A niobium-titanium dual-doped ternary precursor and its preparation method, cathode material and UPS battery

By using a method for preparing niobium-titanium doped ternary precursors, the problems of rapid capacity decay and short cycle life of existing ternary precursors under high-rate discharge were solved, and a positive electrode material with high-rate discharge capability, long cycle life and wide temperature adaptability was prepared to meet the requirements of AI server UPS power supplies.

CN123120712APending Publication Date: 2026-11-17JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611401452.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ternary precursors exhibit rapid capacity decay and insufficient cycle life under high-rate discharge, making it difficult to meet the stringent requirements of AI server UPS power supplies.

Method used

By employing a method for preparing niobium-titanium dual-doped ternary precursors, and by changing the types of doping elements and the co-precipitation feeding method, highly controllable and uniform niobium-titanium dual-doped ternary precursors with uniform particle size distribution and high tap density are prepared. The resulting cathode material can meet the requirements of millisecond-level response, high power density, and long cycle life.

Benefits of technology

The niobium-titanium double-doped ternary precursor achieved a capacity retention rate of ≥88.8% under high-rate discharge, ≥85.8% after 1000 1C charge-discharge cycles, ≥85.2% at -20℃, and ≥85.1% after 500 cycles at 60℃, meeting the stringent requirements of AI server UPS power supplies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application provides a niobium-titanium dual-doped ternary precursor, its preparation method, a cathode material, and a UPS battery. The preparation method of the niobium-titanium dual-doped ternary precursor includes the following steps: mixing a nickel-cobalt-manganese ternary mixed metal salt solution, niobium pentoxide, and titanium dioxide, and ultrasonically dispersing them to obtain a dispersion; simultaneously adding the dispersion, a precipitant solution, and a complexing agent solution to a base solution, and obtaining the niobium-titanium dual-doped ternary precursor through a co-precipitation reaction. By changing the type of doping element raw material and the feeding method of co-precipitation, this application can prepare a niobium-titanium dual-doped ternary precursor with highly controllable and uniform doping. The niobium-titanium dual-doped ternary precursor has a uniform particle size distribution and high tap density. The resulting cathode material can meet the stringent requirements of millisecond-level response, high power density, long cycle life, and wide-temperature operation, solving the technical pain points of existing UPS batteries such as rapid capacity decay and short cycle life under high-rate discharge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of battery materials technology, and relates to a niobium-titanium dual-doped ternary precursor and its preparation method, cathode material and UPS battery. Background Technology

[0002] With the rapid development of artificial intelligence technology, the computing power demand of AI server clusters is growing exponentially, placing extremely high demands on the reliability and stability of power supply. As a critical infrastructure of AI data centers, UPS (Uninterruptible Power Supply) needs to achieve seamless switching within milliseconds (<4ms) in the event of mains power failure, providing continuous and stable power support for AI servers and avoiding computing power loss and data loss due to power outages.

[0003] Traditional UPS power supplies mostly use lead-acid batteries as energy storage units. However, lead-acid batteries have disadvantages such as low energy density, short cycle life (about 500 times), slow charging speed, large size, and heavy weight, making it difficult to meet the needs of high-density deployment and long-term operation of AI servers. Lithium-ion batteries, with their advantages of high energy density, long cycle life (>2000 times), fast charging, and lightweight design, are gradually becoming the mainstream choice for UPS power supplies.

[0004] In lithium-ion battery cathode materials, ternary materials (Ni-Co-Mn-O) are widely used in UPS power supplies due to their high energy density and good rate performance. Ternary precursors, as key precursors for ternary cathode materials, directly affect the electrochemical performance of the final cathode material due to their structure, morphology, and elemental composition. AI server UPS power supplies have the following special requirements, placing higher demands on ternary precursors: 1. High-rate discharge capability: AI servers generate sharp short-term power spikes during training and inference, with peak currents reaching 10 to 20 times the rated current, requiring the battery to quickly release large currents without voltage collapse; 2. Long cycle life: UPS power supplies need to operate in a float charge state for extended periods, occasionally undergoing deep discharge, requiring the battery to have excellent cycle stability under both high-rate cycling and float charge conditions; 3. Wide operating temperature range: AI data center environments experience large temperature fluctuations, requiring the battery to operate stably within a range of -20℃ to 60℃; 4. High safety: UPS power supplies are typically deployed in enclosed spaces, requiring the battery to have excellent thermal stability and safety.

[0005] Existing ternary precursors exhibit rapid capacity decay and insufficient cycle life under high-rate discharge, making it difficult to meet the stringent requirements of AI server UPS power supplies. Therefore, developing a ternary precursor with high-rate discharge capability, long cycle life, and wide temperature adaptability is of great significance for improving the performance of AI server UPS power supplies. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this application aims to provide a niobium-titanium dual-doped ternary precursor, its preparation method, cathode material, and UPS battery. By changing the type of doping element raw material and the feeding method of co-precipitation, this application can prepare a niobium-titanium dual-doped ternary precursor with highly controllable and uniform doping. The niobium-titanium dual-doped ternary precursor has a uniform particle size distribution and high tap density. The cathode material prepared can meet the stringent requirements of millisecond-level response, high power density, long cycle life, and wide-temperature operation, solving the technical pain points of existing UPS batteries such as rapid capacity decay and short cycle life under high-rate discharge.

[0007] To achieve the purpose of this application, the following technical solution is adopted: In a first aspect, this application provides a method for preparing a niobium-titanium dual-doped ternary precursor, the method comprising the following steps: A nickel-cobalt-manganese ternary mixed metal salt solution, niobium pentoxide and titanium dioxide were mixed and ultrasonically dispersed to obtain a dispersion. The dispersion, precipitant solution, and complexing agent solution were simultaneously added dropwise to the base liquid, and a co-precipitation reaction was carried out to obtain a niobium-titanium dual-doped ternary precursor.

[0008] In some possible implementations, the total molar concentration of various metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution is 1.5 mol / L to 2 mol / L.

[0009] In some possible implementations, the amount of niobium pentoxide added is 0.1% to 0.5%, based on the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%.

[0010] In some possible implementations, the amount of titanium dioxide added is 0.05% to 0.2%, based on the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%.

[0011] In some possible implementations, the ultrasonic dispersion time is 40 min to 60 min.

[0012] In some possible implementations, the precipitant solution comprises a sodium hydroxide solution.

[0013] In some possible implementations, the molar concentration of the precipitant solution is 4 mol / L to 6 mol / L.

[0014] In some possible implementations, the complexing agent solution comprises ammonia.

[0015] In some possible implementations, the molar concentration of the complexing agent solution is 2 mol / L to 3 mol / L.

[0016] In some possible implementations, the dropping rate of the dispersion is 0.5 L / h to 1 L / h.

[0017] In some possible implementations, the temperature of the coprecipitation reaction is 50°C to 60°C.

[0018] In some possible implementations, the pH of the coprecipitation reaction is 11 to 11.5.

[0019] In some possible implementations, stirring is performed during the coprecipitation reaction.

[0020] In some possible implementations, the stirring speed is 600 rpm to 700 rpm.

[0021] Secondly, this application provides a niobium-titanium dual-doped ternary precursor, which is prepared by the preparation method described in the first aspect.

[0022] In some possible implementations, the SPAN of the niobium-titanium dual-doped ternary precursor is <0.5.

[0023] In some possible implementations, the crystal plane intensity ratio of the niobium-titanium dual-doped ternary precursor is 0.5 to 1.3.

[0024] In some possible implementations, the tap density of the niobium-titanium dual-doped ternary precursor is 1.8 g / cm³. 3 ~2.1g / cm 3 .

[0025] In some possible implementations, the specific surface area of ​​the niobium-titanium dual-doped ternary precursor is 12 m². 2 / g~18m 2 / g.

[0026] In some possible implementations, the median particle size D50 of the niobium-titanium dual-doped ternary precursor is 8 μm to 15 μm.

[0027] Thirdly, this application provides a cathode material, which is prepared by mixing and sintering a niobium-titanium doped ternary precursor as described in the second aspect with a lithium source.

[0028] In some possible implementations, the lithium source includes lithium hydroxide and / or lithium carbonate.

[0029] In some possible implementations, the sintering temperature is 750°C to 800°C.

[0030] In some possible implementations, the sintering time is 5h to 15h.

[0031] Fourthly, this application provides a UPS battery comprising the positive electrode material as described in the third aspect.

[0032] Compared with the prior art, this application has the following advantages: (1) The method for preparing niobium-titanium dual-doped ternary precursor provided in this application can prepare niobium-titanium dual-doped ternary precursor with highly controllable doping amount and uniform doping by changing the type of raw material of doping element and the feeding method of co-precipitation. The niobium-titanium dual-doped ternary precursor has a uniform particle size distribution and high tap density. The obtained cathode material can meet the stringent requirements of millisecond-level response, high power density, long cycle life and wide temperature operation, and solves the technical pain points of existing UPS batteries with fast capacity decay and short cycle life under high rate discharge.

[0033] (2) The niobium-titanium dual-doped ternary precursor prepared by the method provided in this application can produce a battery with a capacity of more than 233 mAh / g, a capacity retention rate of more than 88.8% under 20C discharge rate, a capacity retention rate of more than 85.8% after 1000 1C charge-discharge cycles, a capacity retention rate of more than 85.2% at -20℃, and a capacity retention rate of more than 85.1% after 500 cycles at 60℃. Detailed Implementation

[0034] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0035] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0036] In this application, "at least two combinations" refers to a quantity greater than or equal to 2 unless otherwise specified. For example, "any one or at least two combinations" means any one of the listed items, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this application. In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or simultaneously containing both A and B. In this application, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.

[0037] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" as used in this application means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this application can be combined with other embodiments that do not conflict with existing technologies. The ordinal numbers "first," "second," "third," and "fourth," etc., used in this application in the expressions "first aspect," "second aspect," "third aspect," and "fourth aspect," are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly specifying the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.

[0038] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict order of execution. The actual order of execution of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order in which they are written or in any order without technical conflict.

[0039] In a first aspect, this application provides a method for preparing a niobium-titanium dual-doped ternary precursor, the method comprising the following steps: A nickel-cobalt-manganese ternary mixed metal salt solution, niobium pentoxide and titanium dioxide were mixed and ultrasonically dispersed to obtain a dispersion. The dispersion, precipitant solution, and complexing agent solution were simultaneously added dropwise to the base liquid, and a co-precipitation reaction was carried out to obtain a niobium-titanium dual-doped ternary precursor.

[0040] This application uses niobium pentoxide and titanium dioxide as the niobium and titanium doping sources, respectively. These are dispersed into nanoscale particles by ultrasonication in a mixed metal salt solution, ensuring uniform dispersion in the dispersion liquid. The doping amount is precisely controlled, and the stable oxide state does not affect the pH and other conditions of the subsequent co-precipitation reaction, thus avoiding dopant segregation. The co-precipitation reaction is then carried out by titration. During the co-precipitation process, the nickel-cobalt-manganese ternary precursor undergoes in-situ nucleation and growth, and the nano-Nb₂O₅ / TiO₂ microcrystals are encapsulated within the primary grains, forming a bulk homogeneous dual-doped structure without surface enrichment or dopant segregation defects. The sphericity and compaction density of the resulting precursor are significantly improved.

[0041] The method described in this application enables niobium pentoxide and titanium dioxide to be uniformly doped in the cathode precursor. During the subsequent sintering process of preparing the cathode material, Nb and Ti can diffuse uniformly into the interior of the layered oxide lattice to form a stable bulk phase doping. Niobium can suppress Li / Ni mixing and improve the stability of the crystal structure; titanium can enhance the electronic conductivity and ionic conductivity of the material and improve the rate performance.

[0042] In some embodiments, the total molar concentration of various metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution is 1.5 mol / L to 2 mol / L, for example: 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2 mol / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0043] In some embodiments, with the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%, the amount of niobium pentoxide added is 0.1% to 0.5%, for example: 0.1%, 0.2%, 0.3%, 0.4% or 0.5%, etc., not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0044] In some embodiments, with the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%, the amount of titanium dioxide added is 0.05% to 0.2%, for example: 0.05%, 0.08%, 0.1%, 0.15% or 0.2%, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0045] In some embodiments, the ultrasonic dispersion time is 40 min to 60 min, for example: 40 min, 45 min, 50 min, 55 min or 60 min, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0046] In some embodiments, the precipitant solution comprises a sodium hydroxide solution.

[0047] In some embodiments, the molar concentration of the precipitant solution is 4 mol / L to 6 mol / L, for example: 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L or 6 mol / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0048] In some embodiments, the complexing agent solution comprises ammonia.

[0049] In some embodiments, the molar concentration of the complexing agent solution is 2 mol / L to 3 mol / L, for example: 2 mol / L, 2.2 mol / L, 2.5 mol / L, 2.8 mol / L or 3 mol / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0050] In some embodiments, the dropping rate of the dispersion is 0.5 L / h to 1 L / h, for example: 0.5 L / h, 0.6 L / h, 0.8 L / h, 0.9 L / h or 1 L / h, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0051] In some embodiments, the temperature of the coprecipitation reaction is 50°C to 60°C, for example: 50°C, 52°C, 55°C, 58°C or 60°C, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0052] In some embodiments, the pH of the coprecipitation reaction is 11 to 11.5, for example: 11, 11.1, 11.2, 11.3, 11.4 or 11.5, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0053] In some embodiments, stirring is performed during the coprecipitation reaction.

[0054] In some embodiments, the stirring speed is 600 rpm to 700 rpm, for example: 600 rpm, 620 rpm, 650 rpm, 680 rpm or 700 rpm, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0055] Secondly, this application provides a niobium-titanium dual-doped ternary precursor, which is prepared by the preparation method described in the first aspect.

[0056] The method described in this application produces a niobium-titanium dual-doped ternary precursor with uniform particle size distribution and high tap density. The doping amount of the doping element in the niobium-titanium dual-doped ternary precursor is highly controllable. The niobium-titanium dual-doped ternary precursor, when used as a cathode material, exhibits an α-Ni(OH)2 type hexagonal crystal structure and a high (001) / (101) diffraction peak intensity ratio, which can provide a good lithium-ion diffusion channel.

[0057] In some embodiments, the SPAN of the niobium-titanium dual-doped ternary precursor is less than 0.5, where SPAN is the particle size distribution span, and SPAN = (D90 - D10) / D50.

[0058] In some embodiments, the crystal plane intensity ratio of the niobium-titanium dual-doped ternary precursor is 0.5 to 1.3, for example: 0.5, 0.8, 1, 1.25 or 1.3, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0059] In some embodiments, the tap density of the niobium-titanium dual-doped ternary precursor is 1.8 g / cm³. 3 ~2.1g / cm 3 For example: 1.8g / cm 3 1.85g / cm 3 1.9g / cm 3 2g / cm 3 Or 2.1g / cm 3 The term "etc." is not limited to the listed values; it also applies to other unlisted values ​​within the range.

[0060] In some embodiments, the specific surface area of ​​the niobium-titanium dual-doped ternary precursor is 12 m². 2 / g~18m 2 / g, for example: 12m 2 / g、13m 2 / g, 15m 2 / g, 16m 2 / g or 18m 2 / g, etc., are not limited to the listed values; other unlisted values ​​within this range also apply.

[0061] In some embodiments, the median particle size D50 of the niobium-titanium dual-doped ternary precursor is 8 μm to 15 μm, for example: 8 μm, 9 μm, 10 μm, 12 μm or 15 μm, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0062] Thirdly, this application provides a cathode material, which is prepared by mixing and sintering a niobium-titanium doped ternary precursor as described in the second aspect with a lithium source.

[0063] The cathode material prepared using the niobium-titanium dual-doped ternary precursor by the method described in this application exhibits a capacity retention of ≥85% under 20C high-rate discharge and ≥90% after 1000 cycles, with stable performance over a wide temperature range of -20℃ to 60℃. This ternary cathode material is particularly suitable for AI server UPS power supplies, meeting their stringent requirements for millisecond-level response, high power density, long cycle life, and wide-temperature operation. It solves the technical pain points of existing UPS power supply lithium batteries, such as rapid capacity decay and short cycle life under high-rate discharge.

[0064] In some embodiments, the lithium source includes lithium hydroxide and / or lithium carbonate.

[0065] In some embodiments, the sintering temperature is 750°C to 800°C, for example: 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0066] In some embodiments, the sintering time is 5h to 15h, for example: 5h, 8h, 10h, 12h or 15h, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0067] Fourthly, this application provides a UPS battery comprising the positive electrode material as described in the third aspect.

[0068] The UPS battery described in this application is a lithium-ion battery used in UPS power systems, mainly for AI servers. The UPS power system for AI servers includes a 48V / 100Ah battery pack made of UPS batteries, a KSTAR 125kW UPS main unit, an intelligent BMS system, and a liquid cooling device.

[0069] Example 1 This embodiment provides a niobium-titanium dual-doped ternary precursor, which is prepared by the following method: NiSO4, CoSO4, and MnSO4 were dissolved in deionized water at a molar ratio of 85:10:5 to prepare a 1.8 mol / L nickel-cobalt-manganese ternary mixed metal salt solution. Nb2O5 and TiO2 powders (in Ni...) were then added to the nickel-cobalt-manganese ternary mixed metal salt solution. 2+ Co 2+ and Mn 2+ The total molar amount is 100%, the molar amount of Nb2O5 is 0.3%, and the molar amount of TiO2 is 0.1%. The dispersion is obtained by ultrasonic dispersion for 45 min. Under a nitrogen atmosphere, a dispersion, a 5 mol / L sodium hydroxide solution, and a 2.5 mol / L ammonia solution were simultaneously added dropwise to a base solution (a mixed solution of ammonia and sodium hydroxide, pH 11.2). The dropwise addition rate of the dispersion was 0.8 L / h, the temperature was controlled at 55 °C, and the pH was 11.2. The co-precipitation reaction was carried out at a stirring speed of 650 rpm for 15 h. After the reaction was completed, the mixture was filtered and washed to obtain a solid with a pH of 7.2. The solid was then dried at 90 °C for 18 h to obtain a niobium-titanium dual-doped ternary precursor. The niobium-titanium dual-doped ternary precursor has a median particle size D50 of 10 μm, a SPAN of 0.42, and a specific surface area of ​​15 m². 2 / g, tap density 1.85g / cm³ 3 The intensity ratio of the (001) / (101) diffraction peaks (i.e., the crystal plane intensity ratio) in the XRD pattern is 1.25.

[0070] Example 2 This embodiment provides a niobium-titanium dual-doped ternary precursor, which is prepared by the following method: NiSO4, CoSO4, and MnSO4 were dissolved in deionized water at a molar ratio of 85:10:5 to prepare a 2 mol / L nickel-cobalt-manganese ternary mixed metal salt solution. Nb2O5 and TiO2 powders (in Ni...) were then added to the nickel-cobalt-manganese ternary mixed metal salt solution. 2 + Co 2+ and Mn 2+ The total molar amount is 100%, the molar amount of Nb2O5 is 0.1%, and the molar amount of TiO2 is 0.05%. The dispersion is obtained by ultrasonic dispersion for 40 min. Under a nitrogen atmosphere, a dispersion, a 6 mol / L sodium hydroxide solution, and a 3 mol / L ammonia solution were simultaneously added dropwise to a base solution (a mixed solution of ammonia and sodium hydroxide, pH 11.5). The dropwise addition rate of the dispersion was 1 L / h, the temperature was controlled at 60 °C, and the pH was 11.5. The co-precipitation reaction was carried out at a stirring speed of 700 rpm for 10 h. After the reaction was completed, the mixture was filtered and washed to obtain a solid with a pH of 7.2. The solid was then dried at 90 °C for 18 h to obtain a niobium-titanium dual-doped ternary precursor. The niobium-titanium dual-doped ternary precursor has a median particle size (D50) of 13 μm, a span of 0.45, and a specific surface area of ​​12 m². 2 / g, tap density 2.05g / cm³ 3 The intensity ratio of the (001) / (101) diffraction peaks (i.e., the crystal plane intensity ratio) in the XRD pattern is 0.55.

[0071] Example 3 This embodiment provides a niobium-titanium dual-doped ternary precursor, which is prepared by the following method: NiSO4, CoSO4, and MnSO4 were dissolved in deionized water at a molar ratio of 85:10:5 to prepare a 2 mol / L nickel-cobalt-manganese ternary mixed metal salt solution. Nb2O5 and TiO2 powders (in Ni...) were then added to the nickel-cobalt-manganese ternary mixed metal salt solution. 2 + Co 2+ and Mn 2+ The total molar amount is 100%, the molar amount of Nb2O5 is 0.5%, and the molar amount of TiO2 is 0.2%); the dispersion is obtained by ultrasonic dispersion for 40 min. Under a nitrogen atmosphere, a dispersion, a 4 mol / L sodium hydroxide solution, and a 2 mol / L ammonia solution were simultaneously added dropwise to a base solution (a mixed solution of ammonia and sodium hydroxide, pH 11). The dropwise addition rate of the dispersion was 0.5 L / h, the temperature was controlled at 50 °C, and the pH was 11. The co-precipitation reaction was carried out at a stirring speed of 600 rpm for 20 h. After the reaction was completed, the mixture was filtered and washed to obtain a solid with a pH of 7.2. The solid was then dried at 90 °C for 18 h to obtain a niobium-titanium dual-doped ternary precursor. The niobium-titanium dual-doped ternary precursor has a median particle size (D50) of 14 μm, a span of 0.45, and a specific surface area of ​​18 m². 2 / g, tap density 1.92g / cm³ 3 The intensity ratio of the (001) / (101) diffraction peaks (i.e., the crystal plane intensity ratio) in the XRD pattern is 0.8.

[0072] Example 4 The only difference between this embodiment and Embodiment 1 is that the amount of niobium pentoxide added is 0.05%, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0073] Example 5 The only difference between this embodiment and Example 1 is that the amount of niobium pentoxide added is 0.6%, while the other conditions and parameters are exactly the same as in Example 1.

[0074] Example 6 The only difference between this embodiment and Embodiment 1 is that the amount of titanium dioxide added is 0.02%, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0075] Example 7 The only difference between this embodiment and Embodiment 1 is that the amount of titanium dioxide added is 0.3%, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0076] Example 8 The only difference between this embodiment and Embodiment 1 is that the dropping rate of the dispersion is 0.2 L / h, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0077] Example 9 The only difference between this embodiment and Embodiment 1 is that the dropping rate of the dispersion is 1.5 L / h, while the other conditions and parameters are exactly the same as in Embodiment 1.

[0078] Comparative Example 1 The only difference between this comparative example and Example 1 is that niobium (niobium oxalate) and titanium (titanium oxysulfate) are doped in the form of ions in the nickel-cobalt-manganese ternary mixed metal salt solution. All other conditions and parameters are exactly the same as in Example 1.

[0079] Comparative Example 2 The only difference between this comparative example and Example 1 is that the dispersion was injected into the base liquid in a co-precipitation reaction at a rate of 5 L / h. All other conditions and parameters were exactly the same as in Example 1.

[0080] Performance testing: The precursors prepared in the examples and comparative examples were mixed with lithium hydroxide at a ratio of Li:M(Ni+Co+Mn) = 1.08:1 and calcined at 780°C for 11 hours in an oxygen atmosphere to obtain the positive electrode material. The positive electrode material was then used to prepare a positive electrode sheet with a ratio of positive electrode material:conductive carbon black:PVDF = 96:2:2. The negative electrode was prepared using graphite-silicon-oxygen composite material. A composite additive electrolyte was injected, and the cells were encapsulated to obtain energy storage single cells. The single cells were connected in series and parallel to form a 48V / 100Ah battery pack. A backup power supply system for an AI server was built by combining a BMS management system, a liquid cooling module, and a commercial UPS host for testing. The test results are shown in Table 1. Table 1 As shown in Table 1, and based on Examples 1 to 3, the niobium-titanium dual-doped ternary precursor prepared by the method provided in this application can produce batteries with a capacity of over 233 mAh / g, a capacity retention rate of over 88.8% under 20C discharge, a capacity retention rate of over 85.8% after 1000 1C charge-discharge cycles, a capacity retention rate of over 85.2% at -20℃, and a capacity retention rate of over 85.1% after 500 cycles at 60℃.

[0081] Comparing Examples 1 and 4-5, it can be seen that the amount of niobium pentoxide added affects the performance of the niobium-titanium dual-doped ternary precursor prepared in this application. Controlling the amount of niobium pentoxide added to 0.1%~0.5% of the total nickel, cobalt, and manganese content yields a niobium-titanium dual-doped ternary precursor with better performance. If the amount of niobium pentoxide added is too large, excess niobium ions will partially occupy lithium sites or transition metal sites, leading to lattice expansion and intensified cation mixing. Simultaneously, it may generate inert impurity phases such as LiNbO3, increasing electrode polarization resistance and reducing the material's initial coulombic efficiency, rate performance, and cycle stability. If the amount of niobium pentoxide added is too small, the niobium doping modification effect is insufficient, failing to effectively suppress microcrack propagation and rock salt phase surface transformation in high-nickel ternary materials during charge and discharge. This results in limited improvement in the material's long cycle life, structural stability, and rate performance, making it difficult to achieve the expected comprehensive electrochemical performance.

[0082] A comparison of Examples 1 and 6-7 shows that the performance of the niobium-titanium dual-doped ternary precursor prepared in this application is affected by the amount of titanium dioxide added. Controlling the amount of titanium dioxide added to 0.05%~0.2% of the total nickel, cobalt, and manganese content yields a niobium-titanium dual-doped ternary precursor with better performance. If the amount of titanium dioxide added is too large, excessive titanium ions will occupy transition metal sites, causing increased lattice distortion and cation mixing. Simultaneously, it may limit the redox reaction rate of the material, leading to increased electrode polarization resistance, reduced initial coulombic efficiency and reversible capacity, and consequently decreased rate performance and cycle stability. If the amount of titanium dioxide added is too small, the titanium doping modification effect is insufficient, failing to effectively increase the interlayer spacing of the lithium-oxygen layer, suppress the H2-H3 phase transition during charge and discharge, and prevent the propagation of microcracks within secondary particles. This results in limited improvement in the material's structural stability, rate performance, and long cycle life, making it difficult to achieve the expected comprehensive electrochemical performance.

[0083] Comparing Examples 1 and 8-9, it can be seen that the dropping rate of the dispersion affects the performance of the niobium-titanium dual-doped ternary precursor prepared by this application. Controlling the dropping rate of the dispersion at 0.5 L / h to 1 L / h yields a niobium-titanium dual-doped ternary precursor with better performance. If the droplet acceleration of the dispersion is too fast, the local concentration of niobium and titanium ions in the reaction system will be instantaneously too high, resulting in uneven distribution of dopant elements on or inside the particles, forming local enrichment or even precipitation of independent niobium titanium oxide impurity phases. This will destroy the uniformity and crystal structure integrity of the precursor, and may also cause drastic fluctuations in the pH of the reaction system, affecting the sphericity and particle size distribution of the precursor, thereby reducing the initial coulombic efficiency, rate performance, and cycle stability of the cathode material after sintering. If the droplet acceleration of the dispersion is too slow, the effective concentration of niobium and titanium ions in the reaction system will remain at a low level for a long time, and the doping efficiency will decrease significantly. Some dopant elements may be lost due to hydrolysis, complexation, or premature precipitation, resulting in the actual doping amount being far lower than the design value. This will prevent the full utilization of the synergistic modification effect of niobium-titanium dual doping on high-nickel cathode materials (such as inhibiting H2–H3 phase transition, slowing down microcrack propagation, and enhancing lattice oxygen stability), while also significantly extending the preparation cycle, reducing production efficiency, and increasing process costs.

[0084] Comparing Example 1 and Comparative Examples 1-2, the preparation method of the niobium-titanium dual-doped ternary precursor provided in this application uses niobium pentoxide and titanium dioxide as the niobium and titanium sources, respectively. These are dispersed into nanoscale particles by ultrasonication in a mixed metal salt solution, resulting in uniform dispersion in the dispersion liquid. The doping amount is precisely controlled, and the stable oxide state does not affect the pH and other conditions of the subsequent co-precipitation reaction, thus avoiding dopant segregation. The co-precipitation reaction is then carried out by titration. During the co-precipitation process, the nickel-cobalt-manganese ternary precursor undergoes in-situ nucleation and growth, and nano-Nb2O5 / TiO2 microcrystals are encapsulated within the primary grains, forming a bulk uniform dual-doped precursor without surface enrichment or dopant segregation defects. The sphericity and compaction density of the prepared precursor are significantly improved.

[0085] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing a niobium-titanium dual-doped ternary precursor, characterized in that, The preparation method includes the following steps: A nickel-cobalt-manganese ternary mixed metal salt solution, niobium pentoxide and titanium dioxide were mixed and ultrasonically dispersed to obtain a dispersion. The dispersion, precipitant solution, and complexing agent solution were simultaneously added dropwise to the base liquid, and a co-precipitation reaction was carried out to obtain a niobium-titanium dual-doped ternary precursor.

2. The preparation method according to claim 1, characterized in that, The total molar concentration of various metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution is 1.5 mol / L to 2 mol / L.

3. The preparation method according to claim 1 or 2, characterized in that, Based on the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%, the amount of niobium pentoxide added is 0.1%~0.5%. And / or, based on the total molar amount of metal ions in the nickel-cobalt-manganese ternary mixed metal salt solution being 100%, the amount of titanium dioxide added is 0.05%~0.2%; And / or, the ultrasonic dispersion time is 40 min to 60 min.

4. The preparation method according to any one of claims 1-3, characterized in that, The precipitant solution includes a sodium hydroxide solution; And / or, the molar concentration of the precipitant solution is 4 mol / L to 6 mol / L; And / or, the complexing agent solution includes ammonia; And / or, the molar concentration of the complexing agent solution is 2 mol / L to 3 mol / L.

5. The preparation method according to any one of claims 1-4, characterized in that, The dropping rate of the dispersion is 0.5 L / h to 1 L / h.

6. The preparation method according to any one of claims 1-5, characterized in that, The temperature for the coprecipitation reaction is 50℃~60℃; And / or, the pH of the coprecipitation reaction is 11 to 11.5; And / or, stirring is performed during the coprecipitation reaction; And / or, the stirring speed is 600 rpm to 700 rpm.

7. A niobium-titanium dual-doped ternary precursor, characterized in that, The niobium-titanium dual-doped ternary precursor is prepared by the preparation method described in any one of claims 1-6.

8. The niobium-titanium dual-doped ternary precursor as described in claim 7, characterized in that, The SPAN of the niobium-titanium dual-doped ternary precursor is <0.5; And / or, the crystal plane intensity ratio of the niobium-titanium dual-doped ternary precursor is 0.5~1.3; And / or, the tap density of the niobium-titanium dual-doped ternary precursor is 1.8 g / cm³. 3 ~2.1g / cm 3 ; And / or, the specific surface area of ​​the niobium-titanium dual-doped ternary precursor is 12 m². 2 / g~18m 2 / g; And / or, the median particle size D50 of the niobium-titanium dual-doped ternary precursor is 8 μm to 15 μm.

9. A positive electrode material, characterized in that, The cathode material is prepared by sintering a niobium-titanium dual-doped ternary precursor as described in claim 7 or 8 with a lithium source.

10. A UPS battery, characterized in that, The UPS battery contains the positive electrode material as described in claim 9.