A sodium-ion battery cathode material with a Na-poor and F-rich surface, its preparation method and application

By coating the surface of sodium-ion battery cathode material with a Na-poor and F-rich spinel structure, the problems of structural instability and poor air stability of the material under high temperature and high pressure were solved, and the material achieved high thermal stability and excellent electrochemical performance.

CN123120655APending Publication Date: 2026-11-17湖州超钠新能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510624759.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials are structurally unstable at high temperatures and high voltages, easily releasing oxygen and causing thermal runaway. Furthermore, their surface air stability is poor, affecting the material's safety and electrochemical performance.

Method used

By coating the surface of sodium ion layered oxide cathode material with a Na-poor and F-rich spinel structure, the conductivity is improved by suppressing interfacial side reactions through F-, and a unique ion diffusion channel is formed, which enhances the thermal stability and cycle performance of the material.

Benefits of technology

It effectively suppressed oxygen release behavior on the material surface, improved the thermal stability and conductivity of the material, improved rate and cycle performance, reduced charge transfer resistance, and enhanced the safety performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120655A_ABST
    Figure CN123120655A_ABST
Patent Text Reader

Abstract

This invention discloses a sodium-ion battery cathode material with a Na-poor and F-rich surface, its preparation method, and its application. The sodium-ion battery cathode material with a Na-poor and F-rich surface comprises a sodium-ion layered oxide bulk material and a spinel-structured compound layer coating the surface of the sodium-ion layered oxide bulk material. The chemical formula of the sodium-ion layered oxide bulk material is Na. x TMO 2‑y F y The chemical formula of the spinel structure compound layer is AB2O. 4‑z F z The preparation method provided by this invention constructs a Na-poor and F-rich spinel structure coating layer on the surface of a layered oxide cathode material, which not only reduces the residual alkali content and improves the material processing performance, but also utilizes the unique structure of the F-rich spinel phase to achieve high rate capability, high thermal stability, and high air stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of sodium-ion battery electrode material preparation technology, specifically relating to a sodium-ion battery cathode material with a Na-poor and F-rich surface, its preparation method, and its application. Background Technology

[0002] With the rapid development of society and the economy, energy and environmental issues have become an increasingly important focus. Lithium-ion batteries, due to their advantages such as high energy density, long cycle life, and low pollution, have been widely used in consumer electronics, energy storage, and electric vehicles. However, the continuous growth in demand for lithium-ion batteries, coupled with the shortage of lithium resources and the resulting price increases, has severely constrained their development. Sodium, belonging to the same Group 1 element as lithium, has similar physicochemical properties. Sodium is the sixth most abundant element in the Earth's crust, with evenly distributed resources and low price, making it a promising candidate for widespread application in energy storage and low-speed electric vehicles.

[0003] The performance of the cathode material is one of the key factors affecting the performance of sodium-ion batteries. Layered oxide cathodes have attracted increasing attention due to their high redox potential, high specific capacity, and low cost. With the marketization of sodium-ion batteries and the introduction of relevant national standards and regulations, the safety performance of sodium-ion batteries has become an urgent issue to be addressed. Similar to lithium-ion batteries, the safety performance of sodium-ion batteries is a systemic problem, directly related to the cathode and anode materials, electrolyte, separator, and runaway conditions. For cathode materials, polyanionic materials, due to their high covalent bond energy of phosphate / sulfate / pyrophosphate polyanions, can support and stabilize the crystal structure of the material, thus exhibiting high thermal stability. Layered oxide cathode materials are prone to oxygen release under high temperature and high voltage, which not only leads to a decrease in the stability of the cathode crystal structure but also allows the released oxygen to act as a fuel for thermal runaway, exacerbating the thermal runaway reaction and further accelerating oxygen release and damaging the crystal structure.

[0004] Currently, researchers mainly improve the structural and thermal stability of layered oxide cathode materials through doping or coating strategies. For example, introducing dopants with high TM-O bond energies during the doping sintering process enhances the stability of the TMO6 octahedral structure, reduces oxygen release behavior at high voltage and high temperature, and thus improves the material's safety performance. However, dopants with high TM-O bond energies, such as Ta, La, Zr, Y, Nb, and W, are generally expensive, and large quantities are required to achieve a significant improvement, resulting in high material costs. The coating strategy typically uses thermally stable polyanionic materials as coating agents to stabilize the surface structure and reduce side reactions such as surface oxygen release and gas generation. However, coating polyanionic materials often results in the polyanionic coating layer containing many impurity phases, affecting the material's electrochemical performance. Summary of the Invention

[0005] The main objective of this invention is to provide a sodium-ion battery cathode material with a Na-poor and F-rich surface, its preparation method, and its application, so as to overcome the shortcomings of the prior art.

[0006] To achieve the aforementioned objectives, the technical solution adopted by this invention includes:

[0007] One aspect of the present invention provides a sodium-ion battery cathode material having a Na-poor and F-rich surface, the chemical formula of which is Na x TMO 2-y F y / AB2O 4-z F z Wherein, 0.44<x≤1.05, 0≤y<0.5, 0<z≤4, TM includes at least one of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Ca, Y, Si, Ta, La, Nb, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, and B, A includes at least one of Li, Na, K, Mg, Cu, Zn, Sr, Ni, and Ca, and B includes at least one of Co, Al, Fe, Mn, Si, Zr, Ti, B, Cr, Cd, and La, and A and B are not the same.

[0008] Another aspect of the present invention provides a method for preparing a sodium-ion battery cathode material having a Na-poor and F-rich surface, comprising:

[0009] Sodium-ion layered oxide bulk material is mixed with a coating agent and sintered to obtain the sodium-ion battery cathode material with a Na-poor and F-rich surface. The coating agent includes source A, source B and fluorine source.

[0010] Another aspect of the present invention provides a sodium-ion battery comprising a positive electrode material, said positive electrode material comprising the aforementioned sodium-ion battery positive electrode material having a Na-poor and F-rich surface.

[0011] Compared with the prior art, the technical solution of the present invention has at least the following advantages:

[0012] The sodium-ion battery cathode material provided by this invention has a Na-poor, F-rich spinel structure coating layer on its surface, wherein the F... - It can effectively suppress the occurrence of interfacial side reactions, and F - This method can reduce charge transfer resistance, which is beneficial for improving material conductivity, rate capability, and cycle performance. The F-rich spinel structure coating can confine oxygen released from the bulk material, contributing to improved material safety. The method provided by this invention is applicable to all layered oxide cathode materials and is simple to operate, suitable for industrial production. Attached Figure Description

[0013] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0014] Figure 1 This is a SEM image of the sodium ion cathode material sample in Example 1 of the present invention;

[0015] Figure 2 This is a SEM image of the sodium ion cathode material sample in Example 2 of the present invention;

[0016] Figure 3 This is a SEM image of the sodium ion cathode material sample in Comparative Example 1 of this invention;

[0017] Figure 4 This is a comparison chart of the charge-discharge curves of batteries made from the positive electrode materials in Example 1 and Comparative Examples 1 and 2 of the present invention.

[0018] Figure 5 This is a comparison chart of the rate performance of batteries made from the cathode materials in Example 1 of the present invention and Comparative Examples 1 and 2.

[0019] Figure 6 This is a comparison chart of the cycle performance of batteries made from the cathode materials in Example 1 and Comparative Examples 1 and 2 of the present invention. Detailed Implementation

[0020] The invention will be more fully understood by reading the following detailed description. However, it should be understood that the detailed description disclosed below is merely exemplary of the invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims and as a representative basis for teaching those skilled in the art to employ the invention in different ways in any suitable detailed embodiment.

[0021] As one aspect of the technical solution of this invention, it relates to a sodium-ion battery cathode material with a Na-poor and F-rich surface, the chemical formula of which is Na x TMO 2-y F y / AB2O 4-z F zWherein, 0.44<x≤1.05, 0≤y<0.5, 0<z≤4, TM includes at least one of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Ca, Y, Si, Ta, La, Nb, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, and B, A includes at least one of Li, Na, K, Mg, Cu, Zn, Sr, Ni, and Ca, and B includes at least one of Co, Al, Fe, Mn, Si, Zr, Ti, B, Cr, Cd, and La, and A and B are not the same.

[0022] In some embodiments, the sodium-ion battery cathode material with a Na-poor and F-rich surface comprises a sodium-ion layered oxide bulk material and a spinel-structured compound layer coated on the surface of the sodium-ion layered oxide bulk material, wherein the chemical formula of the sodium-ion layered oxide bulk material is Na. x TMO 2-y F y The chemical formula of the spinel structure compound layer is Al₂O₃. 4-z F z .

[0023] In this invention, the spinel structure coating has unique ion diffusion channels, which facilitates the diffusion of Na during charging and discharging. + The transport and diffusion of these molecules enhance the rate performance of the material. The spinel-structured coating exhibits good air stability and isolates the bulk material, which has poor air stability, from direct contact with the environment, thus contributing to improved overall air stability of the material.

[0024] In some preferred embodiments, the thickness of the spinel structured compound layer is 2-20 nm.

[0025] In some preferred embodiments, the mass of the spinel structured compound layer is 2-15 wt‰ of the mass of the sodium ion layered oxide bulk material.

[0026] In some preferred embodiments, the sodium ion layered oxide bulk material has an O phase, a P phase, or an O / P mixed phase crystal structure.

[0027] In some embodiments, the sodium-ion battery cathode material with a Na-poor and F-rich surface has an irregular blocky or spherical morphology.

[0028] Layered oxide cathode materials undergo phase transformation processes from layered structure to spinel structure and rock salt phase structure under thermal runaway conditions. The spinel structure has higher thermal stability than the layered structure, can withstand higher thermal runaway temperature, reduces oxygen release behavior on the material surface, and improves the safety performance of the material.

[0029] Conventional layered oxide sodium-ion battery cathode materials are prone to structural oxygen release under high temperature and high voltage. This not only leads to a decrease in the structural stability of the cathode material, but the released oxygen can also act as a combustion promoter during battery thermal runaway, exacerbating the thermal runaway reaction, further accelerating oxygen release and structural damage, and ultimately leading to fire and explosion. In addition, layered oxide sodium-ion battery cathode materials generally have poor air stability, leading to the precipitation of bulk active Na, an increase in the residual alkali content on the surface, and thus causing many problems such as poor processing performance, decreased specific capacity, increased surface side reactions, decreased rate and cycle performance, and gas generation during cycle.

[0030] This invention replaces the oxygen (O) in conventional spinel oxides with the more electronegative sulfur (F) to form a F-rich spinel structure coating layer. This coating layer exhibits higher thermal stability than bulk layered oxides and conventional spinel oxides, reducing oxygen release from the material surface at high temperatures. Simultaneously, the F-rich spinel coating layer can confine the oxygen released from the bulk material, helping to prevent further escalation of thermal runaway. Furthermore, the F in the formed F-rich surface... - It can effectively suppress the occurrence of interfacial side reactions, reduce charge transfer resistance, improve material conductivity, and improve rate and cycle performance.

[0031] The sodium-ion battery cathode material provided by this invention has AB2O formed. 4-z F z On the surface of spinel, O or F ions are arranged in a face-centered cubic close-packed configuration. Low-valence cation A fills 1 / 8 of the tetrahedral voids, high-valence cation B fills 1 / 2 of the octahedral voids, and the remaining 7 / 8 of the tetrahedral voids and 1 / 2 of the octahedral voids are completely empty. This unique structure provides specific channels and spaces for ion transport, which is beneficial for Na during charging and discharging. + The transmission and diffusion of these technologies enable excellent rate performance.

[0032] As another aspect of the technical solution of the present invention, a method for preparing a sodium-ion battery cathode material with a Na-poor and F-rich surface includes:

[0033] Sodium-ion layered oxide bulk material is mixed with a coating agent and sintered to obtain the sodium-ion battery cathode material with a Na-poor and F-rich surface. The coating agent includes source A, source B and fluorine source.

[0034] In some embodiments, the preparation method includes:

[0035] Bulk material Na was obtained by mixing precursors, sodium source, and dopants, followed by sintering. x TMO 2-y F yAlternatively, a solid-state method can be used to obtain bulk material Na by uniformly mixing a metal or non-metal element compound with a sodium source in a stoichiometric ratio and then sintering at high temperature. x TMO 2-y F y .

[0036] Specifically, the steps for preparing sodium-ion battery cathode materials according to the present invention include: 1) obtaining bulk material Na by mixing a precursor, a sodium source, and a dopant, and sintering. x TMO 2-y F y Alternatively, a solid-state method can be used to obtain bulk material Na by uniformly mixing a metal or non-metal element compound with a sodium source in a stoichiometric ratio and then sintering at high temperature. x TMO 2-y F y ;2) The bulk material Na x TMO 2-y F y The mixture is mixed with coating agents (source A, source B, and fluorine source) and sintered to obtain a positive electrode material Na with a Na-poor and F-rich spinel structure surface. x TMO 2-y F y / AB2O 4-z F z The molar ratio of Na is 0.44 to 1.05, and the amounts of other elements are calculated according to the molar ratios of each element in the chemical formula.

[0037] In some preferred embodiments, the sodium source includes any one or a combination of two or more of Na2CO3, NaHCO3, NaOH, Na2O, CH3COONa, etc., but is not limited thereto.

[0038] In some preferred embodiments, the preparation method includes:

[0039] The precursor, sodium source, and dopant are mixed uniformly and subjected to a first sintering treatment to obtain the bulk material Na. x TMO 2-y F y The molar ratio of the precursor, sodium source, and dopant element TM:Na:F is 1:x:y.

[0040] In some more preferred embodiments, the precursor has the chemical formula of any one or more combinations of MCO3, M(OH)2, MC2O4, MO2, etc., wherein M includes any one or more combinations of Ni, Fe, Mn, Cu, Mg, Ti, Zn, Co, etc., but is not limited thereto.

[0041] In some more preferred embodiments, the dopant includes an L-containing compound, wherein L includes any one or more combinations of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Zn, Ca, Y, Si, Ta, La, Nb, Zr, Mg, Al, Sn, Ru, Sr, W, Mo, B, F, etc., but is not limited thereto.

[0042] In some more preferred embodiments, the first sintering process includes: heating to 850-1100°C at a heating rate of 1-10°C / min, holding at that temperature for 6-20 hours, and the sintering atmosphere including air or oxygen.

[0043] In some preferred embodiments, the preparation method includes:

[0044] A bulk material Na is obtained by uniformly mixing a metallic or non-metallic element compound with a sodium source and then sintering it at high temperature. x TMO 2-y F y The molar ratio of the metal or non-metal element compound and the sodium source element TM:Na:F is 1:x:y.

[0045] In some more preferred embodiments, the metal or non-metal element in the metal or non-metal element compound includes any one or more combinations of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Ca, Si, Ta, La, Nb, Y, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, F, etc., but is not limited thereto.

[0046] In some more preferred embodiments, the high-temperature sintering process includes: heating to 850-1100°C at a heating rate of 1-10°C / min, holding at that temperature for 6-20 hours, and the sintering atmosphere including air or oxygen.

[0047] In some embodiments, the preparation method includes:

[0048] The sodium ion layered oxide bulk material is mixed uniformly with a coating agent and subjected to a second sintering treatment to obtain the sodium ion battery cathode material with a Na-poor and F-rich surface. The molar ratio of elements A:B:F in the A source, B source and fluorine source is 1:2:2.

[0049] In some preferred embodiments, the mass ratio of the sodium ion layered oxide bulk material to the coating agent is 1000:2-15.

[0050] In some preferred embodiments, the A source includes, but is not limited to, any one or a combination of two or more of the following: oxides of A, hydroxides of A, carbonates of A, oxalates of A, acetates of A, and nitrates of A.

[0051] In some preferred embodiments, the source of B includes, but is not limited to, any one or a combination of two or more of the following: oxides of B, hydroxides of B, carbonates of B, oxalates of B, acetates of B, and nitrates of B.

[0052] In some preferred embodiments, the fluorine source comprises a fluorine-containing compound. Specifically, the fluorine-containing compound includes any one or a combination of two or more of LiF, NaF, CaF2, MgF2, AlF3, and NH4F, but is not limited thereto. Conventional coating of spinel oxides requires a high coating temperature of 850–1000°C, while common fluorine sources such as CaF2, MgF2, and AlF3 can also act as fluxes to effectively lower the coating temperature and reduce energy consumption.

[0053] In this invention, some fluorine-containing compounds such as LiF, CaF2, MgF2, and AlF3 serve as both fluorine sources to provide F elements for the spinel structure coating layer and A or B sources to provide A or B elements for the spinel structure coating layer. In some fluorine-containing compounds such as NaF, most of the Na elements diffuse into the bulk phase during sintering, and exist in small amounts on the surface in the form of NaOH, Na2CO3, or NaHCO3.

[0054] In some preferred embodiments, the second sintering process includes: heating to 700-1000℃ at a heating rate of 1-10℃ / min, holding at that temperature for 4-10 hours, and the sintering atmosphere including air or oxygen. At a coating temperature of 700-1000℃, the inert residual Na on the surface (such as NaOH, Na2CO3, or NaHCO3) is converted into active Na in the bulk phase, increasing the specific capacity of the material while reducing the residual alkali content on the surface, thus improving the processing performance of the material.

[0055] Sodium-ion layered oxide cathode materials are highly sensitive to H2O and CO2 in the environment. During contact with humid air, Na spontaneously escapes from the bulk Na layer, generating NaOH, Na2CO3, or NaHCO3. These electrochemically inactive residual sodium salts not only degrade the material's processing performance but also increase its impedance, affecting its specific capacity and causing severe gas generation problems. This invention utilizes high-temperature sintering to convert surface inert residual Na (e.g., NaOH, Na2CO3, or NaHCO3) into active Na in the bulk phase during the coating sintering process. This active Na diffuses into the Na layer of the bulk lattice, helping to improve the material's specific capacity. Simultaneously, it reduces the surface residual alkali content, minimizing cross-linking reactions caused by the attack of bases on CH and CF groups in polyvinylidene fluoride (PVDF), thereby improving the material's processing performance.

[0056] As another aspect of the technical solution of the present invention, a sodium-ion battery includes a positive electrode material, wherein the positive electrode material includes the aforementioned sodium-ion battery positive electrode material having a Na-poor and F-rich surface.

[0057] In summary, this invention proposes a novel approach to synthesizing sodium-ion battery cathode materials: coating the surface of conventionally sintered sodium-ion layered oxide cathode materials with a Na-poor and F-rich spinel structure to improve the material's rate capability and safety performance. Furthermore, this synthesis method is simple, low-cost, and easy to industrialize.

[0058] The present invention is further illustrated below by way of examples, but the invention is not limited to the scope of the examples described. All reagents and raw materials used in the following examples are commercially available, and test methods not specifically specified are generally performed under conventional conditions or according to the conditions recommended by the respective manufacturers.

[0059] Example 1

[0060] This embodiment provides a method for preparing a sodium-ion battery cathode material with a Na-poor and F-rich surface, including the following steps:

[0061] 100g Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 The (OH)2 precursor (commercially available), 61.04g Na2CO3, 0.313g TiO2, 0.675g ZrO2 and 0.313g CuO were mixed evenly and then sintered in air at a temperature of 1020℃ for 12h at a heating rate of 2℃ / min. The sintered sample was then pulverized and sieved to obtain the layered bulk material O3-NFM111.

[0062] Subsequently, 100g of the prepared O3-NFM111 was mixed evenly with 0.065g MgF2, 0.098g MgO, and 0.354g Al2O3, and then sintered in air at a temperature of 750℃ for 6 hours at a heating rate of 2℃ / min to obtain a product with MgAl2O3. 3.4 F 0.6 A sodium-ion battery cathode material with a spinel structure coating, wherein the mass of the spinel structure coating accounts for 5 wt‰ of the mass of the layered structure phase material.

[0063] Example 2

[0064] Compared with Example 1, the difference is that the sintering temperature for preparing O3-NFM111 bulk material was 950℃, and the sample morphology was secondary spherical particles.

[0065] Example 3

[0066] This embodiment provides a method for preparing a sodium-ion battery cathode material with a Na-poor and F-rich surface, including the following steps:

[0067] 34.144g Ni(OH)2, 29.406g Fe2O3, 26.126g MnO, 61.04g Na2CO3, 0.313g TiO2, 0.675g ZrO2 and 0.313g CuO were mixed evenly and then sintered in air at a temperature of 1020℃ for 12h at a heating rate of 2℃ / min. The sintered sample was then pulverized and sieved to obtain the layered bulk material O3-NFM111.

[0068] Subsequently, 100g of the prepared O3-NFM111 was mixed evenly with 0.065g MgF2, 0.098g MgO, and 0.354g Al2O3, and then sintered in air at a temperature of 750℃ for 6 hours at a heating rate of 2℃ / min, yielding a product with MgAl2O3... 3.4 F 0.6 A sodium-ion battery cathode material with a spinel structure coating, wherein the mass of the spinel structure coating accounts for 5 wt‰ of the mass of the layered structure phase material.

[0069] Example 4

[0070] This embodiment provides a method for preparing a sodium-ion battery cathode material with a Na-poor and F-rich surface, including the following steps:

[0071] 30.154 g Ni(OH)₂, 25.870 g MnO, 23.615 g TiO₂, and 34.996 g Na₂CO₃ were mixed evenly and sintered in air at a temperature of 900 °C for 12 h at a heating rate of 2 °C / min. The sintered sample was then pulverized and sieved to obtain the layered bulk material P₂-Na. 0.67 Ni 0.33 Mn 0.37 Ti 0.3 O2.

[0072] Subsequently, 100g of the prepared P2-Na 0.67 Ni 0.33 Mn 0.37 Ti 0.3 O2 was mixed evenly with 0.106g LiF and 0.622g Mn3O4 and sintered in air atmosphere at a temperature of 850℃ for 6h and a heating rate of 2℃ / min to obtain a sodium-ion battery cathode material with a LiMn2O3F spinel structure coating layer, wherein the mass of the spinel structure coating layer accounts for 7.5wt‰ of the mass of the layered structure phase material.

[0073] Example 5

[0074] This embodiment provides a method for preparing a sodium-ion battery cathode material with a Na-poor and F-rich surface, including the following steps:

[0075] 26.774 g Ni(OH)₂, 3.843 g Fe₂O₃, 30.730 g MnO, 3.880 g MgO, 7.688 g TiO₂, and 43.363 g Na₂CO₃ were mixed evenly and sintered in air at 950 °C for 12 h at a heating rate of 2 °C / min. The sintered sample was then pulverized and sieved to obtain the layered bulk material P₂ / O₃-Na. 0.85 Ni 0.30 Fe 0.05 Mn 0.45 Mg 0.10 Ti 0.1 O2.

[0076] Subsequently, 100g of the prepared P2 / O3-Na 0.85 Ni 0.30 Fe 0.05 Mn 0.45 Mg 0.10 Ti 0.1O2 was mixed with 0.038g NaF, 0.242g CuO, and 0.489g Co3O4 and sintered in air at a temperature of 850℃ for 6 hours at a heating rate of 2℃ / min to obtain CuCo2O4. 3.7 F 0.3 A sodium-ion battery cathode material with a spinel structure coating, wherein the mass of the spinel structure coating accounts for 7.5 wt‰ of the mass of the layered structure phase material.

[0077] Example 6

[0078] Compared with Example 1, the difference is that the surface of the prepared sodium-ion battery cathode material is MgAl2O. 3.2. F 0.8 Spinel-structured coating.

[0079] Example 7

[0080] Compared with Example 1, the difference is that the surface of the prepared sodium-ion battery cathode material is MgAl2O. 3.8 F 0.2 Spinel-structured coating.

[0081] Example 8

[0082] Compared with Example 1, the difference lies in that the sintering temperature for preparing the O3-NFM111 bulk material was 850℃, the holding time was 20h, and the heating rate was 1℃ / min; MgAl2O 3.4 F 0.6 The sintering temperature for spinel structure coating is 700℃, the holding time is 10h, and the heating rate is 1℃ / min.

[0083] Example 9

[0084] Compared with Example 1, the difference lies in the sintering temperature of the O3-NFM111 bulk material preparation being 1100℃, the holding time being 6h, and the high-temperature sintering treatment being carried out at a heating rate of 10℃ / min; MgAl2O 3.4 F 0.6 The sintering temperature for spinel structure coating is 1000℃, the holding time is 4h, and the heating rate is 10℃ / min.

[0085] Comparative Example 1

[0086] Compared with Example 1, the difference is that the spinel phase MgAl2O is not processed. 3.4 F 0.6 The coating of matter.

[0087] Comparative Example 2

[0088] 100g Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 The (OH)2 precursor (commercially available), 61.04g Na2CO3, 0.313g TiO2, 0.675g ZrO2 and 0.313g CuO were mixed evenly and then sintered in air at a temperature of 1020℃ for 12h at a heating rate of 2℃ / min. The sintered sample was then pulverized and sieved to obtain the layered bulk material O3-NFM111.

[0089] Subsequently, 100g of the prepared O3-NFM111 was mixed evenly with 0.142g of MgO and 0.358g of Al2O3 and sintered in air atmosphere at a temperature of 750℃ for 6h and a heating rate of 2℃ / min to obtain a sodium-ion battery cathode material with a MgAl2O4 spinel structure coating layer, wherein the mass of the spinel structure coating layer accounts for 5wt‰ of the mass of the layered structure phase material.

[0090] SEM comparison of the sodium-ion battery cathode materials prepared in Examples 1 and 2 and Comparative Example 1 Figure 1 , Figure 2 and Figure 3 As shown.

[0091] Figure 1 The image shows the SEM image of the sample in Example 1. The morphology is an irregular blocky shape, exhibiting typical single-crystal morphology characteristics. The particle surface is smooth and there are no residual alkali features. Figure 3 The SEM image of the sample in Comparative Example 1 shows the uncoated spinel phase MgAl2O. 3.4 F 0.6 The sample also exhibited an irregular blocky single-crystal morphology, with fine white spots on the surface of its particles, which were residual alkali precipitated on the surface. Figure 2 The image shows the SEM image of the sample in Example 2. The sample exhibits a spherical morphology, typical of polycrystalline structures, and the primary particle surface is also smooth. A comparison of the SEM images of Examples 1 and 2 with Comparative Example 1 shows that the sample coated with the fluorine-containing spinel phase structure exhibits a significant reduction in residual alkali material on the surface.

[0092] The positive electrode active materials prepared in each embodiment and comparative example were used to fabricate coin-type half-cells, and their electrochemical performance was tested. The specific testing method was as follows: using the sodium-ion battery positive electrode materials recovered and prepared in each embodiment and comparative example as the positive electrode, a metallic sodium sheet as the negative electrode, a glass fiber membrane as the separator, and a NaPF6 / propylene carbonate mixed solution as the electrolyte, a sodium-ion battery was assembled and subjected to charge-discharge tests. The current density was 15 mA / g, the voltage range was 2.5–4.1 V, and the test temperature was 25°C. The test results were recorded in Table 1. Comparison graphs of charge-discharge curves, rate performance, and cycle performance of the batteries prepared with the positive electrode materials of Example 1 and Comparative Examples 1 and 2 are shown below. Figure 4 , Figure 5 and Figure 6 As shown.

[0093] The specific test method for thermal stability is as follows: After the prepared coin cell half-cells are left to stand for 8–12 hours, they are first formed by charging and discharging at a current of 0.1C for 2 cycles, and then charged to 4.1V using the GITT method with a GITT current of 0.05C and a relaxation time of 30 minutes. The fully charged battery is disassembled in a glove box, the positive electrode is removed, and cleaned in DMC solution for 30 minutes. Then, it is vacuum dried under negative pressure in the glove box for 10 minutes. After complete drying, the positive electrode is scraped to remove powder, and a certain amount of positive electrode material powder is weighed and placed into a disposable high-pressure crucible, which is then sealed. The mass difference before and after weighing the crucible is obtained to obtain the sample mass. The test is performed in a DSC device under the following conditions: 50–500℃, N2 atmosphere, N2 flow rate of 50 mL / min, and heating rate of 2℃ / min.

[0094] The electrochemical performance, initial decomposition temperature, and residual alkali content of the sodium-ion battery cathode materials prepared in the above examples and comparative examples are listed in Table 1 below.

[0095] Table 1. Performance Comparison of Prepared Sodium-ion Cathode Materials

[0096]

[0097]

[0098] Comparing Examples 1, 2, and 3, it is evident that the present invention can prepare high-rate, high-safety sodium-ion battery cathode materials through two methods: precursor-dopant mixing-sintering or high-temperature solid-state method. Furthermore, it is applicable to both monocrystalline and polycrystalline samples. The samples prepared by the solid-state method exhibit slightly lower overall performance than those prepared by the co-precipitation method. This is because the co-precipitation process results in a more uniform elemental distribution and better sample consistency.

[0099] Examples 4 and 5 are P2 phase and P2 / O3 mixed phase materials, respectively. They can also be used as spinel-coated matrix materials, and their rate capability, cycle life, and safety are better than those of O3 phase cathode materials.

[0100] By comparing the sample of Example 1 with that of Comparative Example 1, it can be found that the discharge capacity, rate performance, cycle performance and thermal stability of the uncoated Na-poor and F-rich spinel structure sample are all inferior to those of the coated sample, and the residual alkali content is also significantly higher than that of the coated sample. This indicates that the presence of the Na-poor and F-rich spinel structure coating layer has a significant improvement on the overall performance of the matrix sample.

[0101] By comparing the samples of Example 1 and Comparative Example 2, it is shown that the sample with the F-rich spinel structure coating has a higher initial thermal decomposition temperature than the sample with conventional spinel oxide coating, and its improvement in thermal stability is significantly better than that of conventional spinel oxide coating.

[0102] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.

[0103] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A sodium-ion battery cathode material with a Na-poor and F-rich surface, characterized in that, The chemical formula of the sodium-ion battery positive electrode material with Na-poor and F-rich surface is Na x TMO 2-y F y / AB₂O 4-z F z , where 0.44<x≤1.05, 0≤y<0.5, 0<z≤4, TM includes at least one of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Ca, Y, Si, Ta, La, Nb, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, A includes at least one of Li, Na, K, Mg, Cu, Zn, Sr, Ni, Ca, B includes at least one of Co, Al, Fe, Mn, Si, Zr, Ti, B, Cr, Cd, La, and A and B are not the same.

2. The sodium-ion battery cathode material with a Na-poor and F-rich surface according to claim 1, characterized in that, It includes a sodium ion layered oxide bulk material and a spinel-structured compound layer coating the surface of the sodium ion layered oxide bulk material, wherein the chemical formula of the sodium ion layered oxide bulk material is Na. x TMO 2-y F y The chemical formula of the spinel structure compound layer is AB2O. 4-z F z ; Preferably, the thickness of the spinel structure compound layer is 2-20 nm; Preferably, the mass of the spinel structure compound layer is 2-15 wt‰ of the mass of the sodium ion layered oxide bulk material; Preferably, the sodium ion layered oxide bulk material has an O phase, a P phase, or an O / P mixed phase crystal structure.

3. The sodium-ion battery cathode material with a Na-poor and F-rich surface according to claim 1, characterized in that, The sodium-ion battery cathode material with a Na-poor and F-rich surface has an irregular blocky or spherical morphology.

4. The method for preparing the sodium-ion battery cathode material with a Na-poor and F-rich surface as described in any one of claims 1-3, characterized in that, include: Sodium-ion layered oxide bulk material is mixed with a coating agent and sintered to obtain the sodium-ion battery cathode material with a Na-poor and F-rich surface. The coating agent includes source A, source B and fluorine source.

5. The preparation method according to claim 4, characterized in that, include: Bulk material Na was obtained by mixing precursors, sodium source, and dopants, followed by sintering. x TMO 2-y F y Alternatively, a solid-state method can be used to obtain bulk material Na by uniformly mixing a metal or non-metal element compound with a sodium source in a stoichiometric ratio and then sintering at high temperature. x TMO 2-y F y .

6. The preparation method according to claim 5, characterized in that, The sodium source includes any one or a combination of two or more of Na2CO3, NaHCO3, NaOH, Na2O, and CH3COONa.

7. The preparation method according to claim 5, characterized in that, include: The precursor, sodium source, and dopant are mixed uniformly and subjected to a first sintering treatment to obtain the bulk material Na. x TMO 2-y F y The molar ratio of the precursor, sodium source and dopant element TM:Na:F is 1:x:y; Preferably, the chemical formula of the precursor is any one or a combination of two or more of MCO3, M(OH)2, MC2O4, and MO2, wherein M includes any one or a combination of two or more of Ni, Fe, Mn, Cu, Mg, Ti, Zn, and Co; Preferably, the dopant includes an L-containing compound, wherein L includes any one or a combination of two or more of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Zn, Ca, Y, Si, Ta, La, Nb, Zr, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F; Preferably, the first sintering process includes: heating to 850-1100°C at a heating rate of 1-10°C / min, holding at that temperature for 6-20 hours, and the sintering atmosphere including air or oxygen.

8. The preparation method according to claim 5, characterized in that, include: A bulk material Na is obtained by uniformly mixing a metallic or non-metallic element compound with a sodium source and then sintering it at high temperature. x TMO 2-y F y The molar ratio of the metal or non-metal element compound and the sodium source element TM:Na:F is 1:x:y; Preferably, the metallic or non-metallic element in the metallic or non-metallic element compound includes any one or a combination of two or more of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Ca, Si, Ta, La, Nb, Y, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F; Preferably, the high-temperature sintering process includes: heating to 850-1100℃ at a heating rate of 1-10℃ / min, holding at that temperature for 6-20 hours, and the sintering atmosphere including air or oxygen.

9. The preparation method according to claim 4, characterized in that, include: The sodium ion layered oxide bulk material is mixed with a coating agent and subjected to a second sintering treatment to obtain the sodium ion battery cathode material with a Na-poor and F-rich surface. The molar ratio of elements A:B:F in the A source, B source and fluorine source is 1:2:

2. Preferably, the mass ratio of the sodium ion layered oxide bulk material to the coating agent is 1000:2-15; Preferably, the A source includes any one or a combination of two or more of the following: oxides of A, hydroxides of A, carbonates of A, oxalates of A, acetates of A, and nitrates of A. Preferably, the B source includes any one or a combination of two or more of the following: oxides of B, hydroxides of B, carbonates of B, oxalates of B, acetates of B, and nitrates of B. Preferably, the fluorine source includes a fluorine-containing compound; more preferably, the fluorine-containing compound includes any one or a combination of two or more of LiF, NaF, CaF2, MgF2, AlF3, and NH4F. Preferably, the second sintering process includes: heating to 700-1000°C at a heating rate of 1-10°C / min, holding at that temperature for 4-10 hours, and the sintering atmosphere including air or oxygen.

10. A sodium-ion battery, comprising a positive electrode material, characterized in that, The cathode material includes any one of the sodium-ion battery cathode materials with a Na-poor and F-rich surface as described in claims 1-3.