A one-dimensional heterojunction silicon-carbon composite anode material and its preparation method

By using a low-temperature, low-pressure chemical vapor deposition process, in-situ composite materials with four temperature zones—catalyst reduction, heterojunction framework growth, silicon-carbon confined filling, and thin carbon end capping—are achieved in the same reactor. This solves the problems of high energy consumption and poor interfacial bonding in the preparation of silicon-carbon anode materials in existing technologies, and realizes the preparation of silicon-carbon composite materials with high efficiency and low cost.

CN123120710APending Publication Date: 2026-11-17ZHEJIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611636924.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-carbon anode materials suffer from problems such as high energy consumption, loose interfacial bonding, high interfacial impedance, large batch-to-batch differences, and cumbersome processes during preparation, making it difficult to achieve in-situ composite preparation of one-dimensional heterojunction framework and silicon-carbon confinement under low-temperature conditions.

Method used

By employing a low-temperature, low-pressure chemical vapor deposition process, in-situ composite in four temperature zones—catalyst reduction, heterojunction framework growth, silicon-carbon confinement filling, and thin carbon end capping—is achieved within the same reactor through a time-sequential feeding method. This results in a dual-scale synergistic confinement structure of single-walled carbon nanotube bundles and silicon-carbon active components, ensuring interfacial bonding and the continuity of the conductive network.

Benefits of technology

Significantly reducing energy consumption, simplifying the process, improving the cycle stability and electrochemical performance of materials, and reducing costs, this method enables the preparation of highly efficient silicon-carbon composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120710A_ABST
    Figure CN123120710A_ABST
Patent Text Reader

Abstract

A one-dimensional heterojunction silicon-carbon composite anode material and its preparation method are disclosed, belonging to the technical field of lithium-ion battery anode materials. In this material, the silicon-carbon active component at least partially fills the hollow cavity and / or inter-tube gaps of the one-dimensional heterojunction, forming a composite structure with dual-scale synergy of inter-tube gap confinement and particle surface coating. The average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is 1.0 nm to 1.4 nm, and the mass content of the silicon-carbon active component is 5% to 40%. The preparation method employs low-temperature, low-pressure chemical vapor deposition, sequentially completing catalyst reduction and activation, one-dimensional heterojunction framework growth, confined filling of the silicon-carbon active component, and thin carbon end-capping passivation within the same reactor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery anode material technology, specifically to a one-dimensional heterojunction silicon-carbon composite anode material and its preparation method. Background Technology

[0002] As a core component of new energy vehicles and large-scale energy storage, the improvement of lithium-ion batteries' energy density highly depends on the innovation of anode material systems. The theoretical specific capacity of graphite anodes is only 372 mAh / g, which is insufficient to meet the high energy density requirements of power batteries. Silicon-based anodes, due to their ultra-high theoretical specific capacity (approximately 4200 mAh / g for crystalline silicon and approximately 3579 mAh / g for amorphous silicon) and low lithium intercalation potential (approximately 0.4 V vs. Li / Li), offer a significant advantage. + Silicon-based anodes are considered strong candidates for next-generation high-energy-density anode materials due to their advantages such as effectively avoiding lithium dendrite formation, abundant reserves, and environmental friendliness. However, silicon-based anodes experience approximately 300% volume expansion during charge and discharge. Repeated expansion and contraction lead to the pulverization and shedding of active materials, repeated rupture and regeneration of the solid electrolyte interphase (SEI) film, resulting in rapid capacity decay, low coulombic efficiency, and electrode cracking, severely restricting their commercial application.

[0003] To mitigate the volume effect of silicon, current technologies typically combine nano-silicon with carbon materials to form silicon-carbon anodes, utilizing the buffer space and continuous conductive network provided by the carbon matrix to improve cycle stability. Among these, carbon nanotubes (CNTs), with their one-dimensional linear structure, excellent mechanical strength, and electrical conductivity, are widely used as the conductive framework and confinement carrier in silicon-carbon composites. Constructing nanotubes into one-dimensional heterostructures can further enhance their physicochemical properties. For example, some methods involve mechanically mixing CNTs with silicon powder, graphite, etc., to form a slurry, or using multi-walled carbon nanotubes (MWCNTs) to coat the surface of silicon particles to construct a conductive network. However, in the mechanical mixing method, the interface between CNT and silicon is loose and the contact resistance is high, making it difficult for CNT to form an effective three-dimensional confinement structure inside the silicon particles. The conductive network is still prone to breakage during cycling. MWCNT, due to its large tube diameter (usually greater than 5nm), cannot form an effective cavity confinement for silicon clusters at the sub-2nm scale, and its ability to buffer expansion is limited. Furthermore, the separate mass production of high-purity CNT and the secondary dispersion process significantly increase the process complexity and manufacturing cost.

[0004] Another approach involves growing CNTs in situ on silicon or carbon substrates using chemical vapor deposition (CVD) to achieve tighter interfacial bonding. For example, plasma-enhanced CVD (PECVD) or segmented CVD processes can be used to sequentially grow CNTs and deposit silicon in the same reactor, or metal catalysts can be loaded onto the surface of silicon-carbon composite materials and then interconnected in situ using a vapor phase method. However, the above-mentioned routes still have significant shortcomings: First, the conventional silicon CVD deposition temperature is usually as high as 700–1100℃. The high temperature not only consumes a lot of energy, but also aggravates the sintering and agglomeration of catalyst particles, resulting in a wide CNT diameter distribution and poor selectivity. Second, most existing CVD routes are non-in-situ composite modes of "first elongating the tube, then filling it with silicon" or "coating the tube externally", which makes it difficult to achieve dual-scale synergistic confinement of silicon and carbon active components in the hollow cavity of CNTs and the gap between the tube bundles. The silicon-CNT interface still depends on subsequent heat treatment for bonding, and the interface impedance and consistency are difficult to guarantee. Third, the plasma-assisted route has complex equipment that is difficult to scale up, and lacks online monitoring methods for CNT diameter, silicon filling rate and amorphous carbon ratio, resulting in large batch-to-batch differences and cumbersome post-processing (such as acid washing and purification, offline sorting) procedures.

[0005] Furthermore, carbon-based one-dimensional heterostructures, especially single-walled carbon nanotubes (MWCNTs), are more suitable than MWCNTs as one-dimensional supports for silicon-carbon confinement due to their smaller diameter (typically less than 2 nm), higher aspect ratio, and better conductivity. However, the CVD preparation of one-dimensional heterostructures is extremely sensitive to catalyst particle size, reaction temperature, and atmospheric conditions. Traditional high-temperature CVD processes (e.g., 1200–1500 °C) are energy-intensive, incompatible with heat-sensitive silicon-carbon precursors, and often contain large amounts of amorphous carbon and metal residues, requiring repeated purification with strong acids, which poses a significant environmental burden. Existing studies have attempted to reduce the cost of one-dimensional heterostructure preparation through floating catalytic CVD and fluidized bed CVD, but these studies mainly focus on the large-scale preparation of the one-dimensional heterostructure itself and have not effectively combined with in-situ composites with silicon-carbon anodes. This still cannot solve the problem of process redundancy and cost stacking caused by "mass production of high-purity one-dimensional heterostructures alone + secondary dispersion of slurry".

[0006] In summary, existing silicon-carbon anode technologies lack an in-situ composite process that can achieve "one-dimensional heterojunction framework growth - silicon-carbon confined filling - thin carbon end-capping passivation" in the same reactor under low-temperature conditions. It is also difficult to perform real-time closed-loop control of CNT diameter, silicon filling rate and defect degree during the preparation process. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a one-dimensional heterojunction silicon-carbon composite anode material and its preparation method that takes into account low temperature energy saving, dual-scale confined configuration and online consistency control.

[0008] The technical solution adopted by this invention to solve its technical problem is: a one-dimensional heterojunction silicon-carbon composite anode material, comprising a silicon-carbon active component and a one-dimensional heterojunction conductive framework, wherein the one-dimensional heterojunction is a carbon-based one-dimensional heterojunction, the main body of which is a single-walled carbon nanotube bundle, the silicon-carbon active component at least partially fills the inter-tube gaps of the one-dimensional heterojunction and / or is coated on its surface by the one-dimensional heterojunction, forming a composite structure in which the tube confinement and surface coating work together; the average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is 1.0 nm to 1.4 nm, and the mass content of elemental silicon in the silicon-carbon active component, based on the total mass of the composite material, is 5% to 40%.

[0009] The one-dimensional heterojunction refers to a heterostructure composed of carbon nanotube segments with different chirality or diameters along the axial direction, with single-walled carbon nanotube bundles as the basic building blocks. This invention confines the silicon-carbon active component within the hollow cavity and inter-bundle gaps of the one-dimensional heterojunction, forming a dual-scale synergistic confinement structure. This simultaneously suppresses silicon volume expansion at both the nanoscale and micro-network scales, preventing the active material from pulverizing and detaching. The average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is only 1.0~1.4 nm, effectively confining silicon clusters at the sub-2 nm scale, significantly superior to multi-walled carbon nanotubes. The single-walled carbon nanotube content is not less than 99.99%, ensuring high purity and low defect density of the conductive framework. Combined with a silicon-carbon active component content range of 5%~40%, excellent cycle stability can be achieved while maintaining high capacity. Preferably, when the mass content of the silicon-carbon active component is around 25%, the overall performance of the material's specific capacity and cycle life is optimal.

[0010] Preferably, the silicon-carbon active component includes at least one of nano-silicon, amorphous carbon, and in-situ pyrolysis carbon, and a Si-C interface bond is formed between the silicon-carbon active component and the one-dimensional heterojunction.

[0011] Si-C interfacial bonding transforms the simple physical contact between the silicon-carbon active components and the one-dimensional heterostructure into a chemical bond, significantly reducing interfacial contact resistance and improving electron transport efficiency. Simultaneously, this bonding effectively anchors silicon clusters during charge and discharge, preventing them from detaching from the conductive framework during volume expansion and contraction, thereby extending cycle life. The presence of in-situ pyrolyzed carbon further buffers the volumetric stress of silicon and enhances the overall structural integrity of the material.

[0012] Preferably, the configuration of the composite structure is one of the following: (1) The silicon-carbon active component is coated in a one-dimensional heterojunction tube network gap; (2) The silicon-carbon active component is filled into the hollow cavity of a one-dimensional heterojunction, forming a cavity-filling type. (3) Surface co-growth type with silicon as the core, one-dimensional heterojunction as the shell and cracked carbon as the transition layer.

[0013] The three configurations described above are suitable for different application scenarios: the bundled network type has a complete continuous conductive framework and good mass production adaptability, making it suitable for large-scale applications of power batteries; the cavity-filled type completely confines silicon inside the cavity, providing the strongest confinement effect, making it suitable for high-rate, long-cycle scenarios; and the surface co-growth type has the tightest interface bonding and the shortest electron transport path, making it suitable for high-end applications with extremely high energy density requirements. All three configurations are derived from the same in-situ composite process and can be flexibly selected according to battery design requirements, thus expanding the applicability of this invention.

[0014] Preferably, the average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is 1.2 nm, and the mass content of the silicon-carbon active component is about 25%; the total content of metal impurities in the composite anode material is not higher than 200 ppm.

[0015] When the average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is 1.2 nm, it achieves an optimal balance between specific surface area and lumen volume, providing sufficient confinement space for silicon while ensuring high conductivity. The silicon-carbon active component content of approximately 25% achieves a good trade-off between specific capacity and initial efficiency. The total metal impurity content is no higher than 200 ppm, effectively avoiding metal catalytic side reactions, reducing abnormal SEI film growth, and improving battery safety and cycle stability.

[0016] Preferably, the one-dimensional heterojunction forms a continuous three-dimensional conductive network, and the aspect ratio of a single one-dimensional heterojunction is not less than 10. 3 Furthermore, adjacent one-dimensional heterojunctions overlap each other through tube bundle gaps, so that the silicon-carbon active components are confined within the network units surrounded by the three-dimensional conductive network.

[0017] Aspect ratio not less than 10 3 One-dimensional heterojunctions readily form dense, continuous conductive networks. The overlapping of the tube bundles creates a three-dimensional confined space, firmly locking the silicon-carbon active components within the network units, maintaining a complete conductive path even at high silicon content. This structure significantly reduces contact losses during cycling, enabling the electrodes to maintain low impedance and high capacity retention even after long cycles, making it particularly suitable for high-rate fast charging scenarios.

[0018] Preferably, the silicon component in the silicon-carbon active component is spherical nano-silicon particles with a D50 particle size of 30nm~150nm and a specific surface area of ​​15m². 2 / g~60m 2 / g; The surface of the silicon component is coated with the one-dimensional heterojunction conductive framework, and the one-dimensional heterojunction and the surface of the silicon component form a continuous contact.

[0019] Spherical nano-silicon avoids stress concentration at sharp corners. Its D50 particle size of 30~150nm effectively shortens the lithium-ion diffusion path without causing serious side reactions due to excessively small particle size; specific surface area of ​​15~60m² 2 / g facilitates the formation of continuous coating contacts with one-dimensional heterojunctions, ensuring that each silicon particle is covered by a conductive network, thereby improving the utilization rate of active materials and rate performance.

[0020] A method for preparing a one-dimensional heterojunction silicon-carbon composite anode material is disclosed, which employs a low-temperature, low-pressure chemical vapor deposition process and completes the following steps sequentially in the same reactor using a time-sequential feeding method: catalyst reduction and activation → one-dimensional heterojunction framework growth → confined filling of silicon-carbon active components → thin carbon end-capping and passivation; wherein the temperature for growing the one-dimensional heterojunction framework is 450℃~650℃, the temperature for confined filling of silicon-carbon active components is 400℃~600℃, and the growth temperature is at least 150℃ lower than that of conventional silicon chemical vapor deposition processes.

[0021] This invention integrates four steps—catalyst reduction, one-dimensional heterojunction growth, silicon-carbon filling, and thin carbon end-capping—into a single reactor. Continuous in-situ composite is achieved through sequential feeding, eliminating the traditional multi-step process of "preparing CNTs separately and then composited with silicon," significantly simplifying the process and reducing costs. The framework growth temperature of 450℃~650℃ and the filling temperature of 400℃~600℃ are significantly lower than the conventional silicon CVD temperature of 700℃~1100℃, a reduction of at least 150℃. This not only significantly saves energy but also avoids the problems of catalyst sintering and agglomeration and silicon-carbon precursor thermal decomposition and mismatch caused by high temperatures. Preferably, when the growth temperature is reduced by more than 200℃ compared to the conventional process, energy consumption is reduced by about one-third, catalyst activity retention is higher, and the uniformity and selectivity of the one-dimensional heterojunction are further improved.

[0022] Preferably, the preparation method includes the following steps: raw material pretreatment → catalyst loading → in-situ composite in four temperature zones → in-situ passivation and self-cleaning → post-treatment → characterization and electrode compatibility verification. In the aforementioned four-temperature-zone in-situ composite process, the function and conditions of each temperature zone are as follows: First temperature zone (reduction and activation): 250℃~450℃, hydrogen / argon atmosphere, reduction and activation of metal catalyst; Second temperature zone (skeleton growth): 450℃~650℃, alcohol carbon source atmosphere, to grow and form a one-dimensional heterojunction skeleton. Third temperature zone (confined filling): 400℃~600℃, organosilicon precursor atmosphere, deposition of silicon-carbon active components; Fourth temperature zone (passivation end cap): 300℃~500℃, trace olefin atmosphere, forming a thin carbon shell.

[0023] The four temperature zones respectively handle reduction, growth, filling, and passivation functions, integrating the operation of previously separate equipment into a single LPCVD unit. Temperature gradients and atmosphere switching are achieved through boat pushing or gas switching, ensuring continuous and controllable process flow. The first temperature zone's low-temperature reduction maintains the catalyst's nanoscale size; the second temperature zone's low-temperature growth of one-dimensional heterojunctions ensures high selectivity; the third temperature zone's low-temperature silicon-carbon filling prevents silicon grain coarsening at high temperatures; and the fourth temperature zone's low-temperature passivation forms a stable thin carbon shell. Each temperature zone is independently adjustable, facilitating optimization of the process window for different silicon and carbon sources, and demonstrating excellent prospects for industrial scale-up.

[0024] The catalyst is a Fe-Co-Mo multimetallic system supported on zeolite and / or alumina, with a molar ratio of Fe, Co, and Mo of 2.5:2.5:0.2~1.0 and a total metal loading of 1.0wt%~5.0wt% of the support mass. The surface of the support is coated with an alumina and / or magnesium oxide spacer layer with a thickness of 5nm~20nm, which is used to prevent the silicon source vapor from diffusing into the catalyst particles and causing catalyst silanization deactivation.

[0025] Preferably, the total system pressure is 0.1 kPa to 10 kPa and the total gas flow rate is 300 sccm to 1000 sccm; the second temperature zone and the third temperature zone are connected by continuous boat pushing or gas switching, so that the one-dimensional heterojunction growth and silicon-carbon deposition are coupled in situ in the same furnace.

[0026] The low-pressure environment increases the free path of gas molecules, which is beneficial for the uniform diffusion of reactant gases in the tube bundle gaps and on the catalyst surface, thereby improving the uniformity of one-dimensional heterojunction growth and the consistency of silicon filling. A pressure range of 0.1 kPa to 10 kPa and a total gas flow rate of 300 sccm to 1000 sccm allow for precise control of reactant residence time, suppressing gas-phase side reactions. Continuous boat pushing or gas switching enables seamless connection between the two temperature zones, avoiding the damage to catalyst activity and interface purity caused by intermediate air exposure, and ensuring the quality of in-situ coupling.

[0027] Preferably, in the passivation process, a small amount of water vapor is introduced to selectively vaporize and remove the amorphous carbon deposited on the outer wall of the single-walled carbon nanotubes and the surface of the catalyst particles at 300℃~500℃, thereby reducing the acid washing process in the post-treatment; the water vapor treatment time is 10min~15min to avoid excessive oxidation of the single-walled carbon nanotube walls.

[0028] Trace amounts of water vapor can selectively oxidize and remove amorphous carbon from the surface of one-dimensional heterojunctions at passivation temperatures, while simultaneously re-oxidizing deactivated metal catalyst particles into an active state, achieving online catalyst regeneration and extending single-batch operating time. More importantly, this self-cleaning process reduces the content of metal residues and amorphous carbon in the product, allowing for the reduction or even elimination of strong acid washing processes in the post-processing stage, significantly reducing waste acid emissions and environmental costs. The total metal impurity content of the self-cleaned material can be controlled below 200 ppm, meeting the requirements of high-end battery applications.

[0029] Preferably, the alcohol carbon source is ethanol and / or methanol, the organosilicon precursor is hexamethyldisiloxane and / or tetraethyl orthosilicate, and the thickness of the thin carbon shell is 2 nm to 10 nm.

[0030] Both ethanol and methanol are renewable carbon sources with good decomposition activity at low temperature and low pressure, which is beneficial for obtaining high-purity one-dimensional heterojunctions. Hexamethyldisiloxane and tetraethyl orthosilicate contain Si-O bonds in their molecules, which can be decomposed at low temperature to generate silicon-carbon active components, avoiding the use of high-cost and high-risk silane gases. The thickness of the thin carbon shell is controlled at 2nm~10nm, which can effectively isolate the electrolyte and stabilize the SEI film without reducing the specific capacity of the material due to excessive carbon layer thickness.

[0031] Compared with existing technologies, this invention has the following advantages: This invention creatively proposes an integrated solution of "low-temperature LPCVD time-sequential feeding + dual-scale confinement of silicon and carbon in the gaps between single-walled carbon nanotube bundles / on the surface of particles," achieving a high degree of synergy between material structure and preparation process. At the structural level, the confinement of the tube gaps inhibits silicon grain growth, while surface coating and Si-C interface bonding ensure long-term cycling stability. At the process level, the integrated in-situ composite process across four temperature zones significantly simplifies the process; the low-temperature window of 450℃~650℃ is at least 150℃ lower than the conventional silicon CVD window of 700℃~1100℃, resulting in significant energy savings and inhibiting catalyst sintering. The selective vaporization of amorphous carbon using trace amounts of water vapor reduces the acid washing process, thereby simultaneously reducing energy consumption, material consumption, and environmental costs. This solution combines excellent electrochemical performance, process scalability, and economic efficiency. Attached Figure Description

[0032] Figure 1 SEM image of the one-dimensional heterojunction silicon-carbon composite anode material (tube bundle network type) prepared in Example 1 of this invention.

[0033] Figure 2 SEM image of the one-dimensional heterojunction silicon-carbon composite anode material (cavity-filled type) prepared in Example 2 of this invention.

[0034] Figure 3 This is a SEM image of the one-dimensional heterojunction silicon-carbon composite anode material (surface co-growth type) prepared in Example 3 of the present invention.

[0035] Figure 4 The Raman spectrum of the one-dimensional heterojunction silicon-carbon composite anode material (tube bundle network type) prepared in Example 1 of this invention. Detailed Implementation

[0036] The present invention will now be described in detail through examples. Unless otherwise stated, all raw materials used are commercially available.

[0037] Example 1 The steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=80nm, BET specific surface area=30m²) 2 The ZSM-5 molecular sieve (SiO2 / Al2O3 molar ratio = 30, specific surface area 350 m²) was placed in a tube furnace and dried at 120℃ for 2 hours under argon protection for later use. 2 / g) Grind through a 200-mesh sieve, calcine in air at 500℃ for 2 hours to remove the template agent, and then let it cool naturally before use.

[0038] (2) Catalyst support: Fe-Co-Mo trimetallic catalyst was supported on a zeolite support using the equal-volume impregnation method. Fe(NO3)3·9H2O, Co(NO3)2·6H2O and (NH4)6Mo7O were weighed out in a molar ratio of Fe:Co:Mo=2.5:2.5:0.5. 24 • 4H2O was dissolved in deionized water, and pretreated ZSM-5 molecular sieve was added. After stirring evenly, the mixture was allowed to stand at room temperature for 12 hours, dried at 80°C for 6 hours, and then calcined in air at 450°C for 3 hours to obtain the catalyst precursor. The total metal loading was controlled to be 2.5 wt% of the support mass. Subsequently, the catalyst precursor was immersed in a 0.1 mol / L aluminum nitrate solution, and ammonia was slowly added dropwise until pH=8, so that Al(OH)3 precipitate coated the surface of the catalyst precursor. After filtration and washing, the precursor was dried at 80°C and then calcined in air at 400°C for 2 hours to form an Al2O3 spacer layer with a thickness of about 10 nm. This spacer layer is located between the support and the silicon active component and can effectively prevent the catalyst from undergoing silanization deactivation.

[0039] (3) Four-zone LPCVD in-situ composite: The zeolite support with the above-mentioned catalyst was mixed with spherical nano-silicon at a mass ratio of 1:10, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (200 sccm) was introduced to purge for 30 min. Then, each zone was run according to the following procedure: First temperature zone (reduction activation): The furnace temperature is raised to 350℃, hydrogen (200 sccm) and argon (200 sccm) are introduced, the total system pressure is controlled at 5 kPa, and the reduction activation is carried out for 1 hour to reduce Fe-Co-Mo oxide into alloy nanoparticles.

[0040] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 550℃, and the carbon source is switched to ethanol vapor. The ethanol is carried into the furnace by argon gas bubbling. The bubbling argon gas flow rate is 200 sccm, and 200 sccm of argon gas is added at the same time. The total system pressure is maintained at 5 kPa. The growth is carried out for 60 min, and a one-dimensional heterojunction three-dimensional conductive network is formed in situ on the catalyst surface. This network is uniformly coated on the surface of spherical nano-silicon particles and overlaps with each other to form a tube bundle network type confined structure.

[0041] Third temperature zone (silicon-carbon confined filling): The temperature is reduced to 500℃, and the gas source is switched to hexamethyldisiloxane vapor, which is carried by argon gas bubbling. The bubbling argon gas flow rate is 50 sccm, and 300 sccm of argon gas is added. The total system pressure is maintained at 5 kPa. Deposition is carried out for 30 minutes, so that the silicon-carbon active components fill the hollow cavity and tube bundle gap of the one-dimensional heterojunction, forming a dual-scale confined composite structure.

[0042] Fourth temperature zone (passivation and end-capping): The temperature is lowered to 400℃, and propylene (10 sccm) and argon (300 sccm) are introduced. The total system pressure is maintained at 5 kPa for 20 min, forming a thin carbon shell with a thickness of approximately 5 nm on the surface of the composite material. Subsequently, a trace amount of water vapor (0.5 sccm) and argon (200 sccm) are introduced at 400℃ for 10 min to selectively oxidize and remove amorphous carbon, while simultaneously achieving catalyst regeneration and self-cleaning.

[0043] The second to third temperature zones are seamlessly connected by continuous boat pushing and gas switching, enabling one-dimensional heterojunction growth and silicon-carbon deposition to be coupled in situ within the same furnace without air exposure, thus ensuring interface purity.

[0044] (4) Post-treatment: Stop heating and cool naturally to room temperature under argon protection. The obtained product is ultrasonically cleaned twice with deionized water and vacuum dried at 80℃ for 12h. Since the reaction system is a low-pressure gas phase deposition, the catalyst metal is loaded in the pores of the zeolite support in the form of nanoparticles. Most of it remains in the quartz boat residue with the support, and very little metal migrates out with the gas flow.

[0045] (5) Characterization and electrode compatibility verification: See Figure 1SEM characterization of the one-dimensional heterojunction silicon-carbon composite anode material prepared in this embodiment shows that the silicon-carbon active components are uniformly distributed in the gaps and surface of the one-dimensional heterojunction tube bundles, forming a dual-scale confined composite structure. Raman spectroscopy characterization of the one-dimensional heterojunction silicon-carbon composite anode material (tube network type) prepared in Example 1 of this invention yields the following results: Figure 4 As shown. By Figure 4 The spectrum shows the presence of radial breathing mode (RBM) peaks characteristic of single-walled carbon nanotubes, confirming that the conductive framework is composed of single-walled carbon nanotubes. Simultaneously, a distinct characteristic peak of crystalline silicon (520 cm⁻¹) was observed. -1 D peak (1350cm) -1 ) and the sharp G peak (1590cm) -1 The high intensity ratio of G peak to D peak (IG / ID) indicates that the material has good crystallinity and good composite properties between the silicon-carbon active component and the one-dimensional heterojunction conductive framework. Thermogravimetric analysis (TGA, air atmosphere) shows that the mass loss in the 400℃~700℃ range corresponds to the oxidation of the silicon-carbon active component. After normalization, the elemental silicon mass content is approximately 25.0%. The obtained composite negative electrode material was mixed with conductive carbon black and polyvinylidene fluoride at a mass ratio of 90:5:5, and a slurry was prepared using N-methylpyrrolidone as a solvent. The slurry was coated onto a copper foil current collector and dried under vacuum at 110℃ for 12 h. After cutting, CR2032 coin cells were assembled with lithium metal sheet as the counter electrode and the electrolyte being 1 mol / L LiPF6 / ethylene carbonate: diethyl carbonate = 1:1 (volume ratio), with 10% fluoroethylene carbonate added. Electrochemical tests showed that the initial coulombic efficiency at 0.1C was 86.2%, the reversible specific capacity was 1253 mAh / g, the capacity retention rate after 500 cycles at 0.5C was 81.5%, and the electrode full-charge expansion rate was about 17%, demonstrating excellent cycle stability and expansion suppression ability.

[0046] Example 2 This embodiment demonstrates a cavity-filling configuration, and the specific steps are as follows: (1) Raw material pretreatment: Spherical silicon nanoparticles (D50=30nm, BET specific surface area=60m² / g) were placed in a tube furnace and dried at 100℃ for 3h under argon protection for later use. γ-Al2O3 support (specific surface area 200m² / g) was then used. 2 The powder (g) is ground through a 300-mesh sieve, calcined at 600℃ in air for 1.5 hours, and then allowed to cool naturally before use.

[0047] (2) Catalyst loading: Fe-Co-Mo trimetallic catalyst was loaded onto a γ-Al2O3 support using an equal-volume impregnation method. The corresponding nitrate was weighed out at a molar ratio of Fe:Co:Mo = 2.5:2.5:0.2 (i.e., the Mo ratio was taken as the lower limit of 0.2), dissolved in deionized water, added to the pretreated γ-Al2O3 support, stirred evenly, and allowed to stand at room temperature for 10 h. It was then dried at 70 °C for 8 h and calcined in air at 400 °C for 4 h, with the total metal loading controlled at 1.0 wt% of the support mass. Subsequently, an oxide spacer layer with a thickness of approximately 5 nm was formed on the catalyst to prevent silanization deactivation of the catalyst with silicon. The lower Mo ratio and thinner spacer layer in this embodiment help reduce the catalyst particle size, which is beneficial for forming a small-diameter one-dimensional heterojunction.

[0048] (3) Four-zone LPCVD in-situ composite: The γ-Al2O3 support with catalyst was mixed with spherical nano-silicon at a mass ratio of 1:0.05 (i.e., 1 part silicon for every 20 parts support), placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (100 sccm) was then introduced to purge for 40 min. Subsequently, each zone was operated according to the following procedure: First temperature zone (reduction activation): The furnace temperature is raised to 250℃, and hydrogen (100 sccm) and argon (100 sccm) are introduced. The total system pressure is controlled at 0.1 kPa, and the reduction activation is carried out at this temperature for 1.5 h to reduce Fe-Co-Mo oxide into alloy nanoparticles. The lower total pressure increases the free path of gas molecules, which is beneficial for the uniform diffusion of reactant gases in the narrow cavity.

[0049] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 450℃, and the carbon source is switched to methanol vapor. Methanol is carried into the furnace by argon gas bubbling at a flow rate of 50 sccm. At the same time, 250 sccm of argon gas is added to make the total gas flow rate 300 sccm. The total system pressure is maintained at 0.1 kPa. After 90 min of growth, a one-dimensional heterojunction with an average tube diameter of about 1.0 nm and a single-wall selectivity of not less than 99.99% is formed in situ on the catalyst surface. This one-dimensional heterojunction forms a continuous three-dimensional conductive network, with adjacent tube bundles overlapping each other to provide sufficient cavity for subsequent cavity filling.

[0050] The third temperature zone (silicon-carbon confined filling): The temperature is lowered to 400℃, and the gas source is switched to tetraethyl orthosilicate (TEOS) vapor, carried by argon gas bubbling at a flow rate of 30 sccm, with an additional 270 sccm of argon gas added, maintaining a total gas flow rate of 300 sccm. The total system pressure is maintained at 0.1 kPa, and deposition is carried out for 60 minutes. This allows the silicon-carbon active component to fully fill the hollow cavity of the one-dimensional heterojunction, forming a cavity-filled composite structure. The mass content of the silicon-carbon active component is approximately 5%. The lower filling temperature avoids silicon grain coarsening, ensuring that silicon clusters are strictly confined within a sub-2 nm cavity.

[0051] Fourth temperature zone (passivation and end-capping): The temperature is lowered to 300℃, and acetylene (5 sccm) and argon (295 sccm) are introduced at a total gas flow rate of 300 sccm. The total system pressure is maintained at 0.1 kPa for 30 minutes, forming a thin carbon shell with a thickness of approximately 2 nm on the surface of the composite material. Subsequently, a trace amount of water vapor (0.3 sccm) and argon (300 sccm) are introduced at 300℃ for 15 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning, thereby reducing the acid washing process in post-treatment.

[0052] The second to third temperature zones are seamlessly connected by continuous boat pushing and gas switching, so that the growth of one-dimensional heterojunction and silicon-carbon deposition are coupled in situ in the same furnace without air exposure in between, ensuring the purity of the interface and forming Si-C interface bonding between the silicon-carbon active components and the one-dimensional heterojunction.

[0053] (4) Post-treatment: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product twice with deionized water using ultrasonication and dry it under vacuum at 70°C for 16 hours without strong acid washing. The total content of metal impurities in the obtained composite anode material was determined by inductively coupled plasma atomic emission spectrometry to be 120 ppm, which meets the low impurity requirement.

[0054] (5) Characterization and electrode compatibility verification: See Figure 2SEM characterization of the one-dimensional heterojunction silicon-carbon composite anode material prepared in this embodiment shows that the silicon-carbon active component fully fills the hollow cavity of the one-dimensional heterojunction, forming a cavity-filled composite structure. At the open end of the one-dimensional heterojunction, the silicon-carbon active component grows uniformly from the inside of the cavity outwards, effectively filling the cavity while maintaining the integrity of the outer wall. Adjacent tube bundles overlap to form a continuous three-dimensional conductive network, and silicon clusters are strictly confined within the sub-2 nm cavity, achieving one-dimensional cavity confinement of the silicon active component by single-walled carbon nanotubes. Raman spectroscopy (RBM peaks) shows that the average diameter of the one-dimensional heterojunction is approximately 1.0 nm, and the single-wall selectivity is statistically higher than 99.99%. Thermogravimetric analysis shows that the mass content of the silicon-carbon active component is approximately 5%. A coin cell was assembled using the same method as in Example 1, and electrochemical tests were performed. The results show that the initial efficiency at 0.1C is 89.5%, and the reversible specific capacity is 562 mAh / g. After 500 cycles at 0.5C, the capacity retention is 88.3%, and the electrode full-charge expansion rate is approximately 9%.

[0055] Example 3 This embodiment demonstrates a surface co-growth configuration, and the specific steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=150nm, BET specific surface area=15m²) 2 The ZSM-5 molecular sieve (SiO2 / Al2O3 molar ratio = 50, specific surface area 400 m²) was placed in a tube furnace and dried at 150 °C for 1.5 h under argon protection for later use. 2 The silicon nanoparticles (g) were ground through a 150-mesh sieve, calcined at 550°C in air for 3 hours, and then allowed to cool naturally before use. These large-particle-size spherical nano-silicon nanoparticles facilitate the surface co-growth of a silicon core, a one-dimensional heterojunction shell, and a pyrolytic carbon transition layer.

[0056] (2) Catalyst loading: Fe-Co-Mo trimetallic catalyst was loaded onto a zeolite support using an equal-volume impregnation method. The corresponding salts were weighed at a molar ratio of Fe:Co:Mo = 2.5:2.5:1.0, dissolved in deionized water, and pretreated ZSM-5 molecular sieve was added. After stirring evenly, the mixture was allowed to stand at room temperature for 16 h, dried at 90 °C for 5 h, and then calcined in air at 500 °C for 2 h, controlling the total metal loading to be 5.0 wt% of the support mass. Subsequently, the catalyst precursor was immersed in a 0.2 mol / L aluminum nitrate solution, and ammonia was added dropwise until pH = 7, causing Al(OH)3 precipitate to coat its surface. After filtration, washing, and drying, it was calcined in air at 450 °C for 3 h to form an Al2O3 spacer layer with a thickness of approximately 20 nm, preventing silanization deactivation of the catalyst with silicon. A higher Mo ratio helps improve the high-temperature stability of the catalyst, and a thicker spacer layer can inhibit silicon diffusion into the catalyst.

[0057] (3) Four-zone LPCVD in-situ composite: The zeolite support with catalyst was mixed with spherical nano-silicon at a mass ratio of 1:0.67, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (500 sccm) was then introduced to purge for 20 min. Subsequently, each zone was operated according to the following procedure: First temperature zone (reduction activation): The furnace temperature is raised to 450℃, and hydrogen (400 sccm) and argon (400 sccm) are introduced. The total system pressure is controlled at 10 kPa, and the reduction activation is carried out at this temperature for 0.5 h to reduce Fe-Co-Mo oxide into alloy nanoparticles. A higher total pressure is beneficial to improving the partial pressure and deposition rate of the silicon-carbon precursor.

[0058] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 650℃, and the carbon source is switched to a mixture of methanol and ethanol vapor (volume ratio 1:1), which is carried into the furnace by argon gas bubbling. The bubbling argon gas flow rate is 300 sccm, and 400 sccm of argon gas is added at the same time to make the total gas flow rate 1000 sccm. The total system pressure is maintained at 10 kPa. After 30 minutes of growth, a one-dimensional heterojunction shell with an average tube diameter of about 1.4 nm and a single-wall selectivity of not less than 99.99% is formed in situ on the surface of spherical nano-silicon. This shell forms a continuous three-dimensional conductive network and makes continuous contact with the surface of silicon components.

[0059] The third temperature zone (silicon-carbon confined filling): Maintaining 600℃, a mixture of hexamethyldisiloxane (HMDSO) and tetraethyl orthosilicate (TEOS) vapors (molar ratio 1:1) is simultaneously introduced into the furnace, carried by argon bubbling at a flow rate of 150 sccm, with an additional 350 sccm of argon added, maintaining a total gas flow rate of 1000 sccm. The total system pressure is maintained at 10 kPa. Deposition lasts for 15 minutes, during which silicon-carbon active components are simultaneously deposited inside the one-dimensional heterojunction shell, with in-situ pyrolyzed carbon serving as a transition layer. This forms a surface-co-grown composite structure with silicon as the core, a one-dimensional heterojunction as the shell, and pyrolyzed carbon as the transition layer, with an elemental silicon content of approximately 40%. The higher filling temperature and the dual silicon source synergistically enhance the loading of silicon-carbon active components.

[0060] Fourth temperature zone (passivation and end-capping): The temperature is lowered to 500℃, and propylene (50 sccm) and argon (500 sccm) are introduced, with a total gas flow rate of 1000 sccm and a total system pressure maintained at 10 kPa for 10 minutes, forming a thin carbon shell with a thickness of approximately 10 nm on the surface of the composite material. Subsequently, a trace amount of water vapor (2.0 sccm) and argon (500 sccm) are introduced at 500℃ for 5 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning, and reducing the acid washing process in post-treatment.

[0061] The second to third temperature zones are seamlessly connected by continuous boat pushing and gas switching, so that the growth of one-dimensional heterojunction and silicon-carbon deposition are coupled in situ in the same furnace without air exposure in between, ensuring the purity of the interface and forming a tight Si-C interface bond between the silicon-carbon active components and the one-dimensional heterojunction.

[0062] (4) Post-treatment: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product three times with deionized water using ultrasonication, and dry it under vacuum at 90℃ for 10 hours without strong acid washing. The total content of metal impurities in the obtained composite anode material was determined to be 95 ppm by inductively coupled plasma atomic emission spectrometry, which meets the low impurity requirement.

[0063] (5) Characterization and electrode compatibility verification: See Figure 3 The composite material obtained in this embodiment exhibits a typical core-shell structure: spherical nano-silicon as the core, in-situ pyrolytic carbon as the transition layer, and an outer layer of a three-dimensional conductive shell composed of a one-dimensional heterostructure. The silicon core surface is smooth and intact, and the carbon nanotubes in the shell continuously coat the pyrolytic carbon layer, forming a tight Si-C interface bond, which effectively suppresses the volume expansion of silicon and shortens the electron transport path. Raman spectroscopy (RBM peak) shows that the average diameter of the one-dimensional heterojunction is approximately 1.4 nm, and the single-wall selectivity is statistically higher than 99.99%. Thermogravimetric analysis shows that the mass content of silicon-carbon active components is approximately 40%. A coin cell was assembled using the same method as in Example 1, and electrochemical tests were performed. The results showed that the initial efficiency at 0.1C was 82.0%, and the reversible specific capacity was 1752 mAh / g; after 500 cycles at 0.5C, the capacity retention was 74.6%, and the electrode full-charge expansion rate was approximately 26%.

[0064] Example 4 This embodiment demonstrates a tube bundle network configuration, and the specific steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=100nm, BET specific surface area=40m2 / g) was placed in a tube furnace and dried at 130℃ for 2h under argon protection for later use. β-type zeolite (SiO2 / Al2O3 molar ratio=25, specific surface area 380m2 / g) was ground through a 200-mesh sieve, calcined in air at 480℃ for 2.5h, and then naturally cooled for later use.

[0065] (2) Catalyst loading: Fe-Co-Mo trimetallic catalyst was loaded onto a zeolite support using an equal-volume impregnation method. The corresponding salts were weighed in a molar ratio of Fe:Co:Mo = 2.5:2.5:0.6, dissolved in deionized water, and added to the pretreated zeolite. After stirring evenly, the mixture was allowed to stand at room temperature for 14 h, dried at 85 °C for 6 h, and then calcined in air at 480 °C for 3 h, controlling the total metal loading to be 3.5 wt% of the support mass. Subsequently, the catalyst precursor was immersed in a 0.15 mol / L mixed solution of aluminum nitrate and magnesium nitrate (molar ratio 1:1), and ammonia was added dropwise until pH = 8, allowing Al(OH)3 and Mg(OH)2 to co-precipitate and coat its surface. After filtration, washing, and drying, it was calcined in air at 420 °C for 2.5 h to form an Al2O3 / MgO composite spacer layer with a thickness of approximately 12 nm. This layer combines the barrier effect of Al2O3 and MgO on silicon diffusion, further preventing the catalyst from undergoing silanization deactivation.

[0066] (3) In-situ composite and online monitoring of four-zone LPCVD: The zeolite support with catalyst was mixed with spherical nano-silicon at a mass ratio of 1:15, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (300 sccm) was then introduced to purge for 30 min. Subsequently, each temperature zone was run according to the following procedure, and online monitoring was started simultaneously: First temperature zone (reduction and activation): The furnace temperature is raised to 380℃, hydrogen (300 sccm) and argon (300 sccm) are introduced, the total system pressure is controlled at 3 kPa, and the reduction and activation is carried out for 1 hour to reduce Fe-Co-Mo oxide into alloy nanoparticles.

[0067] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 580℃, and the carbon source is switched to ethanol vapor. Ethanol is carried into the furnace by argon gas bubbling at a flow rate of 150 sccm, while 450 sccm of argon gas is added simultaneously, bringing the total gas flow rate to 600 sccm. The total system pressure is maintained at 3 kPa, and growth is carried out for 75 minutes, forming a one-dimensional heterojunction three-dimensional conductive network in situ on the catalyst surface. During the growth process, an in-situ Raman acquisition optical path is set at the observation window of the furnace tube in the second temperature zone, and the RBM region (100 cm⁻¹ to 300 cm⁻¹) spectrum is acquired at 60-second intervals. The tube diameter corresponding to the maximum value of the RBM peak is used as the characterization value of the average tube diameter. At the same time, a residual gas analyzer (RGA) is used to monitor the signal intensity ratio of CH₄, CO, and H₂ in the outlet gas, indirectly reflecting the ethanol conversion rate. When the average pipe diameter of three consecutive samples deviates from the target value by more than ±0.1 nm (1.2 nm), the pipe diameter distribution is converged by manually adjusting the temperature of the second temperature zone (±10℃) and the ethanol / carrier gas flow rate ratio. After this adjustment, the relative standard deviation of pipe diameter between batches is less than ±5%.

[0068] The third temperature zone (silicon-carbon confined filling): The temperature is lowered to 480℃, and the gas source is switched to hexamethyldisiloxane vapor, carried by argon gas bubbling at a flow rate of 80 sccm. An additional 520 sccm of argon gas is added, maintaining a total gas flow rate of 600 sccm. The total system pressure is maintained at 3 kPa. Deposition lasts for 40 minutes, allowing the silicon-carbon active components to fill the hollow cavities and inter-tube gaps of the one-dimensional heterojunction, forming a dual-scale confined composite structure. The mass content of the silicon-carbon active components is approximately 30%. The second and third temperature zones are seamlessly connected through continuous boat pushing and gas switching, enabling in-situ coupling of one-dimensional heterojunction growth and silicon-carbon deposition within the same furnace.

[0069] Fourth temperature zone (passivation and end-capping): Cooling to 420℃, propylene (20 sccm) and argon (400 sccm) are introduced, with a total gas flow rate of 600 sccm and a total system pressure maintained at 3 kPa for 25 minutes, forming a thin carbon shell approximately 6 nm thick on the composite material surface. Subsequently, a trace amount of water vapor (1.0 sccm) and argon (400 sccm) are introduced at 420℃ for 12 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning, thereby reducing the acid washing process in post-processing. Because the framework growth temperature is 580℃ and the filling temperature is 480℃ (at least 150℃ lower than the 700~1100℃ of conventional silicon chemical vapor deposition processes), low-temperature energy saving is achieved, and the metal impurity content of the self-cleaned product is reduced, further reducing post-processing steps.

[0070] (4) Post-processing: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product twice with deionized water using ultrasonication and dry it under vacuum at 80°C for 12 hours without strong acid washing. The total content of metal impurities in the obtained composite anode material was determined by inductively coupled plasma atomic emission spectrometry to be 55 ppm, which is less than 200 ppm and meets the requirements of high-end battery applications.

[0071] (5) Characterization and electrode compatibility verification: Scanning electron microscopy shows that the one-dimensional heterojunction forms a continuous three-dimensional conductive network, with adjacent tube bundles overlapping each other. The spherical silicon nanoparticles are confined within the network units, and the aspect ratio of a single one-dimensional heterojunction is not less than 10. 3 Raman spectroscopy (RBM peaks) showed that the average diameter of the one-dimensional heterojunction was approximately 1.2 nm, the G / D ratio was approximately 20, and the single-wall selectivity was statistically higher than 99.99%. After online monitoring and adjustment, the batch-to-batch diameter fluctuation was less than ±5%. Thermogravimetric analysis showed that the silicon-carbon active component content was approximately 30%. Coin cells were assembled using the same method as in Example 1 and electrochemical tests were performed. The results showed that the initial efficiency at 0.1C was 85.7%, the reversible specific capacity was 1380±40 mAh / g, the capacity retention after 500 cycles at 0.5C was 83.1%, and the electrode full-charge expansion rate was approximately 15%.

[0072] Example 5 The specific steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=80nm, BET specific surface area=30m²) 2 The ZSM-5 molecular sieve (SiO2 / Al2O3 molar ratio = 30, specific surface area 350 m²) was placed in a tube furnace and dried at 120℃ for 2 hours under argon protection for later use. 2 The silicon nanoparticles (g) were ground through a 200-mesh sieve and calcined in air at 500°C for 2 hours to remove the template agent. After natural cooling, they were ready for use. The matching of particle size and specific surface area allows the spherical nano-silicon to shorten the lithium-ion diffusion path and avoid side reactions caused by excessive specific surface area, which is beneficial for forming continuous contact with one-dimensional heterojunctions.

[0073] (2) Catalyst loading: The Fe-Co-Mo trimetallic catalyst was loaded onto the ZSM-5 zeolite support using the equal-volume impregnation method, wherein the preferred molar ratio of Fe, Co, and Mo was 2.5:2.5:0.5, and the preferred total metal loading was 2.5 wt%. Specifically, Fe(NO3)3·9H2O, Co(NO3)2·6H2O, and (NH4)6Mo7O were weighed in a ratio of 2.5:2.5:0.5. 24 • 4H₂O was dissolved in deionized water, and pretreated ZSM-5 molecular sieve was added. After stirring evenly, the mixture was allowed to stand at room temperature for 12 hours, dried at 80°C for 6 hours, and then calcined in air at 450°C for 3 hours to obtain the catalyst precursor. Subsequently, it was immersed in a 0.1 mol / L aluminum nitrate solution, and ammonia was added dropwise until pH=8, causing Al(OH)₃ precipitate to coat its surface. After filtration, washing, and drying, it was calcined in air at 400°C for 2 hours to form an Al₂O₃ spacer layer with a thickness of approximately 10 nm. The preferred Fe:Co:Mo ratio of 2.5:2.5:0.5 can suppress catalyst particle agglomeration while ensuring single-wall selectivity. The combination of a preferred loading of 2.5 wt% and a preferred spacer layer thickness of 10 nm stabilizes the catalyst particle size at approximately 1.5 nm, which is beneficial for growing a one-dimensional heterojunction with an average diameter of 1.2 nm and effectively prevents silanization deactivation of the catalyst with silicon.

[0074] (3) Four-zone LPCVD in-situ composite: The catalyst-supported zeolite support and spherical nano-silicon were mixed uniformly at a mass ratio of 1:10, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (200 sccm) was then introduced to purge for 30 min. Subsequently, each zone was operated according to the following procedure: First temperature zone (reduction activation): The furnace temperature is raised to 350℃, hydrogen (200 sccm) and argon (200 sccm) are introduced, the total system pressure is controlled at 3 kPa, and the reduction activation is carried out for 1 hour to reduce Fe-Co-Mo oxide into alloy nanoparticles.

[0075] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 520℃, and the carbon source is switched to ethanol vapor. The ethanol is carried into the furnace by argon gas bubbling at a flow rate of 200 sccm, while 400 sccm of argon gas is added simultaneously, bringing the total gas flow rate to 600 sccm. The total system pressure is maintained at 3 kPa, and growth is carried out for 60 minutes, forming a one-dimensional heterojunction three-dimensional conductive network in situ on the catalyst surface. This growth temperature of 520℃ (approximately 230℃ lower than the 700℃~1100℃ of conventional silicon chemical vapor deposition processes) reduces energy consumption by about one-third compared to conventional processes, while also achieving higher catalyst activity retention and better tube diameter uniformity. The average tube diameter of the resulting one-dimensional heterojunction is approximately 1.2 nm, with a single-wall selectivity statistically exceeding 99.99% and an aspect ratio of not less than 10. 3 Adjacent tube bundles overlap to form a composite structure with dual-scale synergy between tube bundle gap confinement and particle surface coating.

[0076] Third temperature zone (silicon-carbon confined filling): The temperature is lowered to 460℃, and the gas source is switched to hexamethyldisiloxane (HMDSO) vapor, carried by argon bubbling at a flow rate of 60 sccm, with an additional 540 sccm of argon added, maintaining a total gas flow rate of 600 sccm. The total system pressure is maintained at 3 kPa, and deposition is carried out for 35 minutes. This allows the silicon-carbon active component to fill the hollow cavity and inter-tube gaps of the one-dimensional heterojunction, forming a tube-tube network composite structure. The mass content of the silicon-carbon active component is approximately 25%. This preferred 25% content achieves the best trade-off between specific capacity and first-time efficiency, and allows the silicon-carbon active component to form a Si-C interfacial bond with the one-dimensional heterojunction.

[0077] The fourth temperature zone (passivation and end-capping): The temperature is lowered to 380℃, and propylene (15 sccm) and argon (400 sccm) are introduced, with a total gas flow rate of 600 sccm. The total system pressure is maintained at 3 kPa for 20 minutes, forming a thin carbon shell approximately 5 nm thick on the composite material surface. Subsequently, a trace amount of water vapor (0.8 sccm) and argon (400 sccm) are introduced at 380℃ for 12 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning, thereby reducing the acid washing process in post-processing. Due to the framework growth temperature of 520℃ and the filling temperature of 460℃ (at least 150℃ lower than conventional processes), low-temperature energy saving is achieved, and the metal impurity content of the self-cleaned product is further reduced, controllable below 200 ppm. The second to third temperature zones are seamlessly connected through continuous boat pushing and gas switching, allowing one-dimensional heterojunction growth and silicon-carbon deposition to be coupled in situ within the same furnace, without air exposure in between, ensuring interface purity.

[0078] (4) Post-processing: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product twice with deionized water using ultrasonication and dry it under vacuum at 80°C for 12 hours without strong acid washing. The total content of metal impurities in the obtained composite anode material was determined by inductively coupled plasma atomic emission spectrometry to be 58 ppm, which is far below 200 ppm and meets the requirements of high-end battery applications.

[0079] (5) Characterization and electrode compatibility verification: Scanning electron microscopy showed that the one-dimensional heterojunction formed a continuous three-dimensional conductive network, with adjacent tube bundles overlapping each other. The spherical silicon nanoparticles were confined within the network units, and the aspect ratio of a single one-dimensional heterojunction was not less than 10. 3 The silicon component surface forms a continuous contact with the one-dimensional heterojunction; Raman spectroscopy (RBM peaks) shows that the average diameter of the one-dimensional heterojunction is approximately 1.2 nm, the G / D ratio is approximately 22, and the single-wall selectivity is statistically higher than 99.99%; thermogravimetric analysis shows that the mass content of the silicon-carbon active component is approximately 25%. A coin cell was assembled using the same method as in Example 1 and electrochemical tests were performed. The results showed that the initial efficiency at 0.1C was 87.5%, the reversible specific capacity was 1650 mAh / g; after 500 cycles at 0.5C, the capacity retention was 85.2%, and the electrode full-charge expansion rate was approximately 14%.

[0080] Example 6 The specific steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=100nm, BET specific surface area=40m²) 2 (g) was placed in a tube furnace and dried at 130℃ for 2 hours under argon protection, for later use. β-type zeolite (SiO2 / Al2O3 molar ratio = 25, specific surface area 380 m²) was then used. 2 The powder (g) is ground through a 200-mesh sieve, calcined at 480℃ in air for 2.5 hours, and then allowed to cool naturally before use.

[0081] (2) Catalyst loading: The corresponding salts were weighed with a molar ratio of Fe:Co:Mo = 2.5:2.5:0.5 and a total metal loading of 3.0 wt%, dissolved in deionized water, and pretreated β-type zeolite was added. After stirring evenly, the mixture was allowed to stand at room temperature for 14 h, dried at 85 °C for 6 h, and then calcined in air at 480 °C for 3 h to obtain the catalyst precursor. Subsequently, the catalyst precursor was immersed in a mixed solution of 0.15 mol / L aluminum nitrate and magnesium nitrate (molar ratio 1:1), and ammonia was added dropwise until pH = 8, so that Al(OH)3 and Mg(OH)2 co-precipitated and coated its surface. After filtration, washing, and drying, the mixture was calcined in air at 420 °C for 2.5 h to form an Al2O3 / MgO composite spacer layer with a thickness of about 12 nm. This composite spacer layer has both the dense barrier effect of Al2O3 and the inhibitory effect of MgO on silicon diffusion, which is more conducive to maintaining catalyst activity and preventing silanization deactivation than a single spacer layer.

[0082] (3) Four-zone LPCVD in-situ composite: The catalyst-supported zeolite support and spherical nano-silicon were mixed uniformly at a mass ratio of 1:15, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (300 sccm) was introduced to purge for 30 min. Then, each zone was operated according to the following procedure: First temperature zone (reduction and activation): The furnace temperature is raised to 380℃, hydrogen (300 sccm) and argon (300 sccm) are introduced, the total system pressure is controlled at 5 kPa, and the reduction and activation is carried out for 1 hour to reduce Fe-Co-Mo oxide into alloy nanoparticles.

[0083] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 540℃, and the carbon source is switched to a mixture of methanol and ethanol vapor (volume ratio 1:1), which is carried into the furnace by argon gas bubbling at a flow rate of 250 sccm. Simultaneously, 350 sccm of argon gas is added, bringing the total gas flow rate to 600 sccm. The total system pressure is maintained at 5 kPa, and growth is carried out for 70 minutes, forming a one-dimensional heterojunction three-dimensional conductive network in situ on the catalyst surface. This growth temperature of 540℃ is approximately 210℃ lower than that of conventional silicon chemical vapor deposition, exceeding the preferred value of 200℃. The resulting one-dimensional heterojunction has an average tube diameter of approximately 1.2 nm, a single-wall selectivity of not less than 99.99%, and an aspect ratio of not less than 10. 3 Adjacent tube bundles overlap to form a continuous conductive network. A preferred mixture of methanol and ethanol can regulate cracking activity while ensuring high purity, resulting in a more concentrated tube diameter distribution.

[0084] The third temperature zone (silicon-carbon confined filling): The temperature is lowered to 470℃, and the gas source is switched to a mixed vapor of HMDSO and TEOS (molar ratio 2:1), carried by argon gas bubbling at a flow rate of 100 sccm, with an additional 500 sccm of argon gas added, maintaining a total gas flow rate of 600 sccm. The total system pressure is maintained at 5 kPa. Deposition lasts for 40 minutes, allowing the silicon-carbon active components to fill the hollow cavities and inter-tube gaps of the one-dimensional heterojunction, forming a tube-bubble network composite structure. The mass content of the silicon-carbon active components is approximately 30%. The preferred dual silicon source of HMDSO and TEOS can achieve a higher silicon-carbon deposition rate and more uniform filling at a lower temperature, avoiding local enrichment. The second and third temperature zones are seamlessly connected through continuous boat pushing and gas switching, allowing one-dimensional heterojunction growth and silicon-carbon deposition to be coupled in situ within the same furnace, without air exposure in between.

[0085] Fourth temperature zone (passivation and end-capping): The temperature is lowered to 400℃, and propylene (20 sccm) and argon (400 sccm) are introduced, with a total gas flow rate of 600 sccm and a total system pressure maintained at 5 kPa for 22 minutes, forming a thin carbon shell with a thickness of approximately 6 nm on the surface of the composite material. Subsequently, a trace amount of water vapor (1.0 sccm) and argon (400 sccm) are introduced at 400℃ for 12 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning, and reducing the acid washing process in post-treatment.

[0086] (4) Post-treatment: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product twice with deionized water using ultrasonication, and then vacuum dry at 80℃ for 12 hours without strong acid washing. The total content of metal impurities in the obtained composite negative electrode material was determined by inductively coupled plasma atomic emission spectrometry to be 72 ppm, which meets the requirement of less than 200 ppm.

[0087] (5) Characterization and electrode compatibility verification: Scanning electron microscopy showed that the one-dimensional heterojunction formed a continuous three-dimensional conductive network, with adjacent tube bundles overlapping each other. Spherical silicon nanoparticles were confined within the network units, and the silicon component surface was coated with a one-dimensional heterojunction conductive framework, forming continuous contacts. Raman spectroscopy showed that the average diameter of the one-dimensional heterojunction was about 1.2 nm, the G / D ratio was about 21, and the single-wall selectivity was higher than 99.99%. Thermogravimetric analysis showed that the mass content of silicon-carbon active components was about 30%. Coin half-cells were assembled according to the same method as in Example 1 and electrochemical tests were performed. The results showed that the initial efficiency at 0.1C was 85.0%, the reversible specific capacity was 1800 mAh / g, the capacity retention rate after 500 cycles at 0.5C was 82.4%, and the electrode full-charge expansion rate was about 16%.

[0088] Example 7 The specific steps are as follows: (1) Raw material pretreatment: Spherical nano-silicon (D50=60nm, BET specific surface area=45m2 / g) was placed in a tube furnace and dried at 110℃ for 2.5h under argon protection for later use. ZSM-5 molecular sieve (SiO2 / Al2O3 molar ratio=40, specific surface area 360m2 / g) was ground through a 200-mesh sieve, calcined in air at 520℃ for 2h, and then naturally cooled for later use.

[0089] (2) Catalyst loading: Salts were weighed at a molar ratio of Fe:Co:Mo = 2.5:2.5:0.5 and a total metal loading of 2.5 wt%. These salts were dissolved in deionized water, and pretreated ZSM-5 molecular sieves were added. After stirring evenly, the mixture was allowed to stand at room temperature for 12 h, dried at 80 °C for 6 h, and then calcined in air at 460 °C for 3 h to obtain the catalyst precursor. Subsequently, the precursor was immersed in a 0.1 mol / L aluminum nitrate solution, and ammonia was added dropwise until pH = 8, forming an Al2O3 spacer layer approximately 10 nm thick to prevent silanization deactivation of the catalyst with silicon. This optimized catalyst system and spacer layer combination is beneficial for obtaining high single-wall selectivity and uniform tube diameter.

[0090] (3) In-situ composite and online monitoring of four-zone LPCVD: The zeolite support with catalyst was mixed with spherical nano-silicon at a mass ratio of 1:12, placed in a quartz boat, and pushed into a four-zone tubular low-pressure chemical vapor deposition furnace. The furnace door was closed, and the system was evacuated to a background pressure below 10 Pa. Argon gas (250 sccm) was then introduced for purging for 30 min. Subsequently, each temperature zone was run according to the following procedure, and online monitoring was started simultaneously: First temperature zone (reduction and activation): The furnace temperature is raised to 360℃, hydrogen (250 sccm) and argon (250 sccm) are introduced, the total system pressure is controlled at 4 kPa, and the reduction and activation is carried out for 1 hour to reduce Fe-Co-Mo oxide into alloy nanoparticles.

[0091] Second temperature zone (one-dimensional heterojunction framework growth): The temperature is raised to 530℃, and the carbon source is switched to ethanol vapor. The ethanol is carried into the furnace by argon gas bubbling at a flow rate of 200 sccm, while 400 sccm of argon gas is added simultaneously, bringing the total gas flow rate to 600 sccm. The total system pressure is maintained at 4 kPa, and growth is carried out for 65 minutes, forming a one-dimensional heterojunction three-dimensional conductive network in situ on the catalyst surface. The growth temperature of 530℃ stabilizes the average diameter of the resulting one-dimensional heterojunction at approximately 1.2 nm, and adjacent tube bundles overlap to form a dual-scale confined space.

[0092] The third temperature zone (silicon-carbon confined filling): The temperature is lowered to 450℃, and the gas source is switched to HMDSO vapor, carried by argon bubbling at a flow rate of 70 sccm. An additional 530 sccm of argon is added, maintaining a total gas flow rate of 600 sccm. The total system pressure is maintained at 4 kPa. Deposition lasts for 35 minutes, allowing the silicon-carbon active component to fill the hollow cavity and inter-tube gaps of the one-dimensional heterojunction, forming a tube-tube network composite structure. The mass content of the silicon-carbon active component is approximately 25%. The lower filling temperature avoids silicon grain coarsening and allows for optimal Si-C interfacial bonding between the silicon-carbon active component and the one-dimensional heterojunction. The second and third temperature zones are seamlessly connected through continuous boat pushing and gas switching, enabling in-situ coupling of one-dimensional heterojunction growth and silicon-carbon deposition within the same furnace.

[0093] Fourth temperature zone (passivation and end-capping): The temperature is lowered to 390℃, and propylene (18 sccm) and argon (400 sccm) are introduced, with a total gas flow rate of 600 sccm and a total system pressure maintained at 4 kPa for 20 minutes. This forms a thin carbon shell with a thickness of approximately 5 nm on the surface of the composite material. This optimal thickness effectively isolates the electrolyte and stabilizes the SEI film without reducing the specific capacity due to excessive carbon layer thickness. Subsequently, a trace amount of water vapor (0.9 sccm) and argon (400 sccm) are introduced at 390℃ for 12 minutes to selectively oxidize and remove amorphous carbon, achieving catalyst regeneration and self-cleaning. This reduces the need for acid washing in post-treatment, requiring only deionized water rinsing, significantly reducing waste acid emissions and environmental costs.

[0094] (4) Post-treatment: Stop heating and allow to cool naturally to room temperature under argon protection. Clean the obtained product twice with deionized water using ultrasonication and dry it under vacuum at 80°C for 12 hours without strong acid washing. The total content of metal impurities in the obtained composite anode material was determined by inductively coupled plasma atomic emission spectrometry to be 63 ppm, which is much lower than 200 ppm.

[0095] (5) Characterization and electrode compatibility verification: Scanning electron microscopy showed that the one-dimensional heterojunction formed a continuous three-dimensional conductive network, with adjacent tube bundles overlapping each other. The spherical silicon nanoparticles were confined within the network units, and the aspect ratio of a single one-dimensional heterojunction was not less than 10. 3 The silicon component surface is coated with a one-dimensional heterojunction conductive framework, forming continuous contacts. Raman spectroscopy (RBM peaks) shows that the average diameter of the one-dimensional heterojunction is approximately 1.2 nm, the G / D ratio is approximately 23, the single-wall selectivity is higher than 99.99%, and the batch-to-batch diameter fluctuation is less than ±5% after online Raman closure. Thermogravimetric analysis shows that the mass content of the silicon-carbon active component is approximately 25%. Coin cells were assembled using the same method as in Example 1 and electrochemical tests were performed. The results showed that the initial efficiency at 0.1C was 88.1%, the reversible specific capacity was 1600 mAh / g, the capacity retention after 500 cycles at 0.5C was 86.0%, and the electrode full-charge expansion rate was approximately 13%.

[0096] Comparative Example 1 Commercially available multi-walled carbon nanotubes (MWCNTs, diameter 10-20 nm, length 10-30 μm, purity ≥95%) were used to replace one-dimensional heterojunctions as the conductive framework. Spherical silicon nanotubes (D50=80 nm, BET=30 μm) were also used. 2MWCNTs (containing silicon nanoparticles) were dispersed in N-methylpyrrolidone at a mass ratio of 1:3, ultrasonically dispersed for 2 hours, and then spray-dried to obtain MWCNT / silicon composite particles, in which the silicon content was approximately 25% by mass. These composite particles were mixed with conductive carbon black and polyvinylidene fluoride at a mass ratio of 90:5:5 to form a slurry, which was then coated onto copper foil to assemble CR2032 coin cells. Scanning electron microscopy (SEM) observation showed that MWCNTs only wrapped around or adhered to the surface of the silicon particles and could not penetrate into the silicon particles to form a tubular confinement. The contact between silicon and carbon nanotubes was physical, without Si-C chemical bonding. Raman spectroscopy determined that the G / D ratio of MWCNTs was approximately 12. Electrochemical tests showed that the initial efficiency at 0.1C was 82.0%, and the reversible specific capacity was 1480 mAh / g; after 500 cycles at 0.5C, the capacity retention was only 58.0%, and the electrode full-charge expansion rate was approximately 32%. Since the diameter of MWCNT is much larger than 2nm, it is impossible to form a cavity constraint for silicon clusters at the sub-2nm scale. The volume expansion of silicon during cycling cannot be effectively suppressed, the conductive network gradually breaks, and the cycling stability is significantly worse than that of Embodiment 1 of the present invention.

[0097] Comparative Example 2 A silicon-carbon composite anode was prepared in a conventional two-step atmospheric-pressure high-temperature CVD process within the same reactor. Spherical silicon nanoparticles with a D50 of 80 nm were impregnated with ferric nitrate solution (Fe loading 2.5 wt%), dried, and placed in a tube furnace. Under argon protection, the temperature was raised to 800 °C, and ethylene (100 sccm) was introduced to grow carbon nanotubes for 60 min. Subsequently, hexamethyldisiloxane vapor was used to deposit the silicon-carbon active component at 700 °C for 30 min. Finally, propylene was introduced at 600 °C for passivation for 20 min. The entire growth process was carried out under atmospheric pressure, without using a low-pressure environment. The resulting product was acid-washed with concentrated nitric acid at 60 °C for 4 h to remove the metal catalyst before testing. Scanning electron microscopy and Raman spectroscopy showed that the carbon nanotube diameter distribution in the product was 2–5 nm, with a high content of multi-walled nanotubes and amorphous carbon, and a single-wall selectivity significantly lower than 99.99%, with a G / D ratio of approximately 8. Inductively coupled plasma atomic emission spectrometry (ICP-AES) determined the metal impurity content to be 280 ppm. Electrochemical tests showed that the initial efficiency at 0.1C was 76.5%, and the reversible specific capacity was 1300 mAh / g; after 300 cycles at 0.5C, the capacity retention was only 42.0%, and the electrode's full-charge expansion rate was approximately 40%. Due to the high growth temperature of 800℃ and the silicon deposition temperature of 700℃, the catalyst particles were severely sintered and agglomerated, and the silicon grains were significantly coarsened. Furthermore, the gas-phase reaction of the silicon-carbon precursor was uncontrollable at high temperatures, resulting in poor carbon nanotube selectivity, high interfacial impedance, and a significant deterioration in electrochemical performance, with energy consumption also significantly higher than that of this invention.

[0098] Comparative Example 3 The preparation method is basically the same as in Example 1, except that after passivation and end-capping in the fourth temperature zone, water vapor self-cleaning is not performed. Instead, the cooled product is directly placed in 65wt% concentrated nitric acid and acid-washed at 60°C for 4 hours to remove the metal catalyst. Then, it is washed with deionized water until neutral and vacuum-dried at 80°C for 12 hours. In the obtained composite anode material, the total content of metal impurities measured by inductively coupled plasma atomic emission spectrometry is 180ppm, which is lower than 200ppm. However, Raman spectroscopy shows that the G / D ratio has decreased from 18 in Example 1 to about 9, indicating that strong acid washing has caused significant damage to the one-dimensional heterojunction structure, introduced a large number of structural defects, and destroyed the complete sp. 2 Carbon conjugated network. Electrochemical tests showed that the initial efficiency at 0.1C was 83.1%, and the reversible specific capacity was 1520 mAh / g; after 500 cycles at 0.5C, the capacity retention was 72.0%, and the electrode full-charge expansion rate was approximately 23%, all significantly lower than in Example 1. Furthermore, the acid washing process generates a large amount of waste acid containing metal ions, requiring specialized treatment, which significantly increases environmental costs and process complexity. This invention, however, uses steam self-cleaning to simultaneously remove amorphous carbon and regenerate the catalyst during the passivation stage, eliminating the need for strong acid washing in post-treatment. This protects the one-dimensional heterojunction structure and reduces costs and environmental burden.

Claims

1. A one-dimensional heterojunction silicon-carbon composite anode material, characterized in that, The material comprises a silicon-carbon active component and a one-dimensional heterojunction conductive framework. The one-dimensional heterojunction is a carbon-based one-dimensional heterojunction, the main body of which is a bundle of single-walled carbon nanotubes. The silicon-carbon active component at least partially fills the interstices of the tube bundles in the one-dimensional heterojunction and / or is coated on its surface by the one-dimensional heterojunction, forming a composite structure with synergistic tube confinement and surface coating. The average diameter of the single-walled carbon nanotubes in the one-dimensional heterojunction is 1.0 nm to 1.4 nm, and the content of the single-walled carbon nanotubes is not less than 99.99%. The silicon-carbon active component contains 5% to 40% elemental silicon based on the total mass of the composite material.

2. The one-dimensional heterojunction silicon-carbon composite anode material according to claim 1, characterized in that, The silicon-carbon active component includes at least one of nano-silicon, amorphous carbon, and in-situ pyrolysis carbon, and a Si–C interface bond is formed between the silicon-carbon active component and the one-dimensional heterojunction.

3. The one-dimensional heterojunction silicon-carbon composite anode material according to claim 1, characterized in that, The configuration of the composite structure is one of the following: (1) The silicon-carbon active component is coated in a one-dimensional heterojunction tube network gap; (2) The silicon-carbon active component is filled into the hollow cavity of a one-dimensional heterojunction, forming a cavity-filling type. (3) Surface co-growth type with silicon as the core, one-dimensional heterojunction as the shell and cracked carbon as the transition layer.

4. The one-dimensional heterojunction silicon-carbon composite anode material according to claim 1, characterized in that, The silicon component in the silicon-carbon active component consists of spherical nano-silicon particles with a D50 particle size of 30nm~150nm and a specific surface area of ​​15m². 2 / g~60m 2 / g; The surface of the silicon component is coated with the one-dimensional heterojunction conductive framework, and the one-dimensional heterojunction and the surface of the silicon component form a continuous contact.

5. A method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to any one of claims 1 to 4, characterized in that, The process employs a low-temperature, low-pressure chemical vapor deposition (CVD) process, which sequentially completes the following steps within the same reactor using a time-sequential feeding method: catalyst reduction and activation → one-dimensional heterojunction framework growth → confined filling of silicon-carbon active components → thin carbon end-capping and passivation. The one-dimensional heterojunction framework growth temperature is 450℃~650℃, and the confined filling temperature of the silicon-carbon active components is 400℃~600℃.

6. The method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to claim 5, characterized in that, The preparation method includes the following steps: raw material pretreatment → catalyst loading → four-temperature zone in-situ composite → in-situ passivation and self-cleaning → post-treatment → characterization and electrode compatibility verification; in the four-temperature zone in-situ composite, the function and conditions of each temperature zone are as follows: First temperature zone: 250℃~450℃, hydrogen / argon atmosphere, reduction and activation of metal catalyst; Second temperature zone: 450℃~650℃, alcohol-based carbon source atmosphere, growth to form a one-dimensional heterostructure framework; Third temperature zone: 400℃~600℃, organosilicon precursor atmosphere, deposition of silicon-carbon active components; Fourth temperature zone: 300℃~500℃, trace olefin atmosphere, forming a thin carbon shell.

7. The method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to claim 6, characterized in that, The catalyst is a Fe-Co-Mo multimetallic system supported on zeolite and / or alumina, with a molar ratio of Fe, Co, and Mo of 2.5:2.5:0.2~1.0 and a total metal loading of 1.0wt%~5.0wt% of the support mass; the surface of the support is coated with an alumina and / or magnesium oxide spacer layer with a thickness of 5nm~20nm.

8. The method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to claim 6, characterized in that, The total system pressure is 0.1 kPa to 10 kPa, and the total gas flow rate is 300 sccm to 1000 sccm. The second temperature zone and the third temperature zone are connected by continuous boat pushing or gas switching, so that one-dimensional heterojunction growth and silicon-carbon deposition are coupled in situ in the same furnace.

9. The method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to claim 6, characterized in that, In the in-situ passivation, a small amount of water vapor is introduced to selectively vaporize and remove amorphous carbon deposited on the outer wall of single-walled carbon nanotubes and the surface of catalyst particles at 300℃~500℃; the water vapor treatment time is 10min~15min.

10. The method for preparing a one-dimensional heterojunction silicon-carbon composite anode material according to claim 6, characterized in that, The alcohol carbon source is ethanol and / or methanol, the organosilicon precursor is hexamethyldisiloxane and / or tetraethyl orthosilicate, and the thickness of the thin carbon shell is 2 nm to 10 nm.