A germanium-based anode material and its preparation method

By introducing a porous structure and carbon coating design into germanium-based anode materials, the volume expansion, conductivity, and interface problems of germanium-based anode materials are solved, thereby improving the performance and lifespan of the battery.

CN123120705APending Publication Date: 2026-11-17SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611525769.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Germanium-based anode materials suffer from volume expansion, insufficient conductivity, and interface problems during charge and discharge, resulting in unsatisfactory cycle performance.

Method used

A germanium-based anode material is prepared by using a structure design of germanium-based core, silicon particles deposited in the pores and carbon coating on the surface, forming a porous structure and a carbon coating. The porosity and carbon layer thickness are optimized by combining specific process parameters.

Benefits of technology

It effectively suppresses the volume expansion of germanium-based anode materials, improves conductivity and structural stability, and enhances the coulombic efficiency and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120705A_ABST
    Figure CN123120705A_ABST
Patent Text Reader

Abstract

This application relates to the field of germanium-based anode technology, specifically to a germanium-based anode material and its preparation method. It includes a germanium-based core, silicon particles deposited in the pores of the germanium-based core, and a carbon layer coating the surface of the germanium-based core, wherein the porosity of the germanium-based core is 30%-45%. The technical solution provided in this application can suppress the volume expansion problem of the germanium-based anode material during charge and discharge. The battery formed by the germanium-based anode material provided in this application exhibits good initial coulombic efficiency, initial discharge capacity, cycle capacity retention, and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of germanium-based anode technology, specifically to a germanium-based anode material and its preparation method. Background Technology

[0002] With the rapid development of lithium-ion battery technology, anode materials with high energy density and long cycle life have become a research focus. While traditional anode materials such as graphite possess stable cycle performance, their theoretical specific capacity is relatively low (approximately 372 mAh / g), making it difficult to meet the demands of high-energy-density batteries. Therefore, developing novel anode materials is currently a hot research topic.

[0003] Germanium, as a potential anode material, boasts a theoretical specific capacity as high as 1600 mAh / g, far exceeding that of graphite, attracting widespread attention. However, germanium-based materials also face several challenges in practical applications: 1. Volume change: Germanium undergoes significant volume expansion during charge and discharge, leading to structural damage and decreased cycle performance; 2. Insufficient conductivity: Pure germanium has low conductivity, limiting its performance at high rates; 3. Interface issues: An unstable solid-electrolyte interface (SEI) layer easily forms between germanium and the electrolyte, further affecting the battery's cycle stability and coulombic efficiency. To address these issues, the industry typically employs carbon coating to improve the conductivity of germanium-based anode materials. However, carbon sources cannot completely prevent lithium salt solvents from penetrating to the germanium core, failing to thoroughly resolve the interface issue between germanium and the electrolyte, thus affecting the battery's coulombic efficiency. Furthermore, carbon cannot suppress the volume expansion of germanium-based anode materials during charge and discharge, thereby impacting the structural stability of the anode material and resulting in unsatisfactory cycle performance. Summary of the Invention

[0004] This application provides a germanium-based anode material and its preparation method to solve the problem that the prior art cannot suppress the volume expansion of germanium-based anode materials during charging and discharging, and also cannot solve the technical problems of low coulombic efficiency and poor cycle stability of batteries formed by germanium-based anode materials.

[0005] In a first aspect, this application provides a germanium-based anode material, comprising a germanium-based core, silicon particles deposited in the pores of the germanium-based core, and a carbon layer coated on the surface of the germanium-based core, wherein the porosity of the germanium-based core is 30%-45%.

[0006] In one alternative embodiment, the pore size of the germanium-based core is 10 nm to 100 nm.

[0007] In one alternative embodiment, the thickness of the carbon layer is 10 nm to 50 nm.

[0008] In one alternative embodiment, the silicon particle content of the germanium-based anode material is 35 wt%-50 wt%.

[0009] In one alternative embodiment, the carbon content of the germanium-based anode material is 4 wt%-11 wt%.

[0010] In one alternative embodiment, the pore structure of the germanium-based core includes macropores, with a pore size distribution of 60%-80% and a pore size ≥50 nm.

[0011] In one alternative embodiment, the pore structure of the germanium-based core includes mesopores, with a pore size distribution of 20%-40% and a pore size of 2 nm-50 nm.

[0012] Secondly, this application provides a method for preparing a germanium-based anode material, comprising the following steps. S1, In an inert atmosphere, a germanium source and a metal A source are heat-treated to form an alloy material, wherein the metal A source can undergo a nitriding reaction with a nitrogen-containing atmosphere to obtain a nitride; S2, etching is performed on the nitride to create pores, resulting in a porous material; S3, silicon is deposited in the pores of a porous material using vapor deposition to obtain a precursor; S4, a germanium-based anode material is obtained by mixing a precursor and a carbon source and then heat-treating the mixture.

[0013] In one alternative implementation, step S1 satisfies at least one of the following conditions: (1) The mass ratio of germanium source to metal A source is 1:0.6-1; (2) Increase the temperature of the heat treatment to 450-700℃ at a heating rate of 1-30℃ / min, and hold for 1-5 hours; (3) The metal source A includes magnesium, lithium, or transition metal sources; (4) Inert atmosphere includes at least one of argon and helium.

[0014] In one optional embodiment, the mass ratio of the germanium source to the magnesium source is 1:0.6-0.8; In one optional embodiment, the heating rate is 5-20℃ / min, the heat treatment temperature is 500-650℃, and the holding time is 2-4h.

[0015] In one alternative implementation, step S2 satisfies at least one of the following conditions: (1) The flow rate of the nitrogen-containing atmosphere is 50-100 L / min; (2) The specific steps of the nitriding reaction are to raise the temperature of the nitriding reaction to 600-900℃ at a heating rate of 1-30℃ / min and keep it at that temperature for 2-8 hours; (3) The steps of etching and creating holes in the nitride include mixing the intermediate after the nitriding reaction with an acidic solution under stirring, the acid treatment temperature is 20-80℃, and the acid treatment time is 1-6h.

[0016] In one optional embodiment, the flow rate of the nitrogen-containing atmosphere is 60 L / min to 80 L / min.

[0017] In one optional embodiment, the heating rate during the nitriding reaction is 5-25℃ / min, the temperature of the nitriding reaction is 700℃-800℃, and the holding time is 4h-6h.

[0018] In one alternative embodiment, the acid treatment temperature is 60-80°C, and the acid treatment time is 3-6 hours.

[0019] In one alternative embodiment, the acidic solution includes at least one of hydrochloric acid solution, sulfuric acid solution, or nitric acid solution.

[0020] In one alternative embodiment, the ratio of the intermediate after nitriding reaction to the acidic substance in the acid solution is 1 g: 0.1-1 mol.

[0021] In one optional embodiment, in step S4, the porous material is vapor-deposited in a silane atmosphere at a temperature of 400-550°C for a deposition time of 30-120 min, and the flow rate of the silane atmosphere is 10-100 L / min.

[0022] In one optional embodiment, in step S5, a vapor-phase carbon source is deposited on the surface of the precursor using vapor deposition. The flow rate of the vapor-phase carbon source is 5-50 L / min, the vapor deposition temperature is 900-1200℃, and the holding time is 10-60 min.

[0023] Thirdly, this application provides a battery comprising the aforementioned germanium-based anode material or a germanium-based anode material prepared by the aforementioned method for preparing germanium-based anode materials. Attached Figure Description

[0024] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0025] Figure 1 This is a scanning electron microscope image of the germanium-based anode material obtained in Example 1 of this application; Figure 2This is a transmission electron microscope (TEM) image of the germanium-based anode material obtained in Example 2 of this application; Figure 3 This is a partial high-resolution transmission electron microscope image of the germanium-based anode material obtained in Example 3 of this application. Detailed Implementation

[0026] The following embodiments are provided to better understand this application. However, the following embodiments do not constitute a limitation on the content and scope of protection of this application. Any product that is the same as or similar to this application, derived by anyone under the guidance of this application or by combining the features of this application with other prior art, falls within the scope of protection of this application.

[0027] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0028] This application provides a germanium-based anode material, comprising a germanium-based core, silicon particles deposited in the pores of the germanium-based core, and a carbon layer coating the surface of the germanium-based core, wherein the porosity of the germanium-based core is 30%-45%. Exemplarily, the porosity of the germanium-based core can be 30%, 31%, 32%, 33%, 33.5%, 34%, 35%, 38%, 39%, 40%, 42%, and 45%, or any value or range from 30% to 45%.

[0029] In some alternative embodiments, the pore size of the germanium-based core ranges from 10 nm to 100 nm.

[0030] In some optional embodiments, the thickness of the carbon layer is 10 nm to 50 nm. For example, the thickness of the carbon layer can be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 38 nm, 40 nm, 45 nm, 48 nm, 49 nm, and 50 nm, or any value or range of 10 nm to 50 nm.

[0031] In some optional embodiments, the silicon particle content of the germanium-based anode material is 35wt%-50wt%. For example, the silicon particle content of the germanium-based anode material is 35wt%, 38wt%, 40wt%, 42wt%, 45wt%, 46wt%, 48wt%, 49wt%, and 50wt%, or any value or range of 35wt%-50wt%.

[0032] In some optional embodiments, the carbon content of the germanium-based anode material is 4wt%-11wt%. For example, the carbon content of the germanium-based anode material can be 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, etc., or any value or range of 4wt%-11wt%.

[0033] In some optional embodiments, the pore structure of the germanium-based core includes macropores, with a pore size distribution of 60%-80% and a pore size ≥50nm.

[0034] In some optional embodiments, the pore structure of the germanium-based core includes mesopores with a pore size distribution of 20%-40% and a pore size of 2-50 nm.

[0035] This application provides a method for preparing a germanium-based anode material, comprising the following steps: S1, in an inert atmosphere, heat-treating a germanium source and a metal A source to form an alloy material, wherein the metal A source is capable of undergoing a nitriding reaction with a nitrogen-containing atmosphere to obtain a nitride; S2, etching the nitride to create pores to obtain a porous material; S3, depositing silicon into the pores of the porous material using a vapor deposition method to obtain a precursor; S4, mixing the precursor and a carbon source and heat-treating the mixture to obtain the germanium-based anode material.

[0036] Taking elemental magnesium as the metal source A as an example, the reaction process involved in the above steps is as follows: S1, ; ; S2, (sufficient acidity); S3. ; S4, .

[0037] In some optional embodiments, step S1 satisfies at least one of the following conditions: (1) The mass ratio of germanium source to metal A source is 1:0.6-1; preferably, the mass ratio of germanium source to magnesium source is 1:0.6-0.8; more preferably, the mass ratio of germanium source to metal A source is 1:0.8. This application controls the alloying reaction by adjusting the mass ratio of germanium source to metal A source. If the amount of metal A source added is too small, the alloying reaction will not be sufficient, which will affect the morphology and structure of the final porous germanium; if the amount of metal A source added is too large, some of the unreacted metal A source will become impurities, affecting the subsequent nitriding process, and some will sublimate, resulting in material waste.

[0038] (2) The temperature of the heat treatment is raised to 450-700℃ at a heating rate of 1-30℃ / min, and the holding time is 1-5h; preferably, the heating rate is 5-20℃ / min, the temperature of the heat treatment is 500-650℃, and the holding time is 2-4h.

[0039] (3) The metal source A includes a magnesium source, a lithium source, or a transition metal source, wherein the transition metal source includes Ti, Zr, V, Cr, Mo, and Fe; preferably, the metal source A includes a magnesium source. The magnesium source includes elemental magnesium; the germanium source includes elemental germanium, and the particle size of the elemental magnesium and elemental germanium is 1-5 μm, preferably 1-3 μm.

[0040] (4) The inert atmosphere includes at least one of argon and helium. Argon is preferred.

[0041] This application utilizes the affinity between metal A source and nitrogen atoms. Metal A source and nitrogen gas undergo a nitriding reaction to generate a molten nitride. During the nitriding reaction, the nitride flows and distributes uniformly within the germanium substrate, forming a template intermediate. This intermediate is then removed by acid washing to obtain a porous germanium substrate. In some optional embodiments, step S2 satisfies at least one of the following conditions: (1) The flow rate of the nitrogen-containing atmosphere is 50-100 L / min; preferably, the flow rate of the nitrogen-containing atmosphere is 60 L / min-80 L / min.

[0042] (2) The specific steps of the nitriding reaction are to raise the temperature of the nitriding reaction to 600-900℃ at a heating rate of 1-30℃ / min and hold it for 2-8h; preferably, the heating rate of the nitriding reaction is 5-25℃ / min, the temperature of the nitriding reaction is 700℃-800℃, and the holding time is 4h-6h; when the nitriding reaction temperature is too low and the holding time is too short, the nitriding reaction is insufficient and uneven, which affects the morphology of the porous germanium base, resulting in low porosity of the porous germanium base. The low porosity of the porous germanium base affects the amount of silane deposition, thus resulting in poor electrochemical performance of the final product negative electrode material; when the nitriding reaction temperature is too high and the holding time is too long, although the nitriding reaction can be fully carried out, it will cause the pore structure formed to collapse to a certain extent, resulting in a decrease in porosity, and at the same time, it will also cause a waste of resources and energy, and the synthesis efficiency of the negative electrode material will also decrease. For example, the temperature of the nitriding reaction can be 600℃, 620℃, 650℃, 700℃, 750℃, 780℃, 800℃, 810℃, 850℃, 880℃, and 900℃, or any value or range within 600℃-900℃. The holding time of the nitriding reaction can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, and 8h, or any value or range within 2h-8h.

[0043] (3) Under stirring, the intermediate after nitriding reaction is mixed with an acidic solution for acid treatment. The acid treatment temperature is 20-80℃ and the acid treatment time is 1-6h; preferably, the acid treatment temperature is 60-80℃ and the acid treatment time is 3-6h; the acidic solution includes at least one of hydrochloric acid solution, sulfuric acid solution or nitric acid solution. The stirring method can be magnetic stirring or conventional stirring method in the art. This application removes the template intermediate nitride through the acid treatment step. If the temperature or time of acid treatment is too low or too short, the magnesium nitride cannot be completely removed, which will affect the structure of the material and the final capacity, and have an adverse effect on the electrochemical performance; if the temperature or time of acid treatment is too high or too long, it will also lead to problems such as pore structure collapse, affecting the porosity of the porous germanium-based material, thereby reducing the electrochemical performance of the negative electrode material. For example, the acid treatment temperature can be 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, or 80℃, or any value or range from 20℃ to 80℃. The acid treatment time can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, or 6h, or any value or range from 1 to 6h.

[0044] In some optional embodiments, etching and hole-forming can be achieved by using an excess of acid solution during the etching and hole-forming process. Specifically, the ratio of the intermediate after nitriding reaction to the acid substance in the acid solution is 1g:0.1-1mol.

[0045] In some optional embodiments, in step S4, the porous material is vapor-deposited in a silane atmosphere at a temperature of 400-550°C for 30-120 minutes, with a silane atmosphere flow rate of 10-100 L / min. If the silane atmosphere flow rate is too low, the deposition temperature is too low, or the time is too short, the silane cannot be fully decomposed and uniformly deposited into the pores of the porous germanium, resulting in the anode material's capacity not reaching the expected level. If the silane atmosphere flow rate is too high, the deposition temperature is too high, or the time is too long, it will lead to an excessively high silicon content. In addition to filling the pores, silicon will also deposit on the surface of the porous germanium substrate, exacerbating the overall expansion of the anode material and making it prone to pulverization and cracking during cycling, thus causing failure. For example, the flow rate of the silane atmosphere can be 10 L / min, 20 L / min, 30 L / min, 40 L / min, 50 L / min, 60 L / min, 70 L / min, 80 L / min, 90 L / min, and 100 L / min, or any value or range within the range of 10-100 L / min. The deposition temperature can be 400℃, 420℃, 450℃, 480℃, 500℃, 520℃, 540℃, 545℃, and 550℃, or any value or range within the range of 400-550℃. The deposition time can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, or 120 min, or any value or range within the range of 30-120 min.

[0046] In some optional embodiments, in step S5, a gaseous carbon source is deposited on the surface of the precursor using a vapor deposition method. The flow rate of the gaseous carbon source is 5-50 L / min, the vapor deposition temperature is 900-1200℃, and the holding time is 10-60 min. Preferably, the flow rate of the gaseous carbon source is 5-20 L / min, the vapor deposition temperature is 450-500℃, and the holding time is 60-90 min. When the flow rate of the gas-phase carbon source is too low, the deposition temperature is too low, or the time is too short, the final carbon coating layer is thin and lacks integrity. During cycling, the carbon layer is prone to breakage, exposing the internal structure to the electrolyte, generating more SEI film, increasing battery internal resistance, and leading to decreased charge / discharge efficiency. When the flow rate of the gas-phase carbon source is too high, the deposition temperature is too high, or the time is too long, although the coating effect of the carbon layer can be guaranteed, the resulting carbon layer thickness will be relatively large. On the one hand, since the carbon layer does not intercalate lithium, an excessively thick carbon layer will significantly reduce the overall theoretical capacity; on the other hand, it will hinder the rapid diffusion of lithium ions during charge and discharge, leading to a decrease in the battery's rate performance. For example, the flow rate of the gas-phase carbon source can be 5 L / min, 10 L / min, 15 L / min, 20 L / min, 30 L / min, 35 L / min, 40 L / min, 45 L / min, 50 L / min, or any value or range from 5 to 50 L / min. The deposition temperature can be 900℃, 950℃, 1000℃, 1050℃, 1100℃, 1150℃, and 1200℃, or any value or range within 900-1200℃. The deposition time can be 10 min, 15 min, 20 min, 25 min, 30 min, 40 min, 45 min, 50 min, and 60 min, or any value or range within 10-60 min.

[0047] In some alternative embodiments, the gaseous carbon source includes at least one of methane, ethane, and acetylene.

[0048] The germanium-based anode material obtained by the above method in this application has a porous germanium framework. Silane deposition uniformly fills the pores, improving its theoretical capacity while mitigating silicon volume expansion. An external carbon layer isolates it from electrolyte erosion, further optimizing the material's conductivity and structural stability. Furthermore, this application enables the production of carbon-coated silane-deposited porous germanium-based anode material at low temperatures (below 1200℃) through a two-step furnace loading process with four reactions and a single acid washing step. First, a single atmosphere change in a tube furnace allows for continuous alloying and nitriding reactions. Second, a single acid washing removes the template. Then, a single atmosphere change in a vertical tube furnace allows for continuous CVD silane deposition and CVD carbon coating. After furnace exit, the carbon-coated silane-deposited porous germanium-based material is obtained, which can be used as a lithium-ion battery anode material, significantly improving the cycle performance of silicon materials. The process provided in this application is simple and continuous, saving time. Moreover, the raw materials are inexpensive and readily available, resulting in low costs and facilitating large-scale commercial production.

[0049] The test methods for the porosity, pore size and pore size distribution of the germanium-based core (powder 3 provided in the following examples and comparative examples) provided in this application are determined by mercury porosimetry. Granularity Dv 50 The particle size distribution was determined using a laser particle size analyzer. The carbon and silicon content were determined using ICP-OES. The method for testing the carbon layer thickness is to measure the thickness range of the germanium-based anode material using transmission electron microscopy. The tap density test method shall be in accordance with GB / T 5162-2021 Determination of tap density of metal powders; the specific surface area test method shall be determined by the BET method.

[0050] Example 1 This embodiment provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1) According to the mass ratio of Ge powder to Mg powder of 1:0.8, Ge powder (1-3μm) and Mg powder (1-3μm) are mixed evenly, placed in a tube furnace, heated to 550℃ at a heating rate of 5℃ / min under Ar atmosphere and held for 2h. After cooling, powder 1 is obtained. (2) The atmosphere in step (1) was changed to N2 atmosphere with a flow rate of 70 L / min, and the temperature was increased to 750℃ at a heating rate of 10℃ / min for nitriding reaction. After holding at the temperature for 5 hours, the mixture was cooled and removed to obtain powder II. (3) Place the powder two obtained in step (2) into a beaker, pour in 100 mL of 1 mol / L hydrochloric acid, stir magnetically at 40 °C for 4 h, then filter repeatedly with deionized water until the pH is neutral, and then vacuum dry to obtain powder three. Tests showed that powder 3 is a porous material with a porosity of 43.6%, a pore size of 10-100 nm, and a pore size distribution of 72% macropores and 28% mesopores. (4) Place the powder three obtained in step (3) into a vertical tube furnace, heat it to 450°C in a silane atmosphere with a flow rate of 80 L / min and heat it at a rate of 5°C / min for deposition, hold it at the temperature for 1 h, and then cool it to obtain powder four. (5) Switch the atmosphere in step (4) to an acetylene atmosphere with a flow rate of 10 L / min, heat it to 950 °C at a heating rate of 10 °C / min for carbon coating, keep it at the temperature for 20 min, and then cool it to obtain germanium-based anode material.

[0051] The scanning electron microscope image of the germanium-based anode material prepared in this embodiment is shown below. Figure 1 As shown, after silane deposition and acetylene carbon coating, the porous germanium matrix has a relatively complete overall structure, which is beneficial for processing and can improve the stability and cycle performance of the material.

[0052] The overall transmission electron microscope image of the germanium-based anode material prepared in this embodiment is shown in the image. Figure 2 ) and local high-resolution transmission electron microscopy images ( Figure 3 As shown in the figure, the carbon coating effect of chemical deposition is relatively good. The porous germanium substrate is completely wrapped by the carbon layer. The carbon layer is dense and uniform, and the internal porous structure is intact, leaving room for the expansion of germanium. The thickness of the carbon layer was characterized by high resolution. The thickness of the carbon layer of about 10 nm is moderate and relatively uniform. It can effectively alleviate the problems of volume expansion, insufficient conductivity and side reactions of internal porous germanium and silicon in electrochemical reaction, thereby significantly improving the performance and life of battery.

[0053] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 3.7 μm, a carbon content of 5.2 wt%, a silicon content of 42.4 wt%, and a tap density of 0.89 g / cm³. 3 Its specific surface area is 4.32 m². 2 / g.

[0054] Example 2 This embodiment provides a method for preparing a germanium-based anode material. The specific steps and parameters are the same as in Example 1. The difference is that the mass ratio of Ge powder to Mg powder in step (1) is 1:0.6.

[0055] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 39.1%, a pore size of 10-100 nm, and a pore size distribution of 68% macropores and 32% mesopores.

[0056] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50It has a particle size of 5.5 μm, a carbon content of 7.1 wt%, a silicon content of 38.6 wt%, and a tap density of 0.77 g / cm³. 3 Its specific surface area is 3.93 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0057] Example 3 This embodiment provides a method for preparing a germanium-based anode material. The specific steps and parameters are the same as in Example 1. The difference is that the nitriding reaction temperature in step (2) is 600℃ and the holding time is 2h.

[0058] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 38.8%, a pore size of 10-100 nm, and a pore size distribution of 63% macropores and 37% mesopores.

[0059] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.8 μm, a carbon content of 6.6 wt%, a silicon content of 39.9 wt%, and a tap density of 0.8 g / cm³. 3 The specific surface area is 4.01 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0060] Example 4 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in Example 1. The difference is that the temperature of the nitriding reaction in step (2) is 700℃ and the holding time is 6h.

[0061] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 41.8%, a pore size of 10-100 nm, and a pore size distribution of 69% macropores and 31% mesopores.

[0062] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.6 μm, a carbon content of 5.5 wt%, a silicon content of 40.5 wt%, and a tap density of 0.85 g / cm³. 3 Its specific surface area is 4.77 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0063] Example 5 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in Example 1. The difference is that the temperature of the nitriding reaction in step (2) is 800℃ and the holding time is 4h.

[0064] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 44.9%, a pore size of 10-100 nm, and a pore size distribution of 74% macropores and 26% mesopores.

[0065] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.7 μm, a carbon content of 4.7 wt%, a silicon content of 44.1 wt%, and a tap density of 0.86 g / cm³. 3 The specific surface area is 4.89 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0066] Example 6 This embodiment provides a method for preparing a germanium-based anode material. The specific steps and parameters are the same as in Example 1. The difference is that the nitriding reaction temperature in step (2) is 900℃ and the holding time is 8h.

[0067] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 38.4%, a pore size of 10-100 nm, and a pore size distribution of 64% macropores and 36% mesopores.

[0068] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 5.3 μm, a carbon content of 5.3 wt%, a silicon content of 37.7 wt%, and a tap density of 0.83 g / cm³. 3 Its specific surface area is 6.52 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0069] Example 7 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that the temperature of magnetic stirring in step (3) is 20°C and the stirring time is 2h.

[0070] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 38.8%, a pore size of 10-100 nm, and a pore size distribution of 70% macropores and 30% mesopores.

[0071] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 6.3 μm, a carbon content of 8.9 wt%, a silicon content of 35 wt%, and a tap density of 0.74 g / cm³. 3 Its specific surface area is 3.56 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0072] Example 8 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that the temperature of magnetic stirring in step (3) is 60°C and the stirring time is 3h.

[0073] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 44.1%, a pore size of 10-100 nm, and a pore size distribution of 73% macropores and 27% mesopores.

[0074] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.7 μm, a carbon content of 5.0 wt%, a silicon content of 43.6 wt%, and a tap density of 0.90 g / cm³. 3 Its specific surface area is 4.87 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0075] Example 9 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that the temperature of magnetic stirring in step (3) is 80°C and the stirring time is 6h.

[0076] Upon testing, the powder obtained in step (3) of this embodiment is a porous material with a porosity of 40.7%, a pore size of 10-100 nm, and a pore size distribution of 71% macropores and 29% mesopores.

[0077] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 5.7 μm, a carbon content of 7.2 wt%, a silicon content of 36.9 wt%, and a tap density of 0.82 g / cm³. 3 The specific surface area is 3.98 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0078] Example 10 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that in step (4), the powder obtained in step (3) is placed in a vertical tube furnace and heated to 450°C in a silane atmosphere with a flow rate of 100 L / min at a heating rate of 5°C / min for deposition. The temperature is maintained for 2 hours, and then cooled to obtain powder (4).

[0079] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.4 μm, a carbon content of 5.8 wt%, a silicon content of 48.3 wt%, and a tap density of 0.85 g / cm³. 3 The specific surface area is 4.29 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0080] Example 11 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as those in Example 1. The difference is that in step (4), the powder obtained in step (3) is placed in a vertical tube furnace and heated to 400°C in a silane atmosphere with a flow rate of 90 L / min at a heating rate of 5°C / min for deposition. The temperature is maintained for 1 hour, and then cooled to obtain powder (4).

[0081] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.1 μm, a carbon content of 5.6 wt%, a silicon content of 44.4 wt%, and a tap density of 0.81 g / cm³. 3 Its specific surface area is 5.03 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0082] Example 12 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that in step (4), the powder obtained in step (3) is placed in a vertical tube furnace and heated to 500°C in a silane atmosphere with a flow rate of 70 L / min at a heating rate of 5°C / min for deposition. The temperature is maintained for 1.5 h, and then cooled to obtain powder (4).

[0083] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 3.8 μm, a carbon content of 5.3 wt%, a silicon content of 42.0 wt%, and a tap density of 0.78 g / cm³. 3 The specific surface area is 5.78 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0084] Example 13 This embodiment provides a method for preparing germanium-based anode material. The specific steps and parameters are the same as in embodiment 1. The difference is that in step (4), the powder obtained in step (3) is placed in a vertical tube furnace and heated to 500°C in a silane atmosphere with a flow rate of 50 L / min at a heating rate of 5°C / min for deposition. The temperature is held for 30 min, and then cooled to obtain powder (4).

[0085] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 3.5 μm, a carbon content of 5.0 wt%, a silicon content of 35.3 wt%, and a tap density of 0.72 g / cm³. 3 Its specific surface area is 6.49 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0086] Example 14 This embodiment provides a method for preparing a germanium-based negative electrode material. The specific steps and parameters are the same as those in Example 1. The difference is that in step (5), the flow rate of the acetylene atmosphere in (4) is 50 L / min and the holding time is 30 min.

[0087] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.9 μm, a carbon content of 10.5 wt%, a silicon content of 37.7 wt%, and a tap density of 0.91 g / cm³. 3 Its specific surface area is 2.78 m². 2 / g, the thickness of the carbon layer is 30-50nm.

[0088] Example 15 This embodiment provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1) According to the mass ratio of Ge powder and Mg powder of 1:0.7, Ge powder (1-3μm) and Mg powder (1-3μm) are mixed evenly and placed in a tube furnace. Under Ar atmosphere, the temperature is raised to 500℃ at a heating rate of 15℃ / min and held for 4h. After cooling, powder 1 is obtained. (2) The atmosphere in step (1) was changed to N2 atmosphere with a flow rate of 80 L / min, and the temperature was increased to 650℃ at a heating rate of 5℃ / min for nitriding reaction. After holding at the temperature for 6.5h, the mixture was cooled and removed to obtain powder II. (3) Place the powder two obtained in step (2) into a beaker, pour in 80 mL of 2 mol / L sulfuric acid, stir magnetically at 35°C for 2 h, then filter repeatedly with deionized water until the pH is neutral, and then vacuum dry to obtain powder three. Tests showed that powder 3 is a porous material with a porosity of 42.4%, a pore size of 10-100 nm, and a pore size distribution of 70% macropores and 30% mesopores. (4) Place the powder three obtained in step (3) into a vertical tube furnace, heat it to 450°C in a silane atmosphere with a flow rate of 80 L / min and heat it at a rate of 5°C / min for deposition, hold it at the temperature for 2 hours, and then cool it to obtain powder four. (5) Change the atmosphere in step (4) to a methane atmosphere with a flow rate of 10 L / min, heat it to 1100 °C at a heating rate of 8 °C / min for carbon coating, keep it at the temperature for 20 min, and then cool it to obtain germanium-based anode material.

[0089] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 3.5 μm, a carbon content of 5.4 wt%, a silicon content of 41.7 wt%, and a tap density of 0.91 g / cm³.3 Its specific surface area is 4.27 m². 2 / g, with a carbon layer thickness of 15-40nm.

[0090] Example 16 This embodiment provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1) According to the mass ratio of Ge powder and Mg powder of 1:0.8, Ge powder (1-3μm) and Mg powder (1-3μm) are mixed evenly, placed in a tube furnace, heated to 650℃ at a heating rate of 20℃ / min under Ar atmosphere and held for 3h. After cooling, powder 1 is obtained. (2) The atmosphere in step (1) was changed to N2 atmosphere with a flow rate of 60 L / min, and the temperature was increased to 850℃ at a heating rate of 25℃ / min for nitriding reaction. After holding at the temperature for 6 hours, the mixture was cooled and removed to obtain powder II. (3) Place the powder two obtained in step (2) into a beaker, pour in 2000 mL of 0.1 mol / L nitric acid, stir magnetically at 45 °C for 1.5 h, then filter repeatedly with deionized water until the pH is neutral, and then vacuum dry to obtain powder three. Tests showed that powder 3 is a porous material with a porosity of 44.1%, a pore size of 10-100 nm, and a pore size distribution of 74% macropores and 26% mesopores. (4) Place the powder three obtained in step (3) into a vertical tube furnace, heat it to 500°C in a silane atmosphere with a flow rate of 80 L / min and a heating rate of 30°C / min for deposition, hold for 30 min, and then cool to obtain powder four. (5) Switch the atmosphere in step (4) to an ethane atmosphere with a flow rate of 10 L / min, heat it to 1200 °C at a heating rate of 10 °C / min for carbon coating, hold it at the temperature for 10 min, and then cool it to obtain germanium-based anode material.

[0091] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.0 μm, a carbon content of 4.9 wt%, a silicon content of 43.3 wt%, and a tap density of 0.88 g / cm³. 3 Its specific surface area is 4.43 m². 2 / g, with a carbon layer thickness of 10-30nm.

[0092] Comparative Example 1 This comparative example provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1)-(4) are the same as in Example 1, that is, the powder obtained in step (4) of Example 1 is a germanium-based negative electrode material.

[0093] After testing, the particle size Dv of the germanium-based anode material prepared in this comparative example was found to be... 50 It has a particle size of 3.4 μm, a silicon content of 44.9 wt%, and a tap density of 0.65 g / cm³. 3 The specific surface area is 9.88 m². 2 / g.

[0094] Comparative Example 2 This comparative example provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1)-(3) are the same as in Example 1; (4) Switch the atmosphere in step (3) to an acetylene atmosphere with a flow rate of 10 L / min, heat the powder to 950 °C at a heating rate of 10 °C / min, carbonize it, keep it at the temperature for 20 min, and then cool it to obtain the germanium-based anode material.

[0095] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 4.0 μm, a carbon content of 5.6 wt%, and a tap density of 0.82 g / cm³. 3 Its specific surface area is 4.14 m². 2 / g, the thickness of the carbon layer is 15-40nm.

[0096] Comparative Example 3 This comparative example provides a method for preparing a germanium-based anode material, the specific steps and parameters of which are as follows: (1)-(2) are the same as in Example 1; (3) Place the powder 2 obtained in step (2) into a beaker, pour in 1 mol / L hydrochloric acid, stir magnetically at 20°C for 1 h, then filter repeatedly with deionized water until the pH is neutral, and then vacuum dry to obtain powder 3. The porosity of powder 3 is 29.5%, the pore size is 10-100 nm, and the pore size distribution is 55% macropores and 45% mesopores. (4)-(5) are the same as in Example 1.

[0097] After testing, the particle size Dv of the germanium-based anode material prepared in this embodiment was found to be... 50 It has a particle size of 3.9 μm, a carbon content of 5.0 wt%, a silicon content of 28.8 wt%, and a tap density of 0.87 g / cm³. 3 Its specific surface area is 4.22 m². 2 / g, the thickness of the carbon layer is 10-30nm.

[0098] Experimental Example The germanium-based anode materials obtained in Examples 1-16 and Comparative Examples 1-3 were mixed with binder, conductive agent, and solvent to form a slurry, which was then uniformly coated onto copper foil. After drying and rolling, the anode sheet was obtained. The binder used was lithium polyacrylate (viscosity-average molecular weight 30000 Da), the conductive agent was conductive carbon black, and the solvent was deionized water. The ratio of germanium-based anode material: conductive carbon black: binder: deionized water was 95g:1g:4g:220mL. LB046 (solvent: ethylene carbonate EC: dimethyl carbonate DEC = 1:1, lithium hexafluorophosphate LiPF6) was used as the electrolyte, a polypropylene (PP) membrane as the separator, and a lithium metal sheet as the counter electrode. These components were then assembled with the anode sheet to form a coin cell.

[0099] Each coin cell was assembled in a glove box under an Ar atmosphere. After stabilization, performance tests were performed using a Blue Electric CT2001A electrochemical workstation. The charge / discharge rate was 0.1C, and the charge / discharge voltage range was 0.005V-1.5V. The following tests were performed on the coin cells: initial discharge capacity, initial coulombic efficiency, electrode full charge expansion rate, cycle performance (capacity retention rate after 500 cycles at 1C), and rate performance.

[0100] Initial Coulomb efficiency % = First discharge capacity / First charge capacity × 100%; Electrode expansion rate % when fully charged = (thickness of fully charged negative electrode - thickness of initial negative electrode) / thickness of initial negative electrode × 100%; Capacity retention % after 500 cycles = (Discharge capacity after 500 cycles / Discharge capacity on the third cycle) × 100%; Rate performance % = 2C discharge capacity / 0.1C discharge capacity × 100%; The test results are shown in Table 1 below.

[0101] Table 1 Test Results

[0102] As shown in Table 1, compared to Example 1, the germanium-based anode material provided in Comparative Example 1 has low initial coulombic efficiency, high electrode full-charge expansion rate, and poor cycle capacity retention. This is because the surface of the germanium-based core in the germanium-based anode material provided in Comparative Example 1 is not coated with a carbon source, thus directly exposing the electrolyte to the surface of the anode material. This exacerbates SEI film instability, volume stress concentration, particle pulverization, and continuous side reactions, resulting in low initial coulombic efficiency, high electrode full-charge expansion rate, and poor cycle capacity retention. The germanium-based anode material provided in Comparative Example 2 has low initial discharge capacity because silicon is not deposited inside the germanium-based core, resulting in low theoretical lithium storage capacity and thus low initial discharge capacity. The germanium-based anode material provided in Comparative Example 3 has low initial discharge capacity, high electrode full-charge expansion rate, and poor initial coulombic efficiency and cycle performance retention. This is because the germanium-based core provided in Comparative Example 3 has low porosity, which not only affects the volume expansion suppression effect of the germanium-based anode material but also results in low silicon loading, leading to unsatisfactory electrochemical performance of the anode material. This application uses a germanium-based material with a porosity of 30%-45% as the core, deposits silicon in the pores of the germanium-based core, and coats the surface of the germanium-based core with a carbon layer to form a negative electrode material that exhibits good initial coulombic efficiency, initial discharge capacity, cycle capacity retention, and rate performance.

[0103] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this application.

Claims

1. A germanium-based anode material, characterized in that, It includes a germanium-based core, silicon particles deposited in the pores of the germanium-based core, and a carbon layer coating the surface of the germanium-based core. The porosity of the germanium-based core is 30%-45%.

2. The germanium-based anode material of claim 1, wherein, The pore size of the germanium-based core ranges from 10 nm to 100 nm; And / or, the thickness of the carbon layer is 10 nm-50 nm.

3. The germanium-based anode material of claim 1, wherein, The silicon particle content of germanium-based anode materials is 35wt%-50wt%; And / or, the carbon content of the germanium-based anode material is 4 wt%-11 wt%; And / or, the pore structure of the germanium-based core includes macropores, with a pore size distribution of 60%-80% and a pore size ≥50nm; And / or, the pore structure of the germanium-based core includes mesopores, with a pore size distribution of 20%-40% and a pore size of 2nm-50nm.

4. A method for producing a germanium-based negative electrode material, characterized by, Includes the following steps, S1, In an inert atmosphere, a germanium source and a metal A source are heat-treated to form an alloy material, wherein the metal A source can undergo a nitriding reaction with a nitrogen-containing atmosphere to obtain a nitride; S2, etching is performed on the nitride to create pores, resulting in a porous material; S3, silicon is deposited in the pores of a porous material using vapor deposition to obtain a precursor; S4, a germanium-based anode material is obtained by mixing a precursor and a carbon source and then heat-treating the mixture.

5. The preparation method according to claim 4, characterized in that, Step S1 satisfies at least one of the following conditions: (1) The mass ratio of germanium source to metal A source is 1:0.6-1; (2) The temperature of the heat treatment is raised to 450-700℃ at a heating rate of 1-30℃ / min, and the holding time is 1-5h; (3) The metal source A includes magnesium, lithium, or transition metal sources; (4) Inert atmosphere includes at least one of argon and helium.

6. The preparation method according to claim 5, characterized in that, The mass ratio of the germanium source to the magnesium source is 1:0.6-0.8; And / or, the heating rate is 5-20℃ / min, the heat treatment temperature is 500-650℃, and the holding time is 2-4h.

7. The preparation method according to claim 4, characterized in that, Step S2 satisfies at least one of the following conditions: (1) The flow rate of the nitrogen-containing atmosphere is 50-100 L / min; (2) The specific steps of the nitriding reaction are to raise the temperature of the nitriding reaction to 600-900℃ at a heating rate of 1-30℃ / min and keep it at that temperature for 2-8 hours; (3) The steps of etching and creating holes in nitrides include mixing the intermediate after nitriding reaction with an acidic solution under stirring, and performing acid treatment at a temperature of 20-80℃ for 1-6 hours.

8. The preparation method according to claim 7, characterized in that, The flow rate of the nitrogen-containing atmosphere is 60 L / min-80 L / min; And / or, the heating rate during the nitriding reaction is 5-25℃ / min, the temperature of the nitriding reaction is 700℃-800℃, and the holding time is 4h-6h; And / or, the acid treatment temperature is 60-80℃, and the acid treatment time is 3-6h; And / or, the acidic solution includes at least one of hydrochloric acid solution, sulfuric acid solution or nitric acid solution; And / or, the ratio of the intermediate after nitriding reaction to the acidic substance in the acid solution is 1g:0.1-1mol.

9. The preparation method according to claim 4, characterized in that, In step S4, the porous material is vapor-deposited in a silane atmosphere at a temperature of 400-550℃ for a deposition time of 30-120 min, and the flow rate of the silane atmosphere is 10-100 L / min. And / or, in step S5, a vapor-phase carbon source is deposited on the surface of the precursor using vapor-phase deposition, with a flow rate of 5-50 L / min, a vapor-phase deposition temperature of 900-1200℃, and a holding time of 10-60 min.

10. A battery, characterized in that, The germanium-based anode material includes the germanium-based anode material according to any one of claims 1-3 or the germanium-based anode material prepared by any one of claims 4-9.