Silicon-carbon composite materials, electrochemical devices and electrical equipment

By setting a coating layer of lithium phosphate and/or lithium pyrophosphate on the surface of silicon-carbon material, the problems of high volume expansion rate and SEI film instability during lithium intercalation of silicon-carbon material are solved, the cycle stability and lithium-ion transport efficiency of electrochemical device are improved, and the volume expansion rate is reduced.

CN123120700APending Publication Date: 2026-11-17HUIZHOU LIWINON NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448021.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-carbon materials exhibit high volume expansion during lithium intercalation and instability during cycling, making it difficult for the SEI film to effectively protect them and leading to electrode failure. Furthermore, the initial lithium intercalation potential is high and fluctuates greatly, which easily generates a loosely structured SEI film, further exacerbating lithium loss and electrode polarization.

Method used

A lithium phosphate and/or lithium pyrophosphate coating layer is formed on the surface of a silicon-carbon matrix. The mass percentage content and average thickness of the coating layer are controlled to form a stable PO coordination structure. The adhesion is improved through chemical bonding, and chemical bonding is formed with the Si-OH and C-OH active sites on the surface of the silicon-carbon matrix. This enhances the compactness and deformation resistance of the coating layer, reduces the negative electrode interface transport impedance, and suppresses the expansion of silicon-carbon particles.

Benefits of technology

It improves the cycle stability of the electrochemical device, reduces the volume expansion rate, promotes lithium-ion intercalation/deintercalation and transport at the lithium-ion interface, suppresses interfacial side reactions, reduces active lithium loss, and enhances the electrochemical performance of silicon-carbon composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This application provides a silicon-carbon composite material, an electrochemical device, and an electrical device, belonging to the field of electrochemical energy storage technology. The silicon-carbon composite material of this application includes a silicon-carbon matrix and a coating layer disposed on the surface of the silicon-carbon matrix; the silicon-carbon matrix includes porous carbon material and silicon nanoparticles dispersed in the pores of the porous carbon material; the coating layer includes lithium phosphate and / or lithium pyrophosphate; based on the mass of the silicon-carbon composite material, the mass percentage content W% of the coating layer and the average thickness d nm of the coating layer satisfy: 5 ≤ d / W ≤ 42; where d is 10~400 nm and W is 0.5~10%. The silicon-carbon composite material of this application can improve the cycle stability of the electrochemical device and reduce the volume expansion rate of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrochemical energy storage technology, specifically to silicon-carbon composite materials, electrochemical devices, and electrical equipment. Background Technology

[0002] In recent years, with the rapid development of the new energy industry, lithium-ion batteries, as the most widely used energy storage devices, have advantages such as high energy density, safety and environmental friendliness, and long cycle life. Among them, silicon-carbon materials, as one of the promising anode materials for secondary batteries, have high theoretical specific capacity and excellent fast-charging performance, meeting the current development needs of new energy. Among the many anode materials that have been studied, silicon, which has abundant reserves in nature, has a theoretical specific capacity as high as 4200 mAh / g, more than 10 times that of graphite materials. Moreover, silicon has a low operating voltage, which can avoid the risk of lithium plating on the surface during the charging process.

[0003] However, existing silicon-carbon materials have the following problems: First, the volume expansion rate of silicon-carbon materials after lithium intercalation exceeds 300%. During cycling, the unstable SEI is difficult to effectively protect silicon particles, and it is easy to cause pulverization, expansion, and detachment from the carbon matrix, leading to electrode failure. Second, the initial lithium intercalation potential of silicon-carbon anodes is high and fluctuates greatly, which easily generates a loosely structured SEI film with high impedance. The film layer is prone to repeated rupture and reconstruction, further aggravating lithium loss and electrode polarization. Summary of the Invention

[0004] The purpose of this application is to overcome the shortcomings of the prior art and provide a silicon-carbon composite material, an electrochemical device, and an electrical device.

[0005] To achieve the above objectives, the technical solution adopted in this application is as follows: Firstly, a silicon-carbon composite material is provided, the silicon-carbon composite material comprising a silicon-carbon matrix and a coating layer disposed on the surface of the silicon-carbon matrix; The silicon-carbon matrix includes porous carbon material and silicon nanoparticles dispersed in the pores of the porous carbon material. The coating layer comprises lithium phosphate and / or lithium pyrophosphate; Based on the mass of silicon-carbon composite materials, the mass percentage content W% of the coating layer and the average thickness d nm of the coating layer satisfy: 5≤d / W≤42; where d is 10~400nm and W is 0.5~10%.

[0006] In some embodiments, the particle size of the silicon-carbon composite material satisfies: Dv10 = 4.5–6.5 μm, and or, Dv50 = 8–9 μm, and or, Dv90 = 12.5–15.5 μm.

[0007] In some embodiments, the particle size span of the silicon-carbon composite material is 0.5 to 1.0.

[0008] In some embodiments, the silicon-carbon composite material has a silicon content of 35-60% by mass.

[0009] In a second aspect, an electrochemical device is provided, comprising a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active layer disposed on at least one surface of the negative electrode current collector, the negative electrode active layer comprising the aforementioned silicon-carbon composite material.

[0010] In some embodiments, the electrochemical device further includes an electrolyte comprising boron-containing additives and fluorine-containing additives, wherein the total mass percentage of the boron-containing additives and fluorine-containing additives, based on the mass of the electrolyte, is M, satisfying: 0.1 ≤ M / W ≤ 0.8.

[0011] In some embodiments, the boron-containing additive includes at least one of lithium difluorooxalate borate, lithium bis(oxalate borate), lithium tetrafluoroborate, trimethyl borate, and triethyl borate.

[0012] In some embodiments, the fluorinated additive includes at least one of fluoroethylene carbonate, lithium difluorophosphate, lithium bisfluorosulfonylimide, and lithium trifluoromethanesulfonate.

[0013] Thirdly, an electrical device is provided, including the aforementioned electrochemical device.

[0014] Compared with the prior art, the beneficial effects of this application are as follows: In the silicon-carbon composite material of this application, a coating layer including lithium phosphate and / or lithium pyrophosphate is provided on the surface of the silicon-carbon matrix, and the mass percentage W of the coating layer and the average thickness d of the coating layer satisfy: 5≤d / W≤42; it has the following advantages: lithium phosphate and / or lithium pyrophosphate contain stable PO coordination structures, and lithium phosphate and / or lithium pyrophosphate form chemical bonds with the Si-OH and C-OH active sites on the surface of the silicon-carbon matrix, improving the adhesion of the coating layer and making the coating layer less prone to falling off during cycling. The combined use of lithium phosphate and lithium pyrophosphate can produce a synergistic effect: lithium phosphate mainly improves lithium-ion migration efficiency, while lithium pyrophosphate strengthens the density and deformation resistance of the coating layer; the two phases are intercalated and complementary. The composite coating can directly reduce the negative electrode interface transport impedance, efficiently promote lithium ion intercalation and deintercalation and transport, and suppress the expansion of silicon carbon particles. At the same time, the coating can physically isolate the silicon carbon matrix from direct contact with the electrolyte, suppress interfacial side reactions, and reduce the loss of active lithium. This improves the cycle stability of electrochemical devices containing silicon carbon composite materials and reduces the volume expansion rate of electrochemical devices containing silicon carbon composite materials. Detailed Implementation

[0015] To facilitate understanding of this application, a more complete description will be provided below. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.

[0016] As used in this article: "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0017] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0018] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1-5” is disclosed, the described range should be interpreted as including ranges “1-4”, “1-3”, “1-2”, “1-2 and 4-5”, “1-3 and 4-5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0019] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.

[0020] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has 'a' parts by mass and component B has 'b' parts by mass, it means that the mass ratio of component A to component B is a:b. It is important to understand that, unlike mass percentage content, the sum of the mass parts of all components is not limited to 100 parts.

[0021] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0022] "Particle size Dv10" refers to the diameter that corresponds to when the cumulative diameter distribution percentage of the particles reaches 10%.

[0023] "Particle size Dv50" refers to the diameter that corresponds to when the cumulative diameter distribution percentage of the particles reaches 50%.

[0024] "Particle size Dv90" refers to the diameter that corresponds to when the cumulative diameter distribution percentage of the particles reaches 90%.

[0025] The “Span value” is used to represent the degree of concentration of particle size, and its expression is Span=(Dv90-Dv10) / Dv50.

[0026] In a first aspect, this application provides a silicon-carbon composite material, the silicon-carbon composite material comprising a silicon-carbon matrix and a coating layer disposed on the surface of the silicon-carbon matrix; The silicon-carbon matrix includes porous carbon material and silicon nanoparticles dispersed in the pores of the porous carbon material. The coating layer comprises lithium phosphate and / or lithium pyrophosphate; Based on the mass meter of silicon-carbon composite material, the mass percentage W of the coating layer and the average thickness d of the coating layer satisfy: 5≤d / W≤42; where d is 10~400nm and W is 0.5~10%.

[0027] In the silicon-carbon composite material of this application, a coating layer including lithium phosphate and / or lithium pyrophosphate is formed on the surface of the silicon-carbon matrix, and the mass percentage W of the coating layer and the average thickness d of the coating layer satisfy: 5 ≤ d / W ≤ 42. This has the following advantages: lithium phosphate and / or lithium pyrophosphate contain stable PO coordination structures, and form chemical bonds with the Si-OH and C-OH active sites on the surface of the silicon-carbon matrix, improving the adhesion of the coating layer and making it less prone to detachment during cycling. The combined use of lithium phosphate and lithium pyrophosphate produces a synergistic effect: lithium phosphate primarily enhances lithium-ion migration efficiency, while lithium pyrophosphate strengthens the density and deformation resistance of the coating layer; the two phases are mutually integrated and complementary. The composite coating can directly reduce the negative electrode interface transport impedance, efficiently promote lithium ion intercalation and deintercalation and transport, and suppress the expansion of silicon carbon particles. At the same time, the coating can physically isolate the silicon carbon matrix from direct contact with the electrolyte, suppress interfacial side reactions, and reduce the loss of active lithium. This improves the cycle stability of electrochemical devices containing silicon carbon composite materials and reduces the volume expansion rate of electrochemical devices containing silicon carbon composite materials.

[0028] Specifically, d can be a range of values ​​consisting of one or any two of the following: 10 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, and 400 nm.

[0029] Specifically, W can be a range of values ​​consisting of one or any two of the following: 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.

[0030] In this application, the test method for the mass percentage content W of the coating layer based on the mass meter of silicon-carbon composite material is as follows: Take a mass m1 of silicon-carbon composite material and place it in a muffle furnace, continuously purging it with air. Calcine it at 1000℃ for 4 hours. During calcination, C is converted to CO2 gas and dissipates, while Si is converted to SiO2. The coating layer remains unchanged. The remaining mass of the material after calcination is m2. Immerse the calcined material in dilute sulfuric acid and heat it to 50℃. The coating layer dissolves in the acid, while SiO2 remains insoluble. Filter, wash, and dry the remaining precipitate, then weigh it as m3. Finally, the mass percentage of the coating layer W = (m2 - m3) / m1.

[0031] In this application, the test method for the average thickness d of the coating layer is as follows: 1. Prepare an electron beam transparent sample by coating silicon-carbon particles with lithium phosphate and / or lithium pyrophosphate on the surface; 2. Obtain Z-contrast images of the particles in HAADF mode of a scanning transmission electron microscope, and identify the coating layer region based on the contrast difference between the phosphate and the silicon-carbon matrix; 3. Perform an electron energy loss spectral scan along the radial direction of the particle to collect the characteristic energy loss edges of Li, P, O, Si and / or C, with only the coating layer containing Li and P elements; 4. Determine the thickness of the coating layer based on the Li or P element signal intensity distribution obtained from the line scan.

[0032] The preparation method of the silicon-carbon composite material described in this application is as follows: S1: In a fluidized bed CVD reactor, carbon matrix particles are placed in the reaction chamber, and an inert carrier gas (such as nitrogen or argon) is introduced to keep the particles in a fluidized state. After heating to a specified temperature, a silicon source gas (such as silane) is introduced. The silicon source thermally decomposes on the surface of the carbon matrix and deposits nano-silicon. After a period of deposition, the introduction of silicon source gas is stopped. At a certain temperature, carbon source gas is introduced to perform carbon coating to obtain the first product. S2: Using LiOH·H2O as the lithium source, phosphoric acid (H3PO4) as the phosphorus source, and ethanol-deionized water as the mixed solvent, the molar ratio of lithium and phosphorus sources is controlled, and citric acid is added as a dispersant to obtain the precursor solution. S3: Add the first product to the precursor solution, stir evenly, remove the solvent, and obtain the second product; S4: Under the protection of a protective gas, the second product is heated to 200~240℃ at room temperature and held for 0.5~2h, then heated to 500℃~650℃ and held for 3h. The precursor undergoes a solid-phase reaction and forms a composite coating layer in situ. After cooling, it is sieved to obtain a silicon-carbon composite material.

[0033] In some embodiments, the porous carbon material includes at least one of resin-based carbon material, biomass-based carbon material, and pitch-based carbon material, obtained after carbonization and activation.

[0034] Specifically, resin-based carbon materials include at least one of phenolic resin and furfural resin.

[0035] Specifically, biomass-based carbon materials include at least one of coconut shells, starch, wood, and straw.

[0036] Specifically, asphalt-based carbon materials include at least one of coal tar pitch and petroleum asphalt.

[0037] In some implementations, the porous carbon material is selected from phenolic resin-based materials, and the final particle size and span of the silicon-carbon composite material are determined by the porous carbon material.

[0038] In step S1, the silicon source gas can be one or more of silane, silane, and dichlorosilane. The content, uniformity, and crystallinity of the deposited nano-silicon can be controlled by adjusting the deposition time and deposition temperature.

[0039] In some embodiments, the silicon-carbon composite material has a silicon content of 35-60% by mass; for example, it can be a range of one or any two of 35%, 37%, 40%, 43%, 45%, 48%, 50%, 52%, 55%, 57%, and 60%.

[0040] In this application, the method for testing the mass percentage of silicon in the silicon-carbon composite material is as follows: A mass m1 of silicon-carbon composite material was placed in a muffle furnace and continuously purged with air. It was calcined at 1000℃ for 4 hours. During calcination, C was converted to CO2 gas and emitted, while Si was converted to SiO2. The coating layer remained unchanged. The remaining mass of the material after calcination was m2. The calcined material was then immersed in dilute sulfuric acid and heated to 50℃. The coating layer dissolved in the acid, while SiO2 remained insoluble. The remaining precipitate was filtered, washed, dried, and weighed, yielding a mass m3. The mass percentage of silicon was 7m3 / 15m1.

[0041] To prevent silicon particle growth and crystallization, the deposition temperature needs to be controlled. Too low a temperature results in low deposition efficiency, while too high a temperature causes silicon particles to grow and transform into crystalline silicon, degrading performance. Specifically, the deposition temperature can be a range of 420℃, 450℃, 480℃, 500℃, 530℃, and 550℃, or any combination thereof. In the embodiments and comparative examples of this application, the preferred deposition temperature is 480℃, and the deposition time is 3 hours. After the nano-silicon particles are deposited, they need to be protected with carbon coating. The carbon source gas can be one or a mixture of acetylene, ethylene, and methane. The carbon coating temperature has a significant impact on the quality of the carbon layer; too low a temperature results in poor carbon layer strength and conductivity, while too high a temperature causes the growth of nano-silicon particles. Specifically, the carbon coating temperature can be a range of 500℃, 530℃, 550℃, 580℃, 600℃, 630℃, 650℃, 680℃, and 700℃, or any combination thereof. In the embodiments and comparative examples of this application, the coating temperature is preferably 580°C and the coating time is 2.5h.

[0042] In some embodiments, the lithium source in the precursor solution is lithium hydroxide, the phosphorus source is phosphoric acid, and the solvent is an ethanol-deionized water mixture. To obtain the composite coating layer of lithium phosphate and lithium pyrophosphate, the molar ratio of the lithium source to the phosphorus source needs to be controlled. Specifically, the molar ratio of the lithium source to the phosphorus source can be one or any combination of 2.2:1, 2.3:1, 2.5:1, 2.6:1, 2.7:1, and 2.8:1. In the embodiments of this application, the molar ratio of the lithium source to the phosphorus source is preferably 2.6:1.

[0043] It should be noted that when the molar ratio of lithium source to phosphorus source is 2:1, the reaction product is lithium monopyrophosphate (Li4P2O7), and when the molar ratio is 3:1, the reaction product is lithium monophosphate (Li3PO4). To obtain a lithium phosphate / lithium pyrophosphate composite coating, the molar ratio of lithium source to phosphorus source needs to be controlled between 2.2 and 2.8:1. This ratio range can directionally regulate the component ratio of lithium phosphate and lithium pyrophosphate in the product, so that the two phases form an optimal composite system. When the molar ratio of lithium source to phosphorus source is lower than 2.2:1, the proportion of lithium pyrophosphate in the system is too high, the ion conductivity of the coating layer decreases, the interfacial impedance increases, which is not conducive to the rapid migration of lithium ions. When the molar ratio of lithium source to phosphorus source is higher than 2.8:1, lithium phosphate becomes the dominant phase, the lithium pyrophosphate content is insufficient, it is difficult to fully fill the grain boundary pores, the density and structural toughness of the coating layer deteriorate, and the resistance to deformation and electrolyte erosion weakens. By controlling the molar ratio of lithium source to phosphorus source within the range of 2.2 to 2.8:1, lithium phosphate and lithium pyrophosphate can coexist in a balanced manner and work synergistically. This ensures that the coating layer has excellent lithium-ion conductivity while maintaining high density and structural stability, thus maximizing the technical advantages of the two-phase composite.

[0044] The citric acid added to the precursor solution mainly serves a complexing and dispersing function, preventing the agglomeration of lithium-phosphorus precursors, improving the uniformity of the coating layer, and refining the phosphate grains after calcination. Furthermore, its thermal decomposition is complete, preventing the introduction of impurities and ensuring the electrochemical performance of the material. The added citric acid accounts for 2-3% of the precursor solution's mass. In the examples and comparative examples described herein, the citric acid accounts for 2.5% of the precursor solution's mass.

[0045] In some embodiments, in step S3, the mass of the first product is n1, the mass of the precursor solution is n2, and 0.15n1≤n2≤3.5n2. The precursor solution and the first product are uniformly mixed and stirred for 3-5 hours to achieve uniform mixing, then dried at 80°C using forced air drying. During this process, the lithium source and phosphorus source react to produce lithium phosphate and lithium pyrophosphate precursors, which are uniformly distributed on the surface of the silicon-carbon particles, yielding the second product. In the subsequent heat treatment process, the lithium phosphate and lithium pyrophosphate precursors are transformed into a lithium phosphate and lithium pyrophosphate coating layer, tightly coating the surface of the silicon-carbon particles, ultimately obtaining a composite silicon-carbon material.

[0046] The mass ratio of the coating layer to the composite silicon-carbon material can be controlled by the ratio of n1 to n2. Specifically, n2 can be a range of values ​​consisting of one or any two of the following: 0.15n1, 0.2n1, 0.3n1, 0.5n1, 0.8n1, 1.0n1, 1.5n1, 2.0n1, 2.5n1, 3.0n1, and 3.5n1.

[0047] In this application, the second product obtained needs to be preheated at 200~240℃ for 0.5~2h to remove citric acid, and then held at 500℃~650℃ for 3h to ensure that the precursor is completely converted into a protective layer of lithium phosphate and lithium pyrophosphate. If the heat treatment temperature is too low, the precursor cannot react completely, resulting in poor coating quality; if the temperature is too high, it will damage the silicon-carbon particles, leading to the growth of nano-silicon. Specifically, the heat treatment temperature in step S4 can be a range of 500℃, 520℃, 550℃, 580℃, 600℃, 630℃, 650℃, or any combination of two of these values. In the embodiments and comparative examples herein, the heat treatment temperature is preferably 550℃.

[0048] In some embodiments, the particle size of the silicon-carbon composite material satisfies: Dv10 = 4.5–6.5 μm, and or, Dv50 = 8–9 μm, and or, Dv90 = 12.5–15.5 μm.

[0049] In this application, the particle size of the silicon-carbon composite material is within the above-mentioned range, which can avoid the problems of excessive specific surface area, severe interfacial side reactions, and low initial coulombic efficiency of small-particle-size silicon-carbon composite materials; at the same time, it can also avoid the defects of excessively long lithium-ion transport paths, poor rate performance, and local expansion in large-particle-size silicon-carbon composite materials, so that the silicon-carbon composite material has both lithium-ion transport efficiency and structural stability.

[0050] Specifically, the particle size Dv10 of the silicon-carbon composite material can be a range of one or any combination of 4.5μm, 4.7μm, 4.9μm, 5.1μm, 5.3μm, 5.5μm, 5.7μm, 5.9μm, 6.1μm, 6.3μm, and 6.5μm.

[0051] Specifically, the particle size of the silicon-carbon composite material can be a range of one or any combination of two of the following: 8μm, 8.1μm, 8.2μm, 8.3μm, 8.4μm, 8.5μm, 8.6μm, 8.7μm, 8.8μm, 8.9μm, and 9μm.

[0052] Specifically, the particle size of the silicon-carbon composite material can be one or a combination of two of the following: 12.5 μm, 12.7 μm, 13 μm, 13.3 μm, 13.5 μm, 13.8 μm, 14 μm, 14.2 μm, 14.5 μm, 14.7 μm, 15 μm, 15.3 μm, and 15.5 μm.

[0053] In this application, the particle size of the silicon-carbon composite material is determined by referring to GB / T 19077-2024 "Particle Size Analysis by Laser Diffraction" and is tested using a laser particle size analyzer to obtain the volume particle size distribution curve of the silicon-carbon composite material.

[0054] In some embodiments, the particle size span of the silicon-carbon composite material is 0.5 to 1.0; for example, it can be a range of one or any two of 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, and 1.0.

[0055] In this application, the particle size span value of the silicon-carbon composite material is within the above-mentioned range, which makes the particle size uniformity of the silicon-carbon composite material high. This can avoid the problem of uneven compaction density and local stress concentration of the negative electrode sheet caused by mixing large-particle-size silicon-carbon composite materials and small-particle-size silicon-carbon composite materials.

[0056] In a second aspect, an electrochemical device is provided, comprising a negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active layer disposed on at least one surface of the negative electrode current collector, the negative electrode active layer comprising the aforementioned silicon-carbon composite material.

[0057] This application does not impose any particular limitation on the negative electrode current collector, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of copper foil, aluminum foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, and composite current collectors. In some embodiments, the composite current collector may include, but is not limited to, at least one of carbon copper composite current collectors, nickel copper composite current collectors, and titanium copper composite current collectors.

[0058] In addition to the aforementioned silicon-carbon composite material, the negative electrode active layer of this application may also include negative electrode active materials conventionally used in the art. For example, it may include, but is not limited to, at least one of graphite, hard carbon, soft carbon, silicon suboxide, lithium metal, lithium titanate, metal alloys, metal sulfides, and graphene. Metal alloys include, but are not limited to, at least one of Li-Sn alloys, Li-Sn-O alloys, and Li-Al alloys. Silicon suboxide is SiO₂. x (0.5 <x<1.6)。

[0059] In some embodiments, the negative electrode active layer further includes at least one of a conductive agent, a binder, and a thickener. This application does not impose particular limitations on the conductive agent and binder, as long as they can achieve the purpose of this application. For example, the conductive agent may include, but is not limited to, at least one of metal-based materials and conductive polymers. In some embodiments, the metal-based material may include, but is not limited to, at least one of metal powder and metal fibers, and the metal may include, but is not limited to, at least one of copper, nickel, aluminum, and silver. In some embodiments, the conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polythiophene, polypyrrole, polyaniline, polyacetylene, poly(p-phenylene), and polyfluorene. For example, the binder may include, but is not limited to, at least one of polyvinyl alcohol, hydroxypropyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyolefin ester, polyolefin alcohol, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, and nylon. For example, thickeners may include, but are not limited to, at least one of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and their salts.

[0060] In some embodiments, the negative electrode structure is a negative electrode structure known in the art that can be used in electrochemical devices.

[0061] In some embodiments, the method for preparing the negative electrode sheet is a method known in the art for preparing negative electrode sheets that can be used in electrochemical devices. For example, the negative electrode sheet can be obtained by mixing the components of the negative electrode active layer (including the negative electrode active material, and optionally a conductive agent, binder, and thickener, etc.) in a solvent, and heating the mixture before using the thickener as needed to prepare a negative electrode slurry, and coating and / or spraying the negative electrode slurry onto a negative electrode current collector. In some embodiments, the solvent may include, but is not limited to, at least one of water, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, trimethyl phosphate, acetone, and dipropylene glycol dimethyl ether.

[0062] In some embodiments, the electrochemical device further includes an electrolyte comprising boron-containing additives and fluorine-containing additives, wherein the total mass percentage of the boron-containing additives and fluorine-containing additives, based on the mass of the electrolyte, is M, satisfying: 0.1 ≤ M / W ≤ 0.8.

[0063] In the electrolyte of this application, boron-containing additives form a flexible Li-BO inorganic phase through a film-forming reaction, which improves the toughness of the SEI film, prevents the SEI film from cracking during cycling, reduces interfacial impedance, and optimizes lithium-ion transport kinetics. Fluorine-containing additives can be reduced and decomposed to generate a highly stable LiF crystalline phase, which builds a dense inorganic framework for the SEI film, improves the strength of the SEI film, and promotes lithium-ion transport. The coating layer provides a stable nucleation substrate for electrolyte additives (boron-containing and fluorine-containing additives). The surfaces of lithium phosphate and / or lithium pyrophosphate are rich in PO bonds and active Li sites, which can preferentially adsorb boron and fluorine additive molecules in the electrolyte, reduce the activation energy of the reduction and decomposition of boron-containing and fluorine-containing additives, lower the nucleation barrier of the inorganic phase of the SEI film, and induce the preferential formation of a high-inorganic-phase SEI film dominated by Li-PO, LiF, and Li-BO phases at the interface, reducing the generation of organic by-products. This high-inorganic-phase SEI film has high lithium-ion transport efficiency, excellent mechanical strength and flexibility, which can further optimize lithium-ion transport kinetics, buffer the volume expansion of silicon-carbon composite materials, avoid the pulverization and breakage of silicon-carbon composite materials, and block the continuous side reactions of the electrolyte, significantly improve the cycle life of the electrochemical device, and effectively reduce the volume expansion rate of the electrochemical device.

[0064] Specifically, M / W can be a range of values ​​consisting of one or any two of the following: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, and 0.8.

[0065] The test methods for boron-containing and fluorine-containing additives in electrolytes are as follows: The relative content of boron- or fluorine-containing components in the electrolyte was determined by gas chromatography-mass spectrometry (GC-MS).

[0066] (a) Take the electrolyte sample to be tested under an inert atmosphere, dilute it with an anhydrous organic solvent and filter it; (b) Analysis was performed using gas chromatography-mass spectrometry, and boron- or fluorine-containing components were qualitatively identified by retention time and characteristic ions in the mass spectrometry. (c) Calculate the relative content of boron- or fluorine-containing components based on the peak area of ​​the characteristic ions of each component.

[0067] In some embodiments, the boron-containing additive includes at least one of lithium difluorooxalate borate, lithium bis(oxalate borate), lithium tetrafluoroborate, trimethyl borate, and triethyl borate.

[0068] In some embodiments, the fluorinated additive includes at least one of fluoroethylene carbonate, difluoroethylene carbonate, fluorocarboxylic acid ester, lithium difluorophosphate, lithium difluorosulfonylimide, and lithium trifluoromethanesulfonate.

[0069] In some embodiments, the electrolyte comprises an electrolyte and an organic solvent.

[0070] In some embodiments, this application does not particularly limit the organic solvent, as long as it can achieve the purpose of this application. The organic solvent used in this application can be an organic solvent known in the prior art. For example, the organic solvent can include, but is not limited to, at least one of carbonate compounds, carboxylic acid ester compounds, ether compounds, and other organic solvents. Among them, carbonate compounds can include, but are not limited to, at least one of chain carbonate compounds and cyclic carbonate compounds. Chain carbonate compounds can include, but are not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and methyl ethyl carbonate (EMC). Cyclic carbonates can include, but are not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), and vinyl ethylene carbonate (VEC). Carboxylic acid ester compounds can include, but are not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valproic acid lactone, and caprolactone. The ether compound may include, but is not limited to, at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran. Other organic solvents may include, but are not limited to, at least one of dimethyl sulfoxide, 1,3-dioxolane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, and trioctyl phosphate.

[0071] In some embodiments, the electrolyte may include, but is not limited to, at least one of inorganic lithium salts, fluorine-containing organic lithium salts, and lithium salts containing dicarboxylic acid complexes. The inorganic lithium salt may include, but is not limited to, at least one of LiClO4, LiAsF6, LiPF6, LiBF4, LiSbF6, LiSO3F, LiPO2F2, and LiN(FSO2)2. Fluorinated organic lithium salts may include, but are not limited to, at least one of LiCF3SO3, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,3-hexafluoropropane disulfonylimide lithium, cyclic 1,2-tetrafluoroethane disulfonylimide lithium, LiPF4(CF3)2, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiPF4(CF3SO2)2, LiPF4(C2F5)2, LiPF4(C2F5SO2)2, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, and LiBF2(C2F5SO2)2. Lithium salts containing dicarboxylic acid complexes may include, but are not limited to, at least one of lithium bis(oxalate)borate, lithium difluorooxalateborate [LiBF2(C2O4)], lithium tri(oxalate)phosphate, lithium difluorobis(oxalate)phosphate, and lithium tetrafluoro(oxalate)phosphate.

[0072] In some embodiments, the mass percentage of the electrolyte is a range of one or any combination of two of the following, based on the mass of the electrolyte: 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 12.5%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, and 30%.

[0073] The electrolyte of this application may also include additives other than boron-containing and fluorine-containing additives. For example, additives may include, but are not limited to, at least one of polynitrile compounds and sulfur-containing additives.

[0074] Polynitrile compounds include at least one of dinitrile compounds and trinitrile compounds. Dinitrile compounds are compounds containing two cyano groups (-CN), and may include, but are not limited to, malononitrile, succinic anionizer, glutaronitrile, adiponitrile, heptacyanide, caprylic anionizer, nonadionitrile, decanonitrile, methylmalononitrile, ethylmalononitrile, isopropylmalononitrile, tert-butylmalononitrile, methylsuccinic anionizer, 2-methyleneglutaronitrile, 1,4-dicyano-3-butene, 2,2-dimethylsuccinic anionizer, 2,3-dimethylsuccinic anionizer, 2,3,3-trimethylsuccinic anionizer, 2,2,3,3-tetramethylsuccinic anionizer, 2,3-diethyl-2,3-dimethylsuccinic anionizer, 2,2-diethyl-3,3-dimethylsuccinic anionizer, dicyclohexyl-1,1-dicarboxynitrile, dicyclohexyl-2,2-dicarboxynitrile, dicyclohexyl-3 3-Dicarboxylonite, 2,5-Dimethyl-2,5-hexanedicarboxylonite, 2,3-Diisobutyl-2,3-dimethylbutanedilonite, 2,2-Diisobutyl-3,3-dimethylbutanedilonite, 2-Methylglutaronilonite, 2,3-Dimethylglutaronilonite, 2,4-Dimethylglutaronilonite, 2,2,3,3-Tetramethylglutaronilonite, 2,2,4,4-Tetramethylglutaronilonite, 2,2,3,4-Tetramethylglutaronilonite, 2,3,3,4-Tetramethylglutaronilonite, 1,4-Dicyanopentane, 2,6-Dicyanopentane, 2,7-Dicyanopentane, 2,8-Dicyanopennonane, 1,6-Dicyanopentane, 1,2-Dicyanobenzene, 1,3-Dicyanopenzene, 1,4-Dicyanopenzene, 3,3'- At least one of (ethylenedioxy)dipropionitrile, 3,3'-(ethylenedisulfide)dipropionitrile, 1,4-dicyano-2-butene, and trans-butenedionitrile. Trinitrile compounds are compounds containing three cyano groups (-CN).

[0075] In some embodiments, the electrolyte preparation method is a method known in the art for preparing electrolytes that can be used in electrochemical devices (including batteries). For example, the electrolyte can be obtained by mixing the components of the electrolyte, including organic solvents, electrolytes, and optional additives.

[0076] In some embodiments, the electrochemical device further includes a positive electrode, the positive electrode comprising a positive current collector and a positive active layer disposed on at least one surface of the positive current collector, the positive active layer comprising the aforementioned positive active material.

[0077] In some embodiments, the positive electrode active material may include, but is not limited to, at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium manganese iron phosphate, lithium titanate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, and lithium manganese silicate. The chemical formula of the lithium-rich manganese-based material is γLi2MnO3·(1-γ)LiDO2, where 0 < γ < 1, and D is a transition metal such as nickel, cobalt, or iron. In some embodiments, lithium nickel cobalt manganese oxide includes at least one of NCM901, NCM712, NCM811, NCM622, NCM523, and NCM111. In this application, the surface of the positive electrode material may be coated with a substance of a different composition. Exemplarily, the coated substance may include, but is not limited to, at least one of the following: aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, bismuth oxide, lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, aluminum sulfate, lithium carbonate, calcium carbonate, magnesium carbonate, and carbon. By coating the surface of the positive electrode material with the aforementioned substances, the oxidation reaction of the electrolyte on the surface of the positive electrode material can be suppressed, thereby improving the service life of the electrochemical device.

[0078] In some embodiments, the positive electrode active layer further includes at least one of a conductive agent, a binder, and a thickener. This application does not particularly limit the conductive agent and binder, as long as they can achieve the purpose of this application. For example, the conductive agent may include, but is not limited to, at least one of carbon-based materials, metal-based materials, and conductive polymers. In some embodiments, the carbon-based materials may include, but are not limited to, at least one of graphite, carbon black, acetylene black, Super-P, Ketjen black, carbon fiber, carbon nanotubes, graphene, and amorphous carbon. In some embodiments, the metal-based materials may include, but are not limited to, at least one of metal powder and metal fibers, and the metal may include, but is not limited to, at least one of copper, nickel, aluminum, and silver. In some embodiments, the conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polythiophene, polypyrrole, polyaniline, polyacetylene, and poly(p-phenylene). For example, the binder may include, but is not limited to, at least one of polyvinyl alcohol, hydroxypropyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyolefin ester, polyolefin alcohol, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, and nylon. For another example, the thickener may include, but is not limited to, at least one of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and their salts.

[0079] This application does not impose any particular limitation on the positive electrode current collector, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of aluminum foil, aluminum alloy foil, composite current collector, carbon cloth, and carbon paper. In some embodiments, the composite current collector may include, but is not limited to, an aluminum-carbon composite current collector.

[0080] In some embodiments, the method for preparing the positive electrode sheet is a method known in the art for preparing positive electrode sheets that can be used in electrochemical devices. For example, the positive electrode sheet can be obtained by mixing the components of the positive electrode active layer (including the positive electrode material, and optionally a conductive agent, binder, and thickener, etc.) in a solvent, and heating the mixture before using the thickener as needed to prepare a positive electrode slurry, and coating and / or spraying the positive electrode slurry onto a positive electrode current collector. In some embodiments, the solvent may include, but is not limited to, at least one of water, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, trimethyl phosphate, acetone, and dipropylene glycol dimethyl ether.

[0081] In some embodiments, the electrochemical device further includes a diaphragm disposed between the positive and negative electrode plates to prevent internal short circuits, allow electrolyte ions to pass freely, and not affect the electrochemical charging and discharging process. This application does not impose any particular limitation on the diaphragm, as long as it achieves the purpose of this application. The diaphragm used in this application can be any diaphragm known in the prior art. For example, the type of diaphragm can include, but is not limited to, at least one of woven membranes, nonwoven membranes, microporous membranes, composite membranes, rolled membranes, and spun membranes. The material of the diaphragm can include, but is not limited to, at least one of polyethylene (PE), polyolefins (PO) mainly composed of polypropylene (PP), polyester, cellulose, polyimide (PI), polyamide (PA), spandex, and aramid. Polyester can include, but is not limited to, polyethylene terephthalate (PET).

[0082] In some embodiments, the diaphragm includes a substrate layer. The substrate layer may include, but is not limited to, at least one of a nonwoven fabric, membrane, or composite membrane having a porous structure. The material of the substrate layer may include, but is not limited to, at least one of polyethylene, polypropylene, polyethylene terephthalate, and polyimide. In some embodiments, the substrate layer may include, but is not limited to, at least one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane.

[0083] In some embodiments, the separator further includes a surface treatment layer disposed on at least one surface of the substrate layer. The surface treatment layer may include, but is not limited to, at least one of a polymer layer, an inorganic layer, and a layer formed by a mixture of polymers and inorganic substances. The polymer layer includes polymers. This application does not particularly limit the polymer, as long as it achieves the purpose of this application. For example, the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene). The inorganic layer includes inorganic particles and a binder. This application does not particularly limit the inorganic particles and binder, as long as it achieves the purpose of this application. For example, the inorganic particles may include, but are not limited to, at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. As another example, the binder may include, but is not limited to, at least one of the binders used in the above-mentioned positive or negative electrode active layers.

[0084] In some embodiments, the present application does not have a particular limitation on the thickness of the diaphragm, as long as the purpose of the present application can be achieved. For example, the thickness of the diaphragm is 3 μm to 20 μm.

[0085] The methods for preparing electrochemical devices are well known to those skilled in the art. This application does not impose any particular limitation on the preparation method of the electrochemical device, as long as it can achieve the purpose of this application. For example, the preparation method of the electrochemical device may include, but is not limited to, the following steps: stacking the positive electrode, separator, and negative electrode in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly inside an aluminum-plastic film; injecting electrolyte into the aluminum-plastic film and sealing it to obtain the electrochemical device; or, stacking the positive electrode, separator, and negative electrode in sequence, and then fixing the four corners of the entire stacked structure with tape to obtain a stacked electrode assembly; placing the electrode assembly inside an aluminum-plastic film; injecting electrolyte into the aluminum-plastic film and sealing it to obtain the electrochemical device. In addition, overcurrent protection elements, conductive plates, etc., may be placed in the aluminum-plastic film as needed to prevent pressure rise and overcharging / discharging inside the electrochemical device.

[0086] A third aspect of this application provides an electrical device, including the aforementioned electrochemical apparatus.

[0087] This application does not impose any particular restrictions on the electrical equipment used, as long as it can achieve the purpose of this application. The electrical equipment used in this application can be any electrical equipment known in the prior art. For example, the electrical equipment can include, but is not limited to, at least one of the following: laptop computer, pen input computer, mobile computer, e-book player, portable telephone, portable fax machine, portable copier, portable printer, over-ear stereo headphones, video recorder, LCD TV, portable cleaner, portable CD player, mini CD, transceiver, electronic notebook, calculator, memory card, portable recorder, radio, backup power supply, motor, automobile, motorcycle, electric bicycle, bicycle, lighting fixture, toy, game console, clock, power tool, flashlight, camera, large household electrochemical storage device, and lithium-ion capacitor.

[0088] Example 1 <Preparation of Silicon-Carbon Composite Materials> Porous carbon was placed in a fluidized bed, and silane SiH4 was introduced under nitrogen protection. The SiH4 flow rate was 4 L / min, the flow ratio was 1:1, the deposition temperature was 480℃, and the deposition time was 3 h. After deposition, acetylene gas was introduced under nitrogen protection for carbon coating. The acetylene flow rate was 3 L / min, the flow ratio was 1:1, the coating temperature was 580℃, and the coating time was 2.5 h. After coating, the carbon was cooled in the furnace and then sieved to obtain the first product.

[0089] Dissolve 0.87 g of phosphoric acid, 0.96 g of LiOH·H2O, and 5 g of citric acid in 200 ml of deionized water to obtain a precursor solution. Weigh 50 g of the first product and add it to the precursor solution. Heat the mixture in a 70°C water bath and stir continuously for 3 hours to allow the reaction to proceed fully. Then, dry the mixture at 80°C in a forced-air environment for 3 hours to obtain the second product.

[0090] The second product was placed in a tube furnace, and argon gas was continuously introduced as a protective gas. The temperature was raised to 220°C at a rate of 5°C / min and held for 1 hour. Then, the temperature was raised to 550°C at a rate of 5°C / min and calcined for 3 hours. After furnace cooling, a silicon-carbon composite material was obtained. Based on the mass of the silicon-carbon composite material, the mass percentage W of the coating layer was 2%, and the mass percentage of silicon element was 48.5%. The average thickness d of the coating layer was 10 nm. The particle sizes of the silicon-carbon composite material were: Dv10 = 5.8 μm, Dv50 = 8.6 μm, Dv90 = 12.7 μm, and the particle size span value was 0.8. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0091] <Preparation of Negative Electrode Sheets> Silicon-carbon composite material, thickener sodium carboxymethyl cellulose, binder styrene-butadiene rubber, and conductive agent acetylene black were mixed in a mass ratio of 95.7:0.8:2.5:1. Deionized water was added, and the mixture was stirred in a vacuum mixer to obtain a negative electrode slurry. The negative electrode slurry was uniformly coated on both sides of a copper foil with a thickness of 8 μm. The coated electrode was dried, cold-pressed, and slit to obtain a negative electrode sheet, wherein the total thickness of the negative electrode active layer was 65 μm.

[0092] <Preparation of Positive Electrode> Lithium cobalt oxide (LCO), the positive electrode active material, polyvinylidene fluoride (PVDF), and acetylene black, the conductive agent, were mixed at a mass ratio of 92:4:4. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry. The positive electrode slurry was uniformly coated on both sides of an aluminum foil with a thickness of 9 μm. The electrode sheet coated with the positive electrode slurry was dried, cold-pressed, and slit to obtain a positive electrode sheet with a size of 700 mm * 120 mm, wherein the total thickness of the positive electrode active layer was 80 μm.

[0093] <Preparation of Electrolyte> At room temperature, in an argon-filled glove box (H2O content <1ppm, O2 content <1ppm), ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed evenly in a volume ratio of 1:2:1. Water is removed using a 4Å molecular sieve. Then, triethyl borate and fluoroethylene carbonate are added and mixed evenly to obtain a mixed solvent. Lithium salt LiPF6 was added to a mixed solvent and mixed thoroughly to obtain an electrolyte; wherein the mass concentration of LiPF6 was 1 mol / L, the mass percentage of triethyl borate was 0.8%, and the mass percentage of fluoroethylene carbonate was 0.8%.

[0094] <Preparation of Secondary Batteries> The prepared positive electrode, separator (12μm thick polypropylene separator), and negative electrode are stacked in sequence, with the separator in the middle of the positive and negative electrode. After winding, hot pressing and shaping, and welding of the tabs, a square battery cell is obtained. The square battery cell is placed in an outer packaging aluminum-plastic film and baked in an oven at 85±10℃ for 24 hours. The electrolyte prepared above is injected into the dried battery, and the battery is allowed to stand, form, and be capacity tested to complete the preparation of the secondary battery.

[0095] Example 2 The difference between Example 2 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in <Preparation of Silicon-Carbon Composite Material>.

[0096] In this embodiment, 1.77 g of phosphoric acid, 1.97 g of LiOH·H2O, and 5.22 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0097] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 1.6% and the mass percentage of fluoroethylene carbonate is 1.6%.

[0098] Example 3 The difference between Example 3 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in the <Preparation of Silicon-Carbon Composite Material>.

[0099] In this embodiment, 2.00 g of phosphoric acid, 2.23 g of LiOH·H2O, and 5.24 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0100] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 1.8% and the mass percentage of fluoroethylene carbonate is 1.8%.

[0101] Example 4 The difference between Example 4 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in <Preparation of Silicon-Carbon Composite Material>.

[0102] In this embodiment, 2.23 g of phosphoric acid, 2.49 g of LiOH·H2O, and 5.25 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0103] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 2.0% and the mass percentage of fluoroethylene carbonate is 2.0%.

[0104] Example 5 The difference between Example 5 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in <Preparation of Silicon-Carbon Composite Material>.

[0105] In this embodiment, 2.85 g of phosphoric acid, 3.18 g of LiOH·H2O, and 5.28 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0106] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 2.52% and the mass percentage of fluoroethylene carbonate is 2.52%.

[0107] Example 6 The difference between Example 6 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in the <Preparation of Silicon-Carbon Composite Material>.

[0108] In this embodiment, 3.69 g of phosphoric acid, 4.11 g of LiOH·H2O, and 5.33 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0109] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 3.2% and the mass percentage of fluoroethylene carbonate is 3.2%.

[0110] Example 7 The difference between Example 7 and Example 1 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in <Preparation of Silicon-Carbon Composite Material>.

[0111] In this embodiment, 4.20 g of phosphoric acid, 4.67 g of LiOH·H2O, and 5.36 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0112] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 3.6% and the mass percentage of fluoroethylene carbonate is 3.6%.

[0113] Example 8 The difference between Example 8 and Example 4 is that the <preparation of silicon-carbon composite material> is different.

[0114] In this embodiment, the sieving process after heat treatment of the second product differs from that in Example 4. The particle size of the silicon-carbon composite material is: Dv10 = 6.2 μm, Dv50 = 8.5 μm, Dv90 = 11.3 μm, and the particle size Span value is 0.6. The remaining steps are the same as in Example 4. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0115] Example 9 The difference between Example 9 and Example 4 is that the <preparation of silicon-carbon composite material> is different.

[0116] In this embodiment, the sieving process after heat treatment of the second product differs from that in Example 4. The particle size of the silicon-carbon composite material is: Dv10 = 5.7 μm, Dv50 = 8.9 μm, Dv90 = 14.6 μm, with a particle size Span value of 1. The remaining steps are the same as in Example 4. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0117] Example 10 The difference between Example 10 and Example 4 is that the preparation of the silicon-carbon composite material is different.

[0118] In this embodiment, the sieving process after heat treatment of the second product differs from that in Example 4. The particle size of the silicon-carbon composite material is: Dv10 = 6.9 μm, Dv50 = 8.7 μm, Dv90 = 11.3 μm, and the particle size span value is 0.5. The remaining steps are the same as in Example 4. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0119] Example 11 The difference between Example 11 and Example 4 is that the <preparation of silicon-carbon composite material> is different.

[0120] In this embodiment, the sieving process after heat treatment of the second product differs from that in Example 4. The particle size of the silicon-carbon composite material is: Dv10 = 4.2 μm, Dv50 = 8.6 μm, Dv90 = 15.6 μm, and the particle size span value is 1.2. The remaining steps are the same as in Example 4. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0121] Examples 12-17 The difference between Examples 12-17 and Example 4 is that the mass percentages of triethyl borate and fluoroethylene carbonate in the electrolyte are different.

[0122] Specifically, in Example 12, based on the mass of the electrolyte, the mass percentage of triethyl borate is 0.25% and the mass percentage of fluoroethylene carbonate is 0.25%.

[0123] In Example 13, based on the mass of the electrolyte, the mass percentage of triethyl borate was 0.75% and the mass percentage of fluoroethylene carbonate was 0.75%.

[0124] In Example 14, based on the mass of the electrolyte, the mass percentage of triethyl borate was 1.5% and the mass percentage of fluoroethylene carbonate was 1.5%.

[0125] In Example 15, based on the mass of the electrolyte, the mass percentage of triethyl borate was 2.5% and the mass percentage of fluoroethylene carbonate was 2.5%.

[0126] In Example 16, based on the mass of the electrolyte, the mass percentage of triethyl borate was 0.125% and the mass percentage of fluoroethylene carbonate was 0.125%.

[0127] In Example 17, based on the mass of the electrolyte, the mass percentage of triethyl borate was 3.5% and the mass percentage of fluoroethylene carbonate was 7.5%.

[0128] Comparative Example 1 The difference between Comparative Example 1 and Example 4 is that the mass percentages of H3PO4 and LiOH·H2O in the precursor solution and triethyl borate and fluoroethylene carbonate in the electrolyte are different in <Preparation of Silicon-Carbon Composite Material>.

[0129] In this embodiment, 0.21 g of phosphoric acid, 0.24 g of LiOH·H2O, and 5.14 g of citric acid were dissolved in 200 ml of deionized water to obtain a precursor solution. 50 g of the first product was weighed and added to the precursor solution, and the mixture was heated in a 70°C water bath with continuous stirring for 3 hours to ensure complete reaction. Subsequently, the mixture was dried at 80°C for 3 hours to obtain the second product. The remaining steps were the same as in Example 1. Some performance parameters of the silicon-carbon composite material are shown in Table 1.

[0130] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 0.2% and the mass percentage of fluoroethylene carbonate is 0.2%.

[0131] Comparative Example 2 The only difference between Comparative Example 2 and Example 4 is that trimethyl borate and fluoroethylene carbonate are not used in Comparative Example 2.

[0132] Comparative Example 3 The difference between Comparative Example 3 and Example 4 is that Example 4 uses the first product directly without coating.

[0133] In this embodiment, based on the mass of the electrolyte, the mass percentage of triethyl borate is 3.2% and the mass percentage of fluoroethylene carbonate is 3.2%.

[0134] Comparative Example 4 The difference between Comparative Example 1 and Example 4 is that Example 4 uses the first product directly without coating, and trimethyl borate and fluoroethylene carbonate are not added to the electrolyte.

[0135] Table 1 shows the parameters of the silicon-carbon composite material and the electrolyte, where "W" is the mass percentage of the coating layer based on the mass of the silicon-carbon composite material, "d" is the average thickness of the coating layer, and "M" is the total mass percentage of triethyl borate and fluoroethylene carbonate based on the mass of the electrolyte. B "M" represents the mass percentage of triethyl borate based on the electrolyte mass. F "The mass percentage of fluoroethylene carbonate is based on the mass of the electrolyte."

[0136] Table 1 Performance testing Cyclic performance and volume expansion rate: At 25℃, the secondary battery was charged to 4.3V at a current density of 0.1C, and then discharged to 3V at a current density of 1C. The discharge capacity during this discharge process is Q1. The same battery was cycled under the following conditions: 0.1C charging and 1C discharging, voltage range of 3V~4.3V. The discharge capacity after 100 cycles is Q2, and the capacity retention rate after 100 cycles = Q2 / Q1 × 100%. The volumes of the secondary battery before and after 100 cycles are V, respectively. 前 V 后 Volume expansion rate = (V 后 -V 前 ) / V 前 ×100%; Five tests were conducted for each data set, and the average value was taken.

[0137] The results are shown in Table 2.

[0138] Table 2 By comparing Examples 1-7 with Comparative Example 4, it can be observed that the coated silicon-carbon composite material exhibits higher capacity retention and lower volume expansion rate, indicating that this coating layer can provide volume buffer for silicon-carbon particles, suppress volume expansion during cycling, reduce SEI cracking, and improve capacity retention. Comparing Examples 1-7, it can be found that the overall performance is best when d / W is 20.

[0139] Comparing Examples 1 and 8-11, the results show that controlling the Span value of the silicon-carbon composite material helps to improve the cycle capacity retention rate and reduce the volume expansion of the silicon-carbon composite material. The lower the Span value, the higher the particle size concentration of the silicon-carbon composite material, the more uniform the coating layer, and the better the performance of the silicon-carbon composite material.

[0140] Comparative Examples 4, 2, and 3 show that the coating layer, boron-containing additives, and fluorine-containing additives have a synergistic effect, indicating that when there is a coating layer on the surface of silicon-carbon particles, it can promote the participation of boron-containing additives and fluorine-containing additives in film formation, resulting in a more stable SEI.

[0141] Comparing Examples 4 and 12-16, it can be seen that the M / W ratio affects product performance. When the M / W ratio is too small, the synergistic effect is weak, while when it is large, the amount of boron- and fluorine-containing additives is excessive, resulting in a thicker SEI and affecting performance. Table 2 shows that selecting a suitable d / W ratio, a lower span, and a suitable M / W is beneficial for obtaining silicon-carbon composite materials with better performance.

[0142] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of this application and not to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.

Claims

1. A silicon-carbon composite material, characterized in that, The silicon-carbon composite material includes a silicon-carbon matrix and a coating layer disposed on the surface of the silicon-carbon matrix; The silicon-carbon matrix includes porous carbon material and silicon nanoparticles dispersed in the pores of the porous carbon material. The coating layer comprises lithium phosphate and / or lithium pyrophosphate; Based on the mass of silicon-carbon composite materials, the mass percentage content W% of the coating layer and the average thickness d nm of the coating layer satisfy: 5≤d / W≤42; where d is 10~400nm and W is 0.5~10%.

2. The silicon-carbon composite material as described in claim 1, characterized in that, The particle size of the silicon-carbon composite material satisfies: Dv10 = 4.5~6.5μm, and or, Dv50 = 8~9μm, and or, Dv90 = 12.5~15.5μm.

3. The silicon-carbon composite material as described in claim 1, characterized in that, The particle size span of the silicon-carbon composite material is 0.5~1.

0.

4. The silicon-carbon composite material as described in claim 1, characterized in that, The silicon-carbon composite material contains 35-60% silicon by mass.

5. The silicon-carbon composite material as described in claim 1, characterized in that, The porous carbon material includes at least one of resin-based carbon materials, biomass-based carbon materials, and pitch-based carbon materials.

6. An electrochemical device, characterized in that, The invention includes a negative electrode sheet, the negative electrode sheet comprising a negative current collector and a negative active layer disposed on at least one surface of the negative current collector, the negative active layer comprising a silicon-carbon composite material as described in any one of claims 1 to 5.

7. The electrochemical device as described in claim 6, characterized in that, The electrochemical device further includes an electrolyte, which includes boron-containing additives and fluorine-containing additives. Based on the mass of the electrolyte, the total mass percentage of the boron-containing additives and fluorine-containing additives is M, which satisfies: 0.1≤M / W≤0.8; where M is 0.05~10%.

8. The electrochemical device as described in claim 7, characterized in that, The boron-containing additive includes at least one of lithium difluorooxalate borate, lithium dioxalate borate, lithium tetrafluoroborate, trimethyl borate, and triethyl borate.

9. The electrochemical device as described in claim 7, characterized in that, The fluorinated additives include at least one of fluoroethylene carbonate, lithium difluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium trifluoromethanesulfonate.

10. An electrical appliance, characterized in that, Includes the electrochemical device as described in any one of claims 7 to 9.