A graphite anode material and its preparation method
By coating a graphite anode material with a low-temperature resin carbon layer and a Nb2O5/ZrO2 solid solution doped with Li+ transport sites, a dual-network structure is constructed, which solves the transport and stability problems of graphite anodes in low-temperature environments and achieves high-efficiency low-temperature lithium-ion battery performance.
Patent Information
- Application Number
- CN202611345840.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Graphite anode materials suffer from high lithium-ion intercalation/deintercalation barriers, slow ion transport rates, large interfacial impedance, and unstable SEI films at low temperatures, leading to battery capacity decay and poor cycle stability, which limits their application in low-temperature lithium-ion batteries.
A graphite core is used, which is sequentially coated with a low-temperature resin carbon layer and an outer layer of Nb2O5/ZrO2 solid solution doped with Li+ transport sites to construct high-speed electron channels and high-speed ion channels. A gradient dual network is formed through low-temperature processing to improve ion/electron transport efficiency and interface stability at low temperatures.
It significantly improves the low-temperature rate performance and cycle stability of graphite anodes. At -20℃, the capacity retention rate at 0.5C discharge is ≥85%, the capacity retention rate at 1C after 100 cycles is ≥90%, and the first efficiency is ≥93%. The material structure has good stability and is suitable for low-temperature lithium-ion battery applications.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of anode material technology, and more specifically, relates to a graphite anode material and its preparation method. Background Technology
[0002] Graphite is currently the mainstream choice for lithium-ion battery anode materials due to its advantages such as high specific capacity, good conductivity, and low cost. However, in low-temperature environments (such as -20°C and below), graphite suffers from problems such as high lithium-ion insertion / extraction barriers, slow ion transport rates, high interfacial impedance, unstable SEI film, and easy co-intercalation with electrolyte solvents. These issues lead to significant capacity decay, poor rate performance, and reduced cycle stability, limiting its application in the field of low-temperature lithium-ion batteries.
[0003] To improve the low-temperature performance of graphite anodes, existing technologies mostly employ coating methods using resin-carbon and metal oxide composite layers. However, these methods have significant drawbacks: First, they are mostly simple physical mixtures of resin-carbon with single or mixed oxides, failing to form a gradient functional structure and resulting in poor synergy between electron and ion transport. Second, the oxide loading is too high (5-10 wt%), easily sacrificing the specific capacity and first-efficiency of graphite. Third, they only focus on the construction of the coating structure, neglecting interface control and the design of dedicated low-temperature Li + The improvement in ion transport efficiency at low temperatures is limited due to several factors. Furthermore, some preparation processes require high-temperature treatment (>500℃), which can easily damage the graphite crystal structure and further affect material performance. Therefore, developing a graphite anode material that balances low-temperature performance, initial efficiency, and cycle stability, while also employing a mild processing method, is of great significance. Summary of the Invention
[0004] The purpose of this invention is to provide a graphite anode material and its preparation method. This invention uses graphite as a core, sequentially coating it with a low-temperature resin carbon layer and then doping it with Li. + The low-content Nb2O5 / ZrO2 solid solution outer layer of the transport sites, by constructing a dual network of "high-speed electron channels + high-speed ion channels", achieves dual high-speed ion / electron transport and interface stability at -20℃, significantly improving the low-temperature rate performance and cycle stability of graphite anodes.
[0005] To achieve the above objectives, one aspect of the present invention provides a graphite anode material, comprising: a graphite core, a resin carbon layer coated on the surface of the graphite core, and a Li-doped layer coated on the surface of the resin carbon layer. + The Nb2O5 / ZrO2 solid solution layer at the transport site.
[0006] In this invention, a graphite core is used as the host for lithium-ion insertion / extraction, ensuring the material's high specific capacity. The resin carbon layer provides a continuous conductive network, protects the graphite core from electrolyte erosion, and inhibits electrolyte solvent co-intercalation; it is doped with Li... + The Nb₂O₅ / ZrO₂ solid solution layer at the transport site provides high ionic conductivity and reduces Li₂ conductivity. + The insertion / extraction barrier guides the formation of a stable SEI film; the in-situ doped Li of this invention + The role of transport sites is to construct Li at low temperatures. + A fast transport channel further reduces interface impedance and improves ion transport efficiency.
[0007] In this invention, the graphite core refers to a core made of graphite.
[0008] According to the present invention, preferably, based on the total weight of the graphite core, the content of the Nb₂O₅ / ZrO₂ solid solution is 1-3 wt%; the content of the resin carbon layer is 3-8 wt%; and the content of Li + The content of transport sites is ≤1 wt%.
[0009] According to the present invention, preferably, the resin carbon layer is made of phenolic resin or epoxy resin by low-temperature curing and low-temperature carbonization; The low-temperature curing temperature is 120-180℃, and the low-temperature carbonization temperature is 250-300℃; The thickness of the resin carbon layer is 5-20 nm.
[0010] According to the present invention, preferably, the doped Li + In the Nb2O5 / ZrO2 solid solution layer of the transport site: The molar ratio of Nb to Zr is 1:(0.5-2). The D50 particle size of the Nb2O5 / ZrO2 solid solution is 2-5 nm; Li + The transport sites are Li2CO3 nanocrystals and / or Li3PO4 nanocrystals, wherein the Li + The particle size of the transport sites is 1-2 nm.
[0011] According to the present invention, preferably, the graphite core is natural graphite or artificial graphite; The D50 particle size of the graphite core is 8-15 μm.
[0012] Another aspect of the present invention provides a method for preparing the above-mentioned graphite anode material, the method comprising: (1) The pretreated graphite, resin and first solvent are mixed and stirred evenly, and then cured and carbonized at low temperature to form a resin carbon layer on the graphite surface to obtain resin carbon coated graphite; wherein the temperature of the low temperature curing is 120-180℃ and the temperature of the low temperature carbonization is 250-300℃. (2) Niobium source, zirconium source, lithium source, complexing agent and second solvent are mixed to form a uniform transparent sol; the resin carbon-coated graphite is added to the sol and stirred for adsorption, and then vacuum dried and low temperature heat treated to form Li doped in situ on the surface of the resin carbon layer. + The Nb2O5 / ZrO2 solid solution layer of the transport site; wherein, the low-temperature heat treatment temperature is 280-300℃.
[0013] In this invention, the preparation process (≤300℃ throughout, without high-temperature damage) is characterized by a core feature: the entire process is conducted at low temperatures (≤300℃), avoiding damage to the graphite crystal structure caused by high-temperature treatment. Simultaneously, a low-temperature sol-gel in-situ synthesis method is used to synthesize Nb₂O₅ / ZrO₂ solid solutions and Li₂O₂. + In-situ synthesis of transport sites ensures uniform coating and tight interfacial bonding, thereby improving the stability of material properties.
[0014] According to the present invention, preferably, the preparation method further includes step (3), in which the product obtained in step (2) is ball-milled and sieved to obtain a graphite anode material.
[0015] According to the present invention, preferably, the pretreated graphite is prepared by a method comprising the following steps: washing graphite with acid, then washing it with water until neutral, and drying it to obtain the pretreated graphite; Preferably, the cleaning is ultrasonic cleaning.
[0016] According to the present invention, preferably, in step (1), the resin is a phenolic resin or an epoxy resin; The first solvent is ethanol or acetone; The low-temperature curing time is 2-4 hours; The low-temperature carbonization time is 1-2 hours, and the carbonization process is carried out under nitrogen protection.
[0017] According to the present invention, preferably, in step (2), the temperature of the vacuum drying is 60-80°C; The low-temperature heat treatment process is carried out under nitrogen protection, and the low-temperature heat treatment time is 1-3 hours. The niobium source is NbCl5; the zirconium source is ZrOCl2·8H2O; the lithium source is Li2CO3 and / or Li3PO4; and the complexing agent is citric acid.
[0018] In this invention, preferably, the purity of the niobium source, zirconium source, lithium source, and complexing agent is ≥99.5%, ensuring the in-situ synthesis of Nb₂O₅ / ZrO₂ solid solution and Li + The transport sites have high purity and uniform dispersion.
[0019] The technical solution of the present invention has the following beneficial effects: (1) Novel structure and obvious differentiation: The gradient dual-functional composite coating structure is adopted, which is different from the simple physical mixing coating of the existing technology, and realizes the synergistic optimization of electron and ion transport; (2) Excellent low-temperature performance: through Nb2O5 / ZrO2 solid solution and Li + The synergistic effect of transport sites significantly reduces Li at low temperatures. + Intercalation / deintercalation barrier and interface impedance; capacity retention ≥85% at -20℃ with 0.5C discharge; capacity retention ≥90% after 100 cycles at 1C. (3) Balancing initial efficiency and capacity: Low content (1-3wt%) Nb2O5 / ZrO2 solid solution loading avoids the sacrifice of graphite capacity by high oxide content, with an initial efficiency ≥93%; (4) The process is mild and the cost is controllable: the entire preparation temperature is ≤300℃, no high temperature treatment is required, the graphite structure is avoided, the process is simple and the energy consumption is low, which is suitable for industrial production; (5) Good stability: The gradient double-layer structure inhibits electrolyte solvent co-intercalation, stabilizes the SEI film, improves the cycle stability and service life of the material, and can be widely used in the field of low-temperature lithium-ion batteries.
[0020] Other features and advantages of the present invention will be described in detail in the following detailed description section. Detailed Implementation
[0021] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0022] The present invention is further illustrated by the following examples: In the following embodiments and comparative examples: the performance tests were conducted under the same conditions: the prepared graphite anode material was used as the working electrode, lithium metal as the counter electrode, the electrolyte was 1 mol / L LiPF6-EC / DMC / EMC (volume ratio 1:1:1), the separator was Celgard 2400 from Celgard, LLC, and CR2032 coin cells were assembled for performance testing; specifically, the working electrode was: a negative electrode slurry (area density of 95±5 g / m³) composed of the anode material prepared in the following embodiments and comparative examples, conductive agent SP, CMC, SBR, and deionized water was coated on the upper surface of copper foil. 2 The working electrode is obtained by drying; in the negative electrode slurry, the mass ratio of negative electrode material, conductive agent SP, CMC and SBR is 95:1:1.5:2.5.
[0023] Initial efficiency test: Under 25℃ ambient conditions, charge at a constant current of 0.1C to 0.005V, then charge at a constant voltage until the current drops to 0.01C, and let stand for 30 minutes; then discharge at a constant current of 0.1C to 2.0V; Initial efficiency = Initial discharge capacity / Initial charge capacity 100%.
[0024] Low-temperature rate performance test: At 25℃, the battery was charged at a constant current of 0.1C to 0.005V, then charged at a constant voltage until the current dropped to 0.01C, and left to stand for 30 minutes. After that, the battery was placed in a -20℃ low-temperature constant temperature chamber for 4 hours. At -20℃, the battery was discharged at a constant current of 0.5C, 1C, and 2C to 2.0V, and the discharge capacity at each rate was recorded. The 0.5C capacity retention rate at -20℃ was calculated based on the 0.5C discharge capacity at 25℃. The 2C / 0.5C capacity ratio is the ratio of the 2C discharge capacity at -20℃ to the 0.5C discharge capacity at -20℃.
[0025] Low-temperature cycle performance test: The battery was placed in a -20℃ low-temperature constant temperature chamber for 4 hours; it was charged at 1C constant current to 0.005V at -20℃, then charged at constant voltage until the current dropped to 0.01C, and left to stand for 30 minutes; then it was discharged at 1C constant current to 2.0V to complete one charge-discharge cycle; the above charge-discharge process was repeated for a total of 100 cycles; the capacity retention rate after 100 cycles was calculated based on the first 1C discharge capacity at -20℃.
[0026] Interfacial impedance testing: AC impedance (EIS) testing was conducted using an electrochemical workstation at -20℃. The test amplitude was 5mV, and the scanning frequency range was 100kHz to 0.01Hz. The interfacial impedance values corresponding to the high-frequency semicircular real axis intercept in the impedance spectrum were extracted.
[0027] Example 1 (1) Graphite pretreatment: Take artificial graphite with a D50 particle size of 10.0 μm, ultrasonically clean it with 0.5 mol / L dilute hydrochloric acid for 10 min (ultrasonic power 300 W), rinse it with deionized water until neutral (pH=6.8–7.2), and vacuum dry it at 60℃ for 2 h to obtain pretreated graphite; (2) Inner layer resin coating: 100g of pretreated graphite, 5g of phenolic resin (softening point 85℃, solid content 98%), and 50mL of anhydrous ethanol were mixed and stirred at 300r / min for 30 min until the system was uniform. The mixture was cured at 150℃ and normal pressure for 3h, and then carbonized at 280℃ for 1.5h under nitrogen protection (nitrogen flow rate 50 mL / min). The mixture was then naturally cooled to room temperature to obtain resin carbon coated graphite (resin carbon content 5wt% based on the total weight of the graphite core, resin carbon layer thickness 12nm). (3) Outer coating + doping: 2.5g NbCl5 (purity 99.9%), 2.0g ZrOCl2·8H2O (purity 99.5%), 0.5g Li2CO3 (purity 99.8%), and 3g citric acid (purity 99.5%) were added to 40 mL of deionized water and stirred at 80℃ and 200r / min for 30 min until a uniform and transparent sol was formed; the resin carbon-coated graphite obtained in step (2) was added to the sol and stirred at 25℃ and 300r / min for 2 h for adsorption, and then vacuum dried at 60℃ for 4 h (gauge pressure -0.08 MPa). Subsequently, it was heat-treated at 290℃ for 2 h under nitrogen protection (nitrogen flow rate 50 mL / min) and naturally cooled to room temperature to form Li doped in situ. + The Nb₂O₅ / ZrO₂ solid solution layer at the transport sites (doped with Li based on the total weight of the graphite core) + In the Nb₂O₅ / ZrO₂ solid solution layer of the transport sites: the content of Nb₂O₅ / ZrO₂ solid solution is 2 wt%, the molar ratio of Nb to Zr is 1:1, and the D50 particle size of the Nb₂O₅ / ZrO₂ solid solution is 3 nm; the content of Li₂CO₃ transport sites (Li₂CO₃ nanocrystals) is 0.5 wt%, and the particle size of Li₂CO₃ transport sites is 1-2 nm. (4) Post-processing: The above product is ball-milled for 10 min using a planetary ball mill (300 r / min, ball-to-material ratio 5:1), and sieved to a D50 particle size of 10.2 μm to obtain the final low-temperature high-rate graphite anode material.
[0028] The above-mentioned coin electrode, using the negative electrode material prepared in this embodiment as the working electrode active material, was subjected to performance testing. The specific results are shown in Table 1.
[0029] Comparative Example 1 The only difference between this comparative example and Example 1 is that the outer coating and doping in step (3) are removed; the resin carbon-coated graphite prepared in step (2) is ball-milled for 10 minutes using a planetary ball mill (300 r / min, ball-to-material ratio 5:1), and sieved to a D50 particle size of 10.2 μm to obtain the final graphite anode material.
[0030] The above-mentioned coin electrode, using the negative electrode material prepared in this comparative example as the working electrode active material, was subjected to performance testing. The specific results are shown in Table 1.
[0031] Comparative Example 2 (1) Graphite pretreatment: Same as in Example 1; (2) Inner layer resin coating: Same as in Example 1; (3) Physical mixing treatment of outer layer: Take Nb2O5 powder and ZrO2 powder with the same particle size as in Example 1 (both are 3nm, Nb and Zr molar ratio is 1:1), add them directly to the resin carbon coated graphite powder obtained in step (2) in a solid phase mixing amount of 2wt% relative to the total weight of the graphite core; This comparative example does not add lithium source Li2CO3, does not prepare sol, and does not perform sol adsorption and in-situ heat treatment to generate solid solution; After uniform mixing, the powder intermediate product is obtained.
[0032] (4) Post-processing: The above powder intermediate product was ball-milled for 10 min using a planetary ball mill (300 r / min, ball-to-material ratio 5:1), and large agglomerated particles were removed by sieving to obtain graphite anode material with a D50 particle size of 10.2 μm.
[0033] The above-mentioned coin electrode, using the negative electrode material prepared in this comparative example as the working electrode active material, was subjected to performance testing. The specific results are shown in Table 1.
[0034] Example 2 (1) Graphite pretreatment: Take natural graphite with a D50 particle size of 11.0 μm, ultrasonically clean it with 0.3 mol / L dilute sulfuric acid for 15 min (ultrasonic power 300 W), rinse it with deionized water until neutral (pH=6.8–7.2), and vacuum dry it at 70℃ for 2 h to obtain pretreated graphite; (2) Inner layer resin coating: 100g of pretreated graphite, 3g of epoxy resin (epoxy value 0.51, solid content 98%), and 40 mL of acetone were mixed and stirred at 300 r / min for 30 min until the system was uniform. The mixture was cured at 120℃ and normal pressure for 4 h, and then carbonized at 250℃ for 2 h under nitrogen protection (nitrogen flow rate 50 mL / min). The mixture was then naturally cooled to room temperature to obtain resin carbon coated graphite (resin carbon content 3 wt% based on the total weight of the graphite core, and resin carbon layer thickness 5 nm). (3) Outer coating + doping: 1.2 g NbCl5, 1.6 g ZrOCl2·8H2O (Nb:Zr molar ratio 1:2), 0.3 g Li2CO3, and 2 g citric acid were added to 35 mL of deionized water and stirred at 70℃ and 200 r / min for 40 min until a uniform and transparent sol was formed; the resin carbon-coated graphite obtained in step (2) was added to the sol and stirred at 25℃ and 300 r / min for 2.5 h for adsorption, and then vacuum dried at 70℃ for 3 h (gauge pressure -0.08 MPa). Subsequently, it was heat-treated at 280℃ for 3 h under nitrogen protection (nitrogen flow rate 50 mL / min) and naturally cooled to room temperature to form Li doped in situ. + The Nb₂O₅ / ZrO₂ solid solution layer at the transport sites (doped with Li based on the total weight of the graphite core) + In the Nb₂O₅ / ZrO₂ solid solution layer of the transport sites: the content of Nb₂O₅ / ZrO₂ solid solution is 1 wt%, the molar ratio of Nb to Zr is 1:2, and the D50 particle size of the Nb₂O₅ / ZrO₂ solid solution is 2 nm; the content of Li₂CO₃ transport sites (Li₂CO₃ nanocrystals) is 0.3 wt%, and the particle size of Li₂CO₃ transport sites is 1-2 nm. (4) Post-processing: The above product was ball-milled for 8 min using a planetary ball mill (300 r / min, ball-to-material ratio 5:1), and sieved to a D50 particle size of 11.3 μm to obtain the final low-temperature high-rate graphite anode material.
[0035] The above-mentioned coin electrode, using the negative electrode material prepared in this embodiment as the working electrode active material, was subjected to performance testing. The specific results are shown in Table 1.
[0036] Example 3 (1) Graphite pretreatment: Take artificial graphite with a D50 particle size of 9.5 μm, ultrasonically clean it with 0.6 mol / L dilute nitric acid for 8 min (ultrasonic power 300 W), rinse it with deionized water until neutral (pH=6.8–7.2), and vacuum dry it at 80℃ for 1.5 h to obtain pretreated graphite; (2) Inner layer resin coating: 100 g of pretreated graphite, 8 g of phenolic resin (softening point 85℃, solid content 98%), and 60 mL of anhydrous ethanol were mixed and stirred at 300 r / min for 30 min until the system was uniform. The mixture was cured at 180℃ and normal pressure for 2 h, and then carbonized at 300℃ for 1 h under nitrogen protection (nitrogen flow rate 50 mL / min). The mixture was then naturally cooled to room temperature to obtain resin carbon coated graphite (resin carbon content 8 wt% based on the total weight of the graphite core, and resin carbon layer thickness 20 nm). (3) Outer coating + doping: 4.8 g NbCl5, 2.4 g ZrOCl2·8H2O (Nb:Zr molar ratio 1:0.5), 1.0 g Li2CO3, and 4 g citric acid were added to 45 mL of deionized water and stirred at 80℃ and 200 r / min for 25 min until a uniform and transparent sol was formed; the resin carbon-coated graphite obtained in step (2) was added to the sol and stirred at 25℃ and 300 r / min for 1.5 h for adsorption, and then vacuum dried at 80℃ for 2.5 h (gauge pressure -0.08 MPa). Subsequently, it was heat-treated at 300℃ for 1 h under nitrogen protection (nitrogen flow rate 50 mL / min) and naturally cooled to room temperature to form Li doped in situ. + The Nb₂O₅ / ZrO₂ solid solution layer at the transport sites (doped with Li based on the total weight of the graphite core) + In the Nb₂O₅ / ZrO₂ solid solution layer at the transport site: the content of Nb₂O₅ / ZrO₂ solid solution is 3wt%, the molar ratio of Nb to Zr is 1:0.5, the D50 particle size of the Nb₂O₅ / ZrO₂ solid solution is 5nm, and Li + The content of transport sites (Li₂CO₃ nanocrystals) is 1.0 wt%, Li + The particle size of the transport sites is 1-2 nm. (4) Post-processing: The above product was ball-milled for 12 min using a planetary ball mill (300 r / min, ball-to-material ratio 5:1), and sieved to a D50 particle size of 9.7 μm to obtain the final low-temperature high-rate graphite anode material.
[0037] The above-mentioned coin electrode, using the negative electrode material prepared in this embodiment as the working electrode active material, was subjected to performance testing. The specific results are shown in Table 1.
[0038] Table 1 Test Data Table
[0039] As shown in Table 1, the low-temperature performance (rate and cycle) and interfacial impedance of the materials in Examples 1-3 of the present invention are significantly better than those in Comparative Examples 1 and 2, with Example 1 exhibiting the best overall performance. Furthermore, Examples 1-3, by specifying different solid solution contents, resin carbon contents, and Nb to Zr molar ratios, all achieved excellent low-temperature performance, demonstrating that the gradient bifunctional composite coating structure and preparation method of the present invention can effectively improve the low-temperature performance of graphite anodes.
[0040] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A graphite anode material, characterized in that, The graphite anode material comprises: a graphite core, a resin carbon layer coating the surface of the graphite core, and a Li-doped layer coating the surface of the resin carbon layer. + The Nb2O5 / ZrO2 solid solution layer at the transport site.
2. The graphite anode material according to claim 1, wherein, Based on the total weight of the graphite core, the content of Nb2O5 / ZrO2 solid solution is 1-3 wt%; the content of resin carbon layer is 3-8 wt%; and Li + The content of transport sites is ≤1 wt%.
3. The graphite anode material according to claim 1, wherein, The resin carbon layer is made of phenolic resin or epoxy resin through low-temperature curing and low-temperature carbonization. The low-temperature curing temperature is 120-180℃, and the low-temperature carbonization temperature is 250-300℃; The thickness of the resin carbon layer is 5-20 nm.
4. The graphite anode material according to claim 1, wherein, The Li-doped + In the Nb2O5 / ZrO2 solid solution layer of the transport site: The molar ratio of Nb to Zr is 1:(0.5-2). The D50 particle size of the Nb2O5 / ZrO2 solid solution is 2-5 nm; Li + The transport sites are Li2CO3 nanocrystals and / or Li3PO4 nanocrystals, wherein the Li + The particle size of the transport sites is 1-2 nm.
5. The graphite anode material according to claim 1, wherein, The graphite core is either natural graphite or artificial graphite. The D50 particle size of the graphite core is 8-15 μm.
6. The method for preparing the graphite anode material according to any one of claims 1-5, characterized in that, The preparation method includes: (1) The pretreated graphite, resin and first solvent are mixed and stirred evenly, and then cured and carbonized at low temperature to form a resin carbon layer on the graphite surface to obtain resin carbon coated graphite; wherein the temperature of the low temperature curing is 120-180℃ and the temperature of the low temperature carbonization is 250-300℃. (2) Niobium source, zirconium source, lithium source, complexing agent and second solvent are mixed to form a uniform transparent sol; the resin carbon-coated graphite is added to the sol and stirred for adsorption, and then vacuum dried and low temperature heat treated to form Li doped in situ on the surface of the resin carbon layer. + The Nb2O5 / ZrO2 solid solution layer of the transport site; wherein, the low-temperature heat treatment temperature is 280-300℃.
7. The preparation method according to claim 6, wherein, The preparation method further includes step (3), in which the product obtained in step (2) is ball-milled and sieved to obtain a graphite anode material.
8. The preparation method according to claim 6, wherein, The pretreated graphite is prepared by a method comprising the following steps: cleaning the graphite with acid, then washing it with water until neutral, and drying it to obtain the pretreated graphite. Preferably, the cleaning is ultrasonic cleaning.
9. The preparation method according to claim 6, wherein, In step (1), the resin is phenolic resin or epoxy resin; The first solvent is ethanol or acetone; The low-temperature curing time is 2-4 hours; The low-temperature carbonization time is 1-2 hours, and the carbonization process is carried out under nitrogen protection.
10. The preparation method according to claim 6, wherein, In step (2), the temperature of the vacuum drying is 60-80℃; The low-temperature heat treatment process is carried out under nitrogen protection, and the low-temperature heat treatment time is 1-3 hours. The niobium source is NbCl5; the zirconium source is ZrOCl2·8H2O; the lithium source is Li2CO3 and / or Li3PO4; and the complexing agent is citric acid.