Dry-process cathode materials and their preparation methods, sodium-ion batteries
By coating polyaniline onto a nickel-iron-copper-manganese matrix material to form a polyaniline coating layer, the problems of high investment in wet electrode process equipment and powder shedding caused by PTFE fibrillation are solved, achieving a dry-process positive electrode sheet with high peel strength and low film resistance, thus improving the performance and environmental friendliness of sodium-ion batteries.
Patent Information
- Application Number
- CN202611413229.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional wet electrode processes involve large investments in equipment and high energy consumption. Furthermore, the PTFE fibrillation mechanism results in weak chemical bonding between the fiber web and active particles/foil, leading to easy powder shedding, low peel strength, and high membrane resistance, which negatively impacts processing and electrochemical performance.
A polyaniline-coated nickel-iron-copper-manganese matrix material is used. The polyaniline coating layer is formed through spray drying and static reaction, which enhances the adhesion between the active particles and the foil. It is also mixed with PTFE to form a fibrous structure, which improves the peel strength and reduces the membrane resistance.
It significantly improves the peeling force of dry-process positive electrode, reduces film resistance, improves the long-cycle performance and high-rate discharge performance of the electrode, and reduces production costs and environmental impact.
Smart Images

Figure CN123120698A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, specifically to cathode materials for dry-process cathode sheets and dry-process cathode sheets and their preparation methods, and sodium-ion batteries; more specifically, to cathode materials for dry-process cathode sheets and their preparation methods, dry-process cathode sheets and their preparation methods, and sodium-ion batteries. Background Technology
[0002] The mainstream production method for positive and negative electrode sheets of lithium-ion and sodium-ion batteries is the wet coating process. This process can achieve good interfacial contact between the active material, conductive carbon black, and current collector through the design of the slurry system (the combination of solvent, binder, and conductive agent). However, the wet process is highly dependent on organic solvents such as N-methylpyrrolidone (NMP). Its preparation process involves long-term stirring and dispersion of the slurry, coating and drying, and solvent condensation and recovery. Not only is the equipment investment large and the energy consumption high, but the environmental pressure and recycling costs caused by solvent volatilization are becoming increasingly prominent in large-scale production.
[0003] Compared to traditional wet electrode processes, the novel dry electrode technology eliminates the steps of slurry preparation, wet film coating, solvent drying, and recycling, offering significant advantages in terms of cost and environmental protection. The dry electrode technology involves dry mixing of active materials, conductive agents, and PTFE binders using high-speed airflow or mechanical shear force. This stretches the PTFE particles under high shear stress, forming a network fiber structure that interweaves and fixes the components. The mixture is then directly laminated onto the current collector surface using a hot rolling process.
[0004] However, the cohesive force provided by the PTFE fibrillation mechanism mainly relies on the fiber network formed by PTFE to bind the positive electrode active particles. Since the chemical bonding between the fiber network and the active particles and foil is weak, powder shedding is easy to occur, resulting in low peeling force. In addition, the contact between the active material and the foil is not good, which leads to high membrane resistance and thus affects the processing and electrochemical performance.
[0005] In view of this, the present invention is hereby proposed. Summary of the Invention
[0006] The primary objective of this invention is to provide a positive electrode material for dry-process positive electrode sheets. Polyaniline is a conductive polymer that combines adhesiveness and conductivity. By coating active particles (i.e., nickel-iron-copper-manganese matrix material) with polyaniline, the bonding effect between active particles and between active particles and foil can be enhanced, significantly improving the problem of powder shedding and thus increasing the peeling force of the electrode sheet. At the same time, the tighter contact between active particles and the conductivity of polyaniline itself can significantly reduce the film resistance.
[0007] The second objective of this invention is to provide a method for preparing a cathode material for dry-process cathode sheets.
[0008] A third objective of this invention is to provide a dry-process positive electrode sheet having high peel strength and low film resistance.
[0009] The fourth objective of this invention is to provide a method for preparing a dry-process positive electrode.
[0010] The fifth objective of this invention is to provide a sodium-ion battery.
[0011] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: The present invention first provides a positive electrode material for dry-process positive electrode sheets, which includes a nickel-iron-copper-manganese matrix material and a polyaniline coating layer covering the nickel-iron-copper-manganese matrix material.
[0012] Furthermore, the thickness of the polyaniline coating layer is 0.05~2μm.
[0013] Furthermore, the general formula of the nickel-iron-copper-manganese matrix material is NaNi. x Mn y Fe z Cu 1-x-y-z O2, where 0.1≤x≤0.5, 0.1≤y≤0.5, 0.1≤z≤0.4, and x+y+z<1.
[0014] The present invention further provides a method for preparing a positive electrode material for dry-process positive electrode sheets, comprising the following steps: mixing a nickel-iron-copper-manganese matrix material with an oxidant solution and then spray-drying it to obtain a mixed material; spraying an aniline solution onto the particle surface of the mixed material and allowing it to react statically to form a polyaniline coating layer, thereby obtaining a positive electrode material for dry-process positive electrode sheets.
[0015] Furthermore, the oxidant solution includes an ammonium persulfate solution.
[0016] Furthermore, the molar concentration of the oxidant solution is 0.01 mol / L to 0.1 mol / L.
[0017] Furthermore, the molar concentration of the aniline solution is 0.05 mol / L to 0.3 mol / L.
[0018] Furthermore, the pH value of the aniline solution is 2.0 to 4.0.
[0019] Furthermore, the mass ratio of aniline in the aniline solution to the nickel-iron-copper-manganese matrix material is 0.001~0.03:1.
[0020] Furthermore, the temperature of the static reaction is 0℃~5℃, and the time of the static reaction is 4h~6h.
[0021] The present invention also provides a dry-process positive electrode sheet, comprising the above-mentioned positive electrode material for dry-process positive electrode sheets.
[0022] Furthermore, the peeling force of the dry-process positive electrode is ≥9N / m.
[0023] Furthermore, the film resistance of the dry-process positive electrode is ≤500mΩ.
[0024] The present invention also provides a method for preparing a dry-process positive electrode sheet, comprising the following steps: mixing the dry-process positive electrode sheet with a positive electrode material, a conductive agent and PTFE and then performing a fiberization treatment to obtain a fiberized material; hot-pressing the fiberized material to obtain a self-supporting film; hot-pressing the self-supporting film with a positive electrode current collector to obtain a dry-process positive electrode sheet.
[0025] Furthermore, the mass ratio of the positive electrode material, the conductive agent, and the PTFE used in the dry-process positive electrode sheet is 95~97:1~2:2~3.
[0026] Furthermore, the mixing temperature is ≤19°C.
[0027] Furthermore, the fiberization process is stopped when the temperature reaches 70°C.
[0028] Furthermore, the positive current collector comprises carbon-coated aluminum foil.
[0029] The present invention also provides a sodium-ion battery, comprising the above-mentioned dry-process positive electrode material or the above-mentioned dry-process positive electrode.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: The positive electrode material for dry positive electrode sheets provided by the present invention adopts polyaniline-coated active particles (i.e., nickel-iron-copper-manganese matrix material) which has both adhesiveness and conductivity, which can enhance the bonding effect between active particles and between active particles and foil, significantly improve the problem of powder shedding, and thus improve the peeling force of the electrode sheet; at the same time, the tighter contact between active particles and the conductivity of polyaniline itself can significantly reduce the film resistance. Attached Figure Description
[0031] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0032] Figure 1 A comparison of the peeling force results of the dry-process positive electrode sheets prepared in Examples 1-3 and Comparative Example 1 provided by the present invention; Figure 2 Comparison of film resistance results of dry-process positive electrode sheets prepared in Examples 1-3 and Comparative Example 1 provided by the present invention. Detailed Implementation
[0033] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0034] Unless otherwise specified, in this invention, terms such as "first aspect," "second aspect," "third aspect," and "fourth aspect" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, terms such as "first," "second," "third," and "fourth" serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.
[0035] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0036] Unless otherwise specified, in this invention, "one or more" or "at least one" refers to any one, any two, or any two or more of the listed items. "Several" refers to any two or more.
[0037] In a first aspect, the present invention provides a positive electrode material for dry-process positive electrode sheets, abbreviated as CFM@PANI. The positive electrode material for dry-process positive electrode sheets includes a nickel-iron-copper-manganese matrix material and a polyaniline coating layer covering the outer surface of the nickel-iron-copper-manganese matrix material.
[0038] This invention starts with active materials and provides a positive electrode material for dry-process positive electrode sheets. It has both conductivity and adhesion properties, which can improve the peeling force of dry-process positive electrode sheets and reduce the film resistance of dry-process positive electrode sheets, and has good application prospects.
[0039] Specifically, polyaniline is a conductive polymer that combines adhesiveness and conductivity. Coating active particles (i.e., nickel-iron-copper-manganese matrix material) with polyaniline enhances the adhesion between active particles and between active particles and the foil, significantly improving the problem of powder shedding. This, in turn, increases the peel strength of the electrode, thereby improving long-cycle performance. Simultaneously, the tighter contact between active particles and the inherent conductivity of polyaniline significantly reduce film resistance, which is beneficial for improving high-rate discharge performance.
[0040] In some specific embodiments, the thickness of the polyaniline coating layer is 0.05~2μm, for example 0.05μm, 0.1μm, 0.2μm, 0.25μm, 0.3μm, 0.5μm, 0.75μm, 0.8μm, 1μm, 1.3μm, 1.5μm, 1.7μm or 2μm.
[0041] In some specific embodiments, the general formula of the nickel-iron-copper-manganese matrix material is NaNi. x Mn y Fe z Cu 1-x-y-z O2, where 0.1≤x≤0.5, 0.1≤y≤0.5, 0.1≤z≤0.4, and x+y+z<1. Here, x can be, for example, 0.1, 0.2, 0.3, 0.4, or 0.5; y can be, for example, 0.1, 0.2, 0.3, 0.4, or 0.5; and z can be, for example, 0.1, 0.2, 0.3, or 0.4.
[0042] Secondly, this invention provides a method for preparing a positive electrode material for dry-process positive electrode sheets, which employs an in-situ polymerization method of aniline to coat the surface of active particles with polyaniline, specifically including the following steps: A nickel-iron-copper-manganese (CFM) matrix material is mixed with an oxidant solution and then spray-dried to obtain a mixed material. Specifically, the CFM matrix material is dispersed in an oxidant solution, stirred evenly, and then dried using a spray-drying method to obtain the mixed material.
[0043] Aniline monomer is dissolved in deionized water, and the pH value is adjusted to obtain an aniline solution. The aniline solution is then sprayed onto the surface of the particles of the mixed material at room temperature (e.g., 15~25℃), and allowed to react under low temperature conditions to form a polyaniline (PANI) coating layer in situ. After the reaction is completed, the material is washed with deionized water and ethanol in sequence, and then dried to obtain the dry-process positive electrode material, namely CFM@PANI.
[0044] Understandably, during the static reaction, aniline monomers undergo oxidative coupling polymerization under the action of an oxidant, forming a polyaniline coating layer on the surface of the nickel-iron-copper-manganese matrix material particles in situ. Subsequent washing removes unreacted oxidant, acid used to adjust the pH, water-soluble oligomers, byproducts, and other impurities.
[0045] Compared with conventional CFM cathode materials, i.e. cathode materials without polyaniline coating, the dry cathode sheet prepared using the CFM@PANI of this invention has significantly improved peel strength and significantly reduced film resistance, showing good application prospects.
[0046] In some specific embodiments, the oxidant solution includes an ammonium persulfate (APS) solution.
[0047] In some specific embodiments, the molar concentration of the oxidant solution is 0.01 mol / L to 0.1 mol / L, for example 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, and 0.1 mol / L.
[0048] In some specific embodiments, the molar concentration of the aniline solution is 0.05 mol / L to 0.3 mol / L; for example, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, and 0.3 mol / L.
[0049] In some specific embodiments, the pH value of the aniline solution is 2.0 to 4.0, for example 2.0, 2.2, 2.5, 2.8, 3.0, 3.3, 3.5, 3.7 or 4.0.
[0050] In some specific embodiments, the mass ratio of aniline in the aniline solution to the nickel-iron-copper-manganese matrix material is 0.001~0.03:1, for example 0.001:1, 0.003:1, 0.005:1, 0.008:1, 0.01:1, 0.02:1, 0.03:1.
[0051] In some specific embodiments, the temperature of the static reaction is 0℃~5℃, for example 0℃, 1℃, 2℃, 3℃, 4℃, 5℃.
[0052] In some specific implementations, the settling reaction time is 4h to 6h; for example, 4h, 5h, 6h.
[0053] Thirdly, the present invention provides a dry-process positive electrode sheet, which includes a positive electrode material for dry-process positive electrode sheets.
[0054] This dry-process positive electrode has high peel strength and low film resistance.
[0055] In some specific embodiments, the peeling force of the dry-process positive electrode sheet is ≥9N / m; for example, 9N / m, 10N / m, 11N / m, 12N / m, 13N / m, 14N / m, 15N / m, 16N / m, 18N / m, 20N / m.
[0056] In some specific embodiments, the film resistance of the dry-process positive electrode is ≤500mΩ, for example, 500mΩ, 450mΩ, 400mΩ, 350mΩ, 300mΩ, 250mΩ, 200mΩ, 150mΩ, or 100mΩ.
[0057] Fourthly, the present invention provides a method for preparing a dry-process positive electrode sheet, comprising the following steps: The dry-process positive electrode sheet is uniformly mixed with positive electrode material, conductive agent and PTFE (polytetrafluoroethylene), and then subjected to fiberization treatment to obtain the fiberized material.
[0058] The fibrous material is hot-pressed to obtain a self-supporting membrane.
[0059] The self-supporting membrane is hot-pressed together with the positive electrode current collector to obtain a dry positive electrode sheet.
[0060] Using dry electrode technology can eliminate processes such as slurry preparation, wet film coating, solvent drying and recycling, resulting in low cost and environmental friendliness.
[0061] Furthermore, the dry-processed positive electrode sheet prepared by this method exhibits high peel strength and low film resistance. The increased peel strength can alleviate the contact degradation caused by the continuous expansion and contraction of the active material during cycling, thereby improving long-cycle performance; the reduced film resistance can lower the battery's internal resistance, which is beneficial for improving high-rate discharge performance.
[0062] In some specific embodiments, the mass ratio of the positive electrode material, the conductive agent and the PTFE in the dry-process positive electrode sheet is 95~97:1~2:2~3, for example 95:2:3, 96:1.5:2.5 or 97:1:2.
[0063] In some specific embodiments, the conductive agent includes, but is not limited to, Super P (SP).
[0064] In some specific embodiments, the mixing temperature is ≤19°C. This can suppress premature fibrillation of PTFE and ensure uniform mixing of the components.
[0065] Specifically, the mixing process involves stirring. During stirring, the temperature rises due to friction between particles, and the faster the stirring speed, the faster the temperature rises. PTFE is prone to fibrosis when the temperature exceeds 19°C, which affects uniform dispersion. Therefore, the mixing temperature is set to ≤19°C to ensure uniform dispersion of PTFE.
[0066] In some specific embodiments, the fibrillation process is stopped when the temperature reaches 70°C. This allows for control over the degree of fibrillation of PTFE, terminating the process in a timely manner when the ideal fiber network is achieved, thus preventing excessive fibrillation from deteriorating the electrode performance.
[0067] In some specific embodiments, after the fiberization process, a step of sieving the fiberized material is included to remove excessively large agglomerates or insufficiently dispersed lumps formed during the fiberization process.
[0068] In some specific embodiments, the positive current collector comprises carbon-coated aluminum foil.
[0069] In some specific embodiments, the thickness of the dry-process positive electrode sheet is 100μm~150μm, for example 100μm, 110μm, 120μm, 130μm, 140μm, 150μm.
[0070] Fifthly, the present invention provides a sodium-ion battery comprising the above-mentioned dry-process positive electrode material or the above-mentioned dry-process positive electrode.
[0071] Sodium-ion batteries made using the above-mentioned dry-process cathode material or the above-mentioned dry-process cathode have excellent cycle performance, significantly improved high-rate discharge performance, and broad application prospects.
[0072] In some specific embodiments, the sodium-ion battery also includes a negative electrode, a separator, and an electrolyte, but this invention does not limit these components.
[0073] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0074] Example 1 The method for preparing the cathode material for dry-process cathode sheets provided in this embodiment includes the following steps: (1) Weigh 400g of nickel-iron-copper-manganese matrix material NaNi 0.33 Mn 0.33 Fe 0.3 Cu 0.04O2 was dispersed into 600g of APS solution with a molar concentration of 0.05mol / L and stirred for 2h until homogeneous to obtain a slurry. The slurry was then dried by spray drying to obtain a mixed material.
[0075] (2) Dissolve 4g of aniline monomer in 860ml of deionized water, and then adjust its pH value to 2.5 with hydrochloric acid to obtain an aniline solution with a molar concentration of 0.05mol / L, that is, the mass ratio of aniline to nickel-iron-copper-manganese matrix material is 0.01:1. At room temperature (20℃), the aniline solution is uniformly sprayed on the surface of the mixed material particles; then it is transferred to 3℃ and allowed to stand for 5h to form a polyaniline coating layer; then it is washed with deionized water and ethanol respectively, and dried to obtain the dry-process positive electrode material CFM@PANI, whose polyaniline coating layer has a thickness of 0.5μm.
[0076] The preparation method of the dry-process positive electrode sheet provided in this embodiment includes the following steps: The dry-process positive electrode sheet obtained in this embodiment is mixed evenly with positive electrode material CFM@PANI and conductive agent SP in a mass percentage ratio of 96.0% and 1.5%, respectively. Then, PTFE in a mass percentage of 2.5% is added and stirred at low speed until uniform. During the low-speed stirring process, the temperature does not exceed 19°C (during stirring, the temperature will rise due to interparticle friction, and the faster the stirring speed, the faster the temperature rises; after exceeding 19°C, PTFE is prone to fibrosis, affecting uniform dispersion. Therefore, a low-speed stirring process is set to ensure uniform dispersion of PTFE). Then, rapid stirring is performed for fibrosis treatment. The fibrosis treatment process is stopped when the temperature rises to 70°C, and fibrous material is obtained. The fibrous material is sieved and then hot-pressed to form a self-supporting film. The self-supporting film is then hot-pressed and laminated with carbon-coated aluminum foil to obtain a dry-process positive electrode sheet with a thickness of 146μm.
[0077] Example 2 The method for preparing the cathode material for dry-process cathode sheets provided in this embodiment includes the following steps: (1) Weigh 400g of nickel-iron-copper-manganese matrix material NaNi 0.33 Mn 0.33 Fe 0.3 Cu 0.04 O2 was dispersed into 300g of APS solution with a molar concentration of 0.05mol / L and stirred for 2h until homogeneous to obtain a slurry. The slurry was then dried by spray drying to obtain a mixed material.
[0078] (2) Dissolve 2g of aniline monomer in 860ml of deionized water, and then adjust its pH value to 3.0 with hydrochloric acid to obtain an aniline solution with a molar concentration of 0.25mol / L, that is, the mass ratio of aniline to nickel-iron-copper-manganese matrix material is 0.005:1. At room temperature (20℃), the aniline solution is uniformly sprayed on the surface of the mixed material particles; then it is transferred to 0℃ and allowed to stand for 6h to form a polyaniline coating layer; then it is washed with deionized water and ethanol respectively, and dried to obtain the dry-process positive electrode material CFM@PANI, whose polyaniline coating layer has a thickness of 0.25μm.
[0079] Using the dry cathode material CFM@PANI obtained in this embodiment, a dry cathode sheet was prepared according to the preparation method of the dry cathode sheet in Example 1.
[0080] Example 3 The method for preparing the cathode material for dry-process cathode sheets provided in this embodiment includes the following steps: (1) Weigh 400g of nickel-iron-copper-manganese matrix material NaNi 0.33 Mn 0.33 Fe 0.3 Cu 0.04 O2 was dispersed into 900g of APS solution with a molar concentration of 0.05mol / L and stirred for 2h until homogeneous to obtain a slurry. The slurry was then dried by spray drying to obtain a mixed material.
[0081] (2) Dissolve 6g of aniline monomer in 860ml of deionized water, and then adjust the pH value to 3.5 with hydrochloric acid to obtain an aniline solution with a molar concentration of 0.75mol / L, i.e., the mass ratio of aniline to nickel-iron-copper-manganese matrix material is 0.015:1. At room temperature (20℃), the aniline solution is uniformly sprayed onto the surface of the mixed material particles; then it is transferred to 5℃ and allowed to stand for 4h to form a polyaniline coating layer; then it is washed with deionized water and ethanol respectively, and dried to obtain the dry-process positive electrode material CFM@PANI, whose polyaniline coating layer thickness is 0.75μm.
[0082] Using the dry cathode material CFM@PANI obtained in this embodiment, a dry cathode sheet was prepared according to the preparation method of the dry cathode sheet in Example 1.
[0083] Comparative Example 1 The difference between the preparation method of the dry-process cathode material provided in this comparative example and that in Example 1 is that aniline monomer was not added in step (2). That is, the dry-process cathode material prepared in this comparative example does not have a polyaniline coating layer.
[0084] Using the dry cathode material CFM obtained in this comparative example, a dry cathode sheet was prepared according to the preparation method of the dry cathode sheet in Example 1.
[0085] Experimental Example The peeling force and film resistance of the dry-process positive electrode sheets prepared in each embodiment and each comparative example were tested respectively, and the results are shown in Table 1.
[0086] The peel strength test method is as follows: the dry-process positive electrode sheet is cut into strips 30mm wide, then attached to 20mm wide special 3M tape, rolled tightly, and the peel strength value is tested using a universal tensile testing machine. The membrane resistance test method is as follows: the rolled dry-process positive electrode sheet is placed on a membrane resistance meter, and the membrane resistance data is measured.
[0087] Table 1. Test results of peel force and film resistance of various dry-process positive electrode sheets
[0088] The comparison diagram of the peeling force results of the dry-process positive electrode sheets of Examples 1-3 and Comparative Example 1 is shown in the figure below. Figure 1 As shown in the figure. A comparison of the film resistance results of the dry-process positive electrode sheets in Examples 1-3 and Comparative Example 1 is shown in the figure. Figure 2 As shown.
[0089] Through Table 1 and Figures 1-2 It can be seen that, compared with Comparative Example 1, the dry-process positive electrode sheets prepared in Examples 1-3 have significantly improved peel strength and significantly reduced film resistance.
[0090] This demonstrates that adding a polyaniline coating layer enables the cathode material used in dry-process cathode sheets to possess both conductivity and adhesion.
[0091] Although the present invention has been illustrated and described with specific embodiments, it should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and scope of the present invention; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention; therefore, this means that all such substitutions and modifications that fall within the scope of the present invention are included in the appended claims.
Claims
1. A positive electrode material for dry-process positive electrode sheets, characterized in that, It includes a nickel-iron-copper-manganese matrix material and a polyaniline coating layer covering the nickel-iron-copper-manganese matrix material.
2. The positive electrode material for dry-process positive electrode sheets according to claim 1, characterized in that, The thickness of the polyaniline coating is 0.05~2μm; And / or, the general formula of the nickel-iron-copper-manganese matrix material is NaNi. x Mn y Fe z Cu 1-x-y-z O2, where 0.1≤x≤0.5, 0.1≤y≤0.5, 0.1≤z≤0.4, and x+y+z<1.
3. The method for preparing the positive electrode material for dry-process positive electrode sheets as described in claim 1 or 2, characterized in that, Includes the following steps: The nickel-iron-copper-manganese matrix material was mixed with an oxidant solution and then spray-dried to obtain a mixed material; Aniline solution is sprayed onto the surface of the particles of the mixed material and allowed to react statically to form a polyaniline coating layer, thus obtaining a positive electrode material for dry-process positive electrode sheets.
4. The method for preparing the positive electrode material for dry-process positive electrode sheets according to claim 3, characterized in that, The oxidant solution includes an ammonium persulfate solution; And / or, the molar concentration of the oxidant solution is 0.01 mol / L to 0.1 mol / L.
5. The method for preparing the positive electrode material for dry-process positive electrode sheets according to claim 3, characterized in that, The molar concentration of the aniline solution is 0.05 mol / L to 0.3 mol / L; And / or, the pH value of the aniline solution is 2.0 to 4.0; And / or, the mass ratio of aniline in the aniline solution to the nickel-iron-copper-manganese matrix material is 0.001~0.03:1; And / or, the temperature of the static reaction is 0℃~5℃, and the time of the static reaction is 4h~6h.
6. A dry-process positive electrode, characterized in that, Includes the positive electrode material for dry-process positive electrode sheets as described in claim 1 or 2.
7. The dry-process positive electrode sheet according to claim 6, characterized in that, The peeling force of the dry-process positive electrode sheet is ≥9N / m; And / or, the film resistance of the dry-process positive electrode is ≤500mΩ.
8. The method for preparing a dry-process positive electrode sheet as described in claim 6 or 7, characterized in that, Includes the following steps: The dry-process positive electrode sheet is mixed with positive electrode material, conductive agent and PTFE and then subjected to fiberization treatment to obtain the fiberized material. The fibrous material is hot-pressed to obtain a self-supporting membrane; After hot-pressing the self-supporting membrane with the positive electrode current collector, a dry-process positive electrode sheet is obtained.
9. The method for preparing a dry-process positive electrode sheet according to claim 8, characterized in that, The mass ratio of the positive electrode material, the conductive agent, and the PTFE used in the dry-process positive electrode sheet is 95~97:1~2:2~3; And / or, the temperature of the mixture is ≤19°C; And / or, during the fiberization process, the temperature is raised to 70°C and then stopped; And / or, the positive current collector comprises carbon-coated aluminum foil.
10. A sodium-ion battery, characterized in that, Includes the positive electrode material for dry-process positive electrode as described in claim 1 or 2, or the dry-process positive electrode as described in claim 6 or 7.