, characterized in that, This includes silicon-based negative electrode sheets prepared using the preparation method described in any one of claims 1-3.
8. A lithium-ion battery, characterized in that, It is prepared by the preparation method described in any one of claims 4-6.