Composite positive electrode active material, positive electrode and rechargeable lithium battery
By combining lithium iron phosphate-based compounds and lithium manganese-based oxides into composite positive electrode active materials to form secondary particles, the problem of deterioration in cycle life characteristics of lithium iron phosphate-based positive electrode active materials under high voltage is solved, thereby improving the performance and stability of rechargeable lithium batteries.
Patent Information
- Application Number
- CN202610662902.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-05-11
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
The active material of lithium iron phosphate positive electrode exhibits deterioration in cycle life characteristics under high voltage and has low capacity and energy density, which limits its application in rechargeable lithium batteries.
The composite positive electrode active material is adopted, which consists of lithium iron phosphate-based compounds and lithium manganese-based oxides as the first and second positive electrode active materials. Through particle-based composite, secondary particles are formed, which ensures price competitiveness and improves charging/discharging efficiency, low-temperature discharge capacity, cycle life characteristics and high-temperature storage characteristics.
It improves the charging/discharging efficiency, low-temperature discharge capacity, cycle life characteristics, and high-temperature storage characteristics of rechargeable lithium batteries, while maintaining price competitiveness and improving powder characteristics and particle density.
Smart Images

Figure CN123120664A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to composite positive electrode active materials, positive electrodes, and rechargeable lithium batteries. Background Technology
[0002] Portable information devices (such as cellular phones, laptops, and smartphones) or electric vehicles already use rechargeable lithium batteries with high energy density as their power source. Recently, research has been actively conducted to use rechargeable lithium batteries with high energy density as a power source or energy storage source for hybrid or electric vehicles.
[0003] Furthermore, the increasing demand for high-performance, safe, and reliable novel positive electrode active materials is driven by the expansion and large-scale production of rechargeable lithium batteries. For example, lithium iron phosphate (LiFePO4)-based positive electrode active materials are attracting attention due to their structural stability, high heat resistance, and abundant raw material availability, making them cost-effective.
[0004] However, lithium iron phosphate (LFP) based positive electrode active materials exhibit a degradation in cycle life characteristics at high voltages, thus limiting their operating voltage. LFP-based positive electrode active materials also suffer from low capacity and energy density. Summary of the Invention
[0005] This disclosure provides composite positive electrode active materials, a positive electrode, and a rechargeable lithium battery that have improved charge / discharge efficiency, low-temperature discharge capacity, cycle life characteristics, and high-temperature storage characteristics, while ensuring the price competitiveness of the rechargeable lithium battery, increasing the average voltage, and having improved powder characteristics, and therefore improved pellet (disc) density.
[0006] According to some embodiments of this disclosure, the composite positive electrode active material may be in particulate form, comprising: a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles, and a second positive electrode active material comprising a lithium manganese-based oxide and in the form of primary particles. The particulate form may include a plurality of primary particles of the first positive electrode active material and a plurality of primary particles of the second positive electrode active material.
[0007] In some embodiments, the lithium iron phosphate-based compound may include a compound represented by Chemical Formula 1, a compound represented by Chemical Formula 2, or a combination thereof. Chemical Formula 1 is as follows:
[0008] Li a1 Fe (1-x1) M 1 x1 PO4.
[0009] Where 0.9 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4. M 1 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Chemical formula 2 is as follows:
[0010] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4.
[0011] Where 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, and x² + y² < 1. M 2 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof.
[0012] In some embodiments, based on the total metals other than lithium in the lithium iron phosphate-based compound, the lithium iron phosphate-based compound may include Al, Mg, Ti, V or combinations thereof in an amount ranging from about 0.1 mol% to about 0.5 mol%.
[0013] In some embodiments, the average particle size of the primary particles of the first positive electrode active material may be greater than or equal to about 0.1 μm and less than about 2 μm.
[0014] In some embodiments, the arithmetic mean size of the primary particles of the first positive electrode active material may be less than or equal to about 200 nm. The standard deviation of the arithmetic mean size of the primary particles of the first positive electrode active material may be less than or equal to about 100 nm.
[0015] In some embodiments, the first positive electrode active material may further include a carbon coating layer on the surface of the primary particles.
[0016] In some embodiments, lithium manganese-based oxides may be represented as follows:
[0017] Li a3 Mn x3 M 3 y3 O 4-b3 X b3 .
[0018] Where 0.9 ≤ a³ ≤ 1.8, 1.7 ≤ x³ ≤ 2, 0 ≤ y³ ≤ 0.3, 1.9 ≤ x³ + y³ ≤ 2.1, and 0 ≤ b³ ≤ 0.1. M 3may be Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr, or a combination thereof. X may be F, P, S, or a combination thereof.
[0019] In some embodiments, the lithium manganese-based oxide may be represented by the following formula:
[0020] Li a4 Mn x4 Al y4 Mg z4 M 4 w4 O 4-b4 X b4 .
[0021] where 0.9≤a4≤1.8, 1.7≤x4<2.0, 0<y4≤0.015, 0<z4≤0.010, 0≤w4<0.3, 1.9≤x4+y4+z4+w4≤2.1, and 0≤b4≤0.1. M 4 may be B, Ba, Ca, Ce, Cr, Fe, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr, or a combination thereof. X may be F, P, S, or a combination thereof.
[0022] In some embodiments, the average particle size of primary particles of the second positive electrode active material may be about 2 μm to about 10 μm.
[0023] In some embodiments, the composite positive electrode active material is in the form of a plurality of secondary particles, and the average particle size of the secondary particles of the composite positive electrode active material may be about 3 μm to about 20 μm.
[0024] In some embodiments, based on 100 wt% of the composite positive electrode active material, the composite positive electrode active material may include the first positive electrode active material in an amount of about 50 wt% to about 99 wt%. Based on 100 wt% of the composite positive electrode active material, the composite positive electrode active material may include the second positive electrode active material in an amount of about 1 wt% to about 50 wt%.
[0025] In some embodiments, the number of primary particles of the second positive electrode active material in the particles of the composite positive electrode active material may be 10 or less.
[0026] In some embodiments, the particles of the composite positive electrode active material may include pores. The porosity of the particles of the composite positive electrode active material (which may be the ratio of the area occupied by the pores to the cross-sectional area of the particles of the composite positive electrode active material) may be about 10% to about 50%.
[0027] According to some embodiments of this disclosure, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the above-described composite positive electrode active material.
[0028] A rechargeable lithium battery according to some embodiments of this disclosure may include a positive electrode, a negative electrode, and an electrolyte as described above.
[0029] Composite positive electrode active materials according to some embodiments can ensure price competitiveness, increase average voltage, improve the charge / discharge efficiency, low-temperature discharge capacity, cycle life characteristics and high-temperature storage characteristics of rechargeable lithium batteries, and improve powder characteristics to improve particle density. Attached Figure Description
[0030] Figure 1 A schematic perspective view showing portions of a cylindrical rechargeable lithium battery according to some embodiments of the present disclosure.
[0031] Figure 2 A cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure is shown schematically.
[0032] Figure 3 and 4 Schematic exploded perspective views of pouch-type rechargeable lithium batteries according to some embodiments of the present disclosure.
[0033] Figure 5 This is a scanning electron microscope image of the cross-section of the composite positive electrode active material prepared in Example 3. Detailed Implementation
[0034] Specific embodiments will be described in detail below so that those skilled in the art can readily implement them. However, this disclosure may be embodied in many different forms and is not to be construed as limited to the embodiments set forth herein.
[0035] The terminology used herein is for describing implementation methods and is not intended to limit the invention. Unless the context clearly specifies otherwise, singular expressions include plural expressions.
[0036] The term "combination" refers to a mixture, laminate, complex, copolymer, alloy, blend, or reaction product of the constituent elements.
[0037] Terms such as “comprising,” “including,” or “having” are intended to indicate the presence of the features, quantities, steps, elements, or combinations thereof embodied, but do not preclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.
[0038] In the accompanying drawings, for clarity, the thickness of layers, films, panels, or regions is exaggerated, and throughout the specification, the same reference numerals denote the same elements. It will be understood that when an element, such as a layer, film, region, or substrate, is referred to as being "on" another element, it may be directly on said other element, or there may be intermediate elements present. Conversely, when an element is referred to as being "directly on" another element, there are no intermediate elements present.
[0039] In addition, the term "layer" in this article includes not only the geometry formed on the entire surface when viewed from a plan view, but also the geometry formed on a portion of the surface.
[0040] The average particle size can be measured, for example, by a particle size analyzer, or by transmission electron microscopy (TEM) or scanning electron microscopy (SEM) images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles in each size range, and calculating accordingly. Unless otherwise defined, the average particle size D... 50 This can mean the diameter of particles that have a cumulative volume of 50% in the particle size distribution, where the particles are considered (assumed) to be spherical. Unless otherwise defined, the average particle size is the value obtained by measuring the dimensions of approximately 20 randomly selected particles from scanning electron microscope (SEM) images and calculating the arithmetic mean of the dimensions of approximately 20 randomly selected particles, where the size of each particle is defined as the diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles.
[0041] The word "or" is not interpreted as exclusive; for example, "A or B" is interpreted as including A, B, or A+B.
[0042] The term "metal" is interpreted to include the concepts of common metals, transition metals, and metalloids (semi-metals). As used herein, the term "metalloid" refers to an element that has properties intermediate between those of metals and nonmetals. Examples of metalloids include, but are not limited to, boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te).
[0043] As used herein, the term "primary particle" refers to the smallest unit particle identified as an agglomeration (cluster) of individual particles when observed using a scanning electron microscope (SEM) of the positive electrode active material, where grain boundaries are not clearly distinguishable or are substantially (substantially) unobservable. Primary particles are the basic units constituting secondary particles formed by the aggregation of tens to hundreds of particles, and can exist individually or in a state where a small number (e.g., 20 or fewer) of primary particles are in contact with each other.
[0044] As used herein, the term "secondary particle" refers to an aggregate of primary particles of a given material, and may also be referred to as an assembly (assembly, collection) in this disclosure. Secondary particles have a structure in which primary particles are combined into individual particle forms (rather than a simple physical mixture) through interparticle contact and bonding. When observed using a scanning electron microscope (SEM), secondary particles can be identified as individual particle forms in which multiple primary particles are aggregated. Such secondary particles are distinguished from simple mixtures in which the corresponding particles are independently dispersed. Secondary particles can be formed by processes such as spray drying.
[0045] Composite positive electrode active material
[0046] According to some embodiments, the composite positive electrode active material includes: a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles, and a second positive electrode active material comprising a lithium manganese-based oxide and in the form of primary particles. The composite positive electrode active material has a particulate form comprising a plurality of primary particles of the first positive electrode active material and a plurality of primary particles of the second positive electrode active material.
[0047] Lithium iron phosphate (LFP)-based compounds, exhibiting excellent structural stability, high heat resistance, and competitive pricing, are attracting attention. However, despite offering superior cycle life characteristics, these characteristics deteriorate when used at high voltages, thus limiting their usable voltage.
[0048] Therefore, an attempt was made to simply mix and use lithium manganese-based oxides, which are low-cost materials with high average voltage. Although this improves the average voltage for rechargeable lithium batteries, the initial charge / discharge efficiency, discharge capacity at low temperatures (e.g., -20°C), cycle life characteristics, and high-temperature storage characteristics of rechargeable lithium batteries can be degraded.
[0049] According to some embodiments, the composite positive electrode active material includes lithium iron phosphate-based compounds to ensure the price competitiveness of rechargeable lithium batteries, and includes lithium manganese-based oxides (which can be used at high voltages and are relatively inexpensive compared to lithium iron phosphate-based compounds). Furthermore, the primary particles of the lithium iron phosphate-based compound and the primary particles of the lithium manganese-based oxide agglomerate to form individual secondary particles (a type of assembly), thereby improving the initial charge / discharge efficiency at high voltages, the discharge capacity at low temperatures (e.g., -20°C), cycle life characteristics, and high-temperature storage characteristics for rechargeable lithium batteries.
[0050] First positive electrode active material
[0051] The first positive electrode active material includes a lithium iron phosphate-based compound. By including a lithium iron phosphate-based compound as the first positive electrode active material, the composite positive electrode active material can ensure price competitiveness while also providing excellent structural and thermal stability for rechargeable lithium batteries.
[0052] Lithium iron phosphate-based compounds may include compounds represented by Chemical Formula 1, compounds represented by Chemical Formula 2, or combinations thereof. Chemical Formula 1 is as follows:
[0053] [Chemical Formula 1]
[0054] Li a1 Fe (1-x1) M 1 x1 PO4.
[0055] In chemical formula 1, 0.9 ≤ a1 ≤ 1.5, 0 ≤ x1 ≤ 0.4, and M 1 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a1 ≤ 1.5; for example, 0.90 ≤ a1 ≤ 1.2, or 0.95 ≤ a1 ≤ 1.1. Additionally, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0.001 ≤ x1 ≤ 0.05.
[0056] Chemical formula 2 is as follows:
[0057] [Chemical Formula 2]
[0058] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4.
[0059] In chemical formula 2, 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, x² + y² < 1, and M 2 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a² ≤ 1.5; for example, 0.90 ≤ a² ≤ 1.2, or 0.95 ≤ a² ≤ 1.1. Additionally, 0.1 ≤ x² ≤ 0.9, 0.3 ≤ x² ≤ 0.9, or 0.4 ≤ x² ≤ 0.8 and 0 ≤ y² ≤ 0.4, 0 ≤ y² ≤ 0.3, 0 ≤ y² ≤ 0.2, 0 ≤ y² ≤ 0.1, or 0 ≤ y² ≤ 0.05.
[0060] Lithium iron phosphate-based compounds may include LiFePO4 and LiMn.0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof, but lithium iron phosphate-based compounds are not limited to these.
[0061] Lithium iron phosphate-based compounds may include Al, Mg, Ti, V, or combinations thereof as doping elements, and may include Al, Mg, Ti, V, or combinations thereof in amounts of about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol% or about 0.4 mol% based on the total metals other than lithium.
[0062] Lithium iron phosphate-based compounds may include Ti, Al, or a combination thereof as doping elements, wherein the amount of Ti may be from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%, based on the total metals excluding lithium, and the amount of Al may be from about 0.1 mol% to about 0.5 mol%, based on the total metals excluding lithium. This can improve rate performance and cycle life characteristics for rechargeable lithium batteries.
[0063] M of chemical formula 1 1 And M of chemical formula 2 2 The active material may include Al, Mg, Ti, V, or combinations thereof, which in this case can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In Formulas 1 and 2, based on the total metals excluding lithium, Al, Mg, Ti, V, or combinations thereof may be included in amounts from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol% or about 0.4 mol%, and these amounts can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In chemical formula 1, 0.001≤x1≤0.005, 0.002≤x1≤0.005, 0.003≤x1≤0.005, or x1=0.004, and in chemical formula 2, 0.001≤x2≤0.005, 0.002≤x2≤0.005, 0.003≤x2≤0.005, or x2=0.004, which improves the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries.
[0064] The first positive electrode active material is in the form of primary particles, and the average particle size of the primary particles of the first positive electrode active material may be less than about 2 μm. The average particle size of the primary particles of the first positive electrode active material may be, for example, greater than or equal to about 0.1 μm and less than about 2 μm, about 0.1 μm to about 1.8 μm, about 0.1 μm to about 1.6 μm, about 0.1 μm to about 1.4 μm, about 0.1 μm to about 1.2 μm, about 0.1 μm to about 1 μm, about 0.1 μm to about 0.8 μm, about 0.2 μm to about 0.8 μm, about 0.3 μm to about 0.7 μm, or about 0.5 μm. The average particle size of the primary particles of the first positive electrode active material can be obtained by measuring the size of approximately 20 primary particles of the first positive electrode active material in an electron microscope image of the surface or cross-section of the composite positive electrode active material in the form of secondary particles, and calculating the arithmetic mean of the size of each particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. The average particle size of the primary particles of the first positive electrode active material may be smaller than the average particle size of the primary particles of the second positive electrode active material described below.
[0065] According to some embodiments, the first positive electrode active material may have small and uniform primary particles. Therefore, the composite positive electrode active material possesses high charge / discharge capacity and excellent cycle life characteristics of rechargeable lithium batteries.
[0066] Furthermore, as measured by scanning electron microscopy (SEM) images of the cross-section of the composite positive electrode active material, the arithmetic mean size of the primary particles of the first positive electrode active material constituting the composite positive electrode active material can be less than or equal to about 200 nm, about 50 nm to about 200 nm, or about 100 nm to about 200 nm, and the standard deviation of the arithmetic mean size can be less than or equal to about 100 nm, less than or equal to about 50 nm, or less than or equal to about 30 nm and can be greater than or equal to about 5 nm, greater than or equal to about 10 nm, or greater than or equal to about 12 nm. The arithmetic mean size and standard deviation of the primary particles of the first positive electrode active material can be obtained by measuring the size of about 20 random primary particles of the first positive electrode active material in the SEM image of the cross-section of the composite positive electrode active material and calculating the arithmetic mean and the standard deviation of the arithmetic mean, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0067] The first positive electrode active material may further include a carbon coating layer on the surface of the primary particles. The carbon coating layer can improve the electrical conductivity of the first positive electrode active material and reduce the resistance of the positive electrode.
[0068] The carbon coating may include amorphous carbon and may be formed from, for example, glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, asphalt resins, tar resins, or combinations thereof.
[0069] Specifically, the carbon coating layer can be formed by: placing carbon raw material on the surface of the first positive electrode active material particles, and then performing a firing process. Alternatively, the carbon raw material and primary particles can be mixed and fired to form a carbon coating layer on the surface of the primary particles, or the carbon raw material and secondary particles can be mixed and fired to form a carbon coating layer on the surface of the secondary particles, and then pulverized to prepare primary particles with the carbon coating layer.
[0070] Based on 100% by weight of the first positive electrode active material, a carbon coating layer may be included in an amount from about 0.1% by weight to about 3.9% by weight, for example, from about 0.5% by weight to about 3.9% by weight, from about 1% by weight to about 3.9% by weight, from about 1.5% by weight to about 3.9% by weight, or from about 1.7% by weight to about 3.9% by weight. Based on 100% by weight of the first positive electrode active material, the amount of the carbon coating layer may be greater than or equal to about 1.5% by weight, greater than about 1.5% by weight, greater than or equal to about 1.6% by weight, greater than or equal to about 1.7% by weight, or greater than or equal to about 1.8% by weight. The amount of the carbon coating layer can be determined by completely burning the first positive electrode active material at a high temperature of about 1200°C to about 1400°C in an oxygen atmosphere to convert the carbon and sulfur in the first positive electrode active material into CO2 (or CO) and SO2, respectively. The amount of the carbon coating layer may be based on the amount of carbon in 100% by weight of the first positive electrode active material.
[0071] The first positive electrode active material can be manufactured by known methods or is a commercially available product. For example, the first positive electrode active material can be obtained by pulverizing secondary particles formed by the aggregation of multiple primary particles and includes lithium iron phosphate-based compounds.
[0072] Second positive electrode active material
[0073] The second positive electrode active material includes a lithium manganese-based composite oxide. The lithium manganese-based oxide included in the second positive electrode active material may have a spinel structure. Lithium manganese-based oxides with a spinel structure have a cubic crystal structure, and because they have a three-dimensional crystal structure, lithium ions have short migration paths, high ionic conductivity, and the overall structure does not collapse when lithium ions are removed, making them very stable.
[0074] The lithium manganese-based oxide can be a lithium manganese-based oxide having a spinel structure with LiMn2O4 as its basic composition. In addition to manganese, the lithium manganese-based oxide may further contain aluminum, magnesium, yttrium, or combinations thereof, and may contain no cobalt or may contain very small amounts of cobalt. For example, based on 100 mol% of metals other than lithium, the cobalt content in the lithium manganese-based oxide may be 5 wt% or less, 3 wt% or less, or 1 wt% or less, and may be 0 wt% or more.
[0075] Lithium manganese-based oxides can be represented by the following chemical formula 3:
[0076] [Chemical Formula 3]
[0077] Li a3 Mn x3 M 3 y3 O 4-b3 X b3 .
[0078] In chemical formula 3, 0.9 ≤ a³ ≤ 1.8, 1.7 ≤ x³ ≤ 2, 0 ≤ y³ ≤ 0.3, 1.9 ≤ x³ + y³ ≤ 2.1, and 0 ≤ b³ ≤ 0.1, M 3 X is Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
[0079] In chemical formula 3, 1.8 ≤ x³ ≤ 2 and 0 ≤ y³ ≤ 0.2, 1.9 ≤ x³ ≤ 2 and 0 ≤ y³ ≤ 0.1, or 1.7 ≤ x³ < 2 and 0 <y3≤0.3。
[0080] Specifically, lithium manganese-based oxides can be represented by the following chemical formula 4:
[0081] [Chemical Formula 4]
[0082] Li a4 Mn x4 Al y4 Mg z4 M 4 w4 O 4-b4 X b4 .
[0083] In Chemical Formula 4, 0.9≤a4≤1.8, 1.7≤x4<2.0, 0<y4≤0.015, 0<z4≤0.010, 0≤w4<0.3, 1.9≤x4+y4+z4+w4≤2.1, and 0≤b4≤0.1, M 4 is one or more elements selected from B, Ba, Ca, Ce, Cr, Fe, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y and Zr, and X is one or more elements selected from F, P and S.
[0084] The second positive electrode active material is in the form of primary particles, and the average particle diameter of the primary particles of the second positive electrode active material may be greater than or equal to about 2 μm. The average particle diameter of single particles of the second positive electrode active material may be, for example, about 2 μm to about 10 μm, about 2 μm to about 9.5 μm, about 2.5 μm to about 9 μm, about 3 μm to about 9 μm, about 3 μm to about 7 μm, or about 3 μm to about 5 μm. The average particle diameter of the primary particles of the second positive electrode active material may be larger than the average particle diameter of the primary particles of the aforementioned first positive electrode active material. That is, the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material within the secondary particle may be distinguished based on particle size. The average particle diameter may be obtained as follows: measuring the size of about 20 random particles of the second positive electrode active material from a scanning electron microscope image (wherein the diameter is measured in the case of spherical particles, and the square root of the product of the major axis length and the minor axis length is measured in the case of non-spherical particles), then calculating the arithmetic mean of the sizes of the respective primary particles of the second positive electrode active material.
[0085] The second positive electrode active material may further include a coating layer on the surface of the primary particles. The coating layer may include a compound of an element including Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, S, or a combination thereof. When the coating layer including the compound is formed on the surface of the second positive electrode active material, the contact between the lithium manganese-based oxide and the electrolyte is blocked, thereby suppressing gas generation during charging and discharging and suppressing elution of manganese at high temperature. The coating layer may include ZnO, Al₂O₃, TiO₂, WO 3、 MgO, CaO, B₂O₃, NbO₂, SrO, CrO, Mo₂O₅, Bi₂O₃, SiO₂, or a combination thereof. The coating layer may be present discontinuously or may be present continuously.
[0086] The second positive electrode active material may be manufactured by a known method or may be a commercially available product.
[0087] The second positive electrode active material can be prepared by solid-state reaction methods, etc. For example, a lithium precursor and a manganese precursor can be mixed in a predetermined molar ratio and then heat-treated in an oxygen atmosphere.
[0088] Examples of lithium precursors may include Li2CO3, LiOH and LiNO3, and examples of manganese precursors may include Mn2O3, MnO2 and Mn3O4.
[0089] Mixing can be carried out by dry or wet mixing methods, and can be performed using methods such as ball milling. The mixture can then be calcined in an oxygen or air atmosphere at a temperature of about 600°C to about 1000°C to form a spinel-structured lithium manganese oxide. If necessary, further pulverization, grading, or sieving can be performed.
[0090] The second positive electrode active material can be prepared in the form of secondary particles from which primary particles agglomerate, and the secondary particles can be separated into primary particles during a subsequent wet milling process to form an assembly of composite positive electrode active materials.
[0091] Composite positive electrode active material
[0092] The composite positive electrode active material has the following characteristics: just The particle form of the multiple primary particles of the electrode active material and the multiple primary particles of the second positive electrode active material. The particle form of the composite positive electrode active material can be that of the first... just The composite positive electrode active material is in the form of secondary particles or assemblies, formed by the aggregation of primary particles of the first positive electrode active material and primary particles of the second positive electrode active material. Primary particles of the first and second positive electrode active materials may exist within the composite positive electrode active material particles. The composite positive electrode active material particles are formed by the aggregation of multiple primary particles. Some of the primary particles are primary particles of the first positive electrode active material, and the remaining portion are primary particles of the second positive electrode active material. This structure differs from a core-shell structure in which particles of the first positive electrode active material surround the surface of the core of the second positive electrode active material particles, thus having a shell structure. In this disclosure, the particle form of the composite positive electrode active material may be referred to as the form of secondary particles or assemblies. Particles described as being in the form of secondary particles or assemblies should be understood to refer to composite positive electrode active material particles.
[0093] The particle form of the composite positive electrode active material according to some embodiments differs from the conventional form in which lithium iron phosphate-based compounds and lithium manganese-based composite oxides are mixed. When lithium iron phosphate-based compounds and lithium manganese-based composite oxides are conventionally mixed and used as positive electrode active materials, the following problem exists: after the formation of the electrode plate, with repeated charging and discharging, the high-temperature storage characteristics deteriorate due to the generation of spaces (gap) between the particles of the lithium iron phosphate-based compound and the lithium manganese-based composite oxide. However, the composite positive electrode active material according to some embodiments solves the above problem by having a particle form, specifically a single secondary particle form by agglomerating primary particles of the first positive electrode active material and primary particles of the second positive electrode active material, more specifically an assembly form comprising: a first positive electrode active material in the form of primary particles of the lithium iron phosphate-based compound and a second positive electrode active material in the form of primary particles of the lithium manganese-based composite oxide.
[0094] By tightly agglomerating the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material, the composite positive electrode active material particles can have a spherical or ellipsoidal geometry. The average particle size of the composite positive electrode active material particles can be, for example, about 3 μm to about 20 μm, about 6 μm to about 20 μm, about 6 μm to about 18 μm, about 8 μm to about 18 μm, about 10 μm to about 18 μm, or about 12 μm to about 18 μm. The average particle size of the composite positive electrode active material particles can be obtained by randomly selecting about 20 secondary particles from an electron microscope image of the composite positive electrode active material, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. The average particle size of the composite positive electrode active material particles can be the average particle size of the secondary particles of the composite positive electrode active material.
[0095] The amounts of the first and second positive electrode active materials in the composite positive electrode active material can be appropriately controlled. Based on 100% by weight of the composite positive electrode active material, the first positive electrode active material may be included in an amount of about 50% to about 99% by weight, about 55% to about 95% by weight, or about 60% to about 90% by weight, and based on 100% by weight of the composite positive electrode active material, the second positive electrode active material may be included in an amount of about 1% to about 50% by weight, about 5% to about 45% by weight, or about 10% to about 40% by weight. If the first and second positive electrode active materials in the composite positive electrode active material are included to satisfy the above ranges, the battery can operate (run) at high voltage, and for rechargeable lithium batteries, battery performance (including initial charge / discharge capacity, efficiency, discharge capacity at low temperature (-20°C), and high-temperature storage characteristics) can be improved.
[0096] The composite positive electrode active material may further include a carbon coating layer on the surface of the composite positive electrode active material particles. The carbon coating layer can improve the electrical conductivity of the composite positive electrode active material and thereby reduce the resistance of the positive electrode comprising it. The carbon coating layer may be the same as the carbon coating layer on the surface of the primary particles of the first positive electrode active material of the composite positive electrode active material described above, and therefore a description of the carbon coating layer is omitted in this section.
[0097] The number of primary particles of the second positive electrode active material in the particles of the composite positive electrode active material can be 10 or less, for example 9 or less, 8 or less, 7 or less, or 6 or less and greater than zero, or 1 or more, 2 or more, or 3 or more. For example, the number of primary particles of the second positive electrode active material in the particles of the composite positive electrode active material can be in the range of 1 to 10, 2 to 10, 3 to 10, 3 to 9, 3 to 8, 3 to 7, or 3 to 6. The number of primary particles of the second positive electrode active material in the particles of the composite positive electrode active material can be determined by counting the number of particles with a particle size greater than or equal to about 2 μm within a single composite positive electrode active material particle, where particle size refers to diameter in the case of spherical particles and the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. Here, the number of primary particles of the second positive electrode active material can be the average number of primary particles of the second positive electrode active material in each of a plurality of composite positive electrode active material particles.
[0098] The particles of the composite positive electrode active material may include pores, and the porosity (which is the ratio of the area occupied by the pores to the cross-sectional area of the composite positive electrode active material particles) may be from about 10% to about 50%, for example from about 10% to about 40%, from about 10% to about 30%, or from about 20% to about 30%. The porosity can be obtained by cutting the composite positive electrode active material particles using a focused ion beam (FIB) to obtain a cross-section, and by measuring the ratio of the area occupied by the pores to the cross-sectional area of the composite positive electrode active material particles within the cross-section using an image analysis program such as ImageJ via scanning electron microscopy. The cross-section of the composite positive electrode active material can be obtained by cutting the composite positive electrode active material using a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be acquired, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or a consistent threshold setting method equally applied to all samples. The porosity of the composite positive electrode active material can be the average of the porosities measured for multiple composite positive electrode active materials, and can be obtained, for example, by measuring the porosity of at least 20 individual composite positive electrode active materials and calculating the average porosity of at least 20 individual composite positive electrode active materials. If the porosity in the composite positive electrode active material particles meets the above range, during positive electrode compression, primary particles can fill the spaces between the pores in secondary particles, thereby improving the aggregate density or positive electrode density, and thus improving the capacity characteristics and energy density of the rechargeable lithium battery.
[0099] The agglomerate density of the composite positive electrode active material can be greater than or equal to about 2.4 g / cc, and can be about 2.4 g / cc to about 3 g / cc, about 2.45 g / cc to about 2.9 g / cc, about 2.5 g / cc to about 2.8 g / cc, or about 2.5 g / cc to about 2.6 g / cc. The agglomerate density of the composite positive electrode active material can be measured as follows: 3 g of the composite positive electrode active material is placed in a mold, and the material is held in the mold at 25°C for 30 seconds at a temperature of 4 tonnes. The thickness of the agglomerates is measured, and the agglomerate volume is calculated using the agglomerate thickness and the diameter of the mold. The mass of the composite positive electrode active material is then divided by the calculated volume. If the agglomerate density of the composite positive electrode active material meets the above range, the powder characteristics can be improved, thereby improving the capacity characteristics for rechargeable lithium batteries. If the porosity of the composite positive electrode active material particles meets the above range, during positive electrode compression, the primary particles can further fill the spaces between the pores in the secondary particles, and thus the aggregate density of the composite positive electrode active material can be further improved as it is within the above range, and thus the energy density of the battery can be further increased.
[0100] positive electrode
[0101] According to some embodiments, the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the aforementioned composite positive electrode active material. According to some embodiments, the positive electrode can improve overall battery performance by including the aforementioned composite positive electrode active material, and specifically, can exhibit high capacity, high efficiency, high energy density, and excellent cycle life characteristics while increasing the operating voltage.
[0102] Positive electrode current collector
[0103] There are no particular restrictions on the positive electrode current collector, as long as it is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be an aluminum foil or stainless steel foil with a thickness of about 10 μm to about 15 μm.
[0104] Positive electrode active material layer
[0105] The positive electrode active material layer includes the aforementioned composite positive electrode active material. Specific details of the composite positive electrode active material are the same as described above.
[0106] The amount of composite positive electrode active material may be about 60% to about 99.9% by weight, about 70% to about 99.8% by weight, about 80% to about 99% by weight, or about 90% to about 98% by weight, based on a 100% by weight positive electrode active material layer.
[0107] The positive electrode active material layer may optionally further include a binder, a conductive material, or a combination thereof.
[0108] The binder can be used to ensure good adhesion between composite positive electrode active material particles and to ensure good adhesion of the composite positive electrode active material to the positive electrode current collector. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide (polymers containing ethylene oxide), polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, or nylon, but the binder is not limited to these.
[0109] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes in the battery. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0110] In the positive electrode active material layer, based on 100% by weight of the positive electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the positive electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0111] In addition to the components mentioned above, the positive electrode active material layer may further include other positive electrode active materials without prejudice to the purpose of this disclosure, or may further include irreversible positive electrode additives.
[0112] In addition to the aforementioned composite positive electrode active material, the positive electrode active material layer may further include a positive electrode active material having primary particle form and comprising the aforementioned lithium iron phosphate-based compound (hereinafter, "third positive electrode active material") and / or a positive electrode active material having primary particle form and comprising the aforementioned lithium manganese-based composite oxide (hereinafter, "fourth positive electrode active material"). Here, the third positive electrode active material and / or the fourth positive electrode active material may each be independently those of the first positive electrode active material and / or the second positive electrode active material included in the composite positive electrode active material, which exist in an unassembled and separated state. In this case, the average particle size of the primary particles of the third positive electrode active material may be the same as described above for the first positive electrode active material, and the average particle size of the primary particles of the fourth positive electrode active material may be the same as described above for the second positive electrode active material. Here, the third positive electrode active material and / or the fourth positive electrode active material exist in a non-aggregated, separated state, and do not agglomerate with the aforementioned composite positive electrode active material to form an assembled structure.
[0113] If, in addition to the composite positive electrode active material, the positive electrode active material layer further comprises a third positive electrode active material and / or a fourth positive electrode active material, the weight ratio of the composite positive electrode active material to the third positive electrode active material, the fourth positive electrode active material, or a combination thereof may be from about 1:9 to about 9:1, and may be added appropriately depending on the purpose. The third positive electrode active material in the form of primary particles may further comprise the aforementioned carbon coating layer on the surface of the primary particles, and since the specific details of the carbon coating layer are the same as those described above, those details are omitted in this section.
[0114] Irreversible positive electrode additives are compounds that act as sacrificial positive electrodes, compensating for the irreversible conversion of Li that no longer participates in the charging / discharging reaction by participating in the formation of an SEI (solid electrolyte interphase) film on the surface of the negative electrode during charging / discharging. Irreversible positive electrode additives are compounds that decompose during the formation process to provide Li and do not participate in subsequent charging / discharging processes. By adding such irreversible positive electrode additives, consumed lithium can be replenished, thereby compensating for lithium loss and improving the energy density, cycle life, and stability of rechargeable lithium batteries.
[0115] Irreversible positive electrode additives may include lithium iron-based oxides, lithium cobalt-based oxides, lithium nickel-based oxides, or combinations thereof.
[0116] The lithium iron-based oxide can be Li5FeO4, LiFeO2, LiFe5O8 or a combination thereof, and the use of Li5FeO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and thus greatly achieve the effect of an irreversible positive electrode additive.
[0117] The lithium cobalt-based oxide can be Li6CoO4, and the use of Li6CoO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and thus greatly obtain the effect of an irreversible positive electrode additive.
[0118] The lithium nickel-based oxide can be Li2NiO2, and the use of Li2NiO2 can provide a large amount of lithium during the formation process, which can thus compensate for a large amount of irreversible lithium, and thus greatly achieve the effect of an irreversible positive electrode additive.
[0119] The average particle size D of the irreversible positive electrode additive 50 There are no particular limitations, but it can be, for example, about 0.5 μm to about 20 μm, about 0.5 μm to about 10 μm, about 0.5 μm to about 5 μm, or about 0.5 μm to about 3 μm.
[0120] Rechargeable lithium batteries
[0121] A rechargeable lithium battery according to some embodiments includes the above-described positive electrode, negative electrode, and electrolyte. A rechargeable lithium battery may include a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte.
[0122] According to some embodiments, rechargeable lithium batteries can have generally improved battery performance by including the above-described positive electrode active material, and specifically, can provide improved low-temperature capacity and cycle life characteristics for rechargeable lithium batteries.
[0123] When a rechargeable lithium battery undergoes an initial charge / discharge cycle at a 0.2 C rate and a 0.2 C rate, and this cycle is repeated 50 or more times at a 1 C rate, and the ratio of the discharge capacity of the 50th cycle to the initial discharge capacity is calculated according to Equation 2 (cycle life), the cycle life of the rechargeable lithium battery can be greater than or equal to about 90%. This indicates that rechargeable lithium batteries exhibit improved cycle life characteristics at high voltages compared to rechargeable lithium batteries with a simple mixture of positive electrode active materials. The cycle life of the rechargeable lithium battery can be greater than or equal to about 91%, greater than or equal to about 92%, greater than or equal to about 93%, or greater than or equal to about 94%, and can be less than or equal to about 100%, less than or equal to about 99%, less than or equal to about 98%, less than or equal to about 97%, or less than or equal to about 96%. Equation 2 is as follows:
[0124] [Equation 2]
[0125] Cycle lifetime [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100
[0126] Furthermore, when rechargeable lithium batteries are placed at a high temperature (e.g., approximately 45°C) for 7 days and capacity retention is measured to evaluate high-temperature storage characteristics, the high-temperature capacity retention is greater than or equal to approximately 70%, indicating that the high-temperature storage characteristics of rechargeable lithium batteries are improved compared to rechargeable lithium batteries with simply mixed positive electrode active materials. The high-temperature capacity retention of rechargeable lithium batteries can be greater than or equal to approximately 75% or greater than or equal to approximately 79%, and can be less than or equal to approximately 100%, less than or equal to approximately 95%, or less than or equal to approximately 91%.
[0127] Rechargeable lithium batteries can have cylindrical, prismatic, pouch, or coin-like geometries. Figure 1 This is a schematic diagram showing a cross-section of a cylindrical rechargeable lithium battery cut along a vertical axis according to some embodiments of the present disclosure and an electrode assembly 40 extending from the cylindrical rechargeable lithium battery. Figure 2 This is a cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure. Figure 3 and 4 Each of the following is a schematic exploded perspective view of a pouch-type rechargeable lithium battery according to some embodiments of the present disclosure. The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown).
[0128] The rechargeable lithium battery 100 may include a seal 60 of the sealed housing 50, such as Figure 1 As shown. Additionally, in Figure 2 The rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. The rechargeable lithium battery 100 may include electrode connectors 70, which serve as electrical paths for conducting current generated in the electrode assembly 40 to the outside. The electrode connectors 70 may be as follows: Figure 4 They can be arranged in the same direction as in the middle, or the positive electrode terminal 71 and the negative electrode terminal 72 can be arranged as follows: Figure 3 It is set in the opposite direction as in the middle.
[0129] negative electrode
[0130] The negative electrode for a rechargeable lithium battery includes a negative electrode current collector and a layer of negative electrode active material on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material and may optionally further include a binder, a conductive material, or a combination thereof.
[0131] There are no particular restrictions on the negative electrode current collector, as long as it is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be a copper foil with a thickness of about 10 μm to about 15 μm.
[0132] Negative electrode active materials include materials capable of reversibly inserting / deintercalating lithium ions, lithium metal, lithium metal alloys, materials capable of doping and dedoping lithium, or transition metal oxides.
[0133] Materials capable of reversibly inserting / deintercalating lithium ions can be carbon-based negative electrode active materials, such as crystalline carbon, amorphous carbon, or combinations thereof. Crystalline carbon can be irregular, flake-like, spherical, or fibrous natural or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbonization products, or calcined coke.
[0134] As an alloy of lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.
[0135] Materials capable of doping and dedoping lithium can be Si-based or Sn-based negative electrode active materials. Si-based negative electrode active materials can be silicon, silicon-carbon composites, or SiO₂. x(0<x≤2), a Si-Q alloy (wherein Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements [excluding Si], Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and may for example be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO₂, a Sn alloy, or a combination thereof.
[0136] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter D of the silicon-carbon composite particles 50 may be, for example, from about 0.5 μm to about 20 μm. According to some embodiments, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surfaces of the silicon particles. The silicon-carbon composite may include secondary particles (core) in which silicon primary particles are assembled (aggregated) and an amorphous carbon coating layer (shell) on the surfaces of the secondary particles. Amorphous carbon may also be present between the silicon primary particles; for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be present dispersed in an amorphous carbon matrix.
[0137] The silicon-carbon composite may further include crystalline carbon. The silicon-carbon composite may include: a core including crystalline carbon and silicon particles, and an amorphous carbon coating layer on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon or hard carbon, a mesophase pitch carbonized product, or calcined coke.
[0138] When the silicon-carbon composite includes silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be from about 10 wt% to about 50 wt%, and the amount of amorphous carbon may be from about 50 wt% to about 90 wt%. In addition, when the composite includes silicon, amorphous carbon, and crystalline carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be from about 10 wt% to about 70 wt%, the amount of crystalline carbon may be from about 1 wt% to about 60 wt%, and the amount of amorphous carbon may be from about 15 wt% to about 50 wt%.
[0139] In addition, the thickness of the amorphous carbon coating layer may be from about 5 nm to about 100 nm. The average particle diameter D of the silicon particles (primary particles) 50 may be from about 10 nm to about 1 μm or from about 10 nm to about 200 nm. When no additional definition is provided, the average particle diameter D 50represents the diameter of particles having a cumulative volume of about 50 vol% in the particle size distribution. The silicon particles may be present as elemental silicon, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon may be represented as SiO x (0<x≤2). The atomic ratio of Si:O indicating the oxidation degree may be from about 99:1 to about 33:67.
[0140] The Si-based negative electrode active material or Sn-based negative electrode active material may be mixed with a carbon-based negative electrode active material. When a mixture of the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material is used, the mixing ratio may be about 1:99 to about 90:10 by weight.
[0141] Based on 100 wt% of the negative electrode active material layer, the negative electrode active material may be included in an amount of about 90 wt% to about 99.8 wt% or about 94 wt% to about 99 wt%.
[0142] The binder serves to favorably adhere the negative electrode active material particles to each other, and also serves to adhere the negative electrode active material to the negative electrode current collector. The binder may be a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0143] The non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or a combination thereof.
[0144] The aqueous binder may include styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.
[0145] When an aqueous binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity may be further included. As the cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof may be mixed and used. The alkali metal may be Na, K, or Li.
[0146] The dry binder may be a polymeric material capable of forming fibers and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0147] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0148] Based on 100% by weight of the negative electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the negative electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0149] electrolytes
[0150] The electrolyte used in rechargeable lithium batteries is an electrolyte solution and includes a non-aqueous organic solvent and a lithium salt.
[0151] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of a battery. Non-aqueous organic solvents can be carbonate (carbonate-based) solvents, ester (ester-based) solvents, ether (ether-based) solvents, ketone (ketone-based) solvents, alcohol (alcohol-based) solvents, aprotic solvents, or combinations thereof.
[0152] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butyl carbonate (BC). Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, or caprolactone. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, or tetrahydrofuran. Ketone solvents may include cyclohexanone. Alcohol solvents may include ethanol or isopropanol, and aprotic solvents may include nitriles such as R-CN (where R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups); amides such as dimethylformamide; dioxolane such as 1,3-dioxolane or 1,4-dioxolane; or sulfolane.
[0153] Non-aqueous organic solvents can be used alone or in combination of two or more types, and when two or more types are used in combination, the mixing ratio can be appropriately adjusted depending on the expected battery performance, as is widely understood by those skilled in the art.
[0154] When using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.
[0155] Non-aqueous organic solvents may further include aromatic hydrocarbon organic solvents. Carbonate solvents and aromatic hydrocarbon organic solvents may be mixed and used in a volume ratio of about 1:1 to about 30:1.
[0156] The electrolyte solution may further include vinylene carbonate, vinylene carbonate, or ethylene carbonate compounds to improve battery cycle life.
[0157] Examples of ethylene carbonate compounds may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0158] Lithium salts dissolved in non-aqueous organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts may include at least one of the following: LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).
[0159] The concentration of lithium salt can range from about 0.1 M to about 2.0 M. When the concentration of lithium salt is within this range, the electrolyte solution has suitable ionic conductivity and viscosity. Therefore, excellent performance can be achieved, and lithium ions can move efficiently.
[0160] diaphragm
[0161] Depending on the type of rechargeable lithium battery, a separator may be present between the positive and negative electrodes. The separator may be made of polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer membrane of two or more layers, and may be a hybrid multilayer membrane such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polypropylene three-layer separator, or a polypropylene / polypropylene / polypropylene three-layer separator.
[0162] The diaphragm may include a porous substrate and a coating on one or both surfaces of the porous substrate, comprising organic materials, inorganic materials, or combinations thereof.
[0163] The porous substrate may be a polymer film formed from any of the following polymers: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene ether; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; and polytetrafluoroethylene (e.g., Teflon). ® (TEFLON ® Porous substrates may include glass fibers or composite films of polymers and glass fibers.
[0164] The porous substrate may have a thickness of about 1 μm to about 40 μm, for example, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm.
[0165] Organic materials may include (meth)acrylic acid copolymers, which include a first structural unit and a second structural unit derived from (meth)acrylamide, wherein the second structural unit includes at least one structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.
[0166] Inorganic materials may include the following inorganic particles: Al₂O₃, SiO₂, TiO₂, SnO₂, CeO₂, MgO, NiO, CaO, Ga₂O₃, ZnO, ZrO₂, Y₂O₃, SrTiO₃, BaTiO₃, Mg(OH)₂, boehmite, and combinations thereof, but inorganic materials are not limited to these. The average particle size D of the inorganic particles... 50 It can be about 1 nm to about 2000 nm, for example about 100 nm to about 1000 nm or about 100 nm to about 700 nm.
[0167] Organic and inorganic materials can be mixed in a coating, or coatings containing organic materials and coatings containing inorganic materials can be stacked.
[0168] The coating thickness can be from about 0.5 μm to about 20 μm, for example from about 1 μm to about 10 μm or from about 1 μm to about 5 μm.
[0169] In the following sections, embodiments and comparative examples of the present invention are described. However, the embodiments described below are merely some implementations of the present invention, and the present invention is not limited to the embodiments described below.
[0170] Example 1
[0171] (1) Preparation of composite positive electrode active material
[0172] (Preparation of the active material for the first positive electrode)
[0173] A raw material mixture was prepared by mixing FePO4, as an iron phosphate-based precursor, and Li2CO3, as a lithium raw material, in a molar ratio of 2:1. A carbon raw material was prepared by mixing glucose and polyethylene glycol in a weight ratio of 5:5. Furthermore, 90 wt% of the raw material mixture and 10 wt% of the carbon raw material were mixed to form a slurry, and distilled water as a first solvent was added to the mixture, followed by wet milling to prepare a first slurry. Wet milling was performed using a ball mill. Specifically, approximately 90 wt% of the raw material mixture and approximately 10 wt% of the carbon source material were introduced into a milling vessel with a capacity of approximately 5 L along with approximately 3 kg of zirconia balls and approximately 2 kg of water, and wet milling was performed by rotating the vessel at approximately 100 rpm for approximately 3 hours. During wet milling, TiO2, as a titanium-based raw material, was added, and the amount was adjusted such that Ti accounted for 0.4 mol%, based on the total metals other than lithium in the final lithium iron phosphate-based compound.
[0174] A first slurry, wet-milled, was added to a spray dryer (Büchi Mini SprayDryer B-290) at a rate of 0.5 kg / min and then spray-dried at 200°C to obtain a first dried product. This first dried product was then calcined at 750°C for 8 hours to obtain a first calcined product, which was then pulverized into primary particles at 6000 rpm using an air-jet mill to obtain a first positive electrode active material. Through a pulverization process, the first calcined product, comprising lithium iron phosphate-based compounds, was pulverized into a first positive electrode active material in the form of secondary particles from which multiple primary particles agglomerated, resulting in a first positive electrode active material in which the multiple primary particles did not agglomerate but were instead separated. The first positive electrode active material has an average particle size of 0.5 μm and LiFe... 0.996 Ti 0.004 PO4 is composed of primary particles.
[0175] (Preparation of the active material for the second positive electrode)
[0176] Li₂CO₃ and Mn₂O₃ were mixed in a molar ratio of 1.02:2.0, and then heated from 25°C to 820°C at a heating rate of 5°C / min under an oxygen atmosphere, and held at 820°C for 8 hours to obtain a calcined product. The obtained calcined product was then sieved through a 325-mesh sieve to prepare the second positive electrode active material. At this point, the second positive electrode active material was in the form of secondary particles formed by the agglomeration of multiple primary particles, with an average particle size of 9 μm, and its composition was Li₂CO₃. 1.02 Mn2O4. The secondary particles of the second positive electrode active material are separated into primary particles by a wet milling process performed during the preparation of the composite positive electrode active material as described later, and the separated primary particles subsequently constitute the secondary particles of the composite positive electrode active material prepared by a spray drying process.
[0177] (Preparation of composite positive electrode active material)
[0178] The first and second positive electrode active materials were mixed at a weight ratio of 9:1 for 30 minutes at 15 rpm using a mixer (L5M-A). Water was added as a second solvent, and wet milling was performed to prepare a second slurry. This slurry was then added at 0.5 kg / min to a spray dryer (Büchi Mini Spray Dryer B-290) and spray-dried at 200°C to obtain a second dried product. Wet milling was performed using a ball mill. Specifically, a mixture of approximately 3 kg of zirconia balls, approximately 2 kg of water, and approximately 2 kg of the first and second positive electrode active materials was introduced into a milling vessel with a capacity of approximately 5 L, and the vessel was rotated at approximately 50 rpm for approximately 1 hour. The second dried product is a composite positive electrode active material in the form of secondary particles in which the primary particles of the first and second positive electrode active materials agglomerate.
[0179] (2) Manufacturing of the positive electrode
[0180] A composite positive electrode active material was prepared by mixing polyvinylidene fluoride as a binder and carbon nanotubes as a conductive material at a weight ratio of 96:2:2 (positive electrode active material: binder: conductive material). This composition was dispersed in N-methylpyrrolidone solvent to prepare a positive electrode active material slurry, which was then coated onto a 15 μm thick Al foil, dried, and compressed to fabricate the positive electrode.
[0181] (3) Manufacturing of rechargeable lithium battery cells
[0182] A negative electrode active material slurry was prepared by dispersing 97.5% by weight graphite as the negative electrode active material, 1.5% by weight carboxymethyl cellulose and 1% by weight styrene-butadiene rubber as binders in distilled water. This slurry was coated onto a 10 μm thick Cu foil, then dried and compressed to fabricate the negative electrode.
[0183] A 10 μm thick polyethylene separator is placed between the positive and negative electrodes to fabricate an electrode assembly, which is then inserted into a housing. An electrolyte is injected into the housing to fabricate a rechargeable lithium-ion battery cell (a pouch cell at the 100 mAh level). The electrolyte is prepared by mixing EC (ethylene carbonate): EMC (ethyl methyl carbonate): DMC (dimethyl carbonate) at a volume ratio of 2:4:4 and dissolving 1.15 M LiPF6 in the mixed solvent.
[0184] Examples 2 to 4
[0185] The composite positive electrode active material, positive electrode and rechargeable lithium battery cell according to Examples 2 to 4 are manufactured by a method substantially the same as that in Example 1, except that in the process of the part of Example 1, “(1) Preparation of composite positive electrode active material”, the first positive electrode active material and the second positive electrode active material are mixed at the weight ratio described in Table 1 instead of at a weight ratio of 9:1 when the second slurry is prepared.
[0186] Table 1:
[0187]
[0188] Comparative Examples 1 to 4
[0189] The positive electrode and rechargeable lithium battery cell according to Comparative Examples 1 to 4 were manufactured in substantially the same manner as in Examples 1 to 4, except that: in the process of "(2) Manufacturing of the positive electrode" in Examples 1 to 4, the first positive electrode active material obtained in the process of "(1) Preparation of composite positive electrode active material" and the prepared second positive electrode active material were simply mixed at 15 rpm for 30 minutes using a mixer (L5M-A) at the weight ratio of the first positive electrode active material and the second positive electrode active material according to Examples 1 to 4 as described in Table 1, as the positive electrode active material. In the positive electrode active material, the first positive electrode active material and the second positive electrode active material do not exist in the form of an aggregated assembly, but in a dispersed state.
[0190] Evaluation Example 1: Evaluation of Composite Positive Electrode Active Materials
[0191] (1) Porosity evaluation
[0192] The porosity of the composite positive electrode active materials of Examples 1 to 4 was measured, and the results are shown in Table 2. The porosity was obtained by taking scanning electron microscope images of the cross-section of the secondary particles to measure the ratio of the area of the pores in the cross-section of the secondary particles to the cross-sectional area of the secondary particles of each composite positive electrode active material, and the results are shown in Table 2.
[0193] (2) Particle analysis
[0194] Cross-sectional images of the composite positive electrode active material manufactured in Example 3 were taken using a scanning electron microscope, and the scanning electron microscope images of the cross-section of the composite positive electrode active material manufactured in Example 3 are shown below. Figure 5 middle.
[0195] exist Figure 5 In the diagram, within a single composite positive electrode active material particle, black represents internal pores, and gray represents the first and second positive electrode active materials. Among those marked in gray, the second positive electrode active material refers to particles with a particle size greater than or equal to about 2 μm, while the first positive electrode active material refers to the remaining particles with a particle size less than about 2 μm. Particle size is defined as diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles.
[0196] Reference Figure 5 Multiple first positive electrode active material particles and second positive electrode active material particles agglomerate to form an assembly.
[0197] Similar to Example 3, cross-sectional images of the composite positive electrode active materials manufactured in Examples 1, 2 and 4 were taken using a scanning electron microscope. Based on the images, the average particle size of the secondary particles, the average particle size of the primary particles of the first positive electrode active material, the arithmetic mean size of the first positive electrode active material, the standard deviation of the first positive electrode active material, and the average particle size of the primary particles of the second positive electrode active material were measured and are shown in Table 2.
[0198] Specifically, the average particle size of the secondary particles is obtained as follows: approximately 20 secondary particles are randomly selected from a scanning electron microscope image of the cross-section of the composite positive electrode active material, the size of each secondary particle is measured, and the arithmetic mean of the sizes of each secondary particle is calculated. The size of each secondary particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. The average particle size of the primary particles of the first and second positive electrode active materials is also obtained as follows: approximately 20 primary particles of the first and second positive electrode active materials are randomly selected from the scanning electron microscope images of each composite positive electrode active material, respectively. The size of each primary particle is measured, and the arithmetic mean of the sizes of each primary particle is calculated. The size of each primary particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. In this case, within the composite positive electrode active material, as described above, particles with a particle size of less than about 2 μm are considered primary particles of the first positive electrode active material and their particle size is measured to obtain an arithmetic mean, while particles with a particle size greater than or equal to about 2 μm are considered primary particles of the second positive electrode active material and their particle size is measured to obtain an arithmetic mean.
[0199] The arithmetic mean size and standard deviation of the first positive electrode active material were obtained by measuring the size of any 20 primary particles of the first positive electrode active material from a scanning electron microscope image of the cross-section of the composite positive electrode active material (wherein the particle size is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles), and calculating the arithmetic mean and the standard deviation of the arithmetic mean.
[0200] The number of primary particles of the second positive electrode active material in the composite positive electrode active material was determined by counting the number of particles with a size greater than or equal to about 2 μm in a scanning electron microscope image of the cross-section of the composite positive electrode active material. The particle size was defined as the diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles. Here, the number of primary particles is the average number of primary particles of the second positive electrode active material in multiple composite positive electrode active material particles.
[0201] Unlike Examples 1 to 4, in which the first positive electrode active material and the second positive electrode active material are spray-dried to produce a dried product and then fired into an assembly, Comparative Examples 1 to 4, in which the first positive electrode active material and the second positive electrode active material are simply mixed, show that the first positive electrode active material and the second positive electrode active material exist in a dispersed state, so that it is not necessary to show the evaluation of those comparative examples in Table 2.
[0202] Table 2:
[0203]
[0204] Referring to Table 2, the composite positive electrode active materials of Examples 1 to 4 confirm that the first positive electrode active material is prepared according to its preparation method into primary particles with relatively small and uniform size, and also forms an assembly with the primary particles of the second positive electrode active material.
[0205] Evaluation Example 2: Particle Density Evaluation
[0206] The agglomerate density of the (composite) positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 4 was determined as follows: 3 g of the (composite) positive electrode active material was placed in a mold, and the (composite) positive electrode active material was held in the mold at 25°C for 30 seconds. The thickness of the agglomerate was measured, and the agglomerate volume was calculated using the agglomerate thickness and the diameter of the mold. The mass of the (composite) positive electrode active material was divided by the calculated volume.
[0207] Evaluation Example 3: Evaluation of Battery Performance
[0208] (1) Evaluation of initial charge / discharge capacity and efficiency
[0209] The rechargeable lithium-ion battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were charged at 25°C at a rate of 0.2 C to a battery voltage of 4.45 V and discharged at a rate of 0.2 C to a cutoff voltage of 3.0 V to measure the initial charge / discharge capacity, which was used to calculate the initial efficiency according to Equation 1. The results are shown in Table 3. Equation 1 is as follows:
[0210] [Equation 1]
[0211] Initial efficiency [%] = [Discharge capacity in the first cycle / Charge capacity in the first cycle] × 100.
[0212] (2) Average voltage
[0213] The average voltage of the rechargeable lithium battery cells according to Examples 1 to 4 and Comparative Examples 1 to 4 at 50% SOC (State of Charge) during the initial discharge was measured, and the results are shown in Table 3.
[0214] (3) Low-temperature capacity evaluation
[0215] The rechargeable lithium-ion battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were fully charged to a battery voltage of 4.45V at a rate of 0.2C, and then discharged to 3.0V at a rate of 0.2C in an atmosphere set to -20°C to measure the low-temperature discharge capacity. The results are shown in Table 3.
[0216] (4) Cyclic life characteristic evaluation
[0217] After initial charging and discharging, the rechargeable lithium-ion battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were repeatedly charged at a 1C rate to a battery voltage of 4.45 V, and then discharged at a 1C rate to a cutoff voltage of 3.0 V 50 times. The ratio of the 50th cycle discharge capacity to the initial discharge capacity was calculated according to Equation 2 below, and the results are shown in Table 3. Equation 2 is as follows:
[0218] [Equation 2]
[0219] Cycle lifetime [%] = [Discharge capacity at the 50th cycle / Discharge capacity at the 1st cycle] × 100.
[0220] (5) Evaluation of high temperature storage characteristics
[0221] The rechargeable lithium battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were charged to SOC 98% at a rate of 0.2 C, and then left to stand at 45°C for 7 days in a high-temperature room to measure capacity retention. The results are shown in Table 3.
[0222] (6) Capacity evaluation per volume
[0223] The capacity per volume of the rechargeable lithium battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 was measured by multiplying the density by the capacity, and the results are shown in Table 3.
[0224] Table 3:
[0225]
[0226] Referring to Table 3, when the mixing weight ratio of the first positive electrode active material and the second positive electrode active material is the same, the rechargeable lithium battery cell including the positive electrode active materials (in the form of an assembly) prepared in Examples 1 to 4 is superior to the rechargeable lithium battery cell including the positive electrode active materials (each in the form of a simple mixture) prepared in Comparative Examples 1 to 4 in the following aspects: particle density, initial discharge capacity, efficiency, low-temperature discharge capacity, 1C cycle life, high-temperature storage characteristics, and capacity per volume. In the case of the rechargeable lithium battery cell including the positive electrode active materials prepared in Comparative Examples 1 to 4, the first and second positive electrode active materials are simply mixed, and isolation occurs between the particles due to insufficient electrochemical reaction between different particles. This can lead to a decrease in overall battery performance due to problems with the physical connection between different particles. In particular, the high-temperature storage characteristics of the rechargeable lithium battery can be significantly degraded. Meanwhile, in the case of the positive electrode active material prepared in Examples 1 to 4, the above-mentioned problem is solved by agglomerating the particles of the first and second positive electrode active materials to form a single secondary particle (i.e., an assembly). Therefore, compared with rechargeable lithium battery cells including the positive electrode active materials prepared in Comparative Examples 1 to 4, the high-temperature storage characteristics of rechargeable lithium battery cells having the positive electrode active material of one of the above-described examples are significantly improved.
[0227] While the invention has been described with respect to some embodiments as described above, this disclosure is not limited to the embodiments described above. Rather, this disclosure covers various modifications and equivalent arrangements of the embodiments described above.
[0228] <Description of representative figure labels>
[0229] 100: Rechargeable lithium battery; 10: Positive electrode
[0230] 11: Positive electrode lead connector 12: Positive electrode terminal
[0231] 20: Negative electrode 21: Negative electrode lead connector
[0232] 22: Negative electrode terminal; 30: Diaphragm
[0233] 40: Electrode assembly; 50: Housing
[0234] 60: Seal 70: Electrode terminal
[0235] 71: Positive electrode connector; 72: Negative electrode connector
Claims
1. A composite positive electrode active material, which is in particulate form, said composite positive electrode active material comprising: The first positive electrode active material includes lithium iron phosphate-based compounds and is in the form of primary particles; and The second positive electrode active material includes lithium manganese-based oxides in the form of primary particles. The particulate form includes a plurality of primary particles of the first positive electrode active material and a plurality of primary particles of the second positive electrode active material.
2. The composite positive electrode active material according to claim 1, wherein the lithium iron phosphate-based compound comprises a compound represented by chemical formula 1, a compound represented by chemical formula 2, or a combination thereof: [Chemical Formula 1] Li a1 Fe (1-x1) M 1 x1 PO4, Where 0.9≤a1≤1.5, 0≤x1≤0.4, and M 1 Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof; and [Chemical Formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4, Where 0.9≤a²≤1.5, 0.1≤x²≤0.9, 0≤y²<0.9, x²+y²<1, and M 2 It is Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.
3. The composite positive electrode active material according to claim 1, wherein, based on the total metals other than lithium in the lithium iron phosphate-based compound, the lithium iron phosphate-based compound comprises Al, Mg, Ti, V or combinations thereof in an amount ranging from 0.1 mol% to 0.5 mol%.
4. The composite positive electrode active material according to claim 1, wherein the average particle size of the primary particles of the first positive electrode active material is greater than or equal to 0.1 μm and less than 2 μm.
5. The composite positive electrode active material according to claim 1, wherein the arithmetic mean size of the primary particles of the first positive electrode active material is less than or equal to 200 nm, and The standard deviation of the arithmetic mean size of the primary particles of the first positive electrode active material is less than or equal to 100 nm.
6. The composite positive electrode active material according to claim 1, wherein the first positive electrode active material further comprises a carbon coating layer on the surface of the primary particles.
7. The composite positive electrode active material according to claim 1, wherein the lithium manganese-based oxide is represented by the following: Li a3 Mn x3 M 3 y3 O 4-b3 X b3 , Where 0.9 ≤ a³ ≤ 1.8, 1.7 ≤ x³ ≤ 2, 0 ≤ y³ ≤ 0.3, 1.9 ≤ x³ + y³ ≤ 2.1, and 0 ≤ b³ ≤ 0.1, M 3 X is Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
8. The composite positive electrode active material according to claim 1, wherein the lithium manganese-based oxide is represented by the following: Li a4 Mn x4 Al y4 Mg z4 M 4 w4 O 4-b4 X b4 , where 0.9≤a4≤1.8, 1.7≤x4<2.0, 0<y4≤0.015, 0<z4≤0.010, 0≤w4<0.3, 1.9≤x4+y4+z4+w4≤2.1, and 0≤b4≤0.1, M 4 is B, Ba, Ca, Ce, Cr, Fe, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
9. The composite positive electrode active material according to claim 1, wherein the average particle size of the primary particles of the second positive electrode active material is 2 μm to 10 μm.
10. The composite positive electrode active material according to claim 1, wherein the composite positive electrode active material is in the form of a plurality of secondary particles, and the average particle size of the secondary particles of the composite positive electrode active material is 3 μm to 20 μm.
11. The composite positive electrode active material according to claim 1, wherein, based on 100% by weight of the composite positive electrode active material, the composite positive electrode active material comprises the first positive electrode active material in an amount of 50% by weight to 99% by weight, and The composite positive electrode active material comprises 100% by weight of the composite positive electrode active material, wherein the composite positive electrode active material includes the second positive electrode active material in an amount of 1% to 50% by weight.
12. The composite positive electrode active material according to claim 1, wherein the number of primary particles of the second positive electrode active material in the particles of the composite positive electrode active material is 10 or less.
13. The composite positive electrode active material according to claim 1, wherein the particles of the composite positive electrode active material include pores, and The porosity of the particles of the composite positive electrode active material is 10% to 50%, and the porosity is the ratio of the area occupied by the pores to the cross-sectional area of the particles of the composite positive electrode active material.
14. Positive electrode, including: Positive electrode current collector; and A positive electrode active material layer is disposed on the positive electrode current collector and includes the composite positive electrode active material according to any one of claims 1 to 13.
15. A rechargeable lithium battery, including: The positive electrode according to claim 14; negative electrode; and Electrolytes.