LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode materials, their preparation methods, applications, and lithium-ion batteries

By using LLTO-Li3BO3 gradient coating to coat lithium-rich manganese-based cathode materials, the structural instability and ion conduction efficiency issues during cycling were resolved. This achieved long-term cycling stability and efficient ion transport under high voltage and high rate conditions, simplifying the production process and reducing costs.

CN123120694APending Publication Date: 2026-11-17CENT SOUTH UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611369239.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-rich manganese-based cathode materials are prone to lattice oxygen release during cycling, leading to irreversible structural changes, severe voltage decay, low ionic conductivity, poor rate performance, and violent interfacial reactions, which cannot meet the requirements of long-cycle and high-safety industrial applications.

Method used

By using LLTO-Li3BO3 gradient coating material, and through sol-gel blending coating combined with segmented temperature-controlled calcination, an inner LLTO layer is constructed to provide a fast lithium-ion conduction channel, an outer Li3BO3 layer forms a dense barrier, and a gradient interface in the middle eliminates heterogeneous interface impedance, thus realizing a bidirectional gradient structure.

Benefits of technology

It significantly improves the cycling stability and voltage retention of materials, enhances ion transport efficiency, reduces interfacial impedance, simplifies processes and reduces costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120694A_ABST
    Figure CN123120694A_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery cathode material technology, and more particularly to an LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, its preparation method, applications, and lithium-ion batteries. The LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material includes a core and a shell coating the core. The core is a lithium-rich manganese-based material; the shell comprises an LLTO and Li3BO3 composite material, wherein the LLTO content decreases gradient from the core to the surface, and the Li3BO3 content increases gradient from the core to the surface. This invention innovatively uses LLTO-Li3BO3 as a co-coating material, further enhanced by its bidirectional gradient structure, thus achieving synergy and improving the long-cycle stability of the lithium-rich manganese-based material under high voltage, high rate, and wide temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery cathode material technology, and more particularly to an LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, its preparation method, application, and lithium-ion battery technology. Background Technology

[0002] Lithium-rich manganese-based cathode materials (usually denoted as xLi₂MnO₃·(1-x)LiMO₂, where M is a transition metal such as Ni, Co, or Mn) possess ultra-high specific capacity (theoretical specific capacity can reach over 300 mAh / g, and actual reversible capacity often exceeds 250 mAh / g) and high operating voltage (3.0~4.8V vs Li₂). + With its advantages such as abundant manganese resources and the presence of Li₂O₃, Li₂O₃, and other manganese, it is considered one of the core candidate materials for next-generation high-energy-density lithium-ion batteries, showing broad application prospects in power batteries, energy storage batteries, and other fields. However, this material has significant drawbacks: it is prone to lattice oxygen release during cycling, leading to an irreversible transformation of the layered structure to the spinel phase, causing severe voltage decay (voltage drop of more than 0.5V after hundreds of cycles) and capacity decay; at the same time, its intrinsic ionic conductivity is low (approximately 10⁻⁶ Ω·cm). -8 ~10 -7 The polarization is severe during charging and discharging, resulting in poor rate performance. In addition, the interfacial reaction between the material surface and the electrolyte is intense, and transition metal ions are easily dissolved and catalyze the decomposition of the electrolyte, further exacerbating the deterioration of cycle stability.

[0003] To address these issues, various modification strategies have been developed in existing technologies, including elemental doping (such as doping with Al, Mg, and Zr to strengthen the crystal structure), morphology manipulation (such as preparing nanorods and microspheres to shorten ion diffusion paths), and surface coating (constructing a protective layer to isolate the material from direct contact with the electrolyte). Among these, surface coating has become a research hotspot due to its ease of operation and targeted nature. Commonly used coating materials include metal oxides such as Al₂O₃ and TiO₂, and lithium-based compounds such as LiPO₃ and LiAlO₂. However, these coating materials have significant limitations: metal oxides are mostly insulators or low-ionic conductors, which increase interfacial resistance and sacrifice the material's ion transport efficiency; while lithium-based compounds can provide lithium ions, their chemical stability is insufficient, and they are prone to side reactions with the electrolyte under high voltage, making it difficult to maintain the integrity of the coating layer over a long period. Therefore, they cannot simultaneously solve the problem of synergistic optimization of structural stability, interfacial compatibility, and ion conduction efficiency.

[0004] Despite years of research that has led to certain improvements in the performance of lithium-rich manganese-based cathode materials, existing modification methods struggle to balance high capacity retention, low voltage decay rate and excellent rate performance. As a result, their cycle life (especially under high-voltage and high-rate working conditions) still cannot meet the industrial application requirements for long-cycle batteries (e.g., more than 1000 cycles) and high safety, which limits their popularization in practical battery systems. Therefore, developing a modification technology that can simultaneously solve the problems of structural stability, interface compatibility and ion conduction efficiency of lithium-rich manganese-based materials has become a key breakthrough to promote the industrial application of such materials. Contents of the Invention

[0005] To solve the problems existing in the prior art, the first object of the present invention is to provide an LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, aiming to provide a brand-new cathode active material that takes into account excellent high-voltage, high-rate and long-cycle stability.

[0006] The second object of the present invention is to provide the preparation method and application of the aforementioned LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material.

[0007] The third object of the present invention is to provide a lithium ion battery comprising the aforementioned LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material.

[0008] An LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, comprising a core and a shell coating the core; the aforementioned core is a lithium-rich manganese-based material; the aforementioned shell comprises an LLTO and Li3BO3 composite material, wherein the content of LLTO decreases gradiently in the direction from the core to the surface, and the content of Li3BO3 increases gradiently in the direction from the core to the surface.

[0009] The present invention innovatively adopts LLTO-Li3BO3 as a combined coating material, and further cooperates with its bidirectional gradient structure, which can achieve synergy and improve the long-cycle stability of the lithium-rich manganese-based material under high-voltage, high-rate and wide temperature range conditions.

[0010] In the present invention, the chemical formula of the lithium-rich manganese-based material is xLi2MnO3·(1-x)LiTMO2, wherein TM is at least one of Ni, Co and Mn, and 0<x<1.

[0011] In the present invention, the chemical formula of LLTO is, for example, La (5 / 8)-y Li 3y TiO3, wherein 0<y<0.15, and further can be 0.1~0.13.

[0012] In this invention, the molar ratio of LLTO to Li3BO3 is 1:0.04~0.15, preferably 1:0.06~0.12. Under the preferred ratio, better composition and structural compatibility can be obtained, which helps to further enhance the wide temperature range and fast charging performance of the modified lithium-rich manganese-based material.

[0013] The thickness of the shell coating is 5~50nm.

[0014] As an optional option, the LLTO in the shell is 0.5-5% of the core weight; further, it can be 1-3%, and more preferably 1-2%. The preferred coating amount helps to further enhance the wide-temperature range and fast-charging performance of the modified lithium-rich manganese-based material.

[0015] This invention also provides a method for preparing the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, comprising the following steps:

[0016] Step 1:

[0017] A composite adhesive was prepared by mixing LLTO precursor a, Li3BO3 precursor b, and a chelating agent and carrying out a complexation reaction; the ratio of the amount of chelating agent added to the total molar amount of Ti and La in LLTO precursor a was 1~2.5:1.

[0018] Step 2:

[0019] A lithium-rich manganese-based material and a composite adhesive were mixed and then dried to obtain a coated precursor; the drying temperature was 45~75℃.

[0020] Step 3:

[0021] The coated precursor was subjected to gradient calcination to synthesize and gradient distribute LLTO and Li3BO3, thereby obtaining the LLTO-Li3BO3 gradient coated lithium-rich manganese-based cathode material.

[0022] Gradient calcination includes a first stage of calcination at a temperature of 400~500℃ and a second stage of calcination at a temperature of 600~700℃.

[0023] This invention innovatively employs a sol-gel method for coating, combined with coating conditions and a gradient mechanism. Based on the difference in nucleation behavior between LLTO and Li3BO3, it is possible to unexpectedly construct the composite material with the special bidirectional gradient coating structure in situ. Studies have shown that the material prepared by the method exhibits excellent long-cycle stability under high pressure and high rate.

[0024] This invention differs from conventional single-coating and mixed homogeneous coating methods. It utilizes a unique preparation condition combining sol-gel blend coating and segmented temperature-controlled calcination. Taking advantage of the inherent differences in hydrolytic activity and crystallization nucleation kinetics between LLTO and Li3BO3 precursors, the highly active LLTO precursor preferentially crystallizes near the matrix interface during the low-temperature stage. During the high-temperature stage, the inert boron source gradually crystallizes from the particle surface inwards to generate Li3BO3, spontaneously forming a bidirectional continuous gradient coating structure with an inner layer rich in LLTO and an outer layer rich in Li3BO3. This gradient structure provides a rapid lithium-ion conduction channel through the inner LLTO layer, while the outer Li3BO3 layer forms a dense barrier resistant to electrolyte corrosion. The intermediate gradient interface eliminates interphase interface impedance, synergistically improving the material's high-voltage long-cycle stability and rate performance.

[0025] This invention utilizes a one-step sol-gel co-coating coupled precursor hydrolysis activity differential gradient nucleation + staged low-temperature calcination process to form a coating structure, achieving a triple synergistic effect of "inner layer LLTO constructing continuous fast ion conduction channels + outer layer Li3BO3 constructing a dense anti-side reaction barrier + continuous gradient interface eliminating heterogeneous interface impedance". This significantly improves the cycling stability and voltage retention rate of the material, enhances ion transport efficiency to improve rate performance, and simplifies the coating process and reduces industrial production costs.

[0026] In this invention, precursor material a includes a lanthanum source, a lithium source, and a titanium source.

[0027] The lanthanum source is one of La(NO3)3·6H2O, La2O3, or a mixture thereof;

[0028] The lithium source is one of LiNO3 and Li2CO3 or a mixture thereof;

[0029] The titanium source is one of tetrabutyl titanate, TiCl4, or a mixture thereof; the boron source is one of H3BO3, LiBO2, or a mixture thereof.

[0030] The elements in precursor raw material a are proportioned according to the LLTO stoichiometric ratio.

[0031] Precursor material b includes at least one of boron source and lithium source;

[0032] In precursor b, the molar ratio of Li / B is 2.9~3.2:1.

[0033] Chelating agents include at least one of citric acid, ethylene glycol, glycerol, tartaric acid, and disodium EDTA;

[0034] The ratio of the amount of chelating agent added to the total molar amounts of Ti and La in the precursor raw material a of LLTO is 1.5~2:1;

[0035] The solvent for the complexation reaction is one of deionized water, ethanol, or a mixture thereof.

[0036] In this invention, in step 2, the mixing process is carried out under ultrasonic assistance;

[0037] The ultrasonic dispersion power is 200~500W, the time is 30~60min; the stirring temperature is 40~60℃, and the stirring speed is 300~500r / min;

[0038] The atmosphere for the first and second stages of calcination can be at least one of nitrogen or rare gases.

[0039] The first calcination stage lasts for 1-4 hours, and the second calcination stage lasts for 1-4 hours.

[0040] The present invention also provides an application of the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material, which is used as a cathode active material for the preparation of lithium-ion batteries.

[0041] The present invention also provides a lithium-ion battery comprising the aforementioned LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material.

[0042] The lithium-ion battery of the present invention, except for the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material described in the present invention, may have other known components and structural arrangements.

[0043] Beneficial effects

[0044] The gradient structure reduces interfacial impedance: With no obvious phase interface, lithium-ion transport resistance is significantly reduced, and the interfacial impedance growth rate during cycling is more than 50% lower than that of Al2O3-coated materials. Simultaneously, the high ionic conductivity of lithium lanthanum titanate constructs an efficient transport channel, increasing the lithium-ion diffusion coefficient to 10. -7 ~10 -8 cm 2 / s (2 to 3 orders of magnitude higher than traditional coating materials).

[0045] Synergistic improvement in cycling and voltage stability: Gradient distribution + staged calcination makes the coating layer more stable during cycling, effectively suppressing oxygen release and layered-spinel phase transformation in lithium-rich manganese-based materials. After 200 cycles at 1C, the capacity retention rate is ≥90% (only 50%~60% for uncoated materials), the voltage decay is ≤0.2V (over 0.5V for uncoated materials), and the structural integrity is significantly improved.

[0046] Simple process with controllable cost: The sol-gel method is adopted for coating, which achieves high uniformity of raw material mixing, and the thickness and coating amount of the coating layer are easy to adjust; the calcination temperature (400~700℃) is lower than the high-temperature process (800~1000℃) for traditional oxide coating, reducing energy consumption by 25%~35%; the lanthanum source and titanium source used are both industrially available raw materials, and the overall cost is 40%~50% lower than that of noble metal coating (such as RuO2);

[0047] Strong industrial adaptability: The production process can rely on existing positive electrode material synthesis equipment (ball mill, spray dryer, tube furnace, etc.) without customizing special devices; the coating amount can be flexibly adjusted according to application scenarios (high rate is required for power batteries, long cycle life is required for energy storage batteries), with excellent compatibility for large-scale production, providing a feasible path for the industrial application of lithium-rich manganese-based materials. Brief Description of the Drawings

[0048] Figure 1 The cycle diagram of the button cell prepared in Example 1 at room temperature and 1C;

[0049] Figure 2 is the specific capacity-voltage curve diagram of Example 1. Detailed Description of the Embodiments

[0050] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.

[0051] To achieve the above objectives, the present invention adopts the following technical solutions:

[0052] An optional LLTO-Li3BO3 gradient coated lithium-rich manganese-based positive electrode material, comprising a lithium-rich manganese-based base material, and lithium lanthanum titanate and Li3BO3 coated on the surface layer of the material, wherein the chemical formula of lithium lanthanum titanate (LLTO) is La (5 / 8)-y Li 3y TiO3 (0<y<0.15), preferably y=0.125 (La 0.5 Li 0.375 TiO3).

[0053] An optional preparation method of the LLTO-Li3BO3 gradient coated lithium-rich manganese-based positive electrode material, said preparation method comprising the following steps:

[0054] Step 1: Prepare gradient LLTO-Li3BO3 composite sol; mix lanthanum source, lithium source, and titanium source in a molar ratio of La:Li:Ti = (0.4~0.6):(0.3~0.45):1; the molar ratio of boron source to lithium lanthanum titanate is 0.12:1 in a solvent, stir until completely dissolved, add citric acid or ethylene glycol as a chelating agent to adjust the pH to 3~6, ​​and continue stirring to form a transparent and uniform composite sol that can achieve gradient deposition.

[0055] Step 2: In-situ gradient coating reaction is carried out. The lithium-rich manganese-based matrix powder is added to the above-mentioned gradient composite sol and ultrasonically dispersed at 200-500 W for 30-60 min to ensure thorough particle dispersion. The mixture is then stirred at a constant temperature of 40-60℃ and 300-500 r / min. Utilizing the difference in hydrolysis rates between the titanium and boron sources, LLTO preferentially forms dense nuclei on the matrix surface, while Li3BO3 gradually deposits on the outer surface as the reaction proceeds until the solvent is completely evaporated, obtaining a coated precursor with a gradient composition distribution. The mass ratio of the composite sol to the lithium-rich manganese-based matrix is ​​0.5%-5%.

[0056] Step 3: Calcination and solidification. The gradient-coated precursor is placed in an atmosphere furnace and calcined using a two-stage process.

[0057] First stage calcination: Pre-calcination at 400~500℃ for 1~4 hours to remove organic matter and initially fix the gradient distribution;

[0058] Second stage calcination: calcination at 600~700℃ for 1~4h to crystallize the coated phase without interdiffusion, preserving the radial composition gradient; heating rate 2~5℃ / min, inert gas atmosphere.

[0059] This invention provides an in-situ coated lithium-rich manganese-based cathode material and its preparation method: by combining sol-gel coating with low-temperature calcination, a continuously distributed coating layer with "gradual decrease of LLTO phase and gradual increase of Li3BO3 phase from the matrix outward" is achieved, which not only improves the cycle stability and voltage retention rate of the material, but also enhances the ion transport efficiency to improve rate performance, while simplifying the coating process and reducing the cost of industrial production.

[0060] More preferably, in the preparation of lithium-rich manganese-based matrix materials, the lithium source is one or a mixture of Li2CO3, LiOH·H2O; the manganese source is one or a mixture of MnO2, Mn3O4, Mn(NO3)2·4H2O; the nickel source is one or a mixture of Ni(NO3)2·6H2O, Ni(CH3COO)2, NiCO3, NiSO4, NiO; and the cobalt source is one or a mixture of Co(NO3)2·6H2O, Co(CH3COO)2, CoSO4, Co3O4.

[0061] In a further preferred embodiment, the calcination temperature in the preparation of lithium-rich manganese-based matrix material is 600~900℃, and the calcination time is 5~15h.

[0062] In a further preferred embodiment, in the preparation of lithium-rich manganese-based matrix materials, the ball milling is a planetary ball mill with a ball-to-material mass ratio of 10:1 to 20:1, a rotation speed of 300 to 500 r / min, and a time of 2 to 6 h; the calcination temperature is 600 to 900 °C, the holding time is 5 to 15 h, and the heating rate is 3 to 8 °C / min.

[0063] More preferably, the grinding balls are made of ceramic and have a diameter of 5 mm, and the ratio of the total mass of the grinding balls to the total mass of the lithium / manganese / nickel / cobalt source raw material powder is 10:1 to 20:1.

[0064] More preferably, in the first step, the lanthanum source is one of La(NO3)3·6H2O, La2O3, or a mixture thereof.

[0065] More preferably, in the first step, the lithium source is one of LiNO3, Li2CO3, or a mixture thereof.

[0066] More preferably, in the first step, the titanium source is one of tetrabutyl titanate, TiCl4, or a mixture thereof.

[0067] More preferably, in the first step, the boron source is one of H3BO3, LiBO2, or a mixture thereof.

[0068] More preferably, in the first step, the solvent is one of deionized water, ethanol, or a mixture thereof.

[0069] More preferably, in the first step, the chelating agent is one of citric acid and ethylene glycol; the amount of the chelating agent added is related to the metal ions (La). 3+ Ti 4+ The molar ratio of ) is 1~2.5:1.

[0070] More preferably, in the second step, the ultrasonic dispersion power is 200~500W, the time is 30~60min; the stirring temperature is 40~60℃, and the stirring rate is 300~500r / min.

[0071] The following specific embodiments are provided to better illustrate this application.

[0072] In this invention, unless otherwise stated, the lithium-rich manganese-based matrix material may optionally be 0.5Li₂MnO₃·0.5LiNi. 0.1 Co 0.1 Mn 0.8 O2 can be a commercial product or prepared by the following methods:

[0073] According to the chemical formula 0.5Li₂MnO₃·0.5LiNi 0.1 Co 0.1 Mn 0.8 The following stoichiometric amounts of LiOH·H2O (purity ≥99.5%), MnO2 (purity ≥99.0%), Ni(NO3)2·6H2O (purity ≥99.0%), and Co(NO3)2·6H2O (purity ≥99.0%) were weighed and fed into a planetary ball mill at a ball-to-material mass ratio of 15:1. The milling speed was 400 r / min, and the mixture was milled for 4 hours to obtain a mixed powder.

[0074] The mixed powder was placed in an alumina crucible and then placed in a box sintering furnace. The temperature was increased to 800℃ at 5℃ / min under an air atmosphere and held for 10 hours. The mixture was then cooled to room temperature with the furnace and ground to obtain lithium-rich manganese-based matrix powder (particle size 1~3μm).

[0075] Example 1

[0076] Step 1:

[0077] According to the chemical formula La 0.5 Li 0.375 Weigh out the stoichiometric proportions of TiO3 (LLTO) precursor material a (including La(NO3)3·6H2O (purity ≥99.5%), LiNO3 (purity ≥99.0%), and tetrabutyl titanate (purity ≥98.0%) according to the LLTO stoichiometric ratio), and separately weigh out the Li3BO3 precursor material b (source B, including stoichiometric amounts of lithium nitrate and H3BO3, wherein the molar ratio of H3BO3 to LLTO is 0.12:1). Add the above precursor material a and precursor material b to 50 mL of a mixed solvent of deionized water and ethanol (volume ratio 2:1) and stir to dissolve. Add a complexing agent (citric acid, purity ≥99.5%) (molar ratio of La+Ti metal ions 1.5:1), adjust the pH to 4.5, and stir at 40℃ and 300 r / min for 2 h to form a uniform and transparent sol.

[0078] Step 2: Coating reaction and calcination solidification

[0079] Weigh 10g of lithium-rich manganese-based matrix powder and add it to the sol in step 1 (the LLTO in the sol is 1% of the weight of the lithium-rich manganese-based material). Disperse it ultrasonically at 300W for 45min, and then stir it at 50℃ (drying temperature) and 400r / min until the solvent is completely evaporated to obtain a dry gel-like coated precursor.

[0080] The precursor was placed in an alumina crucible and then placed in a tube sintering furnace. Nitrogen gas was introduced (flow rate 60 mL / min), and a two-stage stepped temperature control process was adopted: first, the temperature was increased to 450℃ at 2℃ / min (T1: low temperature calcination temperature) and held for 2 hours, and then the temperature was increased to 650℃ at 5℃ / min (T2: high temperature calcination temperature) and held for 2 hours. After the holding period, the temperature was cooled to room temperature with the furnace to obtain a lithium-rich manganese-based positive electrode active material with lithium titanate lanthanum-Li3BO3 gradient coating (coating thickness of about 15 nm).

[0081] Step 3: Button cell fabrication and testing

[0082] A slurry was prepared by dispersing the positive electrode active material (lithium-rich manganese-based positive electrode active material with lithium titanate lanthanum-Li3BO3 gradient coating) in NMP according to the mass ratio of SuperP: carbon nanotubes: PVDF = 85:5:3:7. The slurry was then coated onto aluminum foil and vacuum dried at 80℃ for 12 hours before being punched into 2032 specification electrode sheets.

[0083] Using lithium metal as the counter electrode, Celgard 2400 as the separator, and 1 mol / L LiPF6 / EC+DMC+EMC (volume ratio 1:1:1) as the electrolyte, CR2032 (diameter 20 mm, thickness 3.2 mm) coin cells were assembled and tested in the voltage range of 3.0~4.8V.

[0084] Example 2

[0085] Compared to Example 1, the only difference is that in step 2, the LLTO in the sol is 2% of the weight of the lithium-rich manganese-based material;

[0086] In step 2, the complexing agent is twice the total molar amount of La+Ti metal, and the drying temperature is 60℃;

[0087] The low-temperature calcination temperature is 400℃, and the holding time at the low-temperature calcination temperature is 3h;

[0088] The high-temperature calcination temperature is 700℃, and the holding time is 1.5h;

[0089] All other operations and parameters are the same as in Example 1.

[0090] Example 3

[0091] Compared with Example 1, the only difference is that in step 2, the LLTO in the sol is 3% of the weight of the lithium-rich manganese-based material; the low-temperature calcination temperature is 500°C; and the holding time at the low-temperature calcination temperature is 1 hour.

[0092] The high-temperature calcination temperature was 600℃, and the holding time was 3h; other operations and parameters were the same as in Example 1.

[0093] Example 4

[0094] Compared to Example 1, the only difference is that in step 1, the chemical formula of LLTO is La. 0.525 Li 0.3 The molar ratio of B / LLTO in TiO3 and B source is 0.06:1. The total coating amount of coating material and other operations and parameters are the same as in Example 1.

[0095] Comparative Example 1

[0096] Compared with Example 1, the only difference is that the lithium-rich manganese-based active material is used as the positive electrode active material, and the coating treatment in steps 1 and 2 is not performed. The electrode preparation, coin cell assembly and testing operations and parameters in step 3 are the same as in Example 1.

[0097] Comparative Example 2

[0098] Preparation and testing of Al2O3-coated lithium-rich manganese-based cathode materials

[0099] Step 1 (Preparation of Al2O3 coating solution): Calculate the required molar amount of aluminum based on an Al2O3 coating amount of 2%. Weigh Al(NO3)3·H2O (purity ≥99.0%), add an appropriate amount of a mixed solvent of deionized water and ethanol (volume ratio 2:1), and stir to dissolve; add citric acid (to react with Al2O3)... 3+ The pH was adjusted to 4.5 (molar ratio 1.5:1), and the mixture was stirred at 40°C and 300 r / min for 2 hours to form a uniform and transparent aluminum sol.

[0100] Step 2 (coating and calcination): Weigh 10 g of lithium-rich manganese-based matrix powder and add it to the above aluminum sol. Disperse it ultrasonically at 300 W for 45 min, and then stir it at 50℃ and 400 r / min until the solvent is completely evaporated to obtain a dry gel-like coated precursor.

[0101] The precursor was placed in a box sintering furnace and heated to 550°C at 5°C / min in air atmosphere, held for 4 hours, cooled to room temperature with the furnace, and ground to obtain Al2O3-coated lithium-rich manganese-based cathode material.

[0102] The electrode preparation, coin cell assembly, and testing steps are the same as in Example 1;

[0103] Comparative Example 3

[0104] Compared with Example 1, the only difference is that in step 1, only LLTO precursor material is added, and precursor material b is no longer added. The missing Li3BO3 in the coating material is supplemented by an equal weight of LLTO. That is, the total coating amount of the coating material and other operations and parameters are the same as in Example 1.

[0105] Comparative Example 4

[0106] Compared with Example 1, the only difference is that in step 1, only H3BO3 is added to prepare lithium borate with lithium source, and the precursor raw material a for synthesizing LLTO is not added. The amount of coating material and other operations and parameters are the same as in Example 1.

[0107] Comparative Example 5

[0108] Compared with Example 1, the only difference is that the sol-gel liquid phase coating process is abandoned, and solid-phase dry powder direct physical mixing is adopted: the raw materials (precursor raw material a and precursor raw material b) of step 1 are mixed with lithium-rich manganese-based materials in solid phase and then subjected to calcination treatment in step 3. All other operations and parameters are the same as in Example 1.

[0109] Comparative Example 6

[0110] Compared with Example 1, in step 2, no low-temperature heat preservation treatment was performed, and the calcination was carried out directly at the high-temperature calcination temperature T2. Other operations and parameters were the same as in Example 1.

[0111] It is impossible to form a bidirectional gradient structure with an inner layer rich in LLTO and an outer layer rich in Li3BO3.

[0112] Comparative Example 7

[0113] Compared to Example 1, the only difference is that in step 1, the LLTO precursor is replaced with a stoichiometric precursor for the chemical synthesis of LATP (lithium aluminum titanium phosphate), wherein the chemical formula of LATP is Li 1.3 Al 0.3 Ti 1.7 (PO4)3, other operations and parameters are the same as in Example 1.

[0114] Comparative Example 8

[0115] Compared with Example 1, the only difference is that LLTO single-coated powder was prepared according to Comparative Example 3 and Li3BO3 single-coated powder was prepared according to Comparative Example 4. Then, the two modified powders were directly mixed in dry powder (the weight ratio of LLTO and lithium borate in the two dry powders was the same as in Example 1). In-situ cosol gradient coating was not performed. Each particle had an independent coating structure and there was no bidirectional gradient layer inside the single particle.

[0116] Comparative Example 9

[0117] Compared to Example 1, in step 2, the drying temperature is 90°C. All other operations and parameters are the same as in Example 1.

[0118] Comparative Example 10

[0119] Compared to Example 1, in step 1, the total molar ratio of citric acid to La+Ti metal was adjusted to 3.5:1.

[0120] The test results for each case are shown in Table 1:

[0121] Table 1:

[0122]

[0123] The performance test results of the above embodiments and comparative examples were compared, see... Figure 1 and Figure 2 As can be seen from the above comparison results, the beneficial effects of the present invention are as follows:

[0124] Synergistic improvement in cycling and voltage stability: The stable perovskite structure of the lithium titanate lanthanum coating can effectively suppress oxygen release and layered-spinel phase transformation during cycling of lithium-rich manganese-based materials. After 200 cycles at 1C, the capacity retention rate is ≥90% (compared to only 50%~60% for uncoated materials), the total voltage decay is ≤0.2V, and the structural integrity is significantly improved.

[0125] Dual optimization of interface and ion transport performance: The coating layer has high chemical inertness, which can reduce the dissolution of transition metal ions and electrolyte decomposition. The rate of increase of interface impedance during cycling is reduced by more than 50% compared with Al2O3 coated materials. At the same time, the high ionic conductivity of lithium lanthanum titanate constructs an efficient transport channel, with a capacity retention of ≥65% at 5C rate (compared to only 30%~40% for uncoated materials), and the lithium-ion diffusion coefficient is improved to 10. -7 ~10 -8 cm 2 / s (2-3 orders of magnitude higher than traditional coating materials);

[0126] The process is simple and the cost is controllable: the process of this invention is controllable and easy to implement. The lanthanum source and titanium source used are both industrial-grade and readily available raw materials. The overall cost is 40% to 50% lower than that of precious metal coating (such as RuO2).

[0127] Strong industrial adaptability: The production process can rely on existing cathode material synthesis equipment (ball mill, spray dryer, tube furnace, etc.) without the need for customized special equipment; the coating amount can be flexibly adjusted according to the application scenario (power batteries require high rate and energy storage batteries require long cycle time), and it has excellent compatibility for large-scale production, providing a feasible path for the industrial application of lithium-rich manganese-based materials.

[0128] This invention provides an in-situ gradient-coated lithium-rich manganese-based cathode material and its preparation method: by combining sol-gel coating with low-temperature calcination, a continuously distributed coating layer is achieved with "a decreasing gradient of LLTO phase and an increasing gradient of Li3BO3 phase from the matrix outwards". This not only improves the cycle stability and voltage retention rate of the material, but also enhances the ion transport efficiency to improve rate performance, while simplifying the coating process and reducing the cost of industrial production.

Claims

1. A lithium-rich manganese-based cathode material with LLTO-Li3BO3 gradient coating, comprising a core and a shell coating the core; characterized in that, The core is a lithium-rich manganese-based material; the shell comprises an LLTO and a Li3BO3 composite material, wherein the LLTO content decreases in gradient from the core to the surface, and the Li3BO3 content increases in gradient from the core to the surface.

2. The LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that, The chemical formula of the lithium-rich manganese-based material is xLi₂MnO₃·(1-x)LiTMO₂,0 <x<1。 3. The LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that, The chemical formula of LLTO is La (5 / 8)-y Li 3y TiO3, where 0 <y<0.15。 4. The LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that, The molar ratio of LLTO to Li3BO3 is 1:0.04~0.15; The thickness of the shell's coating layer is 5~50nm; The LLTO in the shell is 0.5-5% of the weight of the core; more preferably it can be 1-3%, and even more preferably 1-2%.

5. A method for preparing the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material according to any one of claims 1 to 4, characterized in that the step include: Step 1: A composite adhesive was prepared by mixing LLTO precursor a, Li3BO3 precursor b, and a chelating agent and carrying out a complexation reaction; the ratio of the amount of chelating agent added to the total molar amount of Ti and La in LLTO precursor a was 1~2.5:

1. Step 2: A lithium-rich manganese-based material and a composite adhesive were mixed and then dried to obtain a coated precursor; the drying temperature was 45~75℃. Step 3: The coated precursor was subjected to gradient calcination to synthesize and gradient distribute LLTO and Li3BO3, thereby obtaining the LLTO-Li3BO3 gradient coated lithium-rich manganese-based cathode material. Gradient calcination includes a first stage of calcination at a temperature of 400~500℃ and a second stage of calcination at a temperature of 600~700℃.

6. The preparation method of the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 5, characterized in that, Precursor material a includes lanthanum source, lithium source and titanium source. The lanthanum source is one of La(NO3)3·6H2O, La2O3, or a mixture thereof; The lithium source is one of LiNO3 and Li2CO3 or a mixture thereof; The titanium source is one of tetrabutyl titanate, TiCl4, or a mixture thereof; the boron source is one of H3BO3, LiBO2, or a mixture thereof. Precursor material b includes at least one of boron source and lithium source; Chelating agents include at least one of citric acid and ethylene glycol; The solvent for the complexation reaction is one of deionized water, ethanol, or a mixture thereof.

7. The preparation method of the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 5, characterized in that, In step 2, the mixing process is performed under ultrasound assistance; The ultrasonic dispersion power is 200~500W, the time is 30~60min; the stirring temperature is 40~60℃, and the stirring speed is 300~500r / min; The method for removing the solvent is evaporation.

8. The method for preparing the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material as described in claim 5, characterized in that, The first calcination stage lasts for 1-4 hours, and the second calcination stage lasts for 1-4 hours.

9. The application of the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material according to any one of claims 1 to 4, or the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material prepared by the preparation method according to any one of claims 5 to 8, characterized in that, It is used as a positive electrode active material in the preparation of lithium-ion batteries.

10. A lithium-ion battery, characterized in that, The material comprises the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material according to any one of claims 1 to 4, or the LLTO-Li3BO3 gradient-coated lithium-rich manganese-based cathode material prepared by the preparation method according to any one of claims 5 to 8.