A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery cathode material, its preparation method and application
By modifying sodium-ion battery cathode materials with Ca-Ti dual doping and P2-type coating, the problem of structural instability under high voltage was solved, and the stability and capacity retention of the materials under high voltage were improved, making them suitable for high-energy-density sodium-ion batteries.
Patent Information
- Application Number
- CN202610961605.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing sodium-ion battery cathode materials are structurally unstable under high voltage, exhibiting irreversible phase transitions and electrolyte side reactions, resulting in low capacity retention. Traditional modification strategies are insufficient to achieve a synergistic improvement in structural stability and interfacial compatibility, thus failing to meet the requirements for long-life applications.
By performing Ca-Ti double doping inside the O3-type cathode substrate, a P2-type coating layer matching the substrate lattice is constructed, forming a heterostructure, suppressing phase transitions and constructing fast sodium ion transport channels, thereby enhancing the crystal framework stability and interface protection of the material.
It significantly improves the structural stability and interface compatibility of the material in high-voltage systems, enhances capacity retention and cycle stability, and is suitable for high-energy-density sodium-ion batteries.
Smart Images

Figure CN123120670A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of sodium-ion battery materials technology, specifically to a Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery cathode material, its preparation method, and its application. Background Technology
[0002] With the rapid development of sodium-ion batteries towards higher voltage and higher energy density, O3-type layered oxide cathode materials (especially NaNi) are becoming increasingly important. 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 (NFM) has become the core choice for next-generation energy storage and power sodium batteries due to its advantages such as high specific capacity, moderate operating voltage, and low raw material cost. However, its large-scale application in high-voltage systems above 4.1 V still faces several insurmountable technical bottlenecks.
[0003] On the one hand, Na under high voltage + Deep extraction triggers an irreversible phase transition of O3→P3→OP2 / O1 type, accompanied by severe lattice volume distortion and internal stress accumulation, leading to microcracks in the particles and gradual structural collapse. Simultaneously, transition metals (Fe, Mn) are prone to valence disproportionation and migration into the sodium layer, inducing Jahn... Teller distortion and the release of reactive lattice oxygen exacerbate material structural instability and voltage decay. On the other hand, high voltage significantly intensifies the negative electrode's degradation. Electrolyte interface side reactions and severe electrolyte oxidation and decomposition make it difficult for conventional film-forming components to form a dense and stable CEI film. This results in continuous electrolyte consumption, dissolution of transition metals, and a continuous increase in interfacial impedance. Ultimately, when the battery is cycled at a high voltage of 4.1V, the capacity retention rate is generally less than 60%, which is far from meeting the requirements for long-life applications.
[0004] Meanwhile, traditional modification strategies have significant limitations. While bulk doping (such as Mg, Zn, and Al) can stabilize the crystal structure to some extent, its effect on suppressing interfacial side reactions is limited. Single oxide coatings (Al₂O₃, TiO₂, etc.) can physically block the electrolyte, but they suffer from poor ionic conductivity, low lattice matching with the O₃ matrix, and high interfacial stress leading to easy detachment, which in turn increases the Na₂O content. + Transmission resistance and degraded rate performance. More importantly, most existing technologies only focus on one dimension: bulk stability or interface protection, making it difficult to achieve a synergistic improvement in structural stability and interface compatibility, and thus failing to fundamentally solve the "phase transition" problem under high voltage. crack Side reactions A vicious cycle of "capacity decay".
[0005] For example, Chinese patent application CN121601629A discloses a P2 / P3 mixed-phase sodium-ion battery layered oxide cathode material and its preparation method, which uses wet ball milling and high-temperature solid-state calcination to prepare a material with the chemical formula Na. x Li y Ni a Mn b M c O2 mixed-phase materials. This approach significantly improves the specific capacity, rate capability, and cycle stability in the 2.0-4.0 V voltage range through P2 / P3 mixed-phase and multi-element doping, and the process is simple and easy to mass-produce; however, due to the inherent characteristics of the high-temperature solid-state method, there are problems such as limited mixing uniformity, difficulty in controlling particle size and batch consistency, and high energy consumption, which are not conducive to the stringent requirements of material consistency for high-end power batteries.
[0006] Patent application CN121506897 A discloses an O3 core / P2 shell composite sodium-ion battery layered oxide cathode material and its preparation method. The method involves first preparing an O3 core precursor and a P2 shell precursor using a co-precipitation method, then obtaining the core and shell materials through high-temperature calcination, followed by grinding, mixing, and a second high-temperature solid-state calcination to form a core-shell composite material. While the cathode material prepared by this patent application exhibits high specific capacity, excellent air stability, and outstanding long-cycle performance, effectively combining the high capacity of the O3 phase with the high stability of the P2 phase, and further suppressing phase transitions and improving cycle life through elemental doping, this method suffers from a long and complex process flow. It requires two high-temperature calcinations and two co-precipitation reactions, resulting in high energy consumption and a long production cycle. Furthermore, the co-precipitation and core-shell composite process require strict control of numerous parameters such as pH, temperature, stirring, particle size, and mass ratio, making process control difficult and increasing the pressure to maintain batch consistency, which is not conducive to large-scale, low-cost mass production.
[0007] In summary, bulk structural instability and insufficient interface protection jointly limit the high-voltage O3 The practical application of NFM cathode materials urgently requires the development of a synergistic modification technology that can simultaneously achieve bulk dual-doping for strong stabilization and interface lattice-matched coating. This technology would suppress phase transitions from within and isolate side reactions from without, while maintaining both high ionic conductivity and structural integrity, thereby overcoming the key technological bottlenecks in high-voltage sodium-ion battery cathodes. Summary of the Invention
[0008] This invention aims to solve the problems in the prior art and provides a sodium-ion battery cathode material synergistically modified by Ca-Ti dual doping and P2 coating, its preparation method and application.
[0009] To achieve the above objectives, the first aspect of this application provides a Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery cathode material, wherein the cathode material comprises a Ca-Ti dual-doped O3-type cathode matrix and a P2-type Na-type cathode coated on the surface of the matrix. 2 / 3 Ni1 / 3Mn2 / 3O2 coating layer.
[0010] The inventive concept of this invention is: to perform Ca reaction inside the O3-type positive electrode substrate. Ti double doping stabilizes the crystal framework and suppresses irreversible phase transitions. At the same time, it constructs a P2-type coating layer on the substrate surface that matches the substrate lattice and has excellent ionic conductivity, achieving synergistic enhancement of bulk structure and interface protection. On the one hand, it suppresses structural distortion of cathode materials, dissolution of transition metals, and side reactions of electrolytes under high voltage. On the other hand, it constructs a fast sodium ion transport channel, significantly improving interface stability and structural tolerance, thereby breaking through the bottleneck of rapid capacity decay under high voltage.
[0011] Preferably, in the above-mentioned modified sodium-ion battery cathode material, the chemical formula of the Ca-Ti dual-doped O3-type cathode matrix is Na. 1-a Ca a (Ni1 / 3Fe1 / 3Mn1 / 3-b Ti b O2, where 0.01≤a≤0.05, 0.005≤b≤0.02.
[0012] In the aforementioned modified sodium-ion battery cathode material, preferably, Ca element occupies the Na group. + Lattice sites act as structural pillars, widening interlayer spacing and suppressing phase transitions; Ti elements occupy transition metal sites, strengthening the TM (transition metal matrix). O bonds suppress oxygen defects and lattice distortion.
[0013] In the aforementioned modified sodium-ion battery cathode material, preferably, the mass of the P2-type coating layer is 1.0% to 5.0% of the mass of the Ca-Ti dual-doped O3-type cathode matrix. Within this range, the coating layer can form a uniform and dense physical barrier, suppressing side reactions and structural collapse under high voltage, without significantly increasing interfacial impedance. This allows for the synergistic optimization of the cathode material's cycle stability and sodium-ion transport kinetics.
[0014] In the aforementioned modified sodium-ion battery cathode material, preferably, the average thickness of the P2-type coating layer is 10–50 nm. This thickness range can act as a dense barrier to suppress side reactions, oxygen release, and structural degradation under high voltage, while not significantly hindering the rapid transport of sodium ions and electrons, thus ensuring the high-rate performance and long-cycle stability of the cathode material.
[0015] The average particle size of the Ca-Ti dual-doped O3-type cathode substrate is 2–5 μm. This particle size range can reduce the occurrence of electrolyte side reactions without excessively prolonging the sodium ion diffusion path. At the same time, the internal stress distribution of the particles is uniform, and the resistance to volume deformation is stronger. It can maintain good structural integrity under high voltage conditions, and balance energy density, cycle life and rate performance.
[0016] Preferably, the modified sodium-ion battery cathode material has a specific surface area of 0.5~2.0 m² / g.
[0017] A second aspect of this application provides a method for preparing the modified sodium-ion battery cathode material described above, comprising the following steps:
[0018] (1) Prepare Ni by mixing soluble nickel salt, soluble iron salt, and soluble manganese salt into a mixed solution and then using a co-precipitation method. 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 precursor; (2) The precursor is mixed with sodium source, calcium source and titanium source, and calcined in two stages under an oxidizing atmosphere to obtain Ca-Ti double-doped O3 type cathode matrix; (3) Dissolve the P2 type coating precursor in a solvent, add the Ca-Ti double-doped O3 type cathode matrix obtained in step (2), stir to adsorb, evaporate to dryness, and then calcine again under an oxidizing atmosphere to obtain the Ca-Ti double-doped and P2-coated synergistic modified sodium-ion battery cathode material.
[0019] In the above preparation method, preferably, in step (1), the coprecipitation reaction is controlled at pH 9.5-11, ammonia concentration 3-5 mol / L, and reaction temperature 50-65℃.
[0020] In the above preparation method, preferably, in step (2), the calcium source is one or more of CaCO3 and Ca(CH3COO)2; the titanium source is one of nano-TiO2 and tetrabutyl titanate; the sodium source is sodium carbonate, and the sodium source is in excess by 3-8 mol%; The two-stage calcination process is as follows: first, the temperature is increased to 400-550℃ at a rate of 5-10℃ / min and held for 3-5 hours; then, the temperature is increased to 850-920℃ at a rate of 2-10℃ / min and held for 10-15 hours; the oxidizing atmosphere is air or oxygen.
[0021] In the above preparation method, preferably, in step (3), the P2 type coating layer precursor is sodium acetate, nickel acetate and manganese acetate; the solvent is one or both of ethanol and deionized water; the stirring temperature is 25-80℃, the stirring speed is 400-1000 r / min, and the time is 1-4 h; The secondary calcination process is as follows: the temperature is increased to 600-750℃ at a rate of 2-6℃ / min, and held for 4-8 hours; the oxidizing atmosphere is air or oxygen.
[0022] The third aspect of this application provides the application of the modified sodium-ion battery cathode material according to the above-described method or the modified sodium-ion battery cathode material prepared by the above-described method in a sodium-ion battery.
[0023] In the above applications, preferably, the modified sodium-ion battery cathode material is adapted to a high-voltage system, and the operating voltage range of the high-voltage system is 2.0 to 4.1 V.
[0024] In the above-mentioned applications, preferably, the sodium-ion battery can cycle stably in the high voltage range of 2.0~4.1V, and retains ≥77% capacity after 200 cycles at 1C rate.
[0025] In the above-mentioned applications, preferably, the modified sodium-ion battery cathode material is used to synergistically form a stable and dense CEI film under high voltage systems, thereby improving the structural stability and interface compatibility of the material.
[0026] Compared with the prior art, this application has the following beneficial effects: (1) This invention constructs a P2-type Na that matches the matrix lattice. 2 / 3 The Ni1 / 3Mn2 / 3O2 coating layer achieves uniform coating on the surface of the Ca-Ti dual-doped O3-type cathode substrate. The interfacial bonding between the coating layer and the substrate is strong, effectively avoiding the problems of easy detachment and high interfacial impedance associated with traditional coating materials. The P2-type coating layer itself possesses excellent ionic conductivity and good lattice matching with the substrate, not only acting as a physical barrier to suppress transition metal dissolution and electrolyte side reactions under high voltage, but also constructing a fast sodium ion transport channel, significantly improving the interfacial stability and compatibility of the material in high-voltage systems. Simultaneously, by performing Ca-Ti dual doping within the O3-type substrate, where Ca occupies Na... + Lattice sites act as structural pillars, increasing interlayer spacing and suppressing irreversible phase transitions; Ti occupies transition metal sites, strengthening TM-O bonds and suppressing oxygen defects and lattice distortion; the synergistic effect of the two significantly enhances the crystal framework stability and structural tolerance of the material under high voltage.
[0027] (2) The modified cathode material of this invention achieves dual synergy through Ca-Ti bulk doping + P2 type lattice matching coating. The coating is uniform, the interface bonding is strong, and the structural tolerance is high. The CEI film can be stabilized by the material's own interface optimization, which significantly improves the structural stability and interface compatibility of the material in the 4.1 V high voltage system. The assembled sodium-ion battery can achieve a reversible specific capacity of 134.6 mAh / g and an initial coulombic efficiency of 88.9% at a high charging voltage of 4.1V and a rate of 0.1C. The capacity decay is slow at high rates. After 200 cycles at a rate of 1C, the capacity retention rate can reach 85.7%, which is far better than the unmodified and single-modified samples.
[0028] (3) The method of the present invention adopts a combination process of co-precipitation-solid phase sintering-wet coating. The doping and coating are controllable in steps, and the crystallinity and coating thickness are adjustable. The process is stable, low in cost, and does not require special equipment. It is easy to scale up to achieve industrial production, providing an efficient and feasible technical route for the large-scale development of layered oxide cathodes for high-voltage and long-life sodium-ion batteries.
[0029] (4) The cathode material of the present invention can synergistically form a stable and dense CEI film, which significantly improves the structural stability and interface compatibility of the material in the high voltage system. It is particularly suitable for high voltage sodium-ion battery systems with high energy density requirements and has broad market application prospects. Attached Figure Description
[0030] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0031] Figure 1 The cathode material of Comparative Example 1 and Ca in Example 1 of this invention are X-ray diffraction (XRD) pattern of Ti-doped and P2-coated synergistic modification of layered cathode material for sodium-ion batteries; Figure 2 Ca in Embodiment 1 of the present invention Scanning electron microscope (SEM) image of Ti-doped and P2-coated synergistic modification of layered cathode material for sodium-ion batteries; Figure 3 Ca in Embodiment 1 of the present invention Transmission electron microscope (TEM) image of Ti-doped and P2-coated synergistic modification of layered cathode material for sodium-ion batteries; Figure 4This is a charge-discharge cycle performance curve of the positive electrode materials prepared in Example 1 and Comparative Example 1 of this invention after being assembled into batteries. Detailed Implementation
[0032] To facilitate understanding of this application, the following description will be more comprehensive and detailed in conjunction with the accompanying drawings and preferred embodiments, but the scope of protection of this application is not limited to the following specific embodiments.
[0033] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this application.
[0034] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0035] Example 1: A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery cathode material of the present invention comprises an O3-type layered oxide matrix Na. 0.98 Ca 0.02 (Ni 1 / 3 Fe 1 / 3 Mn 0.32 Ti 0.02 O2, the matrix surface is uniformly coated with P2 type Na 2 / 3 Ni 1 / 3 Mn 2 / The 3O2 coating layer comprises 3 wt% of the Ca-Ti dual-doped O3-type cathode matrix, with a thickness of approximately 25 nm. Ca occupies Na sites, and Ti occupies transition metal sites. The P2-type coating layer forms a lattice-matched heterostructure with a strong interfacial bond and no significant phase separation. The matrix particle size is mainly distributed between 3–5 μm. The specific surface area of this modified sodium-ion battery cathode material is 1.2 m². 2 / g.
[0036] The preparation method of the Ca-Ti dual-doped and P2-coated synergistic modified cathode material in this embodiment includes the following steps: (1) Ni1 / 3Fe1 / 3Mn1 / 3(OH)2 spherical precursor was prepared by co-precipitation method: nickel sulfate, ferric sulfate and manganese sulfate were mixed in a molar ratio of Ni:Fe:Mn=1:1:1 to prepare a 1.5 mol / L mixed salt solution. A complexing agent solution with an ammonia concentration of 4.0 mol / L and a sodium hydroxide solution with a concentration of 4.0 mol / L were also prepared as precipitants.
[0037] A co-precipitation reactor was used. Deionized water was added to the bottom as the base liquid, and the reactor was heated to 60°C and purged with nitrogen to remove oxygen. Under stirring conditions (stirring speed of 600 r / min), the mixed salt solution, complexing agent solution, and precipitant solution were continuously added to the reactor in a parallel flow using peristaltic pumps. The feed rate of the mixed salt solution was 2.0 mL / min, the feed rate of the complexing agent solution (ammonia) was 0.5 mL / min, and the feed rate of the precipitant solution (sodium hydroxide) was automatically adjusted based on real-time pH feedback (initially set at 1.5 mL / min). The total feeding time was controlled to be completed within 4 hours. During the reaction, the reaction temperature was kept constant at 60°C. The pH of the reaction system was stabilized at 10.2 ± 0.1, and the ammonia concentration was maintained at 4.0 ± 0.2 mol / L, by adjusting the feed rates of the sodium hydroxide solution and ammonia. After the feeding was completed, the reaction was continued with stirring for 40 hours (total reaction time 50 hours). After the reaction was completed, the resulting slurry was centrifuged, washed with deionized water, and dried to obtain spherical Ni1 / 3Fe1 / 3Mn1 / 3(OH)2 precursor. The tap density of this precursor was measured to be 1.5 g / cm³ (using a tap density meter with 3000 vibrations), and the median particle size D50 was measured to be 6 μm using a laser particle size analyzer, indicating a uniform particle size distribution (Span < 1.0). (2) The precursor obtained in step (1) was mixed with Na2CO3, CaCO3 and nano TiO2 at a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.05:0.02:1 (5 mol% excess sodium), wherein the molar percentage of Ti was 2% (i.e., the molar ratio of Ti replacing Mn was 2 mol%). After ball milling the mixture for 6 h, it was placed in a muffle furnace and pre-calcined at 500℃ for 4 h at an oxygen atmosphere, and then sintered at 880℃ for 12 h at a high temperature of 3℃ / min. After natural cooling, it was ground to obtain the Ca-Ti double-doped O3 type matrix material Na. 0.98 Ca 0.02 (Ni 1 / 3 Fe 1 / 3 Mn 0.32 Ti 0.02 O2; XRD analysis confirmed that it is a pure phase O3 structure.
[0038] (3) In-situ wet coating: Sodium acetate, nickel acetate, and manganese acetate were dissolved in anhydrous ethanol at a molar ratio of Na:Ni:Mn = 2 / 3:1 / 3:2 / 3, and ultrasonically dispersed to form a uniform solution. The solution was added to the Ca-Ti double-doped O3 matrix material obtained in step (2) at a ratio of 3 wt% of the mass of the P2 coating layer to the mass of the O3 matrix. The mixture was stirred at 600 r / min for 2 h, and then the solvent was evaporated at 80 °C. The dried material was then sintered for 6 h at 650 °C at 5 °C / min in air atmosphere to generate the P2 type Na2 / 3Ni1 / 3Mn2 / 3O2 coating layer in situ on the surface of the O3 matrix. After cooling, the material was sieved to obtain the final product, Ca-Ti double-doped / P2 coated synergistic modified cathode material, denoted as Na 0.98 Ca 0.02 (Ni 1 / 3 Fe 1 / 3 Mn 0.32 Ti 0.02 O2@P2-Na 2 / 3 Ni 1 / 3Mn 2 / 3 O2, Scanning Electron Microscopy (SEM) image as shown Figure 2 As shown, the transmission electron microscope (TEM) image is as follows. Figure 3 As shown.
[0039] Example 2: A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery layered cathode material of the present invention comprises an O3-type layered oxide matrix Na. 0.99 Ca 0.01 (Ni 1 / 3 Fe 1 / 3 Mn 0.329 Ti 0.005 O2, the matrix surface is uniformly coated with P2 type Na 2 / 3Ni 1 / 3 Mn 2 / 3 O2 coating layer; the coating layer accounts for 1 wt% of the mass of the Ca-Ti double-doped O3-type cathode substrate, with a thickness of approximately 25 nm; Ca elements occupy Na sites, and Ti elements occupy transition metal sites; the P2-type coating layer and the O3-type substrate form a lattice-matched heterostructure; the substrate particle size is mainly distributed in the range of 2–4 μm, and the specific surface area is 1.8 m². 2 / g.
[0040] The preparation method of the Ca-Ti dual-doped and P2-coated synergistic modified cathode material in this embodiment includes the following steps: (1) Ni1 / 3Fe1 / 3Mn1 / 3(OH)2 spherical precursor was prepared by co-precipitation method: nickel sulfate, ferric sulfate and manganese sulfate were mixed in a molar ratio of Ni:Fe:Mn=1:1:1 to prepare a 1.5 mol / L mixed salt solution. A complexing agent solution with an ammonia concentration of 3.5 mol / L and a sodium hydroxide solution with a concentration of 4 mol / L were also prepared as precipitants.
[0041] A co-precipitation reactor was used. Deionized water was added to the bottom as the base liquid, and the reactor was heated to 55°C. Nitrogen gas was then introduced to remove oxygen. Under stirring conditions (stirring speed of 600 r / min), the mixed salt solution, complexing agent solution, and precipitant solution were continuously added to the reactor in a parallel flow using peristaltic pumps. The feed rate of the mixed salt solution was 2.0 mL / min, the feed rate of the complexing agent solution (ammonia) was 0.5 mL / min, and the feed rate of the precipitant solution (sodium hydroxide) was automatically adjusted based on real-time pH feedback (initially set at 1.5 mL / min). The total feeding time was controlled to be completed within 4 hours. During the reaction, the reaction temperature was kept constant at 55°C. The pH of the reaction system was stabilized at 10.8 ± 0.1, and the ammonia concentration was maintained at 3.5 ± 0.2 mol / L, by adjusting the feed rates of the sodium hydroxide solution and ammonia. After the feeding was completed, the reaction was continued with stirring for 8 hours (total reaction time 12 hours). After the reaction was completed, the resulting slurry was centrifuged, washed with deionized water, and dried to obtain a spherical Ni1 / 3Fe1 / 3Mn1 / 3(OH)2 precursor. The tap density of the precursor was tested to be 1.5 g / cm³ (measured using a tap density meter with 3000 vibrations).
[0042] (2) The precursor obtained in step (1) was mixed with Na2CO3, Ca(CH3COO)2 and tetrabutyl titanate in a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.03:0.01:1 (sodium excess 3 mol%), wherein the molar percentage of Ti was 0.5% (i.e., the molar ratio of Ti replacing Mn was 0.5 mol%). After ball milling the mixture for 5 h, it was pre-calcined at 450 °C for 5 h at a rate of 5 °C / min under an oxygen atmosphere, and then sintered at 860 °C for 14 h at a rate of 3 °C / min to obtain the Ca-Ti double-doped O3 type matrix material Na 0.99 Ca 0.01 (Ni 1 / 3 Fe 1 / 3 Mn 0.329 Ti 0.005 O2; (3) Wet coating: The P2 type precursor (sodium acetate, nickel acetate, and manganese acetate in the ratio of Na:Ni:Mn = 2 / 3:1 / 3:2 / 3) is dispersed in deionized water and mixed with the matrix at a ratio of 1 wt% of coating layer mass fraction. The mixture is stirred for 3 h and dried at 70℃ for 8 h. Then, it is sintered at 600℃ for 8 h in air atmosphere to obtain the final product Ca-Ti double doped / P2 coated synergistic modified cathode material.
[0043] Example 3: A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery layered cathode material of the present invention comprises an O3-type layered oxide matrix Na. 0.97 Ca 0.03 (Ni 1 / 3 Fe 1 / 3 Mn 0.31 Ti 0.01 O2, the matrix surface is uniformly coated with P2 type Na 2 / 3 Ni 1 / 3Mn 2 / 3 An O2 coating layer; the coating layer accounts for 5 wt% of the matrix and has a thickness of approximately 45 nm; Ca elements occupy Na sites, and Ti elements occupy transition metal sites; the P2-type coating layer and the O3-type matrix form a lattice-matched heterostructure; the particle size of the cathode material matrix is approximately 4–5 μm, and the specific surface area is 0.8 m². 2 / g.
[0044] The preparation method of the Ca-Ti dual-doped and P2-coated synergistic modified cathode material in this embodiment includes the following steps: (1) Ni was prepared by co-precipitation method 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor: Prepare a 1.5 mol / L mixed salt solution by mixing nickel sulfate, ferric sulfate, and manganese sulfate in a molar ratio of Ni:Fe:Mn=1:1:1. Also prepare a complexing agent solution with a concentration of 4.5 mol / L ammonia water and a 4 mol / L sodium hydroxide solution as a precipitant.
[0045] A co-precipitation reactor was used. Deionized water was added to the bottom of the reactor as the base solution, and the mixture was heated to 62°C. Nitrogen gas was then introduced to remove oxygen. Under stirring conditions, a mixed salt solution, a complexing agent solution, and a precipitant solution were added to the reactor in a parallel stream. The reaction temperature was controlled at 62°C. The pH of the reaction system was stabilized at 10.5 and the ammonia concentration was maintained at 4.5 mol / L by adjusting the dropping rates of sodium hydroxide solution and ammonia water. The reaction was continuously stirred for 40 hours. After the reaction, the resulting slurry was centrifuged, washed, and dried to obtain spherical Ni. 1 / 3 Fe 1 / 3 Mn 1 / 3(OH)2 precursor.
[0046] (2) The precursor was mixed with Na2CO3, CaCO3 and nano TiO2 at a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.08:0.03:1 (8 mol% excess sodium), wherein the molar percentage of Ti was 1% (i.e., the molar ratio of Ti replacing Mn was 1%). After ball milling for 8 h, the mixture was pre-calcined at 520℃ for 3.5 h under an oxygen atmosphere by raising the temperature at 5℃ / min, and then sintered at 900℃ for 13 h by raising the temperature at 2℃ / min to obtain the double-doped matrix Na. 0.97 Ca 0.03 (Ni 1 / 3 Fe 1 / 3 Mn 0.31 Ti 0.01 )O2.
[0047] (3) Wet coating: Sodium acetate, nickel acetate, and manganese acetate were dissolved in deionized water at a molar ratio of Na:Ni:Mn = 2 / 3:1 / 3:2 / 3, and ultrasonically dispersed for 15 min to form a uniform coating precursor solution (total metal ion concentration of 0.2 mol / L). The Ca-Ti double-doped O3 matrix material obtained in step (2) was added to the above solution at a ratio of 5 wt% of the P2 coating layer mass to the O3 matrix mass. The mixture was stirred at 600 r / min for 2 h at room temperature to ensure that the coating precursor solution fully wetted the surface of the matrix particles. The solvent was then evaporated at 85 °C, and the dried material was ground through a 200-mesh sieve. The resulting powder was placed in a muffle furnace and heated to 700 °C at a heating rate of 5 °C / min under an oxygen atmosphere. The mixture was then held at this temperature for 5 h to sinter, so that the P2 type Na2 / 3Ni1 / 3Mn2 / 3O2 coating layer was generated in situ on the surface of the O3 matrix. After natural cooling, the material is ground through a 200-mesh sieve to obtain the final product, Ca-Ti dual-doped / P2-coated synergistic modified cathode material.
[0048] Example 4: A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery layered cathode material of the present invention comprises an O3-type layered oxide matrix Na. 0.96 Ca 0.04 (Ni 1 / 3 Fe 1 / 3 Mn 0.315 Ti 0.015 O2, the matrix surface is uniformly coated with P2 type Na 2 / 3Ni 1 / 3 Mn 2 / 3An O2 coating layer; the coating layer accounts for 2 wt% of the matrix and has a thickness of approximately 20 nm; Ca elements occupy Na sites, and Ti elements occupy transition metal sites; the P2-type coating layer and the O3-type matrix form a lattice-matched heterostructure; the particle size of the cathode material matrix is 3–4 μm, and the specific surface area is 1.5 m². 2 / g.
[0049] The preparation method of the Ca-Ti dual-doped and P2-coated synergistic modified cathode material in this embodiment includes the following steps: (1) Ni was prepared by co-precipitation method 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor: Prepare a 1.5 mol / L mixed salt solution by mixing nickel sulfate, ferric sulfate, and manganese sulfate in a molar ratio of Ni:Fe:Mn=1:1:1. Also prepare a complexing agent solution with a concentration of 5.0 mol / L ammonia water and a 4 mol / L sodium hydroxide solution as a precipitant.
[0050] A co-precipitation reactor was used. Deionized water was added to the bottom of the reactor as the base solution, and the mixture was heated to 65°C. Nitrogen gas was then introduced to remove oxygen. Under stirring conditions, a mixed salt solution, a complexing agent solution, and a precipitant solution were added to the reactor in a parallel stream. The reaction temperature was controlled at 65°C. The pH of the reaction system was stabilized at 11 by adjusting the dropping rates of sodium hydroxide solution and ammonia water, and the ammonia concentration was maintained at 5.0 mol / L. The reaction was continuously stirred for 40 hours. After the reaction, the resulting slurry was centrifuged, washed, and dried to obtain spherical Ni. 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 precursor.
[0051] (2) The precursor was mixed with Na2CO3, Ca(CH3COO)2 and tetrabutyl titanate in a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.06:0.04:1 (sodium excess 6 mol%), wherein the molar percentage of Ti was 1.5% (i.e., the molar ratio of Ti replacing Mn was 1.5%). After ball milling for 7 h, the mixture was pre-calcined at 550 °C for 3 h under an oxygen atmosphere by raising the temperature at 5 °C / min, and then sintered at 920 °C for 10 h by raising the temperature at 3 °C / min to obtain the double-doped matrix Na. 0.96 Ca 0.04 (Ni 1 / 3 Fe 1 / 3 Mn 0.315 Ti 0.015 O2; (3) Wet coating: Sodium acetate, nickel acetate and manganese acetate are dispersed in a mixed solvent of ethanol and deionized water (volume ratio 1:1) at a molar ratio of Na:Ni:Mn = 2 / 3:1 / 3:2 / 3. The mixture is mixed with the substrate at a mass fraction of 2 wt% of the coating layer, stirred for 2.5 h, and dried at 75 °C for 7 h. Then, it is sintered again at 680 °C for 7 h in air atmosphere to obtain the final product, Ca-Ti double doped and P2 coated synergistic modified cathode material.
[0052] Example 5: A Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery layered cathode material of the present invention comprises an O3-type layered oxide matrix Na. 0.995 Ca 0.005 (Ni 1 / 3 Fe 1 / 3 Mn 0.327 Ti 0.008 O2, the matrix surface is uniformly coated with P2 type Na 2 / 3Ni 1 / 3 Mn 2 / 3 An O2 coating layer; the coating layer accounts for 4 wt% of the matrix and has a thickness of approximately 35 nm; Ca occupies Na sites, and Ti occupies transition metal sites; the P2-type coating layer and the O3-type matrix form a lattice-matched heterostructure; the particle size of the cathode material matrix is 2–5 μm, and the specific surface area is 0.5 m². 2 / g.
[0053] The preparation method of the Ca-Ti dual-doped and P2-coated synergistic modified cathode material in this embodiment includes the following steps: (1) Ni was prepared by co-precipitation method 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor: Prepare a 1.5 mol / L mixed salt solution by mixing nickel sulfate, ferric sulfate, and manganese sulfate in a molar ratio of Ni:Fe:Mn=1:1:1. Also prepare a complexing agent solution with a concentration of 3.0 mol / L ammonia water and a 4 mol / L sodium hydroxide solution as a precipitant.
[0054] A co-precipitation reactor was used. Deionized water was added to the bottom of the reactor as the base solution, and the mixture was heated to 50°C. Nitrogen gas was then introduced to remove oxygen. Under stirring conditions, a mixed salt solution, a complexing agent solution, and a precipitant solution were added to the reactor in a parallel stream. The reaction temperature was controlled at 50°C. The pH of the reaction system was stabilized at 9.8 by adjusting the dropping rates of sodium hydroxide solution and ammonia water, and the ammonia concentration was maintained at 3.0 mol / L. The reaction was continuously stirred for 40 hours. After the reaction was completed, the resulting slurry was centrifuged, washed, and dried to obtain spherical Ni. 1 / 3 Fe 1 / 3 Mn1 / 3 (OH)2 precursor.
[0055] (2) The precursor obtained in step (1) was mixed with Na2CO3, CaCO3 and nano TiO2 in a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.04:0.005:1 (sodium excess 4 mol%), wherein the molar percentage of Ti was 0.8% (i.e. the molar ratio of Ti replacing Mn was 0.8%). After ball milling for 6 h, the mixture was pre-calcined at 400℃ for 5 h at a temperature of 5℃ / min under an oxygen atmosphere, and then sintered at 850℃ for 15 h at a temperature of 3℃ / min to obtain a double-doped matrix. (3) Wet coating: Sodium acetate, nickel acetate, and manganese acetate were dissolved in anhydrous ethanol at a molar ratio of Na:Ni:Mn = 2 / 3:1 / 3:2 / 3 and ultrasonically dispersed for 15 min to form a uniform coating precursor solution (total metal ion concentration of 0.2 mol / L). The Ca-Ti double-doped O3 matrix material obtained in step (2) was added to the above solution at a ratio of 4 wt% of the P2 coating layer mass to the O3 matrix mass. The mixture was stirred at 600 r / min for 3 h at room temperature to ensure that the coating precursor solution fully wetted the surface of the matrix particles. The solvent was then evaporated at 80 °C, and the dried material was ground through a 200-mesh sieve. The resulting powder was placed in a muffle furnace and heated to 750 °C at a heating rate of 5 °C / min under an oxygen atmosphere. The mixture was then held at this temperature for 4 h to allow the P2 type Na2 / 3Ni1 / 3Mn2 / 3O2 coating layer to be generated in situ on the surface of the O3 matrix. After natural cooling, the material is ground through a 200-mesh sieve to obtain the final product, Ca-Ti dual-doped / P2-coated synergistic modified cathode material.
[0056] Comparative Example 1: This comparative example uses pure phase Na (Ni) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, the preparation method of which includes the following steps: (1) Ni was prepared using the same co-precipitation method as in Example 1. 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor; (2) The precursor obtained in step (1) was mixed with Na2CO3 at a ratio of Na:(Ni+Fe+Mn)=1.05:1 and ball-milled for 6 h; then, under an oxygen atmosphere, it was pre-calcined at 500℃ for 4 h at a heating rate of 5℃ / min, and then sintered at 880℃ for 12 h at a heating rate of 5℃ / min. After cooling and grinding, pure phase Na(Ni) was obtained. 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0057] The XRD patterns of pure Na(Ni1 / 3Fe1 / 3Mn1 / 3)O2 in this comparative example and the Ca-Ti dual-doped and P2-coated synergistic modified sodium-ion battery cathode material prepared in Example 1 are shown below. Figure 1 As shown. By Figure 1 As can be seen, both samples exhibit typical diffraction peaks (space group R) of O3-type layered oxide structure. The absence of impurity phase formation (m) indicates that the Ca-Ti dual doping and P2 coating did not disrupt the O3-type main phase structure. Compared with the pure phase material of Comparative Example 1, the (003) and (104) characteristic diffraction peaks of the modified material in Example 1 shifted to lower angles, which is attributed to Ca²⁺. + Occupying Na sites expands the interlayer spacing, Ti 4+ Occupying transition metal sites enhances the bond energy of the TM-O bond. Simultaneously, the (003) / (104) peak intensity ratio increases significantly after modification, indicating a reduction in cation mixing, which is beneficial for Na… + Rapid transport. In addition, no obvious P2 phase diffraction peaks were observed in the modified sample, which may be due to the low content (3 wt%) and thin thickness (about 25 nm) of the P2 coating layer, which is below the detection limit of the XRD instrument. This also indirectly proves that the P2 coating layer is uniformly dispersed on the surface of the O3 matrix, rather than forming an independent aggregate phase.
[0058] Comparative Example 2: This comparative example is Ca. The preparation method of Ti dual-doped cathode material includes the following steps: (1) Ni was prepared using the same co-precipitation method as in Example 1. 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor; (2) The precursor obtained in step (1) was mixed with Na2CO3, CaCO3 and nano TiO2 at a stoichiometric ratio of Na:Ca:(Ni+Fe+Mn+Ti)=1.05:0.02:1 (5 mol% excess sodium), wherein the molar percentage of Ti was 2 mol% (i.e., Ti accounted for 2 mol% of the total molar number of Ni+Fe+Mn). After ball milling the mixture for 6 h, it was placed in a muffle furnace and pre-calcined at 500℃ for 4 h under an oxygen atmosphere, and then sintered at 880℃ for 12 h at 5℃ / min. After natural cooling and grinding, the Ca-Ti dual-doped cathode material was obtained.
[0059] Comparative Example 3: The comparative example is a P2-coated cathode material, and its preparation method includes the following steps: (1) Ni was prepared using the same co-precipitation method as in Example 1.1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 spherical precursor; (2) Sintering with Na2CO3 to obtain an undoped pure phase O3 type matrix; (3) Using the same wet coating process as in Example 1, 3 wt% of P2 type layered oxide was coated on the surface of the pure phase substrate and sintered at 650°C for 6 h to obtain a cathode material coated only with P2.
[0060] Electrochemical performance was tested using CR2032 coin cells. The positive electrode was prepared by mixing the active material, polyvinylidene fluoride (PVDF) binder, and N-methylpyrrolidone (NMP) solvent at a mass ratio of 8:1:1. Specifically, 1.6 g of active material was mixed with 3.33 g of PVDF solution (8 wt%, dissolved in NMP), and an additional 3.15 g of NMP was added to adjust the slurry viscosity. The mixture was then ball-milled in a planetary ball mill with five ZrO2 balls to obtain a uniformly dispersed positive electrode slurry.
[0061] The uniform slurry was coated onto the aluminum foil current collector and dried in a vacuum drying oven at 80℃ for 24 h. The CR2032 coin cell was assembled using metallic sodium as the counter electrode and a mixed solution of 1 mol / L NaClO4 dissolved in EC / DMC / EMC (volume ratio 1:1:1) as the electrolyte.
[0062] The constant current charge-discharge test was conducted in the voltage range of 2.0–4.1 V. The first four cycles were performed once each at a rate of 0.1 C, 0.2 C, 0.5 C and 1 C, respectively. After that, the cycle continued at a rate of 1 C until the 103rd cycle (i.e., the cycle was performed at a rate of 1 C from the 5th to the 103rd cycle).
[0063] The results of the electrochemical performance tests are shown in Table 1.
[0064] Pure phase Na (Ni) in Comparative Example 1 1 / 3 Fe 1 / 3 Mn 1 / 3 The charge-discharge cycle performance curves of the sodium-ion battery cathode materials synergistically modified by O2 and P2 coating prepared in Example 1 are shown in the figure. Figure 4 As shown.
[0065] Table 1: Comparison of electrochemical performance of batteries assembled from positive electrode sheets prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention
[0066] As shown in Table 1, the cathode material with Ca-Ti dual doping and P2 coating synergistic modification of the present invention has significantly better electrochemical performance than the unmodified sample and the single-modification comparison sample.
[0067] The cathode materials obtained in Examples 1-5 of this invention have an initial discharge capacity of 129.4-134.6 mAh / g at 0.1C and an initial coulombic efficiency of 87.6%-88.9%. After 200 cycles at a high voltage range of 2.0-4.1V and a 1C rate, the capacity retention rate is ≥77%, with a maximum of 85.7%, demonstrating excellent reversible capacity, cycle stability, and rate performance.
[0068] Comparative Example 1 is undoped, uncoated pure phase NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 cathode material exhibits extremely poor cycle stability. After 200 cycles at 1C and 2.0–4.1V, the capacity retention rate is only 53.5%, indicating that pure phase materials are prone to phase transitions and collapse under high voltage, and the interfacial side reactions are severe.
[0069] Comparative Example 2 only used Ca-Ti double doping without P2 coating. Although the bulk structure was stabilized to a certain extent and the initial discharge capacity and coulombic efficiency were improved, due to the lack of effective interface protection, electrolyte erosion and transition metal dissolution were still serious. The capacity retention rate after 200 cycles was only 68.5%, which was significantly lower than that of the synergistic modification example.
[0070] Comparative Example 3 only uses P2 coating without Ca-Ti double doping. Although it can suppress interfacial side reactions to a certain extent, it cannot solve the problems of irreversible phase transformation of O3 phase and lattice distortion under high voltage. The material bulk structure is not stable enough, and the capacity retention rate after 200 cycles is only 62.3%, with limited performance improvement.
[0071] The above results fully demonstrate that the present invention, through the synergistic effect of Ca-Ti dual doping and P2 coating, can simultaneously achieve bulk structure enhancement and interface protection, effectively suppress irreversible phase transitions, alleviate lattice distortion, reduce interfacial side reactions and lower interfacial impedance, so that the cathode material still has high specific capacity, excellent rate performance and ultra-long cycle stability under high voltage system, and its comprehensive performance is significantly better than that of single modified or unmodified materials.
[0072] The above are merely preferred embodiments of this application. It should be noted that this application is not limited to the above embodiments. For those skilled in the art, several improvements and modifications can be made without departing from the principles of this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should also be considered within the scope of protection of this application.
Claims
1. A Ca-Ti double-doped and P2-coated synergistically modified sodium-ion battery cathode material, characterized in that, The positive electrode material comprises a Ca-Ti double-doped O3-type positive electrode matrix, and a P2-type Na 2 / 3 Ni1 / 3Mn2 / 3O2 coating layer.
2. The modified sodium-ion battery cathode material of claim 1, wherein, The chemical formula of the Ca-Ti dual-doped O3-type cathode matrix is Na. 1-a Ca a (Ni1 / 3Fe1 / 3Mn1 / 3-b Ti b O2, where 0.01≤a≤0.05, 0.005≤b≤0.
02.
3. The modified sodium-ion battery cathode material of claim 1, wherein, The mass of the P2-type coating layer is 1.0 to 5.0% of the mass of the Ca-Ti double-doped O3-type cathode substrate.
4. The modified sodium-ion battery cathode material of claim 1, wherein, The average thickness of the P2-type coating layer is 10–50 nm; the average particle size of the Ca-Ti dual-doped O3-type cathode substrate is 2–5 μm.
5. The modified sodium-ion battery cathode material of claim 1, wherein, The specific surface area of the modified sodium-ion battery cathode material is 0.5~2.0 m² / g.
6. A method of producing the modified sodium-ion battery cathode material according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Prepare Ni by mixing soluble nickel salt, soluble iron salt, and soluble manganese salt into a mixed solution and then using a co-precipitation method. 1 / 3Fe 1 / 3 Mn 1 / 3 (OH)2 precursor; (2) The precursor is mixed with sodium source, calcium source and titanium source, and calcined in two stages under an oxidizing atmosphere to obtain Ca-Ti double-doped O3 type cathode matrix; (3) Dissolve the P2 type coating precursor in a solvent, add the Ca-Ti double-doped O3 type cathode matrix obtained in step (2), stir to adsorb, evaporate to dryness, and then calcine again under an oxidizing atmosphere to obtain the Ca-Ti double-doped and P2-coated synergistic modified sodium-ion battery cathode material.
7. The preparation method according to claim 6, characterized in that, In step (1), the coprecipitation reaction is controlled at pH 9.5-11, ammonia concentration 3-5 mol / L, and reaction temperature 50-65℃.
8. The preparation method according to claim 6, characterized in that, In step (2), the calcium source is one or more of CaCO3 and Ca(CH3COO)2; the titanium source is one of nano-TiO2 and tetrabutyl titanate; the sodium source is sodium carbonate, and the sodium source is in excess by 3-8 mol% The two-stage calcination process is as follows: first, the temperature is increased to 400-550℃ at a rate of 5-10℃ / min and held for 3-5 hours; then, the temperature is increased to 850-920℃ at a rate of 2-10℃ / min and held for 10-15 hours; the oxidizing atmosphere is air or oxygen.
9. The preparation method according to claim 6, characterized in that, In step (3), the P2 type coating layer precursor is sodium acetate, nickel acetate and manganese acetate; the solvent is one or both of ethanol and deionized water; the stirring temperature is 25-80℃, the stirring speed is 400-1000 r / min, and the stirring time is 1-4 h. The secondary calcination process is as follows: the temperature is increased to 600-750℃ at a rate of 2-6℃ / min, and held for 4-8 hours; the oxidizing atmosphere is air or oxygen.
10. The application of a modified sodium-ion battery cathode material according to any one of claims 1 to 5 or a modified sodium-ion battery cathode material prepared by any one of claims 6 to 9 in a sodium-ion battery.
Citation Information
Patent Citations
Composite sodium ion battery layered oxide positive electrode material and preparation method thereof
CN121506897A
Layered oxide positive electrode material of P2 / P3 mixed-phase sodium-ion battery and preparation method of layered oxide positive electrode material