A negative electrode material and its preparation method, and a lithium-ion battery
By using bio-oil as a carbon source and combining hydrothermal method and carbonization treatment to prepare porous carbon composite silicon nanoparticles-silicon-carbon anode materials, the problem of volume expansion of silicon-based anode materials during charge and discharge is solved, realizing the application of lithium-ion batteries with high energy density and long cycle life, while reducing costs and making it suitable for large-scale production.
Patent Information
- Application Number
- CN202611305772.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, silicon-based anode materials undergo volume expansion during charging and discharging, leading to pulverization and shedding, which makes it difficult to meet the requirements of high energy density and long cycle life. Furthermore, commonly used carbon sources are expensive and have complex preparation processes, making it difficult to achieve large-scale applications.
Using bio-oil as a carbon source, porous carbon composite silicon nanoparticles—silicon-carbon anode materials—are prepared through a hydrothermal method combined with carbonization. The process is simple and easy to scale up. The material has a moderate silicon content and a porous structure, which buffers the volume expansion of silicon and improves cycle stability.
The prepared porous carbon-silicon nanoparticle silicon-carbon anode material exhibits excellent electrochemical performance in lithium-ion batteries, improving the cycle stability of the material and the energy density of the battery, reducing costs, and conforming to the concept of sustainable development.
Smart Images

Figure CN123120680A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of batteries, specifically relating to a negative electrode material and its preparation method, and a lithium-ion battery using the negative electrode material. Background Technology
[0002] In recent years, with the rapid popularization and development of portable electronic devices and electric vehicles, traditional graphite anodes can no longer meet the current market demand for high energy density and long cycle life, necessitating the search for next-generation lithium-ion battery anode materials. Compared to carbon-based anode materials, silicon is an alloyed lithium-intercalating material with a theoretical lithium intercalation capacity as high as 4200 mAh / g. It is also abundant, safe, and non-toxic, making it the most promising lithium-ion battery anode material. However, in existing technologies, silicon undergoes volume expansion (~380%) during charging and discharging, leading to defects such as material pulverization and detachment. To overcome these problems, researchers have proposed various strategies, among which the composite construction of silicon nanoparticles and carbon materials to create silicon-carbon composites is considered an effective method. Carbon materials can not only buffer the volume expansion of silicon but also improve the conductivity of the material. Currently, commonly used carbon sources include graphene, carbon nanotubes, and organic polymers, but these carbon sources are costly and have complex preparation processes, making large-scale application difficult. Summary of the Invention
[0003] Based on the problems existing in the prior art, the present invention provides a method for preparing porous carbon composite silicon nanoparticles-silicon carbon anode materials using bio-oil as a carbon source.
[0004] The silicon-carbon anode material provided by this invention has a silicon content of 47%-53wt%, a specific capacity of 1800-2000mAh / g, and a specific surface area of 3.0-6.5 m². 2 / g, total pore volume 0.1~0.005 cc / g, powder resistivity 1.0-10Ω·cm.
[0005] The anode was prepared using the silicon-carbon anode material and assembled into a 4Ah pouch cell. The initial coulombic efficiency at 0.8V was 80-84.5%, and the capacity retention rate after 200 cycles at 0.5C was 95.0-98.5%.
[0006] The silicon-carbon anode material of this invention has a moderate silicon content and a porous structure, which can effectively buffer the volume expansion of silicon and improve the cycle stability of the material.
[0007] The method for preparing porous carbon-silicon composite nanoparticle-silicon-carbon anode material provided by the present invention includes the following steps: 1) Preparation of silicon nanoparticles: The silicon source, reducing agent and surfactant are dissolved in a solvent and heated under an inert atmosphere to obtain a silicon nanoparticle dispersion. 2) Bio-oil pretreatment: The bio-oil is filtered and dehydrated to obtain refined bio-oil; 3) Preparation of mixed solution: The silicon nanoparticle dispersion obtained in step 1) is mixed with the refined bio-oil obtained in step 2), a catalyst is added, and the mixture is stirred evenly to obtain a mixed solution; 4) Hydrothermal reaction: The mixed solution obtained in step 3) is transferred to a hydrothermal reactor for hydrothermal reaction to obtain hydrothermal products; 5) Carbonization treatment: The hydrothermal product obtained in step 4) is carbonized in an inert atmosphere to obtain porous carbon composite silicon nanoparticle silicon-carbon anode material, i.e. primary silicon-carbon anode material.
[0008] This invention uses bio-oil as a carbon source, which is widely available, inexpensive, and environmentally friendly, in line with the concept of sustainable development. It uses a hydrothermal method combined with carbonization to prepare porous carbon composite silicon nanoparticle silicon-carbon anode materials. The process is simple and easy to scale up. Moreover, the resulting material has a moderate silicon content and a porous structure, which can effectively buffer the volume expansion of silicon and improve the cycle stability of the material.
[0009] In step 1) of the above method, the silicon source is selected from one or more of tetraethyl orthosilicate, sodium silicate, and silicon dioxide; The reducing agent is selected from one or more of the following: hydrazine hydrate, sodium borohydride, and ascorbic acid; The surfactant is selected from one or more of the following: cetyltrimethylammonium bromide, polyvinylpyrrolidone, and sodium dodecyl sulfate; The solvent is selected from one or more of the following: water, ethanol, and ethylene glycol; The mass ratio of the silicon source (based on silicon) to the reducing agent and surfactant can be 10-30: 5-20: 1-5. The heating reaction is carried out at a temperature of 120–180°C for 3–8 hours. The solid content of silicon nanoparticles in the obtained silicon nanoparticle dispersion is 4%-20%.
[0010] In step 2), the bio-oil is one or more of vegetable oil, animal oil, and waste cooking oil.
[0011] In step 3), the volume ratio of the silicon nanoparticle dispersion to the refined bio-oil is 1:2 to 1:10. The catalyst is selected from one or more of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid; Based on the total mass of refined bio-oil, the amount of catalyst added is 1wt% to 6wt%.
[0012] In step 4), the hydrothermal reaction is carried out at a temperature of 160-220°C for 6-24 hours. The heating rate of the hydrothermal reaction is 1-5℃ / min; In step 5), the inert atmosphere is one or both of nitrogen and argon. The carbonization process is carried out at a temperature of 600-900℃ for 2-6 hours.
[0013] The method further includes, after step 5), performing chemical vapor deposition carbon coating on the obtained primary silicon-carbon anode material to obtain a silicon-carbon anode material.
[0014] The inert gas used in the chemical vapor deposition carbon coating is argon. The carbon precursor gas is at least one of methane, ethane, propane, ethylene, propylene, and acetylene; The flow rate of the carbon precursor gas is 2–10 L / min; The inlet gas flow rate ratio of inert gas to carbon precursor gas is 10 to 5:1; The temperature for carbon coating by vapor deposition is 500–800℃, the time is 2–6 h, and the heating rate can be 1–5℃ / min.
[0015] The primary silicon-carbon anode material or silicon-carbon anode material prepared by the above method also falls within the protection scope of this invention.
[0016] The application of the aforementioned silicon-carbon anode material in lithium-ion batteries also falls within the scope of protection of this invention.
[0017] The present invention also provides a lithium-ion battery, wherein the negative electrode of the lithium-ion battery is prepared using the above-mentioned silicon-carbon negative electrode material.
[0018] The present invention has the following beneficial effects: 1) This invention uses bio-oil as a carbon source, which is widely available, inexpensive, and environmentally friendly, and is in line with the concept of sustainable development; 2) This invention uses a hydrothermal method combined with carbonization to prepare porous carbon composite silicon nanoparticle silicon-carbon anode materials. The process is simple and easy to scale up. 3) The porous carbon composite silicon nanoparticle silicon-carbon anode material prepared by this invention has a porous structure, which can effectively buffer the volume expansion of silicon and improve the cycle stability of the material. 4) The silicon-carbon anode material prepared by this invention has excellent electrochemical performance and can be applied to high-energy-density lithium-ion batteries. Attached Figure Description Figure 1 This is a SEM image of the cross-section of the composite material prepared in Example 1 of the present invention after argon ion beam cutting.
[0019] Figure 2 The image shown is the XRD pattern of the composite material prepared in Example 1 of this invention.
[0020] Figure 3 This is a comparison chart of the cycle performance of Embodiment 1 of the present invention and a commercial product. Detailed Implementation
[0021] The present invention will now be described in further detail with reference to specific embodiments. The given embodiments are merely illustrative of the invention and not intended to limit its scope. The embodiments provided below can serve as a guide for further improvements by those skilled in the art and do not constitute a limitation on the invention in any way.
[0022] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0023] Example 1: Preparation of silicon-carbon anode material for lithium-ion batteries The method for preparing the silicon-carbon anode material for lithium-ion batteries described in this embodiment includes the following steps: 1. Dissolve 10 g tetraethyl orthosilicate, 0.71 g hydrazine hydrate and 0.10 g hexadecyltrimethylammonium bromide in 9 mL of water, and heat at 120 °C for 6 hours under nitrogen protection to obtain a silicon nanoparticle dispersion (the solid content of silicon nanoparticles is 6.56%). 2. Filter and dehydrate 40 mL of soybean oil to obtain refined soybean oil; 3. Mix the silicon nanoparticle dispersion obtained in step 1 with the refined soybean oil obtained in step 2, add 0.8 mL of concentrated sulfuric acid, and stir until homogeneous to obtain a mixed solution.
[0024] 4. Transfer the mixed solution obtained in step 3 to a hydrothermal reactor, heat at a rate of 3℃ / min, react at 180℃ for 12 hours, and allow to cool naturally to room temperature after the reaction to obtain the hydrothermal product. 5. The hydrothermal product obtained in step 4 is carbonized in a nitrogen atmosphere at a carbonization temperature of 700℃ for 4 hours to obtain a porous carbon composite silicon nanoparticle silicon-carbon anode material. 6. Transfer the silicon-carbon anode material obtained in step 5 into a CVD deposition furnace, purge with argon gas at a rate of 20 L / min for 40 min, continue to purge with argon gas at a rate of 20 L / min, purge with acetylene gas at a rate of 2 L / min, heat up at a rate of 1 °C / min, carbonization coating temperature at 500 °C, hold for 2 h, and then allow to cool naturally. After sieving, obtain the final anode active material.
[0025] Figure 1 The image shows a cross-sectional SEM image of the prepared composite material after argon ion beam cutting.
[0026] Figure 2 The image shows the XRD pattern of the prepared composite material.
[0027] Example 2: Preparation of silicon-carbon anode material for lithium-ion batteries 1. Dissolve 10 g of tetraethyl orthosilicate, 0.9 g of ascorbic acid and 0.28 g of polyvinylpyrrolidone in 15 mL of ethylene glycol, and heat at 130 °C for 4 hours under nitrogen protection to obtain a silicon nanoparticle dispersion (the solid content of silicon nanoparticles is 4.96%). 2. Filter and dehydrate 60mL of waste cooking oil to obtain refined waste cooking oil; 3. Mix the silicon nanoparticle dispersion obtained in step 1 with the refined waste cooking oil obtained in step 2, add 1.5 mL of concentrated sulfuric acid, and stir evenly to obtain a mixed solution; 4. Transfer the mixed solution obtained in step 3 to a hydrothermal reactor, heat at a rate of 3℃ / min, react at 180℃ for 12 hours, and allow to cool naturally to room temperature after the reaction to obtain the hydrothermal product. 5. The hydrothermal product obtained in step 4 is carbonized in an argon atmosphere at a carbonization temperature of 700℃ for 4 hours to obtain a porous carbon composite silicon nanoparticle silicon-carbon anode material.
[0028] 6. Transfer the silicon-carbon anode material obtained in step 5 into a CVD deposition furnace, purge with argon gas at a rate of 30 L / min for 40 min, continue to purge with argon gas at a rate of 30 L / min, purge with acetylene gas at a rate of 3 L / min, raise the temperature at a rate of 1 °C / min, set the carbonization coating temperature to 600 °C, hold for 4 h, allow to cool naturally after completion, and sieve to obtain the final anode active material.
[0029] Example 3: Preparation of silicon-carbon anode material for lithium-ion batteries 1. Dissolve 10 g of silicon dioxide, 2.4 g of sodium borate and 0.92 g of sodium dodecyl sulfate in 20 mL of ethanol, and heat at 180 °C for 8 hours under nitrogen protection to obtain a silicon nanoparticle dispersion (the solid content of silicon nanoparticles is 16.7%). 2. Filter and dehydrate 50mL of palm oil to obtain refined palm oil; 3. Mix the silicon nanoparticle dispersion obtained in step 1 with the refined palm oil obtained in step 2, add 3 mL of concentrated sulfuric acid, and stir until homogeneous to obtain a mixed solution; 4. Transfer the mixed solution obtained in step 3 to a hydrothermal reactor, heat at a rate of 3℃ / min, react at 220℃ for 24 hours, and allow to cool naturally to room temperature after the reaction to obtain the hydrothermal product. 5. The hydrothermal product obtained in step 4 is subjected to carbonization treatment under a nitrogen atmosphere. The carbonization temperature is 900℃ and the carbonization time is 6 hours to obtain porous carbon composite silicon nanoparticle silicon-carbon anode material.
[0030] 6. Transfer the silicon-carbon anode material obtained in step 5 into a CVD deposition furnace, purge with argon gas (40 L / min) for 40 min, then continue to purge with argon gas at a rate of 40 mL / min, acetylene gas at a rate of 4 L / min, heating rate of 5 °C / min, carbonization coating temperature of 800 °C, and holding time of 6 h. After completion, allow it to cool naturally, sieve, and obtain the final anode active material.
[0031] Comparative Example 1 The difference between the preparation method and Example 1 is that in step 2, graphene of equal mass is used instead of refined soybean oil.
[0032] Comparative Example 2 The difference between the preparation method and Example 1 is that the hydrothermal reaction temperature in step 4 is 100℃.
[0033] The positive electrode of the full cell uses commercially available ternary material NCM622. The ternary material NCM622 active material, conductive agent SuperP, and binder PVDF are mixed in a mass ratio of 94:3:3, and stirred with N-methylpyrrolidone (NMP) as solvent to form a uniform positive electrode slurry. The slurry is then coated onto a 16μm aluminum foil current collector, resulting in a single-sided areal density of 188 g / m². 2 A commercially available Celgard 2400 single-layer polypropylene (PP) microporous membrane with a thickness of 20 μm and a porosity of 40% was selected to effectively block contact between the positive and negative electrodes and prevent internal short circuits in the battery. The electrolyte adopted a conventional electrolyte system for commercial lithium-ion batteries, specifically formulated as follows: the base solvents were ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1; the conductive lithium salt was lithium hexafluorophosphate (LiPF6) at a molar concentration of 1 mol / L; functional additives included 5 wt% fluoroethylene carbonate (FEC) and 2 wt% vinylene carbonate (VC). These additives stabilized the SEI film on the electrodes and mitigated interfacial damage caused by the volume expansion of silicon materials. The battery was assembled into a 4Ah pouch cell.
[0034] The negative electrode material, conductive agent Super P, single-arm carbon nanotubes, and binder polyacrylic acid (PAA, diluted to 3% solid content) prepared in this embodiment of the invention are mixed in a mass ratio of 92:3:2:3 and stirred with water as a solvent to form a uniform negative electrode slurry. The slurry is coated onto an 8μm copper foil current collector, and the single-sided areal density of the negative electrode is 74 g / m². 2 .
[0035] Table 1 Electrochemical and material physical properties of the examples and comparative products
[0036] As can be seen from the above examples, in Example 1, the material prepared by the process of this invention showed improved initial charge-discharge efficiency and capacity retention compared to the comparative example, indicating that the design of this scheme improved the electrochemical performance of the material to a certain extent. Figure 3 It can also be seen that the material's cycle performance has been slightly improved.
[0037] The present invention has been described in detail above. Those skilled in the art will recognize that the invention can be practiced in a wide range of ways with equivalent parameters, concentrations, and conditions without departing from its spirit and scope, and without requiring unnecessary experiments. While specific embodiments have been provided, it should be understood that further modifications can be made to the invention. In summary, according to the principles of the invention, this application is intended to include any changes, uses, or improvements to the invention, including changes made using conventional techniques known in the art that depart from the scope disclosed herein.
Claims
1. A silicon-carbon anode material having a silicon content of 47%-53 wt%, a specific capacity of 1800-2000 mAh / g, and a specific surface area of 3.0-6.5 m². 2 / g, total pore volume 0.1~0.005 cc / g, powder resistivity 1.0-10Ω·cm.
2. The silicon-carbon anode material according to claim 1, characterized in that, The anode was prepared using the silicon-carbon anode material and assembled into a 4Ah pouch cell. The initial coulombic efficiency at 0.8V was 80-84.5%, and the capacity retention rate after 200 cycles at 0.5C was 95.0-98.5%.
3. A method for preparing the silicon-carbon anode material according to claim 1 or 2, comprising the following steps: 1) Preparation of silicon nanoparticles: The silicon source, reducing agent and surfactant are dissolved in a solvent and heated under an inert atmosphere to obtain a silicon nanoparticle dispersion. 2) Bio-oil pretreatment: The bio-oil is filtered and dehydrated to obtain refined bio-oil; 3) Preparation of mixed solution: The silicon nanoparticle dispersion obtained in step 1) is mixed with the refined bio-oil obtained in step 2), a catalyst is added, and the mixture is stirred evenly to obtain a mixed solution; 4) Hydrothermal reaction: The mixed solution obtained in step 3) is transferred to a hydrothermal reactor for hydrothermal reaction to obtain hydrothermal products; 5) Carbonization treatment: The hydrothermal product obtained in step 4) is carbonized in an inert atmosphere to obtain porous carbon composite silicon nanoparticle silicon-carbon anode material, i.e. primary silicon-carbon anode material.
4. The method according to claim 3, characterized in that, In step 1), the silicon source is selected from one or more of tetraethyl orthosilicate, sodium silicate, and silicon dioxide; The reducing agent is selected from one or more of the following: hydrazine hydrate, sodium borohydride, and ascorbic acid; The surfactant is selected from one or more of the following: cetyltrimethylammonium bromide, polyvinylpyrrolidone, and sodium dodecyl sulfate; The solvent is selected from one or more of the following: water, ethanol, and ethylene glycol; The mass ratio of the silicon source (based on silicon) to the reducing agent and surfactant is 10-30: 5-20: 1-5. The heating reaction is carried out at a temperature of 120–180°C for 3–8 hours. The solid content of silicon nanoparticles in the obtained silicon nanoparticle dispersion is 4%-20%.
5. The method according to claim 3, characterized in that, In step 2), the bio-oil is one or more of vegetable oil, animal oil, and waste cooking oil.
6. The method according to claim 3, characterized in that, In step 3), the volume ratio of the silicon nanoparticle dispersion to the refined bio-oil is 1:2 to 1:
10. The catalyst is selected from one or more of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid; Based on the total mass of refined bio-oil, the amount of catalyst added is 1wt% to 6wt%.
7. The method according to claim 3, characterized in that, In step 4), the hydrothermal reaction is carried out at a temperature of 160-220°C for 6-24 hours. The heating rate of the hydrothermal reaction is 1-5℃ / min.
8. The method according to claim 3, characterized in that, In step 5), the inert atmosphere is one or both of nitrogen and argon. The carbonization process is carried out at a temperature of 600-900℃ for 2-6 hours.
9. The method according to claim 3, characterized in that, The method further includes, after step 5), performing chemical vapor deposition carbon coating on the obtained primary silicon-carbon anode material to obtain a silicon-carbon anode material.
10. The method according to claim 9, characterized in that, The inert gas used for the chemical vapor deposition carbon coating is argon. The carbon precursor gas is at least one of methane, ethane, propane, ethylene, propylene, and acetylene; The flow rate of the carbon precursor gas is 2–10 L / min; The inlet gas flow rate ratio of inert gas to carbon precursor gas is 10 to 5:1; The temperature for carbon coating by vapor deposition is 500–800℃, the time is 2–6 h, and the heating rate can be 1–5℃ / min.
11. A lithium-ion battery, wherein the negative electrode of the lithium-ion battery is prepared using the silicon-carbon negative electrode material as described in claim 1 or 2.