Core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material and its preparation method

By growing V-MOF precursors in situ on the surface of lithium manganese iron phosphate to form an LVP@C core-shell structure, the problem of insufficient modification of lithium manganese iron phosphate cathode material was solved, achieving synergistic improvement of lithium-ion and electron conduction, suppressing manganese dissolution and lattice distortion, and improving the cycle stability and high-temperature performance of the battery.

CN123120682APending Publication Date: 2026-11-17XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611319040.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium manganese iron phosphate cathode materials suffer from problems such as a single modification mechanism, insufficient structural stability, weak interfacial bonding, and low ion conduction efficiency in high-performance power batteries and large-scale energy storage batteries. They cannot effectively suppress manganese dissolution and lattice distortion, resulting in poor voltage decay and cycle stability.

Method used

A vanadium-based metal-organic framework (V-MOF) precursor was grown in situ on the surface of lithium manganese iron phosphate using a solvothermal method. The core-shell structure of lithium vanadium phosphate (LVP) and carbon network was formed by precise temperature control calcination, thus constructing an LVP@C/LMFP core-shell composite cathode material. This achieved a synergistic improvement in lithium-ion and electron conduction and formed a stable physical isolation shell.

Benefits of technology

It significantly inhibits manganese ion dissolution, alleviates lattice distortion, improves the rate performance and long-cycle stability of the material, forms a continuous conductive network, enhances mechanical stability, and improves the high-temperature performance and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120682A_ABST
    Figure CN123120682A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery cathode materials, specifically to a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material and its preparation method. The material comprises a lithium manganese iron phosphate core and an LVP@C shell coating its surface. The shell is obtained by calcining a V-MOF precursor grown in situ on the core surface. During preparation, V-MOF is first grown in situ on the LMFP surface, then mixed with a lithium source and a phosphorus source and calcined, transforming the V-MOF into a fast-ion conductor of lithium vanadium phosphate with a NASICON structure and derived carbon. This invention achieves uniform composite of LVP and carbon on the LMFP surface through in-situ V-MOF conversion, resulting in high bonding strength between the modified layer and the substrate. It simultaneously improves the material's electronic conductivity and ion diffusion coefficient, effectively suppresses manganese leaching and Jahn-Teller distortion, and improves the rate performance and cycle stability of the cathode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery cathode material technology, specifically to a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material and its preparation method. Background Technology

[0002] Lithium manganese iron phosphate (LMFP) possesses advantages such as a high voltage platform (4.1V), high theoretical capacity, and low raw material cost, making it a cost-effective cathode material for lithium-ion batteries. Currently, the industry's conventional preparation and modification techniques mainly involve synthesizing a pure-phase LMFP matrix via a high-temperature solid-state method and then modifying the material surface using a single carbon coating. This method only improves the electronic conductivity of LMFP through the surface carbon layer, without addressing the intrinsic lattice defects and manganese leaching issues. While it remains the mainstream technology for industrial applications at present and meets basic battery charge-discharge performance requirements, it is not suitable for the long-term cycling conditions of high-performance power batteries and large-scale energy storage batteries.

[0003] Existing LMFP modification technologies generally suffer from problems such as a single modification mechanism, insufficient structural stability, weak interfacial bonding, and low ion conduction efficiency, making it difficult to simultaneously address the four core pain points of LMFP: lattice distortion, manganese dissolution, voltage decay, and low conductivity. Regarding elemental doping, while lattice occupancy through single or small amounts of metal ions (such as Al, V, Ti, Mg, etc.) can slightly optimize cell parameters, it does not significantly improve the performance of Mn in lithium manganese iron phosphate. 3+ The effects of dissolution and Jahn-Teller distortion suppression are limited, failing to fundamentally alleviate lattice distortion and structural collapse during charge and discharge processes, resulting in significant capacity decay over long-term cycling. Regarding carbon coating, high-temperature pyrolysis of carbon sources such as glucose and sucrose is often used to prepare carbon layers. While this can improve electronic conductivity, the carbon layer and the LMFP substrate are only physically attached, with weak bonding. During cycling, the carbon layer is prone to detachment and cracking due to electrolyte erosion and volume changes, failing to effectively prevent contact between the electrolyte and active materials. Manganese ion dissolution remains a prominent issue, and the carbon layer itself lacks fast lithium-ion conduction capabilities, limiting the rate performance improvement. For phosphate coating, vanadium phosphate and iron phosphate are often directly ball-milled and mixed. This results in poor coating density and uniformity, easily leading to localized excessive thickness or voids. This not only hinders lithium-ion transport but also increases interfacial impedance. Furthermore, such coatings have low lattice matching with LMFPs, making the heterogeneous interface prone to defects and resulting in poor cycling stability.

[0004] For example, the literature "Improved LiMn" 0.6 Fe 0.4The study, titled "PO4 lattice stability and lithium-ion diffusion via Li3V2(PO4)3 and carbon co-coating for better electrochemical performance," describes a process where lithium vanadium phosphate (LVP) powder and lithium LMFP are simply physically blended using solid-state ball milling, followed by spray drying and high-temperature calcination to prepare LVP / carbon-coated LMFP core-shell materials. This process relies solely on physical adhesion for coating, resulting in point-contact coating, which is highly susceptible to localized excessive build-up, large-area substrate exposure, and free, independent LVP impurity particles. Furthermore, due to the difference in lattice expansion coefficients between the two phases, the composite material is prone to interfacial cracking during cycling, leading to coating layer detachment, phase separation, and long-term modification failure.

[0005] Therefore, there is an urgent need to develop an integrated modification method for lithium manganese iron phosphate that can simultaneously improve electron / ion conduction, suppress manganese dissolution and lattice distortion, and ensure a strong bond between the coating layer and the substrate. Summary of the Invention

[0006] In view of this, the present invention provides a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material and its preparation method, using lithium manganese iron phosphate (LiMn) x Fe y Using PO4 (LMFP) as the core, vanadium-based metal-organic framework (V-MOF) precursors of different concentrations are grown in situ on the surface of LMFP particles using a solvothermal method. After compounding with lithium and phosphorus sources, the precursors are calcined in an inert environment with precise temperature control. Utilizing the V-MOF topological derivatization transformation principle, the vanadium nodes in the V-MOF react with exogenous lithium and phosphorus to generate NASICON-type fast ion conductor lithium vanadium phosphate Li3V2(PO4)3 (LVP) in situ. At the same time, the organic ligands undergo pyrolysis to generate a three-dimensional continuous porous carbon network in situ, thus constructing an LVP@C / LMFP core-shell composite cathode.

[0007] The technical solution of this invention is implemented as follows: In a first aspect, the present invention provides a core-shell type V-MOF-derived LVP@C coated lithium manganese iron phosphate cathode material, which includes a core and a shell coating the surface of the core; the core includes lithium manganese iron phosphate; the shell includes lithium vanadium phosphate and carbon; The shell is obtained by calcining a V-MOF precursor, which is grown in situ on the surface of the core.

[0008] Preferably, the thickness of the shell layer is 12~50 nm.

[0009] Preferably, the carbon accounts for 2.5 to 7.5 wt% of the total mass of the cathode material.

[0010] Specifically, the thickness of the LVP / C shell and the carbon content exhibit a synergistic coupling relationship, jointly determining the material's conductivity, ion diffusion capability, and the shell's protective effect on the inner substrate. If the shell is too thin and the carbon content is insufficient, it is difficult to form a continuous conductive network, resulting in a significant increase in charge transfer impedance. Furthermore, the presence of microscopic pores and defects in the shell makes it easier for the electrolyte to corrode the substrate material, exacerbating Mn dissolution and the Jahn-Teller effect, thus degrading rate performance and cycle stability. Conversely, if the shell is too thick and the carbon content is too high, the lithium-ion diffusion path will become longer, blocking the ion channels inside the LVP, intensifying concentration polarization, and significantly reducing the discharge capacity at high rates. Carbon is an inactive component, and excessive carbon will reduce the material's specific capacity, sacrificing the cell's energy density. Only by controlling the shell thickness and carbon content to an appropriate range can an ultra-thin, continuously distributed LVP / C composite protective shell be constructed, balancing the high lithium-ion transport rate, a complete electron conduction network, and a long-lasting physical barrier against manganese dissolution, thereby achieving a synergistic improvement in rate performance and cycle life.

[0011] More preferably, the lithium manganese iron phosphate has the chemical formula LiMn 0.5 Fe 0.5 The chemical formula of the lithium vanadium phosphate is Li3V2(PO4)3.

[0012] In a second aspect, the present invention provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material as described in the first aspect, comprising the following steps: S1. Disperse lithium manganese iron phosphate powder in a solvent containing vanadium source and organic ligand, and carry out a solvothermal reaction to grow V-MOF precursor on the surface of lithium manganese iron phosphate to obtain V-MOF@lithium manganese iron phosphate composite intermediate. S2. The V-MOF@lithium manganese iron phosphate composite intermediate is mixed with a lithium source and a phosphorus source and calcined under an inert atmosphere to convert the V-MOF precursor into lithium vanadium phosphate and carbon, thereby obtaining the core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate material.

[0013] More preferably, step S1 further includes: redispersing the obtained V-MOF@lithium manganese iron phosphate composite intermediate in a solvent containing a vanadium source and an organic ligand, and performing a solvothermal reaction again to allow the V-MOF precursor to grow a second time on the surface of the composite intermediate.

[0014] Specifically, compared to the single-step single-layer V-MOF coating followed by calcination, this invention also employs a two-step solvothermal double-layer V-MOF coating followed by unified calcination modification method. The second V-MOF layer can selectively fill defects such as thin film areas and microscopic gaps present in the single-layer coating. After calcination, a complete double-layer LVP@C gradient core-shell structure without exposed surfaces is formed, constructing a dual manganese ion barrier, significantly inhibiting Mn dissolution and Jahn-Teller distortion, and alleviating voltage decay. The multi-level interface can hierarchically disperse the charge and discharge lattice stress, preventing shell cracking and detachment. At the same time, the two V-MOF ligands are carbonized to form a hierarchically interconnected porous carbon conductive network, simultaneously accelerating lithium-ion and electron transport, reducing interface impedance, and independently controlling the growth thickness of the two MOF layers. Under the same total coating load, it achieves better material compaction density, rate performance, and long-cycle stability.

[0015] Preferably, the vanadium source in step S1 includes one of vanadium acetylacetonate, vanadium trichloride, or ammonium metavanadate, the organic ligand includes one of terephthalic acid, 2-aminoterephthalic acid, or trimesoic acid, and the solvent includes N,N-dimethylformamide; the lithium source in step S2 includes lithium carbonate, and the phosphorus source includes phosphoric acid.

[0016] Preferably, the mass ratio of lithium manganese iron phosphate in step S1 to the total amount of vanadium source added in step S1 is 5:(0.25-0.8); the mass ratio of vanadium source in step S1 to lithium source and phosphorus source in step S2 is (0.25-0.8):(0.5-0.8):(0.2-0.5).

[0017] More preferably, in step S1, the mixture is dispersed in a solvent containing a vanadium source and an organic ligand, wherein the mass ratio of the organic ligand to the vanadium source is (0.5-2):1; the solvothermal reaction temperature is 80-160 °C and the reaction time is 6-24 h.

[0018] Preferably, the calcination in step S2 specifically includes: heating to 350-450°C at a rate of 1-5°C / min and holding for 1-3 h, then heating to 650-800°C at a rate of 2-10°C / min and holding for 4-12 h; the inert gas includes at least one of nitrogen, argon or helium.

[0019] More preferably, after the calcination is completed, the process further includes: rapidly cooling to 500°C at 10°C / min, holding at that temperature for 1 hour, and then annealing.

[0020] Specifically, annealing can release the lattice thermal stress generated by high-temperature calcination, repair lattice distortion, reduce crystal defects, and regulate the grain boundary structure. On the other hand, it can suppress abnormal grain coarsening, homogenize the valence state of vanadium, reduce the generation of impurity phases, and optimize the carbon coating layer generated in situ by V-MOF pyrolysis to build a continuous conductive network. Ultimately, it can reduce lithium-ion migration resistance, reduce charge-discharge polarization, improve the rate performance and long-cycle stability of the material, alleviate powder hard agglomeration, and improve powder processing performance.

[0021] Thirdly, the present invention provides a lithium-ion battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that the positive electrode comprises a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate positive electrode material as described in the first aspect.

[0022] Compared with the prior art, the advantages of the present invention are as follows: (1) This invention utilizes the in-situ coordination growth of V-MOF on the surface of LMFP to uniformly anchor the MOF precursor on the surface of LMFP particles, and then forms an LVP@C coating layer through topological transformation, achieving ultra-thin, complete, and uniform coating without free impurity particles, with high interfacial bonding strength, solving the problems of uneven coating, weak interfacial bonding, and easy phase separation and peeling during cycling in traditional ball milling coating.

[0023] (2) The LVP generated by the present invention has a NASICON-type three-dimensional lithium-ion diffusion channel, which, together with the conductive carbon network formed by the in-situ carbonization of MOF organic ligands, synergistically enhances the conduction rate of lithium ions and electrons, reduces the electrode interface impedance, and improves the rate performance and low-temperature performance of the material.

[0024] (3) The dense LVP@C coating layer of the present invention forms a physical isolation shell, which isolates the electrolyte from the erosion of the LMFP surface and inhibits the irreversible dissolution of manganese ions; at the same time, a gradient transition interface is formed between LVP and LMFP to buffer Mn 3+ The local lattice strain caused by the Jahn-Teller effect weakens the accumulation of lattice distortion during repeated charge and discharge processes, thus mitigating voltage decay during long cycles.

[0025] (4) In this invention, the organic ligands in the V-MOF are carbonized in situ to form a three-dimensional continuous porous carbon skeleton, which provides a through-type transport channel for electrons and at the same time enhances and toughens the coating layer, improves the mechanical stability of the core-shell structure, and avoids cracks or peeling due to volume expansion and contraction during cycling. Attached Figure Description

[0026] Figure 1 This is a SEM image of the uncoated lithium manganese iron phosphate cathode material in Comparative Example 1 of this invention; Figure 2This is a schematic diagram of the core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material prepared according to the present invention. Detailed Implementation

[0027] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0028] Compared with existing modification technologies, this invention relies on an integrated coating modification strategy of core-shell V-MOF-derived LVP@C to achieve multiple synergistic gains in crystal structure regulation, interface optimization, and ion dynamics enhancement. It breaks through the technical bottleneck of traditional co-coating modification and has unique technical effects and performance advantages that have not been achieved by existing technologies.

[0029] like Figure 2 As shown, firstly, a tightly bonded LVP fast ion conductor shell is formed by high-temperature topological transformation of the in-situ grown V-MOF precursor, constructing a stable core-shell heterostructure. This structure can significantly suppress lattice distortion and the Jahn-Teller effect in the LMFP system during charge-discharge cycling through physical confinement, fundamentally alleviating the problems of crystal structure pulverization and collapse. Unlike the simple physical blending and coating process of LVP and carbon materials used in existing technologies, this invention innovatively introduces in-situ transformation technology of the V-MOF precursor, abandoning the loose bonding mode of traditional external modification, and achieving a strong bonding effect between the shell and the LMFP substrate at the molecular scale.

[0030] Secondly, the continuous and dense in-situ derived LVP coating effectively isolates the electrolyte from direct corrosion of the cathode substrate, significantly suppressing the irreversible dissolution of manganese ions during cycling, and greatly improving the problems of voltage plateau decay and rapid capacity decay in lithium manganese iron phosphate materials during long-term cycling. Compared with conventional coatings that achieve basic corrosion protection and structural stability, the coatings have uneven porosity and insufficient density, and cannot effectively suppress manganese dissolution and lattice distortion under high temperature and high rate conditions. However, this invention relies on the uniform framework structure of V-MOF to form a non-porous, fully covered, and highly dense integrated protective shell after high-temperature conversion, which can achieve long-term suppression of manganese dissolution under wide temperature range and long cycle period, solving the technical pain point of continuous voltage decay over long cycle.

[0031] Meanwhile, by utilizing the ordered pore structure of the V-MOF metal-organic framework, a continuous through-type ion / electron dual transport network is formed after topological transformation, which significantly reduces the charge transfer impedance at the electrode interface, effectively improves the lithium-ion diffusion coefficient and electronic conductivity, and enables the composite material to have excellent high-rate adaptability.

[0032] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Furthermore, in the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0033] In this document, the terms “containing,” “comprising,” or “including” are open-ended expressions, meaning they include the contents specified in this invention but do not exclude other aspects.

[0034] In this document, the terms “optional,” “optionally,” or “optional” generally refer to an event or condition that may, but may not, occur, and the description includes both cases in which the event or condition occurs and cases in which the event or condition does not occur.

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.

[0036] Unless otherwise specified, all raw materials used in this invention are purchased from the market, and all purchased chemicals are used directly without purification.

[0037] Example 1 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of N,N-dimethylformamide (DMF) solution and ultrasonically dispersed for 30 min.

[0038] Add 0.25 g of vanadium acetylacetonate and 0.5 g of terephthalic acid to the above dispersion, stir to dissolve, and transfer to a 100 mL reaction vessel. React at 160 °C for 12 h using a solvothermal method. After cooling, centrifuge and wash three times alternately with DMF and ethanol. Dry under vacuum at 60 °C for 12 h to obtain the V-MOF / LMFP intermediate.

[0039] (3) Place 5.3g of V-MOF / LMFP intermediate, 0.5g of lithium carbonate and 0.2g of phosphoric acid obtained in step (2) into a tube furnace, pre-carbonize at 350 ℃ for 1 h at 1 ℃ / min under nitrogen atmosphere, then calcine at 650 ℃ for 4 h at 2 ℃ / min, cool naturally to room temperature, grind through a 200 mesh sieve to obtain LVP@C / LMFP core-shell composite cathode material.

[0040] Example 2 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0041] (2) Add 0.5 g of vanadium acetylacetonate and 1.0 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to a 100 mL reaction vessel, and react solvothermically at 160 °C for 12 h. The post-treatment is the same as in Example 1.

[0042] (3) Place 5.6g of V-MOF / LMFP intermediate, 0.6g of lithium carbonate and 0.3g of phosphoric acid obtained in step (2) into a tube furnace, pre-carbonize at 450℃ for 1.5 h at 5℃ / min under nitrogen atmosphere, then calcine at 8℃ / min to 800℃ for 12 h, cool naturally to room temperature, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell composite cathode material.

[0043] Example 3 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0044] (2) Add 0.6 g of vanadium acetylacetonate and 1.2 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to a 100 mL reaction vessel, and react solvothermically at 160 °C for 12 h. The post-treatment is the same as in Example 1.

[0045] (3) Place 5.8g of V-MOF / LMFP intermediate, 0.7g of lithium carbonate and 0.4g of phosphoric acid obtained in step (2) into a tube furnace, pre-carbonize at 450℃ for 1.5 h at 5℃ / min under nitrogen atmosphere, then calcine at 8℃ / min to 800℃ for 12 h, cool naturally to room temperature, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell composite cathode material.

[0046] Example 4 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0047] (2) Add 0.8 g of vanadium acetylacetonate and 1.6 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to a 100 mL reaction vessel, and react solvothermically at 160 °C for 12 h. The post-treatment is the same as in Example 1.

[0048] (3) Place 6.0g of V-MOF / LMFP intermediate, 0.8g of lithium carbonate and 0.5g of phosphoric acid obtained in step (2) into a tube furnace, pre-carbonize at 450℃ for 3 h at 5℃ / min under nitrogen atmosphere, then calcine at 800℃ for 12 h at 10℃ / min, cool naturally to room temperature, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell composite cathode material.

[0049] Example 5 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0050] (2) Add 0.2 g of vanadium acetylacetonate and 0.4 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to a 100 mL reaction vessel, react with solvent at 160 °C for 8 h, cool and centrifuge, wash with DMF and ethanol alternately 3 times, and vacuum dry at 60 °C for 12 h to obtain V-MOF / LMFP intermediate.

[0051] (3) The above intermediate was redispersed in 50 mL DMF, and 0.4 g vanadium acetylacetonate and 0.8 g terephthalic acid were added. The reaction was carried out at 160 °C for 12 h. After cooling, the intermediate was centrifuged and washed three times with DMF and ethanol alternately. The intermediate was dried under vacuum at 60 °C for 12 h to obtain the bilayer coated V-MOF / LMFP intermediate.

[0052] (4) Place 5.8 g of the double-layer coated V-MOF / LMFP intermediate, 0.7 g of lithium carbonate, and 0.4 g of phosphoric acid obtained in step (3) into a tube furnace for stepwise calcination and conversion: Step 1: Pre-carbonize at 400℃ for 2 hours under nitrogen atmosphere, increasing the temperature by 2℃ / min; Step 2: Switch to argon atmosphere, increase the temperature to 750℃ at 5℃ / min and calcine for 8 hours; Step 3: Rapidly cool to 500℃ at 10℃ / min, hold for 1 h, anneal, allow to cool naturally, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell composite cathode material.

[0053] Example 6 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0054] Add 0.6 g of vanadium acetylacetonate and 1.2 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to a 100 mL reaction vessel, and react solvothermically at 160 °C for 12 h. Post-treatment is the same as in Example 1.

[0055] (3) Place 5.8 g of the V-MOF / LMFP intermediate, 0.7 g of lithium carbonate, and 0.4 g of phosphoric acid obtained in step (2) into a tube furnace for stepwise calcination and conversion: Step 1: Pre-carbonize at 400 °C for 2 h under nitrogen atmosphere, increasing the temperature by 2 °C / min; Step 2: Switch to argon atmosphere, increase the temperature to 750℃ at 5℃ / min and calcine for 8 hours; Step 3: Rapidly cool to 500℃ at 10℃ / min, hold for 1 h, anneal, allow to cool naturally, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell material.

[0056] Example 7 This embodiment provides a method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Take commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) was dispersed in 50 mL of DMF and ultrasonically dispersed for 30 min.

[0057] (2) Add 0.2 g of vanadium acetylacetonate and 0.4 g of terephthalic acid to the above dispersion, stir to dissolve, transfer to 100 mL reaction vessel, react with solvent at 160 °C for 8 h, cool and centrifuge, wash with DMF and ethanol alternately 3 times, and vacuum dry at 60 °C for 12 h to obtain V-MOF / LMFP intermediate.

[0058] (3) The above intermediate was redispersed in 50 mL DMF, 0.4 g vanadium acetylacetonate and 0.8 g terephthalic acid were added, and the reaction was carried out at 160 °C for 12 h. After cooling, the intermediate was centrifuged, washed three times with DMF and ethanol alternately, and dried under vacuum at 60 °C for 12 h to obtain the bilayer coated V-MOF / LMFP intermediate.

[0059] (4) Place 5.8g of the double-layer coated V-MOF / LMFP intermediate, 0.7g of lithium carbonate and 0.4g of phosphoric acid obtained in step (3) in a tube furnace, pre-carbonize at 450℃ for 1.5 h at 5℃ / min under nitrogen atmosphere, then calcine at 800℃ for 12 h at 8℃ / min, cool naturally to room temperature, grind through a 200-mesh sieve to obtain LVP@C / LMFP core-shell material.

[0060] Comparative Example 1 This comparative example uses uncoated lithium iron phosphate cathode material with the chemical formula LiMn. 0.5 F e0.5 PO4. Its SEM image is as follows. Figure 1 As shown.

[0061] Comparative Example 2 This comparative example provides a method for preparing a non-V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, including the following steps: (1) Weigh 0.6g of acetylacetone vanadium oxide, 0.5g of glucose, 0.4g of phosphoric acid and 0.2g of lithium carbonate and dissolve them in deionized water. Then heat at 60℃ for 10 min, cool to room temperature, wash and dry to obtain LVP powder.

[0062] (2) Weigh commercial LMFP powder (LiMn) 0.5 Fe 0.55 g of PO4 (D50=300 nm) and 0.6 g of LVP powder were ground and mixed evenly in a sand mill.

[0063] (3) The mixture in step (2) was placed in a tube furnace and pre-carbonized at 450 °C for 1.5 h at 5 °C / min under a nitrogen atmosphere, and then calcined at 8 °C / min for 12 h at 800 °C. After cooling naturally to room temperature, it was ground through a 200-mesh sieve to obtain non-V-MOF derived LVP@C / LMFP core-shell material.

[0064] Comparative Example 3 This comparative example provides a method for preparing LVP@C-coated lithium manganese iron phosphate cathode material grown in situ using V-MOF, including the following steps: (1) Weigh 0.6 g of vanadium acetylacetonate and 1.2 g of terephthalic acid and dissolve them in 50 mL of DMF solution. React the mixture at 160 °C for 12 h using a solvothermal method. After cooling, centrifuge the mixture and wash it three times with DMF and ethanol alternately. Dry it under vacuum at 60 °C for 12 h to obtain V-MOF powder.

[0065] (2) Weigh commercial LMFP powder (LiMn) 0.5 Fe 0.5 5 g of PO4 (D50=300 nm) and 0.6 g of the pure V-MOF powder prepared above were placed in a sand mill and thoroughly ground and mixed to uniformly disperse the two powders, thus obtaining a powder mixture of V-MOF and LMFP mechanically blended.

[0066] (3) The mixture in step (2) was placed in a tube furnace and pre-carbonized at 450 °C for 1.5 h at 5 °C / min under a nitrogen atmosphere, and then calcined at 8 °C / min for 12 h at 800 °C. After cooling naturally to room temperature, it was ground through a 200-mesh sieve to finally obtain the non-in-situ grown LVP@C / LMFP composite cathode material.

[0067] The cathode materials prepared in Examples 1-7 and Comparative Examples 1-3 of this invention were assembled into micro-button batteries, and the same preparation process and testing conditions were used to carry out electrochemical performance testing and material structure characterization. All comparative test conditions were kept consistent to ensure that the test results were comparable and valid.

[0068] The fabrication process for micro-button batteries includes: (1) Positive electrode preparation steps: The positive electrode active materials, conductive agent (carbon black) and binder (PVDF) obtained in Examples 1-7 and Comparative Examples 1-3 are uniformly dispersed in N-methylpyrrolidone (NMP) solvent at a mass ratio of 8:1:1. The mixture is stirred in a vacuum stirring device to form a uniform, stable and non-agglomerated positive electrode slurry. The obtained positive electrode slurry is uniformly coated on the surface of aluminum foil current collector, dried to remove organic solvent, and then rolled to adjust the compaction density of the electrode. Finally, it is cut into electrodes with a diameter of 12 mm for use.

[0069] (2) Negative electrode preparation steps: Commercial graphite is used as the negative electrode active material. Graphite, conductive carbon black and sodium carboxymethyl cellulose are uniformly dispersed in deionized water at a mass ratio of 8:1:1 and stirred thoroughly to prepare a uniform negative electrode slurry. The negative electrode slurry is uniformly coated on the surface of the copper current collector, dried and rolled, and then cut into electrode sheets with a diameter of 12 mm for later use.

[0070] (3) Button cell assembly: In an anhydrous and oxygen-free argon protective glove box, the positive electrode, negative electrode, separator and electrolyte prepared above are used as assembly materials and assembled into CR2032 type button cells according to standard procedures; after assembly, the cells are left to stand for 24 hours to ensure that the electrolyte fully wets the pores of the positive and negative electrodes and eliminates the influence of the wetting difference on the electrochemical test results.

[0071] Electrochemical performance testing and material structure characterization include: (1) Rate performance test: The assembled button cell was tested for rate charge and discharge performance using the Blue Battery Test System. The test voltage range was 2.5V~4.3V. Constant current charge and discharge tests were conducted at three rates: 0.1C, 0.33C and 1C. The discharge specific capacity and capacity retention rate at different rates were recorded.

[0072] (2) Cyclic performance test: At room temperature, each embodiment and comparative example were cycled 500 times at a voltage window of 2.5~4.3V and a 1C rate, and the discharge capacity retention rate was recorded.

[0073] (3) Characterization of coating thickness and carbon content: The microstructure of each sample was characterized by transmission electron microscopy, the coating thickness of lithium manganese iron phosphate was statistically analyzed, and the coating uniformity, integrity and thickness difference under different coating processes were compared. The carbon content of each sample surface was quantitatively detected by elemental analysis.

[0074] The performance test results of each embodiment and comparative example are detailed in Table 1.

[0075] Table 1. Comparison of electrochemical performance between each example and the comparative example.

[0076] As shown in Examples 1-4, with the increase of vanadium source dosage, the coating thickness and carbon content increase simultaneously, and the 0.1C specific capacity and long-cycle capacity retention gradually increase. In Example 3, after the coating and carbon content were increased, a complete LVP / C composite protective layer was formed, and the cycle stability was significantly improved. However, when the vanadium source dosage was increased to 0.8 g (Example 4), the coating thickness and carbon content continued to increase, but the 0.1C specific capacity and cycle performance began to decline. This indicates that if the coating thickness increases and the carbon content increases, it may lead to a longer lithium-ion diffusion path, blocking the ion channels inside the LVP and reducing electrochemical performance. On the other hand, if the coating thickness is too thin and the carbon content is too low, it may lead to discontinuities in the conductive network and microscopic defects in the isolation barrier, resulting in poor electrochemical performance.

[0077] Example 5 employed a double-layer V-MOF coating combined with annealing, achieving a specific capacity of 157.15 mAh / g at 0.1C and a capacity retention of 95.8% after 500 cycles, both optimal values ​​among all samples. This demonstrates that double-layer coating effectively eliminates the microscopic gaps of single-layer coating, forming a denser protective shell; calcination combined with annealing facilitates the full conversion of the double-layer V-MOF, promoting LVP crystal form perfection and carbon network structure optimization.

[0078] Example 6 employs a single-layer V-MOF coating combined with an annealing process, achieving a 0.1C specific capacity of 155.9 mAh / g and a capacity retention of 94.2% after 500 cycles, which is lower than the performance of the double-layer V-MOF coating (Example 5). Compared to the dense and complete double-layer coating structure of Example 5, the single-layer V-MOF coating suffers from insufficient uniformity, micropores, and coating defects, failing to form a continuous and dense protective shell. During charge and discharge, the electrolyte easily erodes the LMFP matrix through the coating gaps, causing dissolution of the active material and instability of the crystal structure; simultaneously, the LVP@C conductive network constructed by the single-layer coating has poor continuity, resulting in lower lithium-ion transport and electronic conductivity efficiency.

[0079] Example 7 employed a double-layer V-MOF coating without annealing. The 0.1C specific capacity was 156.2 mAh / g, and the capacity retention after 500 cycles was 94.7%, lower than that of the double-layer V-MOF coating (Example 5). Compared to the coating-coupled annealing process of Example 5, the simple double-layer coating without annealing relaxation resulted in residual lattice stress and structural defects after high-temperature calcination. V-MOF conversion was insufficient, LVP crystal integrity was inadequate, and the carbon conductive network distribution was less uniform. Significant lattice distortion accumulated during cycling, leading to greater ion transport resistance and an inability to fully utilize the structural advantages of the dense double-layer coating. This resulted in lower reversible capacity and cycling stability compared to the annealed double-layer coating system, demonstrating that annealing can further improve the crystal structure and optimize the carbon network, synergistically enhancing electrochemical performance in conjunction with double-layer coating.

[0080] Comparative Example 1: Pure LMFP without any modification treatment has no conductive or protective shell, no fast ion conduction channels, and cannot suppress manganese dissolution. Its specific capacity and cycle retention rate are the lowest among all groups, verifying the gain effect of the modification scheme of the present invention.

[0081] Comparative Example 2 uses glucose as a single carbon source to carbon-coat LMFP, which is a traditional physical coating process. This differs fundamentally from the LVP@C composite coating structure derived in situ from a V-MOF precursor in this application, in terms of carbon source, coating mechanism, and interface structure. In the comparative example, the LVP is not derived from a V-MOF precursor, and glucose is a small-molecule carbon source. The pyrolysis process cannot achieve in-situ nucleation and chemical bonding on the LMFP surface. The coating layer only adheres to the particle surface through physical adsorption, resulting in poor coating uniformity and a tendency for carbon layer agglomeration and local accumulation, with a maximum local thickness reaching 60 nm. This leads to discontinuous coating and localized exposed defects, increasing electrode impedance and hindering lithium-ion transport, making it impossible to construct a stable and complete surface protective layer. Although Comparative Example 2 introduces both LVP and carbon components, this non-V-MOF-derived LVP@C coating layer is physically bonded to the LMFP substrate, resulting in weak interfacial bonding and uneven coating. Its 0.1C specific capacity and cycle retention are lower than those of the example, demonstrating that in-situ derivation growth has significant advantages over physical composites.

[0082] Comparative Example 3 involved the in-situ growth of V-MOF / monolayer coating, followed by the independent preparation of V-MOF and subsequent mechanical blending with LMFP to obtain a composite material. This method only involved physical coating, resulting in weak interfacial bonding, a thick coating layer (55 nm), poor continuity, and numerous defects, leading to an incomplete conductive network. During cycling, the electrolyte easily eroded the LMFP matrix, causing structural damage and hindering ion transport. The electrochemical performance was significantly worse than that of the in-situ coated sample, further demonstrating the superiority of the in-situ growth process.

[0083] The embodiments described above are some, but not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material, characterized in that, It includes a core and a shell covering the surface of the core; the core includes lithium manganese iron phosphate; the shell includes lithium vanadium phosphate and carbon; The shell is obtained by calcining a V-MOF precursor, which is grown in situ on the surface of the core.

2. The core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material according to claim 1, characterized in that, The thickness of the shell is 12~50 nm.

3. The core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material according to claim 1, characterized in that, The carbon content is 2.5 to 7.5 wt% of the total mass of the cathode material.

4. A method for preparing a core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: S1. Disperse lithium manganese iron phosphate powder in a solvent containing vanadium source and organic ligand, and carry out a solvothermal reaction to grow V-MOF precursor on the surface of lithium manganese iron phosphate to obtain V-MOF@lithium manganese iron phosphate composite intermediate. S2. The V-MOF@lithium manganese iron phosphate composite intermediate is mixed with a lithium source and a phosphorus source and calcined under an inert atmosphere to convert the V-MOF precursor into lithium vanadium phosphate and carbon, thereby obtaining the core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate material.

5. The preparation method according to claim 4, characterized in that, Step S1 further includes: redispersing the obtained V-MOF@lithium manganese iron phosphate composite intermediate in a solvent containing vanadium source and organic ligand, and performing a solvothermal reaction again to allow the V-MOF precursor to grow a second time on the surface of the composite intermediate.

6. The preparation method according to claim 5, characterized in that, The vanadium source in step S1 includes one of vanadium acetylacetonate, vanadium trichloride, or ammonium metavanadate; the organic ligand includes one of terephthalic acid, 2-aminoterephthalic acid, or trimesoic acid; and the solvent includes N,N-dimethylformamide. The lithium source in step S2 includes lithium carbonate, and the phosphorus source includes phosphoric acid.

7. The preparation method according to claim 6, characterized in that, The mass ratio of lithium manganese iron phosphate in step S1 to the total amount of vanadium source added in step S1 is 5: (0.25-0.8); the mass ratio of vanadium source in step S1 to lithium source and phosphorus source in step S2 is (0.25-0.8): (0.5-0.8): (0.2-0.5).

8. The preparation method according to claim 4, characterized in that, The calcination in step S2 specifically includes: heating to 350-450 ℃ at a rate of 1-5 ℃ / min and holding for 1-3 h, then heating to 650-800 ℃ at a rate of 2-10 ℃ / min and holding for 4-12 h.

9. The preparation method according to claim 8, characterized in that, After calcination, the process further includes: rapidly cooling to 500°C at 10°C / min, holding at that temperature for 1 hour, and then annealing.

10. A lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The cathode material comprises the core-shell V-MOF-derived LVP@C-coated lithium manganese iron phosphate cathode material as described in any one of claims 1 to 3.