A method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot" process

The one-pot method for preparing multilayer coated silicon-carbon composite anode materials solves the problems of complex processes and high energy consumption in existing technologies, and realizes low-cost large-scale production and preparation of high-performance materials with high specific capacity and good cycle stability.

CN123120692APending Publication Date: 2026-11-17CHONGQING INST OF GREEN & INTELLIGENT TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611361382.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing silicon-carbon anode materials suffer from long process flows, high energy consumption, and poor batch consistency, making it difficult to achieve low-cost large-scale production. Furthermore, the electrochemical performance of the materials is inferior to that of traditional methods, especially in achieving both high specific capacity and long cycle life.

Method used

A one-pot method for preparing multilayer coated silicon-carbon composite anode materials includes feeding nano-silicon powder, solid carbon source, graphene dispersion and solvent into the material at one time, followed by integrated stirring, drying and heat treatment. The components are mixed and heat-treated under specific ratios and conditions to form a multilayer coated structure of silicon core-amorphous carbon layer-graphene layer.

Benefits of technology

This approach achieves extreme simplification of the process flow, reduces production costs, improves the specific capacity and cycle stability of the material, and ensures that the material possesses good conductivity and structural stability while exhibiting high-efficiency electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120692A_ABST
    Figure CN123120692A_ABST
Patent Text Reader

Abstract

This invention discloses a one-pot method for preparing multilayer coated silicon-carbon composite anode materials, belonging to the field of lithium-ion battery manufacturing technology. The method includes the following steps: Step S1: Adding nano-silicon powder, solid carbon source, graphene dispersion, and solvent to a stirring device according to a preset ratio and stirring to obtain a composite slurry; Step S2: Performing solid-liquid separation on the composite slurry, and drying the wet material obtained after solid-liquid separation to obtain a silicon-carbon precursor; Step S3: Performing heat treatment on the silicon-carbon precursor under an inert atmosphere to obtain the silicon-carbon composite anode material. This invention integrates the one-pot feeding of nano-silicon powder, solid carbon source, graphene dispersion, and solvent, along with stirring, drying, and heat treatment, eliminating intermediate separation, purification, and multiple transfers. This solves the problems of cumbersome traditional processes, high energy consumption, and poor batch consistency, achieving extreme process simplification, shortening the cycle, and reducing costs, making low-cost, large-scale production of silicon-carbon anodes possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery preparation technology, and particularly relates to a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method". Background Technology

[0002] Silicon-based materials possess extremely high theoretical specific capacity (4200 mAh / g), thus being considered the most promising anode materials for next-generation lithium-ion batteries. However, existing methods for preparing silicon-carbon anode materials are cumbersome and lengthy, involving multiple steps. Taking the preparation of typical coated silicon-carbon materials as an example, it usually requires the separate preparation or pretreatment of carbon and silicon sources, followed by multiple processes such as liquid-phase mixing, drying, grinding, and multi-stage heat treatment. Furthermore, multiple material transfers and separation and purification of intermediate products are necessary between each process. These methods suffer from problems such as long process flows, high energy consumption, and difficulty in controlling batch consistency, which not only increases production costs but also reduces production efficiency, hindering the large-scale production of materials. In particular, while chemical vapor deposition (CVD) can obtain a uniform and dense carbon coating layer on the silicon surface with excellent product performance, this method requires huge equipment investment, precise temperature and gas path control systems, and has a complex process and limited capacity, making it difficult to achieve large-scale, low-cost industrial applications. This seriously hinders the widespread adoption of silicon-carbon anode materials in the low-to-mid-end market.

[0003] To reduce the preparation cost and process complexity of silicon-carbon anode materials, researchers are actively exploring simplified synthesis routes. Existing technologies have attempted to directly obtain the product by mixing all raw materials in one step followed by heat treatment. For example, silicon powder, carbon source, and conductive agent are mixed in a liquid phase in one step, followed by ball milling and subsequent sintering. This one-pot process eliminates the separation, washing, and pretreatment steps of intermediate products, significantly shortening the production cycle, reducing material loss and energy consumption, and showing great potential for reducing production costs. Regarding ball milling, high-energy ball milling not only achieves uniform dispersion of components at the micro-nano scale but also utilizes mechanochemical effects to promote the generation of fresh active sites on the silicon particle surface, which is beneficial for the subsequent chemical anchoring of the carbon layer. This provides favorable conditions for one-step processes.

[0004] However, the simplified processes reported so far often face a common technical contradiction: the simplification of the process flow is often accompanied by a decrease in the controllability of the material's microstructure, resulting in electrochemical performance inferior to materials prepared by traditional multi-step or CVD methods, especially in achieving both high specific capacity and long cycle life—two core indicators. Furthermore, while some one-pot methods achieve one-step mixing, subsequent processing still requires additional reduction treatments, acid etching, or stepwise heating, failing to truly achieve ultimate process simplification. How to ensure a significantly simplified process flow while maintaining the specific capacity (>2500 mAh / g) and cycle stability required for commercial lithium-ion batteries is a key technical challenge for the low-cost, large-scale production of silicon-carbon anode materials.

[0005] Therefore, there is an urgent need in this field for a silicon-carbon material preparation method that is simple in process, low in cost, easy to scale up for production, and can ensure that the material has good electrochemical performance, so as to break through the cost bottleneck of the commercial application of silicon-carbon anode materials. Summary of the Invention

[0006] Based on the technical problems existing in the prior art, the present invention provides a method for preparing multilayer coated silicon-carbon composite anode materials in a "one-pot" manner.

[0007] According to the technical solution of the present invention, a method for preparing multilayer coated silicon-carbon composite anode materials by a "one-pot method" is provided, comprising the following steps: Step S1: Add nano-silicon powder, solid carbon source, graphene dispersion and solvent to a stirring device according to a preset ratio and stir to obtain composite slurry; Step S2: Perform solid-liquid separation on the composite slurry, and dry the wet material obtained after solid-liquid separation to obtain a silicon-carbon precursor; Step S3: Heat-treat the silicon-carbon precursor under an inert atmosphere to obtain a silicon-carbon composite anode material.

[0008] A further improvement of the present invention is that the solid carbon source includes one or two of glucose or sucrose, phenolic resin and asphalt powder.

[0009] A further improvement of the present invention is that the graphene dispersion is an N-methylpyrrolidone solution or an aqueous dispersion.

[0010] A further improvement of the present invention is that the sum of the masses of the nano-silicon powder, the solid carbon source, and the graphene dispersion is the total mass; The nano-silicon powder accounts for 60% to 70% of the total mass. The solid carbon source accounts for 10% to 15% of the total mass. The graphene dispersion accounts for 15% to 25% of the total mass.

[0011] A further improvement of the present invention is that the solid content of the graphene dispersion is 5%.

[0012] A further improvement of the present invention is that, in step S1, the stirring device is a ball mill, the rotation speed of the ball mill is 600 rpm to 1000 rpm, and the stirring duration is 8 h to 12 h.

[0013] A further improvement of the present invention is that, in step S2, the drying temperature is 80°C to 100°C and the drying duration is 12 hours.

[0014] A further improvement of the present invention is that, in step S3, the temperature of the heat treatment is 600℃~800℃.

[0015] A further improvement of the present invention is that, in step S3, the heat treatment includes a heating stage and a holding stage, wherein the heating stage lasts for 60 min to 120 min and the holding stage lasts for 2 h to 4 h.

[0016] A further improvement of the present invention is that the solvent is deionized water.

[0017] Compared with the prior art, the above-mentioned technical solution of the present invention has the following beneficial technical effects: 1. This invention integrates the feeding of nano-silicon powder, solid carbon source, graphene dispersion and solvent into a single process, followed by stirring, drying and heat treatment. This eliminates the need for intermediate separation and purification and multiple transfers, solving the problems of cumbersome traditional processes, high energy consumption and poor batch consistency. It achieves extreme process simplification, shortens the cycle and reduces costs, making low-cost large-scale production of silicon-carbon anodes possible.

[0018] 2. This invention uses one or two of glucose or sucrose, phenolic resin and asphalt powder as solid carbon sources. Taking advantage of their good water solubility, low pyrolysis temperature and dense film formation, the carbon source fully encapsulates the nano-silicon particles and forms an amorphous carbon inner layer that is closely attached to the silicon core after pyrolysis. This solves the problems of weak silicon-carbon interface bonding and discontinuous coating, effectively buffers the volume expansion of silicon, and improves the cycle stability of the material.

[0019] 3. This invention introduces graphene using N-methylpyrrolidone solution or water-based dispersion, allowing few-layer graphene to uniformly enter the slurry in a pre-dispersed state. This avoids sheet aggregation and allows for flexible matching with oil and water phase systems. It solves the problems of uneven dispersion and difficulty in constructing conductive networks when graphene is directly fed in, achieving uniform distribution and outer coating of graphene, enabling the material to form a continuous conductive network and improving conductivity.

[0020] 4. This invention achieves a balance between the active silicon phase, the carbon-forming coating phase, and the conductive phase by synergistically proportioning nano-silicon powder, solid carbon source, and graphene dispersion at 60%~70%, 10%~15%, and 15%~25%, respectively. This solves the problem of incomplete coating or capacity dilution caused by imbalanced proportions, and achieves both complete coating and conductive network under high silicon content, giving the material both high specific capacity and structural stability.

[0021] 5. This invention uses a graphene dispersion with a solid content of 5%, which makes the graphene sheets stably dispersed, without stacking or agglomerating, and with suitable fluidity, facilitating precise proportioning and uniform mixing. It solves the problems of excessive viscosity and easy agglomeration due to excessive solid content, and excessive medium introduction and prolonged drying time due to excessive solid content. It achieves uniform introduction of graphene and controllable slurry state, making mixing and drying more efficient and batch consistency better.

[0022] 6. In step S1, the present invention uses high-energy ball milling at 600 rpm to 1000 rpm for 8 h to 12 h. The impact shearing and mechanochemical effects of the grinding media cause the components to be dispersed into micro- and nano-sized particles, generating active sites on the silicon surface. The difference in particle size density is used to form centrifugal stratification, which solves the problems of uneven dispersion and weak interfacial bonding. It achieves uniform mixing and preliminary stratification and coating, which facilitates the subsequent firm anchoring of the carbon layer.

[0023] 7. In step S2, the present invention uses drying at 80℃~100℃ for 12h to gradually remove residual solvent, allowing nano-silicon, solid carbon source and graphene to be deposited in situ and adhere to each other during solvent evaporation. This solves the problems of particle migration, delamination and carbon layer defects caused by excessively rapid drying and solvent residue. It realizes the preparation of silicon-carbon precursor with fixed composition and complete structure, making heat treatment more uniform and carbon layer more dense.

[0024] 8. In step S3, the present invention employs heat treatment at 600℃~800℃ to fully pyrolyze and carbonize the solid carbon source, forming a stable amorphous carbon layer and firmly bonding the graphene. At the same time, it avoids residue at excessively low temperatures and silicon grain growth and graphene damage at excessively high temperatures. This solves the problem of incomplete carbonization and high-temperature degradation, achieving a balance between dense carbon layers and stable silicon phases, giving the material both electrical conductivity and cycle performance.

[0025] 9. This invention divides the heat treatment into a 60-120 minute heating stage and a 2-4 hour holding stage. The steady heating allows for the orderly pyrolysis of the carbon source and avoids violent boiling that could disperse the particles. The sufficient holding stage ensures that the carbon layer is dense and firmly bonded. This solves the problems of carbon layer defects caused by rapid heating and weak bonding due to insufficient holding. It enables the controllable formation of a multi-layer coating structure and ensures the integrity of the material coating and the continuity of electrical conductivity.

[0026] 10. This invention uses deionized water as a dispersion solvent to provide a clean liquid medium for nano-silicon powder, solid carbon source and graphene, and completely removes them after drying without leaving any residue in the product. At the same time, it avoids the influence of impurities such as metal ions and chloride ions in ordinary water on purity, solves the problem of electrochemical performance degradation caused by impurities, achieves uniform dispersion of each component and high-purity preparation, and improves product consistency and stability. Attached Figure Description

[0027] The accompanying drawings are provided to better understand the invention and are not intended to unduly limit the scope of the invention. Wherein: Figure 1 This is a scanning electron microscope image of the silicon-carbon composite anode material prepared by using a ball mill as a stirring device in the "one-pot method" for preparing multilayer coated silicon-carbon composite anode material of the present invention. Figure 2 This is a scanning electron microscope image of the silicon-carbon composite anode material prepared by using a mechanical stirring device as the stirring device in the "one-pot method" for preparing multilayer coated silicon-carbon composite anode material of the present invention. Figure 3 This is a transmission electron microscope image of the silicon-carbon composite anode material prepared by the "one-pot method" of the present invention for preparing multilayer coated silicon-carbon composite anode material. Figure 4 This is the Raman spectrum of the silicon-carbon composite anode material prepared by the "one-pot method" of the present invention for preparing multilayer coated silicon-carbon composite anode material; Figure 5 This is a long-cycle performance curve of the silicon-carbon composite anode material prepared by the "one-pot method" of the present invention for preparing multilayer coated silicon-carbon composite anode materials. Detailed Implementation

[0028] The following description, in conjunction with the accompanying drawings, illustrates exemplary embodiments of the present invention, including various details to aid understanding. These details should be considered merely exemplary. Therefore, those skilled in the art will recognize that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the invention. Similarly, for clarity and brevity, descriptions of well-known functions and structures are omitted in the following description.

[0029] This invention discloses a one-pot method for preparing multilayer coated silicon-carbon composite anode materials, belonging to the field of lithium-ion battery manufacturing technology. The method includes the following steps: Step S1: Adding nano-silicon powder, solid carbon source, graphene dispersion, and solvent to a stirring device in a preset ratio and stirring to obtain a composite slurry; Step S2: Performing solid-liquid separation on the composite slurry, and drying the resulting wet material to obtain a silicon-carbon precursor; Step S3: Heat-treating the silicon-carbon precursor under an inert atmosphere to obtain the silicon-carbon composite anode material. This invention integrates the one-pot feeding of nano-silicon powder, solid carbon source, graphene dispersion, and solvent with stirring, drying, and heat treatment, eliminating intermediate separation, purification, and multiple transfers. This solves the problems of cumbersome traditional processes, high energy consumption, and poor batch consistency, achieving extreme process simplification, shortening the cycle, and reducing costs, making low-cost, large-scale production of silicon-carbon anodes possible.

[0030] The technical solution of the present invention will now be described in detail with reference to specific embodiments and accompanying drawings.

[0031] Example 1 This embodiment provides a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method," which includes the following steps: Step S1: Add nano-silicon powder, solid carbon source, graphene dispersion and solvent to a stirring device according to a preset ratio and stir to obtain composite slurry; The "one-pot method" refers to adding all solid components and their dispersion medium that constitute the final material into the same container at once, completing the mixing and preliminary composite process without any separate preparation, separation, washing, or purification of any components. This integrates the traditional multi-stage raw material pretreatment, liquid-phase mixing, and pre-coating of silicon-carbon materials into a single step. Steps S1, S2, and S3 are sequentially connected and use the same batch of materials: Step S1 achieves uniform dispersion and in-situ pre-coating of each component in the liquid phase; Step S2 removes the liquid phase medium to obtain a silicon-carbon precursor with a fixed composition; Step S3 completes carbonization and bonding simultaneously through a single thermal conversion. No intermediate product transfer is required throughout the process, resulting in a short process flow, low material loss, and easy batch consistency control. In some embodiments, nano-silicon powder and solid carbon source dry powder can be premixed and then added together with graphene dispersion and solvent, or all components can be added simultaneously at once. During stirring, the system remains in a flowable slurry state until all components are fully wetted and uniformly dispersed, resulting in a composite slurry without significant stratification or agglomeration.

[0032] Step S2: Perform solid-liquid separation on the composite slurry, and dry the wet material obtained after solid-liquid separation to obtain a silicon-carbon precursor; Solid-liquid separation is used to remove excess liquid phase and grinding media introduced in step S1 from the composite slurry. In some embodiments, filtration, vacuum filtration, pressure filtration, or centrifugation is employed. When ball milling is used in step S1 and the system contains hard grinding beads, the grinding beads are preferentially filtered through a screen for retention and reuse, resulting in a wet material (wet filter cake). Drying is used to further remove residual solvent from the wet material, allowing the nano-silicon powder, solid carbon source, and graphene dispersed in the liquid phase to deposit in situ and adhere to each other during solvent evaporation, forming a solid silicon-carbon precursor with a composition consistent with the feed ratio and fixed relative positions of each component. In some embodiments, drying is performed using vacuum drying, forced-air drying, or spray drying, with vacuum drying being preferred to efficiently remove solvent at a lower temperature and avoid oxidation of nano-silicon and organic carbon sources. The resulting block or cake-shaped precursor is ground and sieved to obtain a precursor powder with uniform particle size for heat treatment in step S3.

[0033] Step S3: Heat-treat the silicon-carbon precursor under an inert atmosphere to obtain a silicon-carbon composite anode material.

[0034] The inert atmosphere is used to isolate oxygen and prevent high-temperature oxidation of nano-silicon and combustion loss of carbon components during pyrolysis. In some embodiments, argon, nitrogen, or a combination thereof are used, with high-purity argon being preferred. The heat treatment is carried out in a tube furnace, box furnace, or rotary furnace, with the precursor placed in an alumina crucible or graphite crucible. During the heating process, the solid carbon source gradually melts, pyrolyzes, and carbonizes, forming an amorphous carbon coating layer on the surface of the nano-silicon particles. The graphene sheets adhere to and anchor to the outside of the carbon layer under the shrinkage effect of carbonization and bridge between adjacent particles, forming a multi-layered coating structure from the inside out, consisting of a silicon core, an amorphous carbon layer, and a graphene layer. After the heat treatment, the material is cooled to room temperature in the furnace under the protection of the inert atmosphere. After grinding and sieving, the silicon-carbon composite anode material is obtained. The entire thermal conversion is completed in one step, without the need for reduction, acid washing, or step-by-step etching in addition to carbonization, achieving integrated mixing, drying, and sintering.

[0035] Specifically, the solid carbon source includes one or two of glucose or sucrose, phenolic resin, and asphalt powder. Glucose and sucrose are water-soluble sugar carbon sources, which can easily dissolve and disperse uniformly in water-based slurries and fully encapsulate nano-silicon particles. They also have low pyrolysis temperatures and moderate residual carbon rates. After pyrolysis, they form a dense amorphous carbon inner layer that is tightly bonded to the silicon core, which buffers the volume expansion of silicon and prevents direct contact between silicon and the electrolyte. In some embodiments, a combination of glucose and sucrose is used to balance solubility and carbonization rate. To further enhance the multilayer coating effect, in other embodiments, the solid carbon source also includes a second carbon source with a pyrolysis temperature higher than that of glucose or sucrose. The second carbon source includes one or more of asphalt powder and phenolic resin. The low-temperature carbon source pyrolyzes first at a lower temperature to form a dense inner carbon layer, while the high-temperature carbon source pyrolyzes at a higher temperature to form a tough outer carbon layer. The two work together to construct a gradient multilayer coating structure with strong bonding and distinct layers.

[0036] Specifically, the graphene dispersion is an N-methylpyrrolidone solution or an aqueous dispersion. The graphene dispersion uses pre-exfoliated and dispersed few-layer graphene as the conductive phase. The N-methylpyrrolidone (NMP) dispersion has good compatibility with oily systems and subsequent electrode coating processes. The aqueous dispersion uses water as the dispersion medium, making it environmentally friendly and low-cost. The choice between the two can be made based on the solubility of the solid carbon source and the solvent system. In some embodiments, when the solid carbon source is water-soluble such as glucose or sucrose and the solvent is deionized water, an aqueous graphene dispersion is preferred to form a uniform aqueous phase system. In the finished product, graphene forms a three-dimensional conductive network and an outermost flexible conductive coating, which not only compensates for the insufficient conductivity of amorphous carbon but also buffers the volume deformation of silicon during lithium insertion / extraction processes. Some layers also bridge between adjacent particles, improving the overall structure and the integrity of the conductive network.

[0037] Specifically, the total mass is the sum of the masses of the nano-silicon powder, solid carbon source, and graphene dispersion; the nano-silicon powder accounts for 60% to 70% of the total mass; the solid carbon source accounts for 10% to 15% of the total mass; and the graphene dispersion accounts for 15% to 25% of the total mass. The above mass ratios are calculated based on the sum of the masses of the nano-silicon powder, solid carbon source, and graphene dispersion, with the sum of their mass percentages being 100%. Each component is taken within the above range and balanced with the others. The solvent added in step S1, as a dispersion medium, is not included in the total mass; its amount is sufficient to ensure that the system is a flowable and stirable slurry. Nano-silicon powder, as the active phase providing capacity, accounts for 60%–70% to ensure high specific capacity of the material; solid carbon source, as the carbon-forming coating phase, accounts for 10%–15% to form a continuous and complete amorphous carbon layer on the surface of silicon particles; graphene dispersion, as the conductive and outer coating phase, accounts for 15%–25% to provide sufficient conductive network and outer sheet coating. Too high a proportion of nano-silicon will result in insufficient carbon coating and easy pulverization and detachment during cycling due to volume expansion; too low a proportion will sacrifice the overall specific capacity; too high a proportion of solid carbon source or graphene dispersion will dilute the active silicon content and reduce reversible capacity.

[0038] Specifically, the solid content of the graphene dispersion is 5%. Solid content refers to the mass fraction of graphene solid phase in the graphene dispersion. At a solid content of 5%, the graphene sheets are stably dispersed and less prone to aggregation, and the dispersion has suitable fluidity, facilitating quantitative proportioning and uniform mixing. Based on a 5% solid content, the actual mass of graphene solid phase introduced into the system by the dispersion is 5% of the dispersion's mass; the total mass of the dispersion is included in the aforementioned total mass during proportioning calculations. Excessive solid content increases the dispersion's viscosity, making graphene prone to aggregation and difficult to disperse uniformly; insufficient solid content introduces excessive dispersion medium, prolonging subsequent solid-liquid separation and drying time, and increasing energy consumption.

[0039] Specifically, in step S1, the stirring equipment is a ball mill, and the speed of the ball mill during stirring is 600 rpm to 1000 rpm, with a stirring duration of 8 h to 12 h. Step S1 preferably uses a wet high-energy ball mill for stirring and mixing. The ball mill can be a planetary ball mill, a stirred ball mill, or a sand mill. The grinding media is hard grinding beads; in some embodiments, zirconium oxide beads (zirconia beads) are used. The mass ratio of material to grinding beads is 1:10 to 1:20. Ball milling, on the one hand, uses the impact and shearing of the grinding beads to uniformly disperse nano-silicon powder, solid carbon source, and graphene at the micro-nano scale and break up soft agglomerates. On the other hand, it utilizes the mechanochemical effect to generate fresh active sites on the surface of silicon particles, making the pyrolytic carbon layer easier to chemically anchor with silicon and improving interfacial bonding. Simultaneously, utilizing the differences in particle size and density among the three components, the material is arranged in a gradient under the centrifugal action of the high-speed ball mill. The denser silicon particles tend to be in the inner layer, and the lightweight sheet-like graphene tends to be in the outer layer, forming a preliminary layered coating during the mixing stage. A rotation speed of 600 rpm to 1000 rpm and a time of 8 h to 12 h can balance dispersion uniformity and mechanical activation effect: if the rotation speed is too low or the time is too short, the dispersion and activation will be insufficient; if the rotation speed is too high or the time is too long, impurities will be easily introduced and the silicon particles will be excessively refined, increasing side reactions. In other embodiments, high-speed mechanical stirring can also replace ball milling, achieving uniform dispersion and layered pre-coating without adding grinding media, and the morphology of the obtained material is basically the same as that of the ball milling method.

[0040] Specifically, in step S2, the drying temperature is 80℃~100℃, and the drying duration is 12 hours. A drying temperature of 80℃~100℃ and a drying time of 12 hours allow residual solvent to evaporate fully and gradually, avoiding rapid heating that could lead to solvent boiling, particle migration, and disruption of the established layered arrangement. Within this temperature range, carbon sources such as glucose and sucrose do not undergo significant pyrolysis, but are fixed to the surface of silicon particles only as the solvent precipitates. In some embodiments, a vacuum oven is used for drying. The vacuum environment lowers the solvent boiling point, accelerates removal, and inhibits oxidation. The resulting blocky precursor is ground and sieved to obtain powder, increasing the heating area in step S3 and ensuring uniform heat treatment. Too low a temperature or too short a time will leave solvent residue, which can easily lead to pores and carbon layer defects during subsequent heat treatment; too high a temperature may cause sugars to melt and clump prematurely or undergo localized oxidation, which is detrimental to maintaining the uniformity of the precursor composition and particle size.

[0041] Specifically, in step S3, the heat treatment temperature is 600℃~800℃. The heat treatment temperature is the highest temperature reached during the holding stage. 600℃~800℃ allows for complete pyrolysis and carbonization of the solid carbon source, forming a stable amorphous carbon layer, and ensures a strong bond between graphene and silicon-carbon particles. Simultaneously, it prevents the growth and agglomeration of nano-silicon grains and damage to the graphene sheet structure at excessively high temperatures. In some embodiments, the temperature is increased from room temperature to 600℃~800℃ at a controllable rate of approximately 5℃ / min. If the temperature is too low, the carbon source will not pyrolyze completely, leaving residual organic components and heteroatoms, resulting in insufficient conductivity and density of the carbon layer. If the temperature is too high, energy consumption will increase, silicon particle growth will be accelerated, and some carbon components may undergo excessive graphitization or silicon-carbon side reactions, which will ultimately impair cycle performance.

[0042] Specifically, in step S3, the heat treatment includes a heating stage and a holding stage. The heating stage lasts for 60-120 minutes, and the holding stage lasts for 2-4 hours. The heating stage is used to gradually increase the temperature of the precursor at a set rate, allowing trace amounts of residual solvent to be removed, and the solid carbon source to soften, melt, and slowly pyrolyze in sequence, avoiding rapid heating that could cause component boiling, gas generation that could disperse particles and carbon layer defects. The heating stage lasts for 60-120 minutes, corresponding to a stable and controllable heating rate, allowing the low-temperature carbon source and the high-temperature carbon source to form carbon in an orderly manner within different temperature ranges, which is beneficial for forming a multi-layered coating with distinct layers. The heating rate can be adjusted accordingly within this time range based on the target temperature. The heat preservation stage is used to maintain the highest temperature for 2 to 4 hours, allowing the carbon source to fully carbonize, the amorphous carbon layer to densify, and the bonding between graphene and the carbon layer, and between the carbon layer and the silicon core to be strong, thereby improving the integrity of the coating and the continuity of conductivity. If the heat preservation time is too short, carbonization and bonding will be insufficient; if it is too long, it will easily lead to silicon grain growth, increased energy consumption, and limited performance gains. After the heat preservation is completed, heating is stopped, and the material is discharged after cooling to room temperature in the furnace under an inert atmosphere.

[0043] Specifically, the solvent used is deionized water.

[0044] The solvent, serving as the liquid-phase dispersion medium in step S1, wets and carries the nano-silicon powder, solid carbon source, and graphene for uniform dispersion. This ensures that the components achieve particle-scale uniform mixing and in-situ pre-coating in the liquid phase. The solvent is then removed through solid-liquid separation and drying in step S2, leaving no residue in the final product. Using deionized water avoids the impact of impurities such as metal ions and chloride ions on material purity and electrochemical performance. Furthermore, deionized water exhibits good compatibility with glucose, sucrose, and water-based graphene dispersions, is low-cost, and pollution-free. In some embodiments, the solvent dosage is based on forming a flowable composite slurry, and the deionized water is evaporated during the drying process. When using an NMP-based graphene dispersion, NMP or a mixture of NMP and water can also be used as the dispersion medium to match the dispersion system.

[0045] The silicon-carbon composite anode material obtained through the above steps has a multi-layer coating structure of silicon core, amorphous carbon layer, and graphene layer. The carbon layer is complete, firmly bonded, and has a continuous conductive network, which can effectively buffer the volume expansion of silicon. While significantly simplifying the process and reducing costs, the material maintains high specific capacity and good cycle stability.

[0046] Specifically, such as Figure 3 The image shown is a transmission electron microscope (TEM) image of the silicon-carbon composite anode material provided in this embodiment. The inner layer shows the lattice fringes of the nano-silicon particles, while the outer layer exhibits a multi-layered coating structure. The outermost layer of the silicon particles is initially coated with an amorphous carbon layer without lattice fringes, followed by a few-layer graphene layer, which is clearly visible.

[0047] Specifically, such as Figure 4 The figure shows the Raman spectrum of the silicon-carbon composite material prepared by ball milling or stirring according to this embodiment. As can be seen from the figure, at approximately 520 cm⁻¹... -1 The Raman characteristic peaks of silicon nuclei appear at approximately 1350 cm⁻¹. -1 Approximately 1580 cm -1 Characteristic peaks of the D and G bands of carbon materials appear at approximately 2700 cm⁻¹. -1 The presence of a characteristic 2D band peak indicates the presence of a graphene structure in the outer carbon layer. Furthermore, the variation in peak intensity ratio and width between the D and G bands reflects the presence of an amorphous carbon interlayer. In addition, the D and G bands prepared by both methods are located in the same position, demonstrating the reproducibility of the one-pot preparation method.

[0048] Specifically, such as Figure 5 The figure shows the long-cycle performance of the silicon-carbon anode prepared based on the composite anode material. As can be seen from the figure, after 400 cycles at a current density of 2.1 A / g, the discharge specific capacity of the silicon-carbon anode remains above 1000 mAh / g, while the capacity of the pure silicon anode rapidly decays to below 100 mAh / g. Furthermore, the coulombic efficiency of the material remains stable above 90% throughout the entire cycle, significantly higher than that of the pure silicon anode. These results indicate that the silicon-carbon composite material prepared using the one-pot method can effectively buffer the volume expansion of silicon and significantly improve the cycle stability of the electrode.

[0049] Example 2 This embodiment provides a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method," which includes the following steps: Step S1: In a ball mill jar, add 13 parts of nano-silicon powder, 2 parts of glucose, 1 part of asphalt powder, 40 parts of NMP graphene dispersion (5% solid content), and 10 parts of deionized water all at once. Then add hard grinding beads (such as zirconium beads, with a material-to-grinding-bead mass ratio of 1:10-1:20), seal, and ball mill at 800-1000 rpm for 10 hours to obtain a uniform black composite slurry.

[0050] Step S2: Filter the ball-milled slurry to separate the zirconium beads, and then place the filtered wet filter cake in a vacuum oven at 80-100℃ for 12 hours to dry, obtaining a black block precursor.

[0051] Step S3: The dried precursor is ground into powder and placed in an alumina crucible for sintering in an argon-protected tube furnace. The temperature is increased to 750-850℃ at a rate of 5℃ / min and held for 3 hours. Heating is then stopped, and the material is cooled to room temperature in the furnace to obtain a silicon-carbon composite anode material with a multilayer amorphous carbon coating structure. In this process, glucose pyrolyzes first at a lower temperature to form a dense inner carbon layer that is tightly bonded to the silicon core; asphalt powder pyrolyzes at a higher temperature to form a tough outer carbon layer. The two work together to construct the multilayer coating structure.

[0052] The properties of the material obtained in this embodiment were characterized: The material obtained in this embodiment was fabricated into electrodes using conventional processes and assembled into CR2032 coin cells for testing. Constant current charge-discharge tests were conducted within a voltage range of 0.005-2V and a current density of 0.05C. The initial discharge specific capacity reached 2750 mAh / g, with an initial efficiency of 88%. After 200 cycles at a current density of 0.5C, the capacity retention was 87%. This multi-carbon source "one-pot method" successfully prepared silicon-carbon anode materials with excellent electrochemical performance while greatly simplifying the process.

[0053] Specifically, such as Figure 1 The image shown is a scanning electron microscope (SEM) image of the silicon-carbon composite anode material provided in this embodiment. The material was stirred using a ball mill, resulting in spherical or near-spherical particles that were relatively uniformly dispersed. Thin, flake-like graphene layers with wrinkled and curled edges were clearly visible on the outer layer of the particles, with some graphene sheets forming bridges between the particles. The multilayer structure had distinct boundaries, was completely coated, and showed no obvious damage or detachment.

[0054] Example 3 This embodiment provides a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method," which includes the following steps: Step S1: In a ball mill jar, add 13 parts of nano-silica powder, 2 parts of glucose, 1 part of phenolic resin, 40 parts of water-based graphene dispersion (5% solid content), and 10 parts of deionized water all at once. Then add zirconium beads (material to zirconium beads mass ratio of 1:10), seal, and ball mill at 600-800 rpm for 12 hours to obtain a uniform composite slurry.

[0055] Step S2: Filter the ball-milled slurry to separate the zirconium beads, and then place the filtered wet filter cake in a vacuum oven at 80°C for 12 hours to dry it to obtain the precursor.

[0056] Step S3: Grind the dried precursor into powder, heat it to 700-800℃ in a tube furnace under argon protection at a heating rate of 5℃ / min, hold it at that temperature for 2 hours, and then cool it to room temperature with the furnace to obtain a multilayer coated silicon-carbon composite anode material.

[0057] According to the test, the material prepared in this embodiment has a first-cycle discharge specific capacity of 2680 mAh / g, an initial efficiency of 87%, and a capacity retention rate of 86% after 200 cycles at 0.5C.

[0058] Example 4 This embodiment provides a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method," which includes the following steps: Step S1: In a ball mill jar, add 13 parts of nano-silica powder, 2 parts of sucrose, 1 part of pitch powder, 40 parts of NMP graphene dispersion (5% solid content), and 10 parts of deionized water all at once. Then add zirconium beads (material to zirconium beads mass ratio of 1:10), seal, and ball mill at 900-1000 rpm for 8 hours to obtain a uniform composite slurry.

[0059] Step S2: Filter the ball-milled slurry to separate the zirconium beads, and then place the filtered wet filter cake in a vacuum oven at 80°C for 12 hours to dry it to obtain the precursor.

[0060] Step S3: Grind the dried precursor into powder, heat it to 750-850℃ in a tube furnace under argon protection at a heating rate of 5℃ / min, hold it at that temperature for 2 hours, and then cool it to room temperature with the furnace to obtain a multilayer coated silicon-carbon composite anode material.

[0061] According to the test, the material prepared in this embodiment has a first-cycle discharge specific capacity of 2720 mAh / g, an initial efficiency of 87%, and a capacity retention rate of 85% after 200 cycles at 0.5C.

[0062] Example 5 This embodiment provides a method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method," which includes the following steps: Step S1: In a mixing tank, add 13 parts of nano-silica powder, 2 parts of glucose, 1 part of phenolic resin, 40 parts of NMP graphene dispersion (5% solid content), and 10 parts of deionized water all at once. Then add zirconium beads (material to zirconium beads mass ratio of 1:10), seal, and ball mill at 700-800 rpm for 11 hours to obtain a uniform composite slurry.

[0063] Step S2: Filter the ball-milled slurry to separate the zirconium beads, and then place the filtered wet filter cake in a vacuum oven at 80°C for 12 hours to dry it to obtain the precursor.

[0064] Step S3: Grind the dried precursor into powder, heat it to 700-800℃ in a tube furnace under argon protection at a heating rate of 5℃ / min, hold it at that temperature for 4 hours, and then cool it to room temperature with the furnace to obtain a multilayer coated silicon-carbon composite anode material.

[0065] According to the test, the material prepared in this embodiment has a first-cycle discharge specific capacity of 2600 mAh / g, an initial efficiency of 86%, and a capacity retention rate of 84% after 200 cycles at 0.5C.

[0066] Specifically, such as Figure 2 The image shown is a scanning electron microscope (SEM) image of the silicon-carbon composite anode material provided in this embodiment. Mechanical stirring was used during the preparation process. The material consists of spherical or near-spherical particles, which are relatively uniformly dispersed. The multilayer structure is also intact, with no obvious damage or detachment observed. The morphology is similar to... Figure 1 The results are consistent with the ball milling method, proving that the one-pot method has repeatable morphology.

[0067] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the above-described division of functional units and modules is merely an example. In practical applications, the above functions can be assigned to different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit. Furthermore, the specific names of the functional units and modules are only for easy differentiation and are not intended to limit the scope of protection of this application. The specific working process of the units and modules in the above system can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here.

[0068] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can occur depending on design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method", characterized in that, Includes the following steps: Step S1: Add nano-silicon powder, solid carbon source, graphene dispersion and solvent to a stirring device according to a preset ratio and stir to obtain composite slurry; Step S2: Perform solid-liquid separation on the composite slurry, and dry the wet material obtained after solid-liquid separation to obtain a silicon-carbon precursor; Step S3: Heat-treat the silicon-carbon precursor under an inert atmosphere to obtain a silicon-carbon composite anode material.

2. The method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method" according to claim 1, characterized in that, The solid carbon source includes one or two of glucose or sucrose, phenolic resin, and asphalt powder.

3. The method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method" according to claim 1, characterized in that, The graphene dispersion is an N-methylpyrrolidone solution or an aqueous dispersion.

4. The method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method" according to claim 1, characterized in that, The sum of the masses of the nano-silicon powder, solid carbon source, and graphene dispersion is the total mass. The nano-silicon powder accounts for 60% to 70% of the total mass. The solid carbon source accounts for 10% to 15% of the total mass. The graphene dispersion accounts for 15% to 25% of the total mass.

5. The method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method" according to claim 1, characterized in that, The solid content of the graphene dispersion is 5%.

6. The method for preparing multilayer coated silicon-carbon composite anode materials by a "one-pot method" according to claim 1, characterized in that, In step S1, the stirring device is a ball mill, and the speed of the ball mill during stirring is 600 rpm to 1000 rpm, and the stirring duration is 8 h to 12 h.

7. The method for preparing multilayer coated silicon-carbon composite anode materials using a "one-pot method" according to claim 1, characterized in that, In step S2, the drying temperature is 80℃~100℃, and the drying duration is 12h.

8. The method for preparing multilayer coated silicon-carbon composite anode materials by a "one-pot method" according to claim 1, characterized in that, In step S3, the temperature of the heat treatment is 600℃~800℃.

9. The method for preparing multilayer coated silicon-carbon composite anode materials by a "one-pot method" according to claim 1, characterized in that, In step S3, the heat treatment includes a heating stage and a holding stage. The heating stage lasts for 60 min to 120 min, and the holding stage lasts for 2 h to 4 h.

10. The method for preparing multilayer coated silicon-carbon composite anode materials by a "one-pot method" according to claim 1, characterized in that, The solvent used is deionized water.