A method for preparing an oxygen ion conductor-modified lithium-rich manganese-based cathode material and its application

By constructing a eutectic phase structure of lithium-rich manganese-based cathode material modified with oxygen ion conductor, the problems of insufficient anion kinetic performance and structural instability were solved, and the performance of lithium-ion battery cathode material with high specific energy and long life was improved.

CN123120690APending Publication Date: 2026-11-17XIAN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611352447.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Lithium-rich manganese-based cathode materials suffer from problems such as low coulombic efficiency in the first cycle, rapid voltage decay during cycling, and large electrochemical polarization, which lead to capacity degradation and low electronic conductivity, affecting their rate performance.

Method used

By constructing an oxygen ion conductor-modified lithium-rich manganese-based cathode material, a ball milling method combined with a low-temperature calcination process was used to composite the oxygen ion conductor La4Mn5Si4O22 with a lithium-rich manganese-based substrate oxide to form a eutectic phase structure, which promotes oxygen ion transport and inhibits irreversible phase transition.

Benefits of technology

The discharge specific capacity and cycle stability of the material were significantly improved. The capacity reached 314.31 mAh/g in the first cycle, the capacity retention rate reached 97.83% after 100 cycles, the retention rate reached 96.01% after 1 C cycle, and the voltage decay was reduced to 1.051 mV/cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120690A_ABST
    Figure CN123120690A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an oxygen-ion conductor-modified lithium-rich manganese-based cathode material and its application. The preparation method includes the following steps: dissolving a lithium source, a nickel source, a cobalt source, and a manganese source in water to obtain a precursor solution; preparing precursor powder using a high-temperature spray drying method; then performing high-temperature sintering to obtain a lithium-rich manganese-based material; ball milling and mixing the oxygen-ion conductor precursor and the lithium-rich manganese material; and finally obtaining the oxygen-ion conductor-modified lithium-rich manganese cathode material under different sintering conditions. This invention constructs a novel eutectic phase composite structure, organically combining the oxygen-ion conductor with the lithium-rich manganese-based cathode material to form a highly efficient oxygen ion rapid migration channel. This structure can significantly improve the anion redox kinetics performance of the material and enhance structural stability. Ultimately, the obtained cathode material exhibits both high specific capacity and excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion batteries, specifically relating to a method for preparing an oxygen-ion conductor modified lithium-rich manganese-based cathode material and its application. Background Technology

[0002] With the development of "energy transformation" and the proposal of "dual carbon" goals, the new energy industry is booming. In terms of manufacturing industrial policies, new energy vehicles have been listed as a key development area, and lithium-ion batteries are the mainstream power batteries in this field. In recent years, the country has vigorously promoted the reform of the automotive industry, greatly stimulating the progress of the electric vehicle industry and enabling China's electric vehicle industry to flourish. Lithium-ion batteries, as an energy storage device integrating high energy density, long cycle life, and environmental friendliness, have rapidly penetrated into multiple key areas such as electric vehicles, portable smart devices, and aerospace since their successful commercialization, becoming an integral part of modern society and greatly impacting our lives. From small portable consumer devices to large-scale automotive power systems and grid energy storage systems, lithium-ion batteries are gradually meeting the increasingly diverse energy storage and supply needs. In commercialized lithium-ion batteries, the cost of cathode materials accounts for more than 30% and is closely related to the battery's energy density and cycle life. Developing low-cost, high-energy-density, and long-life lithium-ion battery cathode materials is currently a research hotspot in academia and industry. Among lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, ternary materials, and lithium-rich manganese-based cathode materials, lithium-rich manganese-based morphological oxides have the advantages of low cost and high specific capacity, and have the potential to become the cathode material for the next generation of high-energy-density lithium-ion batteries.

[0003] Lithium-rich manganese-based solid solution (xLiMO2·(1-x)Li2MnO3, where M is a transition metal such as Ni, Co, or Mn, LRMO) is a rapidly developing cathode material in recent years, possessing advantages such as high specific capacity (up to 300 mAh / g) and low cost, making it a cathode material with great application potential. Unlike other cathode materials, the ultra-high specific capacity of lithium-rich manganese-based solid solution materials is attributed to an additional anion charge compensation mechanism, namely O 2- Directly participating in redox reactions significantly improves the specific capacity and energy density of materials. However, lithium-rich manganese-based materials suffer from low initial coulombic efficiency, rapid voltage decay during cycling, and large electrochemical polarization, leading to capacity degradation. Furthermore, the low electronic conductivity of lithium-rich manganese-based materials results in poor rate performance, thus affecting their fast-charging performance. Therefore, modifying lithium-rich manganese-based materials to improve their initial coulombic efficiency, suppress voltage decay, and enhance cycle capacity and rate performance has become a crucial issue that urgently needs to be addressed.

[0004] In recent years, oxygen ion conductors have attracted widespread attention due to their rich intrinsic oxygen vacancies with high oxygen adsorption and storage capacity, as well as their low oxygen ion migration barrier. Introducing oxygen ion conductors into lithium-rich manganese-based oxides can form novel eutectic phase structures, potentially creating efficient oxygen ion transport channels at the interface and thus improving the anion dynamics performance of lithium-rich manganese-based cathode materials. However, how to efficiently composite oxygen ion conductors with lithium-rich manganese-based layered oxides through controllable processes and clarify their structure-property relationship remains a significant challenge. Summary of the Invention

[0005] This invention provides a method for preparing an oxygen ion conductor modified lithium-rich manganese-based cathode material and its application. By constructing a novel eutectic phase structure, the method solves problems such as insufficient anion kinetic performance and structural instability, thereby improving the discharge specific capacity and cycle stability of the battery.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing an oxygen ion conductor-modified lithium-rich manganese-based cathode material includes the following steps: Step 1: Dissolve lithium source, nickel source, cobalt source and manganese source in water according to the molar ratio of Li:Ni:Co:Mn=1.53:0.165:0.165:0.665, and add complexing agent to obtain precursor solution; Step 2: The precursor solution is prepared into precursor powder by high-temperature spray drying; then the precursor powder is sintered at 1000℃ for 20 minutes to obtain lithium-rich manganese cathode powder material. Step 3: Combine the lithium-rich manganese cathode material obtained in Step 1 with the oxygen ion conductor La4Mn5Si4O 22 The precursor material was placed in a ball mill jar at a molar ratio of 1:0.01; Step 4: The ball mill jar containing lithium-rich manganese powder and oxygen ion conductor is subjected to ball milling, with ethanol added as a dispersant during the ball milling process. Step 5: The ball-milled lithium-rich manganese cathode material and the oxygen ion conductor mixture are sintered in a muffle furnace at a temperature of 250℃~450℃ for 3 hours. After natural cooling, the oxygen ion conductor modified lithium-rich manganese-based cathode material is obtained.

[0007] Furthermore, the lithium source, nickel source, cobalt source, and manganese source are lithium acetate, nickel acetate, cobalt acetate, and manganese acetate, respectively, and the total concentration in the precursor solution is 0.15 mol / L.

[0008] Furthermore, in step one, the complexing agent is citric acid monohydrate, and the concentration of the complexing agent is 0.3 mol / L.

[0009] Furthermore, in step two, the inlet temperature of the spray dryer is 230℃, the outlet temperature is 115℃, the peristaltic pump speed is 600~800mL / h, the needle frequency is 25Hz, and the spray pressure is 0.1~0.5MPa; the atmosphere for spray drying is one or more of air and oxygen.

[0010] Furthermore, in step three, the molar ratio of lithium-rich manganese cathode material to oxygen ion conductor is 1:0.01.

[0011] Furthermore, in step four, the ball milling conditions are 400 rpm for 6 hours.

[0012] Furthermore, in step five, the ball-milled lithium-rich manganese cathode material and the oxygen ion conductor mixture are sintered at a heating rate of 5°C / min and a calcination temperature of 350°C for 3 hours.

[0013] Furthermore, in step three, the oxygen ion conductor La4Mn5Si4O 22 The precursor materials are lanthanum oxide, manganese oxide, and silicon oxide.

[0014] Application of the oxygen ion conductor modified lithium-rich manganese-based cathode material prepared by the above method in the cathode of lithium-ion batteries.

[0015] Furthermore, at a high voltage of 4.8 V, the initial discharge capacity at 0.1 C reached 314.31 mAh / g, and the capacity retention rate after 100 cycles reached 97.83%; the initial discharge capacity at 1 C was 239.39 mAh / g, and the retention rate after 600 long cycles reached 96.01%. At the same time, the average voltage decay during cycling decreased to 1.051 mV / cycle, demonstrating a significant improvement in structural stability.

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses ball milling combined with calcination to modify lithium-rich manganese-based cathode materials. This process is simple to operate and easy to scale up. Specifically, the ball milling process mixes the oxygen ion conductor precursor with the lithium-rich manganese-based material in an ethanol solution through mechanical energy to achieve uniform dispersion and effectively avoid agglomeration. At the same time, the high-energy collisions during the ball milling process can introduce defect sites on the particle surface, promoting the interfacial solid-phase reaction in the subsequent calcination stage. The subsequent calcination temperature is controlled in the range of 250-450℃, which is much lower than the traditional high-temperature sintering (≥800℃), significantly reducing energy consumption and avoiding the risk of excessive grain growth or irreversible phase transformation at high temperatures.

[0017] (2) This invention successfully constructed a novel eutectic phase structure on the surface and interface of lithium-rich manganese-based cathode materials. Oxygen ion conductor La4Mn5Si4O 22By utilizing its inherent oxygen vacancies, the active surface lattice oxygen is significantly suppressed, effectively curbing oxygen release during deep delithiation and promoting highly reversible anionic redox reactions. Simultaneously, the introduction of the oxygen ion conductor modulates the local coordination environment, lowers the oxygen ion migration barrier, and activates more anions to participate in charge compensation. This eutectic phase structure also effectively suppresses irreversible phase transitions during cycling, preventing layered structure collapse and overall performance degradation, ultimately achieving excellent comprehensive electrochemical performance. This eutectic phase structure consists of the oxygen ion conductor La4Mn5Si4O 22 The eutectic phase is formed by matching the lattice of lithium-rich manganese-based layered oxides, exhibiting a coherent or semi-coherent interface at the atomic scale. This structural design brings two core advantages: First, the abundant intrinsic oxygen vacancies in the eutectic structure form efficient channels for rapid oxygen ion migration, significantly reducing the migration energy barrier for oxygen ions, thereby greatly enhancing the anion redox kinetics of lithium-rich manganese-based cathode materials. Second, the eutectic structure effectively suppresses the dissolution and migration of transition metal ions during cycling. Traditional lithium-rich manganese-based materials are prone to irreversible phase transitions from layered structures to spinel / rock salt phases under high pressure, leading to rapid capacity and voltage decay. However, the eutectic structure constructed in this invention significantly suppresses this phase transition through the capture of active oxygen by interfacial oxygen vacancies and the uniform distribution of lattice stress.

[0018] (3) The modified material of this invention exhibits excellent electrochemical performance under high voltage conditions (4.8 V). The initial discharge specific capacity at 0.1 C rate is as high as 314.31 mAh / g, and the capacity retention rate reaches 97.83% after 100 cycles; the initial capacity at 1 C rate is 239.39 mAh / g, and the retention rate reaches 96.01% after 600 long cycles. At the same time, the average voltage decay during cycling is reduced to 1.051 mV / cycle, which proves the significant improvement in structural stability.

[0019] In summary, this invention successfully constructed a eutectic phase structure through a simple ball milling method combined with a calcination process, achieving a synergistic enhancement of the anion dynamics performance and structural stability of lithium-rich manganese-based cathode materials, and providing a practical and feasible technical path for developing high-energy-density and long-life lithium-ion battery cathode materials. Attached Figure Description

[0020] Figure 1 X-ray diffraction data of lithium-rich manganese-based cathode materials prepared in Examples 1-3 and Comparative Example 1; Figure 2 The image shows the elemental distribution data obtained by electron microscopy for the lithium-rich manganese-based cathode material prepared in Example 2. Figure 3 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 1 at 0.1C. Figure 4The data for the first charge-discharge curve of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 1 at 0.1C; Figure 5 The data for the first charge-discharge curve of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 2 at 0.1C; Figure 6 The data for the first charge-discharge curve of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 3 at 0.1C; Figure 7 The data for the first charge-discharge curve of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 2 at 0.1C. Figure 8 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 3 at 0.1C. Figure 9 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 4 at 0.1C. Figure 10 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 5 at 0.1C. Figure 11 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 6 at 0.1C. Figure 12 The first charge-discharge curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 7 at 0.1C. Figure 13 Data on the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 1 at 0.1C for 100 cycles; Figure 14 The data for the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 1 after 100 cycles at 0.1C are shown. Figure 15 The data for the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 2 after 100 cycles at 0.1C are shown. Figure 16 The data for the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 3 after 100 cycles at 0.1C are shown. Figure 17 Data on the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 2 at 0.1C for 100 cycles; Figure 18 Data on the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 4 at 0.1C for 100 cycles; Figure 19 Data on the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 5 at 0.1C for 100 cycles; Figure 20Electrochemical performance cycling data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 1 at 1C for 600 cycles. Figure 21 The data are the electrochemical performance cycle curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 1 at 1C for 600 cycles. Figure 22 The data are the electrochemical performance cycle curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 2 at 1C for 600 cycles. Figure 23 The data are the electrochemical performance cycle curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 3 at 1C for 600 cycles. Figure 24 Electrochemical performance cycling data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 2 at 1C for 600 cycles. Figure 25 Electrochemical performance cycling data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 4 at 1C for 600 cycles. Figure 26 Electrochemical performance cycling data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 5 at 1C for 600 cycles; Figure 27 The average voltage decay curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 1 at 1C for 600 cycles of electrochemical performance. Figure 28 The average voltage decay curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 1 under 600 cycles of electrochemical performance at 1C. Figure 29 The data are the average voltage decay curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 2, after 600 cycles of electrochemical performance at 1C. Figure 30 The data shows the average voltage decay curve of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 3 at 1C for 600 cycles of electrochemical performance. Figure 31 The average voltage decay curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 2 under 600 cycles of electrochemical performance at 1C. Figure 32 The average voltage decay curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 4 under 600 cycles of electrochemical performance at 1C. Figure 33 The average voltage decay curve data of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 5 under 600 cycles of electrochemical performance at 1C. Figure 34Cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Comparative Example 1 under different rate conditions (0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C); Figure 35 The data are the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 1 under different rate conditions (0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C). Figure 36 The data are the cycling curves of the lithium-rich manganese-based cathode material assembled in Example 2 under different rate conditions (0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C). Figure 37 The data shows the cycling curves of the battery assembled with the lithium-rich manganese-based cathode material prepared in Example 3 under different rate conditions (0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C). Figure 38 The images are scanning electron microscope (SEM) images of the lithium-rich manganese-based cathode material prepared in Comparative Example 1 before cycling and after cycling 600 times at 1C. Figure 39 The images are scanning electron microscope (SEM) images of the lithium-rich manganese-based cathode material prepared in Example 2 before cycling and after cycling 600 times at 1C. Figure 40 Transmission electron microscopy (TEM) images of the lithium-rich manganese-based cathode materials assembled in Comparative Example 1 and Example 2 after 600 cycles at 1C. Detailed Implementation

[0021] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0022] This invention uses lithium-rich manganese cathode material with specific elemental composition, and introduces oxygen ion conductors through ball milling and calcination processes. By controlling the calcination temperature of the oxygen ion conductors, the structure of the lithium-rich manganese-based cathode material is modified.

[0023] Example 1

[0024] Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this embodiment, the oxygen ion conductor precursor is La4Mn5Si4O. 22 It is prepared from lanthanum oxide, manganese oxide and silicon oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 250°C and a heating rate of 5°C / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LMSO-250.

[0025] Example 2

[0026] The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1, the main difference being that the calcination temperature in step seven is adjusted to 350 ℃. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this embodiment, the oxygen ion conductor precursor is La4Mn5Si4O. 22 It is prepared from lanthanum oxide, manganese oxide and silicon oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 350℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LMSO-350.

[0027] Example 3

[0028] The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1, the main difference being that the calcination temperature in step seven is adjusted to 450 ℃. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this embodiment, the oxygen ion conductor precursor is La4Mn5Si4O. 22 It is prepared from lanthanum oxide, manganese oxide and silicon oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 450℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LMSO-450.

[0029] Comparative Example 1 The preparation process is basically the same as in Example 1, except that oxygen ion conductor modification was not performed (i.e., no oxygen ion conductor precursor was added, and the subsequent ball milling and low-temperature calcination steps were not performed). The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained, which is denoted as LRMO. Comparative Example 2 The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1. The main difference is that the oxygen ion conductor precursor used is Zr. 0.92 Sr 0.08 O2 (prepared from zirconium dioxide and strontium oxide); and the calcination temperature in step seven is 350 ℃, the heating rate is 5 ℃ / min, and the calcination time is 3 hours. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this comparative example, the oxygen ion conductor precursor is Zr. 0.92 Sr 0.08 O2 is prepared from zirconium dioxide and strontium oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 350℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LZSO-350.

[0030] Comparative Example 3 The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1. The main difference is that the oxygen ion conductor precursor used is Rb5BiMo4O. 16 (Prepared from rubidium carbonate, bismuth trioxide, and molybdenum oxide); and the calcination temperature in step seven is 350 ℃, the heating rate is 5 ℃ / min, and the calcination time is 3 hours. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this comparative example, the oxygen ion conductor precursor is Rb5BiMo4O. 16 It is prepared from rubidium carbonate, bismuth trioxide and molybdenum oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 350℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LRBO-350.

[0031] Comparative Example 4 The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1. The main difference is that the oxygen ion conductor precursor used is Rb5BiMo4O. 16 (Prepared from rubidium carbonate, bismuth trioxide, and molybdenum oxide); and the calcination temperature in step seven is 400 ℃, the heating rate is 5 ℃ / min, and the calcination time is 3 hours. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this comparative example, the oxygen ion conductor precursor is Rb5BiMo4O. 16 It is prepared from rubidium carbonate, bismuth trioxide and molybdenum oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 400℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LRBO-400.

[0032] Comparative Example 5 The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1. The main difference is that the oxygen ion conductor precursor used is Pr2Ni. 0.8 Mo 0.2 O4 (prepared from praseodymium nitrate, nickel oxide, and molybdenum oxide); and the calcination temperature in step seven is 300 ℃, the heating rate is 5 ℃ / min, and the calcination time is 3 hours. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this comparative example, the oxygen ion conductor precursor is Pr₂Ni. 0.8 Mo 0.2 O4 is prepared from praseodymium nitrate, nickel oxide, and molybdenum oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LPNO-300.

[0033] Comparative Example 6 The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1. The main difference is that the oxygen ion conductor precursor used is Pr2Ni. 0.8 Mo 0.2 O4 (prepared from praseodymium nitrate, nickel oxide, and molybdenum oxide); and the calcination temperature in step seven is 350 ℃, the heating rate is 5 ℃ / min, and the calcination time is 3 hours. The specific steps are as follows: Step 1: Synthesis of materials 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in a ball mill jar at a molar ratio of 1:0.01. In this comparative example, the oxygen ion conductor precursor is Pr₂Ni. 0.8 Mo 0.2 O4 is prepared from praseodymium nitrate, nickel oxide, and molybdenum oxide; Step 5: The lithium-rich manganese-based matrix oxide and the oxygen ion conductor precursor placed in the ball mill jar are ball-milled. Step 6: Set the ball milling parameters to 400 rpm and 6 hours, and add 40 mg of ethanol as a dispersant during the ball milling process; Step 7: The ball-milled mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 350℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LPNO-350.

[0034] The preparation process of the oxygen ion conductor modified lithium-rich manganese-based cathode material is basically the same as that in Example 1, the main difference being that in step four, the mixing method of the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor is changed from ball milling to grinding in an agate mortar. The specific steps are as follows: Step 1, Comparative Example 7 Synthetic material 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 was prepared by dissolving 18.92 g of lithium acetate dihydrate, 4.85 g of nickel acetate tetrahydrate, 4.86 g of cobalt acetate tetrahydrate and 19.85 g of manganese acetate tetrahydrate in 1 L of deionized water to prepare a mixed salt solution. 0.3 mol / L of complexing agent citric acid monohydrate (63.04 g) was added to the solution and stirred on a magnetic stirrer for 30 minutes to mix the solution evenly, thus obtaining the precursor solution. Step 2: Pump the precursor solution into the spray dryer, selecting an inlet air temperature of 230 ℃, an outlet air temperature of 115 ℃, a peristaltic pump speed of 600~800 ml / h, a needle frequency of 25 Hz, and a spray pressure of 0.1~0.5 MPa; Step 3: Collect the precursor powder after spraying, place it in a corundum boat, put it into a crucible and calcine it in a muffle furnace. The heating rate is 3 ℃ / min. After heating to 1000 ℃, hold it for 20 minutes. During this time, fresh air is continuously introduced into the muffle furnace. After cooling with the furnace, lithium-rich manganese base oxide is obtained. Step 4: Place the calcined lithium-rich manganese-based substrate oxide and the oxygen ion conductor precursor in an agate mortar at a molar ratio of 1:0.01 and grind them thoroughly. In this embodiment, the oxygen ion conductor precursor is La4Mn5Si4O.22 It is prepared from lanthanum oxide, manganese oxide and silicon oxide; Step 5: Grind the lithium-rich manganese-based base oxide and the oxygen ion conductor precursor placed in the agate mortar. Step 6: The ground mixture is placed in a quartz crucible and sintered in a muffle furnace at a temperature of 350℃ and a heating rate of 5℃ / min. After holding at this temperature for 3 hours, it is naturally cooled. The quartz crucible is then removed to obtain the oxygen ion conductor modified lithium-rich manganese-based cathode material, denoted as LMSO-M350.

[0035] The lithium-rich manganese cathode materials obtained from Examples 1-3 and Comparative Examples 1-7 through oxygen ion conductor modification, the conductive agent (Super P), and the binder (sodium carboxymethyl cellulose, CMC) were mixed in a mass ratio of 85:10:5 to form a slurry. The slurry was stirred at 800 rpm / min for 6 hours until it became homogeneous. Then, it was coated onto an aluminum foil current collector using a doctor blade with a thickness of 0.15 mm to obtain a cathode sheet. The cathode sheet was placed in a vacuum oven and dried at 110°C for 20 hours to obtain a lithium-rich manganese-based cathode sheet.

[0036] Lithium-rich manganese-based positive electrode sheets were cut into 10 mm diameter circular sheets and dried in a vacuum oven at 115°C for 10 hours. Then, they were assembled into button cells in an argon-filled glove box with oxygen and water content both below 0.01 ppm. The assembled button cells were then placed in an oven for activation at 45°C for 40 hours. After removal, the cycle performance of the cells was tested at different current densities.

[0037] Electrochemical performance testing was conducted using 2025 coin cells on a Xinwei testing system. Lithium metal sheets were used as the reference and counter electrodes, Celgard-2400 as the separator, and Xinzhoubang 3045I as the electrolyte. The test voltage range was 2.0–4.8 V. The test temperature was 28±1 ℃. The first three cycles were activated at a 0.1 C rate (1 C = 200 mAh / g), and cycling at a 1 C rate began from the fourth cycle. Specific performance test results are shown in Table 1.

[0038] Table 1

[0039] As can be seen from Table 1, the present invention uses La4Mn5Si4O 22As a precursor for oxygen ion conductors, lithium-rich manganese-based cathode materials were modified using a ball milling method combined with calcination. The modified lithium-rich manganese-based cathode material (LMSO-350), prepared under calcination conditions of 350 ℃ for 3 hours, exhibited optimal electrochemical performance: a first-cycle discharge specific capacity of 314.31 mAh / g at 0.1 C, with a capacity retention of 97.83% after 100 cycles; and a discharge capacity of 239.39 mAh / g at 1 C, with a retention of 96.01% after 600 long cycles. Simultaneously, the average voltage decay during cycling decreased to 1.051 mV / cycle, demonstrating a significant improvement in structural stability.

[0040] like Figure 1 As shown: Analysis of the X-ray diffraction results of Examples 1-3 and Comparative Example 1 shows that a weak (311) diffraction peak was observed in the 29°-31° range of LMSO-350, which corresponds to La4Mn5Si4O. 22 The oxygen ion conductor exhibits a monoclinic C² / m structure. Furthermore, the modification of the oxygen ion conductor did not alter the layered structure of the lithium-rich manganese-based material, nor did it have any other impact on its internal structure.

[0041] like Figure 2 As shown: As can be seen from the electron microscopy scanning elemental distribution diagram of the lithium-rich manganese-based cathode material in Example 2, Mn, Ni, Co, O, Si and La are uniformly distributed inside the particles, indicating that Si and La elements have been successfully incorporated. This shows that the oxygen ion conductor and the lithium-rich manganese cathode material are uniformly distributed, forming a eutectic phase structure.

[0042] like Figures 3-6 As shown: As shown by the first-cycle charge-discharge curves of Examples 1-3 and Comparative Example 1 at 0.1 C, the introduction of the oxygen ion conductor significantly improves the first-cycle discharge specific capacity of the lithium-rich manganese cathode material. This is mainly attributed to the formation of a eutectic phase structure between the oxygen ion conductor and the lithium-rich manganese cathode material. This structure constructs an efficient oxygen ion transport path, significantly reducing the oxygen ion migration barrier, thereby significantly improving the anion dynamics performance within the electrode and promoting the reversibility of the anion redox reaction. Furthermore, the first-cycle coulombic efficiency of the modified sample is significantly better than that of the unmodified sample, further indicating that the eutectic phase structure effectively suppresses irreversible oxygen release during the first charge. During the high-temperature calcination stage, excessively high calcination temperatures can cause irreversible changes in the surface structure of the lithium-rich manganese induced by the oxygen ion conductor, thereby sacrificing reactive sites and causing first-cycle capacity decay. However, the performance of the modified material is still superior to that of the unmodified material.

[0043] like Figure 7-12 As shown: As shown by the first-cycle charge-discharge curves at 0.1 C of Examples 2 and Comparative Examples 2-7, the introduction of the oxygen ion conductor in Example 2 significantly improved the discharge specific capacity of the lithium-rich manganese cathode material. All samples with introduced oxygen ion conductors exhibited improved first-cycle discharge specific capacities compared to the unmodified material, with LMSO-350 prepared in Example 2 showing the best performance, reaching a first-cycle discharge specific capacity of 314.31 mAh / g, significantly higher than Comparative Examples 2-7. Comparative Example 7 used agate mortar and pestle grinding instead of ball milling for mixing, and the resulting LMSO-M350 sample had a significantly lower first-cycle capacity than Example 2, indicating that the mixing method significantly affects the modification effect. During ball milling, the oxygen ion conductor precursor and the lithium-rich manganese-based material are uniformly dispersed in the ethanol solution through mechanical energy, effectively avoiding particle agglomeration. Furthermore, the high-energy collisions during ball milling can introduce defect sites on the particle surface, promoting the interfacial solid-phase reaction in the subsequent calcination stage, thereby forming a more stable eutectic phase structure. Therefore, ball milling is superior to simple agate mortar grinding. It is worth noting that the calcination temperature must be strictly controlled when introducing an oxygen ion conductor into a lithium-rich manganese-based material and performing a secondary calcination. Excessively high secondary calcination temperatures can induce irreversible changes in the surface structure of the lithium-rich manganese, destroying the integrity of the layered structure, thereby sacrificing reactive sites and exacerbating the initial capacity decay. Therefore, this invention controls the secondary calcination temperature at 350 °C, which ensures sufficient contact between the oxygen ion conductor and the lithium-rich manganese matrix to form a stable eutectic phase structure, while avoiding structural damage caused by high temperatures, thus achieving optimal electrochemical performance.

[0044] like Figure 13-19 As shown: The electrochemical performance cycling curves of Examples 1-3 and Comparative Examples 1, 2, 4, and 5 at 0.1 C show that all samples introducing oxygen ion conductors exhibit better cycling stability than the unmodified lithium-rich manganese-based cathode material. Among them, the LMSO-350 cathode material prepared in Example 2 demonstrates the best capacity retention capability, with a capacity retention rate as high as 97.83% after 100 cycles, significantly better than the unmodified sample (Comparative Example 1, approximately 68.34%) and other modified samples (Comparative Examples 2, 4, and 5, with retention rates of 82.23%, 95.03%, and 88.53%, respectively).

[0045] like Figures 20-33 As shown: As shown by the electrochemical cycling curves of Examples 1-3 and Comparative Examples 1, 2, 4, and 5 at 1 C for 600 cycles, the introduction of the oxygen ion conductor not only increases the battery's charge-discharge capacity but also significantly improves its cycle stability. Specifically, the LMSO-350 cathode material prepared in Example 2 achieved a capacity retention of 96.01% after 600 cycles at 1 C, far exceeding the unmodified sample (Comparative Example 1, approximately 53.83%) and other modified samples (Comparative Examples 2, 4, and 5, with retention rates of 89.36%, 87.85%, and 81.29%, respectively). Furthermore, the voltage decay of LMSO-350 was effectively suppressed (average only 1.051 mV per cycle), far lower than the unmodified sample (approximately 1.375 mV / cycle), indicating that the eutectic phase structure effectively suppressed irreversible phase transitions and lattice oxygen release during cycling, thereby significantly improving the material's voltage stability. Oxygen ion conductor La4Mn5Si4O 22 The abundant intrinsic oxygen vacancies within the crystal effectively suppress the irreversible release of lattice oxygen, reducing structural degradation during cycling. Suitable oxygen ion conductor types and calcination temperatures (350 °C) facilitate the formation of a stable eutectic phase structure, thereby effectively suppressing capacity decay during cycling.

[0046] like Figures 34-37 As shown: As shown in the rate performance curves of Examples 1-3 and Comparative Examples 1, 2, 4, and 5 at 1 C, the discharge specific capacity of each battery decreases as the test current density gradually increases. Among all samples, the LMSO-350 cathode material prepared in Example 2 exhibits the highest discharge specific capacity at all rates. When the current density is reduced from 10 C to 0.1 C, the discharge capacity of LMSO-350 can recover to 315.97 mAh / g, demonstrating excellent rate reversibility and structural stability. This advantage is attributed to the efficient oxygen ion transport channels constructed by the eutectic phase structure, which effectively reduces polarization at high current densities, while good interfacial stability ensures efficient capacity recovery after rapid charge and discharge.

[0047] like Figures 38-40 As shown: Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) images of the cathode materials from Examples 2 and 1 after 600 cycles at 1 C reveal that the unmodified lithium-rich manganese cathode material exhibits severe degradation of its internal layered structure after 600 cycles, with most of it transforming into spinel or rock salt phases and forming numerous nanopores, leading to rapid capacity decay. In contrast, the LMSO-350 cathode material prepared in Example 2 maintains good structural integrity after cycling, with no significant particle breakage or collapse. Only a thin, uniform spinel phase protective layer forms on its surface, while the internal layered phase structure remains intact, demonstrating excellent structural stability and resistance to phase transitions. This indicates that the eutectic phase structure can effectively suppress irreversible structural degradation during long-term cycling, thereby significantly improving the cycle life of lithium-rich manganese-based cathode materials.

[0048] In summary, Example 2 is the best embodiment.

[0049] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for preparing an oxygen ion conductor modified lithium-rich manganese-based cathode material, characterized in that: Includes the following steps: Step 1: Dissolve lithium source, nickel source, cobalt source and manganese source in water according to the molar ratio of Li:Ni:Co:Mn=1.53:0.165:0.165:0.665, and add complexing agent to obtain precursor solution; Step 2: The precursor solution is prepared into precursor powder by high-temperature spray drying; then the precursor powder is sintered at 1000 °C for 20 minutes to obtain lithium-rich manganese cathode powder material. Step 3: Combine the lithium-rich manganese cathode material obtained in Step 1 with the oxygen ion conductor La4Mn5Si4O 22 The precursor material was placed in a ball mill jar at a molar ratio of 1:0.01; Step 4: The ball mill jar containing lithium-rich manganese powder and oxygen ion conductor is subjected to ball milling, with ethanol added as a dispersant during the ball milling process. Step 5: The ball-milled lithium-rich manganese cathode material and the oxygen ion conductor mixture are sintered in a muffle furnace at a temperature of 250 ℃~450 ℃ for 3 hours. After natural cooling, the oxygen ion conductor modified lithium-rich manganese-based cathode material is obtained.

2. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step one, the lithium source, nickel source, cobalt source, and manganese source are lithium acetate, nickel acetate, cobalt acetate, and manganese acetate, respectively, and the total concentration in the precursor solution is 0.15 mol / L.

3. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step one, the complexing agent is citric acid monohydrate, and the concentration of the complexing agent is 0.3 mol / L.

4. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step two, the inlet temperature of the spray dryer is 230 ℃, the outlet temperature is 115 ℃, the peristaltic pump speed is 600~800mL / h, the needle frequency is 25 Hz, and the spray pressure is 0.1~0.5 MPa; the atmosphere for spray drying is one or more of air and oxygen.

5. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step three, the molar ratio of lithium-rich manganese cathode material to oxygen ion conductor is 1:0.

01.

6. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step four, the ball milling conditions are 400 rpm for 6 hours.

7. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step five, the ball-milled lithium-rich manganese cathode material and the oxygen ion conductor mixture are sintered at a heating rate of 5 ℃ / min and a calcination temperature of 350 ℃ for 3 hours.

8. The method for preparing the oxygen ion conductor modified lithium-rich manganese-based cathode material according to claim 1, characterized in that: In step three, the oxygen ion conductor La4Mn5Si4O 22 The precursor materials are lanthanum oxide, manganese oxide, and silicon oxide.

9. The application of an oxygen ion conductor modified lithium-rich manganese-based cathode material prepared by the preparation method as described in claim 1 in the cathode of a lithium-ion battery.

10. The application according to claim 9, characterized in that: At a high voltage of 4.8 V, the initial discharge capacity at 0.1 C reached 314.31 mAh / g, and the capacity retention rate after 100 cycles was 97.83%; the initial discharge capacity at 1 C was 239.39 mAh / g, and the retention rate after 600 long cycles was 96.01%. At the same time, the average voltage decay during cycling decreased to 1.051 mV / cycle, demonstrating a significant improvement in structural stability.