A carbon-coated bismuth nanosphere / graphite sheet composite material, its preparation method and application

By using a sandwich structure of carbon-coated bismuth nanospheres/graphite sheets, the problems of low charge transfer efficiency and large volume change of sodium-ion battery anode materials under low temperature conditions were solved, achieving high capacity and stable electrochemical performance.

CN123120675APending Publication Date: 2026-11-17TIANJIN POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611241830.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sodium-ion battery anode materials have low charge transfer efficiency at low temperatures, while bismuth-based materials exhibit large volume changes during charge and discharge, leading to pulverization of the electrode structure and limiting Na+ diffusion and electron conduction.

Method used

A sandwich structure is formed by using carbon-coated bismuth nanospheres/graphite sheets. The carbon-coated bismuth nanospheres are anchored between the graphite sheets to build mechanical support and a conductive network, which avoids volume expansion and promotes sodium ion co-intercalation.

Benefits of technology

It improves the rate performance and low-temperature performance of the battery, enhances the conductivity and stability of the electrodes, and solves the structural stability problem of bismuth-based materials during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120675A_ABST
    Figure CN123120675A_ABST
Patent Text Reader

Abstract

This invention provides a carbon-coated bismuth nanosphere / graphite sheet composite material, its preparation method, and its application. The composite material comprises bismuth nanospheres, a carbon layer, and graphite sheets. The bismuth nanospheres are coated by the carbon layer and anchored between the graphite sheet layers, forming a sandwich structure. The composite material is prepared from the following raw materials in parts by weight: 100 parts graphite, 10-1000 parts bismuth source, 10-1000 parts carbon source, 200-10000 parts acid, and 1000-50000 parts solvent. When the composite material of this invention is used as a negative electrode material for sodium-ion batteries, the carbon protective layer and graphite sheets work synergistically to construct a mechanical support framework and a three-dimensional conductive network, which can effectively suppress the volume expansion of the bismuth negative electrode during charge and discharge, and significantly improve the conductivity and cycle stability of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrode materials, and in particular relates to a carbon-coated bismuth nanosphere / graphite sheet composite material, its preparation method and application. Background Technology

[0002] With the global energy transition and the continued expansion of the energy storage market, sodium-ion batteries (SIBs), as an emerging electrochemical energy storage technology, have gradually gained widespread attention due to their advantages such as abundant sodium resources in the Earth's crust, low raw material preparation costs, and environmentally friendly production and use. Among the components of a sodium-ion battery, the performance of the anode material plays a crucial role in the overall battery performance. An ideal sodium-ion battery anode material needs to possess high specific capacity, good cycle stability, and excellent rate performance, while maintaining good electrochemical performance at low temperatures to meet the needs of various application scenarios such as electric vehicles, energy storage power stations, and portable electronic devices.

[0003] However, the practical application of SIBs is limited by negative electrode reaction kinetics, among which Na + The high desolvation energy barrier is particularly prominent. At low temperatures, traditional anode materials (such as hard carbon) require Na... + Complete desolvation is required for storage, which leads to a sharp drop in charge transfer efficiency and severely impacts the overall battery performance. In contrast, graphite in ether electrolytes can be desolvated by Na... + - Solvent co-intercalation avoids the desolvation process. Combined with the low freezing point of ether solvents (such as diethylene glycol dimethyl ether), this mechanism significantly improves the low-temperature performance of SIBs. Furthermore, some metal sulfides, titanates, conjugated polymers, and bismuth-based materials also exhibit similar sodium storage mechanisms in ether-based electrolytes. Bismuth-based materials, due to their high theoretical specific capacity (385 mAh g⁻¹),... -1 Bi anodes have attracted much attention due to their excellent low-temperature tolerance. However, Bi anodes undergo approximately 350% volume change during charge and discharge, which can easily lead to electrode structure pulverization. Simultaneously, their semi-metallic properties also limit the potential for Na... + Diffusion and electron conduction. Therefore, how to maintain high capacity through structural design while solving the stability and conductivity problems of Bi anodes has become a key challenge in developing high-performance low-temperature anode materials. Summary of the Invention

[0004] In view of this, the present invention aims to overcome the defects in the prior art and proposes a carbon-coated bismuth nanosphere / graphite sheet composite material, its preparation method and application.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented as follows: The present invention provides a carbon-coated bismuth nanosphere / graphite sheet composite material, characterized in that: the composite material includes bismuth nanospheres, a carbon layer and graphite sheets, wherein the bismuth nanospheres are coated by the carbon layer and anchored between the graphite sheet layers to form a sandwich structure.

[0006] Furthermore, based on the total mass of the composite material, the content of the bismuth nanospheres is 10-80%, the content of the carbon layer is 1-10%, and the content of the graphite is 10-90%, with the sum of the three being 100%.

[0007] Furthermore, the composite material is prepared from the following raw materials in parts by weight: 100 parts graphite, 10-500 parts bismuth source, 10-1000 parts carbon source, 200-10000 parts acid, and 1000-50000 parts solvent.

[0008] Furthermore, the bismuth source is at least one of bismuth chloride, bismuth sulfate, bismuth nitrate, bismuth citrate, bismuth acetylacetone, bismuth oxynitrate, bismuth ethylenediaminetetraacetate, or potassium bismuth tartrate.

[0009] Furthermore, the carbon source is at least one of glucose, deoxyglucose, xylose, fructose, galactose, lactose, mannose, arabinose, ribose, deoxyribose, lysolose, sucrose, maltose, cellobiose, trehalose, mesobiose, raffinose, stachyose, fructooligosaccharides, xylooligosaccharides, L-glucose, inositol, sorbitol, tagatose, hydroxymethylfurfural, furfural, glyceraldehyde, thulose, glucosyl alcohol, gluconic acid, gluconolactone, erythrose, starch, cellulose, salicylic acid, malic acid, tartaric acid, ascorbic acid, lactic acid, gallic acid, sorbitol, mannitol, polyethyleneimine, polyacrylonitrile, polydopamine, polyvinylpyrrolidone, polyaniline, urea, melamine, dicyandiamide, glucosamine, or chitosan.

[0010] Furthermore, the acid is at least one selected from hydrochloric acid, nitric acid, sulfuric acid, citric acid, formic acid, acetic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, trichloroacetic acid, or dichloroacetic acid; the concentration of the acid is 0.1-10 M. The solvent is at least one of ethylene glycol, propylene glycol, butanediol, glycerol, diacetone alcohol, diethylene glycol, triethylene glycol, 1,6-hexanediol, polyethylene glycol, 2-pyrrolidone, N-methylpyrrolidone, N-vinylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, or water.

[0011] Furthermore, the graphite is at least one of flake graphite, microcrystalline graphite, expanded graphite, graphite nanosheets, porous graphite, and heteroatom-doped graphite.

[0012] This invention also provides a method for preparing carbon-coated bismuth nanospheres / graphite sheets composite materials, comprising the following steps: Acid and solvent are mixed evenly to obtain an acidic mixed solution. Bismuth source and carbon source are added to the acidic mixed solution, and then graphite is added. After stirring, a solvothermal reaction is carried out. After the reaction is completed, the obtained product is washed, dried, ground and calcined in sequence to obtain the composite material.

[0013] Furthermore, the temperature of the solvothermal reaction step is 80-250 ℃, and the reaction time is 1-48 hours; the temperature of the calcination step is 300-1200 ℃, the heating rate is 0.1-30 ℃ / min, and the calcination time is 0.5-20 hours; the calcination step is carried out under an inert atmosphere or a vacuum.

[0014] This invention also provides an application of a carbon-coated bismuth nanosphere / graphite sheet composite material in the preparation of a sodium-ion battery anode.

[0015] This invention constructs a "graphite sheet / carbon-coated bismuth nanosphere / graphite sheet" sandwich structure by in-situ generating carbon layers to coat bismuth nanospheres and directly loading them onto the surface of graphite sheets. This structure overcomes the shortcomings of two existing technologies: Firstly, in traditional Bi / C core-shell structures, the carbon-coated bismuth nanospheres (with diameters ranging from 10 to 500 nm) only have point contact with each other, and volume expansion under high-rate or long-cycle conditions easily leads to the breakage of interparticle connections, causing deactivation of the active material; secondly, in ordinary Bi / graphite composites, there is a lack of strong interfacial bonding between bismuth particles and graphite sheets, resulting in high contact resistance, and bismuth particles are prone to agglomeration and detachment from the graphite surface. Furthermore, this invention utilizes the confinement effect generated by the solvothermal reaction in a closed reactor. The limited space between the graphite sheet layers confines the growth of bismuth nanospheres, ensuring their uniform size and natural separation by the graphite sheets, avoiding agglomeration of bismuth particles during synthesis, and providing ideal unit cells for the subsequent construction of three-dimensional networks.

[0016] In the above structure, the carbon layer serves as an electron transport channel and stress buffer interface, firmly anchoring the bismuth nanospheres onto the graphite sheet skeleton. The volume expansion stress generated during charging and discharging is rapidly dispersed throughout the graphite network through the carbon layer, avoiding local stress concentration and electrical contact failure, while simultaneously achieving low-impedance electron transport.

[0017] Compared with the prior art, the present invention has the following advantages: In the carbon-coated bismuth nanosphere / graphite sheet composite material of the present invention, bismuth nanospheres are coated with carbon layers and uniformly anchored between graphite sheets to form a sandwich structure. The carbon protective layer and graphite sheets work together to effectively suppress the volume expansion of the bismuth anode during charging and discharging through mechanical support and conductive network construction, thereby improving the electrode conductivity and stability. At the same time, when an ether-based electrolyte is selected, sodium ions can co-intercalate with solvent molecules into the interlayer of bismuth and graphite, avoiding the traditional desolvation process, significantly accelerating the sodium ion reaction kinetics, and improving the rate performance and low-temperature performance of the battery. Attached Figure Description

[0018] Figure 1 The image shown is the XRD pattern of the composite material described in Example 1 of this invention. Figure 2 This is a SEM image of the composite material described in Example 1 of the present invention; Figure 3 The image shown is an HRTEM image of the composite material described in Example 1 of this invention. Detailed Implementation

[0019] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art. Unless otherwise specified, the experimental reagents used in the following embodiments are conventional biochemical reagents; and the experimental methods described are conventional methods.

[0020] The present invention will be described in detail below with reference to the embodiments.

[0021] Example 1 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 4000 parts of 1 M hydrochloric acid and 20000 parts of N,N-dimethylformamide were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth chloride and 50 parts of polyacrylonitrile were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. Then, it was placed in a vacuum oven at 70 °C and dried for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0022] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a certain rate and held constant for 5 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0023] The resulting composite material was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate as the positive electrode material, and the electrochemical performance was tested.

[0024] Figure 1 The XRD pattern of the prepared composite material was compared with the standard spectra of bismuth (PDF#85-1329) and graphite (PDF#41-1487), indicating that the composite material contains both metallic bismuth and graphite phases.

[0025] Figure 2 The image shows a SEM image of the prepared composite material. It can be seen from the image that bismuth exhibits the morphology of nanospheres and is uniformly dispersed between the graphite sheets, presenting an overall sandwich structure. The size of the bismuth nanospheres is approximately between 60-160 nm.

[0026] Figure 3 The HRTEM image of the prepared composite material shows that the surface of the bismuth nanospheres is coated with a carbon layer with a thickness of approximately 11 nm.

[0027] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0028] Example 2 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 0.5 M nitric acid and 5000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 50 parts of bismuth nitrate and 200 parts of glucose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 160 °C for 8 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0029] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 3 °C for 3 min under a vacuum atmosphere. -1 The temperature is increased to 450°C at a certain rate and held constant for 10 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0030] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0031] Example 3 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 2 M sulfuric acid and 10000 parts of propylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 100 parts of deoxyglucose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 200 °C for 5 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0032] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 2 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 350°C at a rising rate and held constant for 20 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0033] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0034] Example 4 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 9000 parts of 0.2 M sulfuric acid and 1000 parts of polyethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth sulfate and 200 parts of xylose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 240 °C for 3 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0035] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 1 °C for 1 min under an argon atmosphere.-1 The temperature is increased to 650°C at a rising rate and held constant for 10 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0036] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0037] Example 5 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 3 M formic acid and 20000 parts of butanediol were mixed evenly to prepare an acidic mixture. Then, 500 parts of bismuth citrate and 500 parts of fructose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 170 °C for 8 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0038] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under a nitrogen atmosphere. -1 The temperature is increased to 700°C at a certain rate and held constant for 10 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0039] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0040] Example 6 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 3 M acetic acid and 20000 parts of glycerol were mixed evenly to prepare an acidic mixture. Then, 300 parts of bismuth acetylacetonate and 300 parts of galactose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 120 °C for 48 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0041] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 30 °C for 3 min under an argon atmosphere. -1 The temperature is increased to 1000°C at a rising rate, held at a constant temperature for 0.5 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0042] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0043] Example 7 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 200 parts of 10 M nitric acid and 50,000 parts of glycerol were mixed thoroughly to prepare an acidic mixture. Then, 50 parts of bismuth nitrate and 200 parts of lactose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 100 °C for 48 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0044] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 1100°C at a rising rate, held at a constant temperature for 0.5 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0045] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0046] Example 8 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M trifluoromethanesulfonic acid and 30000 parts of diacetone alcohol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth oxynitrate and 400 parts of mannose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 90 °C for 36 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0047] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0048] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0049] Example 9 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M p-toluenesulfonic acid and 30000 parts of diethylene glycol were mixed evenly to prepare an acidic mixture. Then, 50 parts of bismuth ethylenediaminetetraacetate and 70 parts of arabinose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 110 °C for 24 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0050] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0051] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0052] Example 10 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M trichloroacetic acid and 30000 parts of triethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth chloride and 300 parts of ribose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of expanded graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 130 °C for 24 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0053] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0054] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0055] Example 11 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M dichloroacetic acid and 30000 parts of 1,6-hexanediol were mixed evenly to prepare an acidic mixture. Then, 500 parts of bismuth chloride and 600 parts of deoxyribose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of expanded graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 140 °C for 24 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0056] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0057] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0058] Example 12 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 30000 parts of 2-pyrrolidone were mixed thoroughly to prepare an acidic solution. Then, 50 parts of potassium bismuth tartrate and 50 parts of lysose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of flake graphite were added to the resulting solution and stirred until evenly dispersed. The solution was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 250 °C for 24 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0059] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0060] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0061] Example 13 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 20000 parts of N-methylpyrrolidone were mixed thoroughly to prepare an acidic solution. Then, 100 parts of bismuth nitrate and 200 parts of sucrose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of flake graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 230 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0062] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0063] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0064] Example 14 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 20000 parts of N-vinylpyrrolidone were mixed thoroughly to prepare an acidic solution. Then, 100 parts of bismuth nitrate and 200 parts of maltose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of flake graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 220 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0065] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0066] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0067] Example 15 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 20000 parts of N-ethylpyrrolidone were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of cellobiose were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 220 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0068] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0069] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0070] Example 16 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 20000 parts of N,N-dimethylformamide were mixed thoroughly to prepare an acidic solution. Then, 300 parts of bismuth nitrate and 400 parts of trehalose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure uniform dispersion. The solution was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 190 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0071] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0072] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0073] Example 17 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid and 30000 parts of dimethyl sulfoxide were mixed thoroughly to prepare an acidic solution. Then, 900 parts of bismuth nitrate and 800 parts of mesnothiose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure uniform dispersion. The solution was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 220 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0074] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0075] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0076] Example 18 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 1000 parts of 1 M nitric acid were mixed with 30000 parts of water to prepare an acidic solution. Then, 500 parts of bismuth nitrate and 500 parts of raffinose were added to this solution and stirred until completely dissolved. Next, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The solution was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 150 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0077] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere.-1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0078] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0079] Example 19 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 10,000 parts of 1 M nitric acid and 30,000 parts of ethylene glycol were mixed thoroughly to prepare an acidic solution. Then, 500 parts of bismuth nitrate and 400 parts of stachyose were added to this solution and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure uniform dispersion. The solution was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0080] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 3 °C for 3 min under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0081] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0082] Example 20 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of fructooligosaccharides were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0083] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 700°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0084] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0085] Example 21 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of xylooligosaccharides were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0086] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 700°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0087] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0088] Example 22 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of L-glucose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0089] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 700°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0090] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0091] Example 23 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of inositol were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0092] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0093] The content of each component in the obtained composite material was determined according to the method described below. It was then used as the negative electrode material in conjunction with sodium vanadium phosphate as the positive electrode material to assemble a sodium-ion battery for electrochemical performance testing. The content of each component and the results of the electrochemical performance tests are shown in Table 1.

[0094] Example 24 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of sorbitol were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0095] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0096] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0097] Example 25 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of tagatose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0098] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere.-1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0099] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0100] Example 26 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of hydroxymethylfurfural were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of flake graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0101] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0102] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0103] Example 27 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of furfural were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of sulfur-doped graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0104] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0105] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0106] Example 28 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of glyceraldehyde were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of phosphorus-doped graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0107] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0108] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0109] Example 29 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of thioglycolate were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of nitrogen-doped graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0110] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0111] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0112] Example 30 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of glucosamine were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of porous graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0113] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0114] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0115] Example 31 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M sulfuric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 300 parts of gluconic acid were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of graphite nanosheets were added to the resulting solution and stirred to disperse them evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0116] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0117] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0118] Example 32 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 5000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 250 parts of glucono-delta-lactone were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of expanded graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0119] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0120] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0121] Example 33 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 2 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of erythrose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0122] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0123] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0124] Example 34 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 2 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of starch were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0125] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0126] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0127] Example 35 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 2 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of cellulose were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0128] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0129] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0130] Example 36 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of salicylic acid were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0131] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0132] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0133] Example 37 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 0.5 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of malic acid were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0134] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0135] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0136] Example 38 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 0.5 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of tartaric acid were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0137] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0138] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0139] Example 39 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 0.5 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of ascorbic acid were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then placed in a vacuum oven at 70 °C and dried for 12 hours. Finally, the dried sample was removed and ground into powder.

[0140] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0141] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0142] Example 40 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 0.5 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 200 parts of lactic acid were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0143] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0144] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0145] Example 41 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 200 parts of gallic acid were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to ensure even dispersion. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant reached 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0146] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0147] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0148] Example 42 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 300 parts of bismuth nitrate and 300 parts of sorbitol were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0149] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0150] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0151] Example 43 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 300 parts of bismuth nitrate and 300 parts of mannitol were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0152] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0153] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0154] Example 44 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 300 parts of bismuth nitrate and 700 parts of polyethyleneimine were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0155] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0156] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0157] Example 45 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 300 parts of bismuth nitrate and 150 parts of polydopamine were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then placed in a vacuum oven at 70 °C and dried for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0158] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 10 °C for 1 min under an argon atmosphere. -1 The temperature is increased to 800°C at a certain rate and held constant for 2 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0159] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0160] Example 46 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 500 parts of polyvinylpyrrolidone were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0161] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere.-1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0162] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0163] Example 47 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 200 parts of bismuth nitrate and 100 parts of polyaniline were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0164] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0165] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0166] Example 48 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 500 parts of urea were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The supernatant was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0167] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0168] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0169] Example 49 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 500 parts of melamine were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0170] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0171] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0172] Example 50 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 500 parts of dicyandiamide were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then placed in a vacuum oven at 70 °C and dried for 12 hours. Finally, the dried sample was removed and ground into powder.

[0173] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0174] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0175] Example 51 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 100 parts of chitosan were added to this mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred until evenly dispersed. The mixture was transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. It was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0176] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0177] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0178] Example 52 A method for preparing a carbon-coated bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis: 2000 parts of 1 M nitric acid and 50000 parts of ethylene glycol were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth nitrate and 500 parts of glucosamine were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was removed and ground into powder.

[0179] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate, held constant for 2 hours, and then cooled to room temperature with the furnace body to obtain the composite material.

[0180] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0181] Comparative Example 1 A method for preparing a bismuth nanosphere / graphite sheet composite material includes the following steps: (1) Solvent thermal synthesis 4000 parts of 1 M hydrochloric acid and 20000 parts of N,N-dimethylformamide were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth chloride were added to the mixture and stirred until completely dissolved. Subsequently, 100 parts of microcrystalline graphite were added to the resulting solution and stirred to disperse it evenly. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then placed in a vacuum oven at 70 °C and dried for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0182] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate and held constant for 5 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0183] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0184] Comparative Example 2 A method for preparing a carbon-coated bismuth nanosphere composite material includes the following steps: (1) Solvent thermal synthesis: 4000 parts of 1 M hydrochloric acid and 20000 parts of N,N-dimethylformamide were mixed evenly to prepare an acidic mixture. Then, 100 parts of bismuth chloride and 50 parts of polyacrylonitrile were added to the mixture and stirred until completely dissolved. The mixture was then transferred to a stainless steel reactor and subjected to a solvothermal reaction at 180 °C for 12 hours. After the reactor cooled to room temperature, the product was centrifuged and washed until the pH of the supernatant was 7. The product was then dried in a vacuum oven at 70 °C for 12 hours. Finally, the dried sample was taken out and ground into powder.

[0185] (2) Tubular furnace calcination: The powder sample was placed in a tube furnace and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature is increased to 600°C at a rising rate and held constant for 5 hours. Then, the temperature is cooled to room temperature with the furnace body to obtain the composite material.

[0186] The content of each component in the obtained composite material was determined according to the method described below, and it was used as the negative electrode material to assemble a sodium-ion battery with sodium vanadium phosphate positive electrode material for electrochemical performance testing. The content of each component and the electrochemical performance test results are shown in Table 1.

[0187] Table 1 shows the component content of the composite material described in the embodiments and comparative examples of the present invention and the electrochemical performance of the assembled sodium-ion battery.

[0188] Table 1 Note: Specific capacity at room temperature is 10 A g. 1 The data obtained at -40 °C shows a specific capacity of 0.1 Ag. -1 The data obtained from the two tests are different, so direct numerical comparison is not appropriate; the cycle stability is at 5A g. -1 Data obtained from 1000 cycles at current density.

[0189] Methods for determining the component content of composite materials: The contents of bismuth nanospheres, carbon layers, and graphite in the composite material of the present invention were determined by the following method: (1) Determination of bismuth content: Accurately weigh a composite material with a mass of m0, add excess dilute nitric acid (1 M), and ultrasonically disperse for 30 minutes. The metallic bismuth reacts with the nitric acid to form a soluble bismuth salt that enters the solution, while the carbon layer and graphite are insoluble in the nitric acid and exist as insoluble matter. After the reaction is complete, filter and collect the insoluble matter, wash repeatedly with deionized water until neutral, dry, and weigh the insoluble matter, recording the mass as m1. The bismuth content in the composite material is then calculated using formula (I): Bismuth content (wt%) = (m0) m1) / m0×100%(I) (2) Determination of carbon layer content: To determine the carbon layer content in the composite material, a graphite-free carbon-coated bismuth nanosphere control sample was prepared under identical conditions (bismuth source type and amount, carbon source type and amount, acid type and amount, solvent type and amount), solvothermal reaction conditions, and calcination conditions. This control sample consisted only of metallic bismuth and a carbon layer.

[0190] Using the same method as in step (1), weigh a control sample with a mass of m0', add excess dilute nitric acid to dissolve the metallic bismuth, filter and collect the insoluble matter (i.e., the carbon layer), wash and dry it, and weigh the mass of the carbon layer, which is recorded as m. C The mass ratio of carbon layer to bismuth in the control sample is calculated according to formula (II): Carbon layer / bismuth mass ratio = m C ' / (m0' m C (II) Since the control sample and the composite material are identical in all raw material types, amounts, and synthesis conditions except for graphite, the mass ratio of carbon layer to bismuth in both is consistent. Based on the mass of bismuth in the composite material measured in step (1), the carbon layer content in the composite material is calculated according to formula (III): Carbon layer content (wt%) = Carbon layer / bismuth mass ratio × Bismuth content (wt%) (III) (3) Determination of graphite content: The total mass of the composite material is 100%. After deducting the bismuth content and carbon layer content, the remainder is the graphite content, calculated according to formula (IV): Graphite content (wt%) = 100% Bismuth content (wt%) Carbon layer content (wt%) (IV) According to the above method, the composite materials obtained in each embodiment of the present invention contain 10-80% bismuth nanospheres, 1-10% carbon layers, and 10-90% graphite by weight, with the sum of the three being 100%.

[0191] Analysis of the relationship between the content of each component and electrochemical performance: As shown in Table 1, the room temperature specific capacity and low temperature specific capacity of the composite material both increase with the increase of bismuth nanosphere content. For example, in Example 17, the bismuth nanosphere content was 72.9%, and its room temperature specific capacity was as high as 108.9 mAh g⁻¹. 1 , The specific capacity at 40℃ is 149.2 mAh g. 1 In Example 12, the bismuth nanosphere content was only 11.9%, and its room temperature specific capacity was 66.5 mAh g⁻¹. 1 , The specific capacity at 40℃ is 91.6 mAh g. 1 This is mainly due to the theoretical sodium storage capacity of bismuth (385 mAh g). 1 The bismuth content is much higher than that of graphite, so increasing the bismuth content helps to improve the overall sodium storage capacity of the composite material.

[0192] However, the higher bismuth content also brought some negative effects. In Example 17, the bismuth content was 72.9%, and the capacity retention after 1000 cycles was only 84%; while in Example 12, the bismuth content was 11.9%, and the cycle stability was as high as 94%. The cycle stability of Examples 11 (bismuth content 70.6%) and 19 (bismuth content 63.8%) was only 85% and 86%, respectively, both lower than the examples with lower bismuth content (such as Examples 1, 2, 7, 9, and 12, whose stability was all above 92%). This indicates that while increasing the bismuth content is beneficial for improving specific capacity, it also exacerbates the damage to the electrode structure caused by volume expansion during charge and discharge, leading to a decrease in cycle stability.

[0193] Considering the balance between specific capacity and cycling stability, this invention preferably uses bismuth nanospheres with a content of 25-75 wt%. Within this range, the composite material can achieve a high specific capacity (generally around 82 mAh g⁻¹ at room temperature). 1 above, The specific capacity at 40℃ is generally around 110 mAh g. 1 (Above), while maintaining good cycling stability (capacity retention is generally above 85% after 1000 cycles). Those skilled in the art can adjust the content of each component within the above range according to actual application needs to obtain a composite material that balances high capacity and long cycle life.

[0194] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A carbon-coated bismuth nanosphere / graphite sheet composite material, characterized in that: The composite material comprises bismuth nanospheres, carbon layers, and graphite sheets. The bismuth nanospheres are coated with carbon layers and anchored between the graphite sheet layers, forming a sandwich structure.

2. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 1, characterized in that: Based on the total mass of the composite material, the content of the bismuth nanospheres is 10-80%, the content of the carbon layer is 1-10%, and the content of the graphite is 10-90%, with the sum of the three being 100%.

3. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 1, characterized in that: The composite material is prepared from the following raw materials in parts by weight: 100 parts graphite, 10-1000 parts bismuth source, 10-1000 parts carbon source, 200-10000 parts acid, and 1000-50000 parts solvent.

4. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 3, characterized in that: The bismuth source is at least one of bismuth chloride, bismuth sulfate, bismuth nitrate, bismuth citrate, bismuth acetylacetone, bismuth oxynitrate, bismuth ethylenediaminetetraacetate, or potassium bismuth tartrate.

5. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 3, characterized in that: The carbon source is at least one of glucose, deoxyglucose, xylose, fructose, galactose, lactose, mannose, arabinose, ribose, deoxyribose, lysolose, sucrose, maltose, cellobiose, trehalose, mesobiose, raffinose, stachyose, fructooligosaccharides, xylooligosaccharides, L-glucose, inositol, sorbitol, tagatose, hydroxymethylfurfural, furfural, glyceraldehyde, thulose, glucosyl alcohol, gluconic acid, gluconolactone, erythrose, starch, cellulose, salicylic acid, malic acid, tartaric acid, ascorbic acid, lactic acid, gallic acid, sorbitol, mannitol, polyethyleneimine, polyacrylonitrile, polydopamine, polyvinylpyrrolidone, polyaniline, urea, melamine, dicyandiamide, glucosamine, or chitosan.

6. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 3, characterized in that: The acid is at least one of hydrochloric acid, nitric acid, sulfuric acid, citric acid, formic acid, acetic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, trichloroacetic acid, or dichloroacetic acid; the concentration of the acid is 0.1-10 M; the solvent is at least one of ethylene glycol, propylene glycol, butanediol, glycerol, diacetone alcohol, diethylene glycol, triethylene glycol, 1,6-hexanediol, polyethylene glycol, 2-pyrrolidone, N-methylpyrrolidone, N-vinylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, or water.

7. The carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 3, characterized in that: The graphite mentioned is at least one of flake graphite, microcrystalline graphite, expanded graphite, graphite nanosheets, porous graphite, and heteroatom-doped graphite.

8. The method for preparing the carbon-coated bismuth nanosphere / graphite sheet composite material according to any one of claims 1-7, characterized in that: Includes the following steps: Acid and solvent are mixed evenly to obtain an acidic mixed solution. Bismuth source and carbon source are added to the acidic mixed solution, and then graphite is added. After stirring, a solvothermal reaction is carried out. After the reaction is completed, the obtained product is washed, dried, ground and calcined in sequence to obtain the composite material.

9. The method for preparing the carbon-coated bismuth nanosphere / graphite sheet composite material according to claim 8, characterized in that: The temperature of the solvothermal reaction step is 80-250 ℃, and the reaction time is 1-48 hours; the temperature of the calcination step is 300-1200 ℃, the heating rate is 0.1-30 ℃ / min, and the calcination time is 0.5-20 hours; the calcination step is carried out under an inert atmosphere or a vacuum.

10. The application of the carbon-coated bismuth nanosphere / graphite sheet composite material according to any one of claims 1-7, characterized in that: The application of the aforementioned composite material in the preparation of sodium-ion battery anodes.