Composite positive electrode active material, method for preparing composite positive electrode active material and rechargeable lithium battery
By preparing composite positive electrode active materials, including lithium iron phosphate-based compounds, lithium manganese-based oxides, and irreversible positive electrode additives, the problem of deterioration in cycle life characteristics of lithium iron phosphate-based positive electrode active materials under high voltage was solved, the charge/discharge capacity and efficiency of rechargeable lithium batteries were improved, the low-temperature discharge capacity and cycle life characteristics were enhanced, and the capacity per volume was increased.
Patent Information
- Application Number
- CN202610662535.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-05-13
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium iron phosphate-based positive electrode active materials suffer from deteriorated cycle life characteristics at high voltages, limiting the operating voltage of rechargeable lithium batteries. They also exhibit low capacity and energy density, and are deficient in initial charge/discharge efficiency, low-temperature discharge capacity, and cycle life characteristics.
Composite positive electrode active materials, including lithium iron phosphate-based compounds, lithium manganese-based oxides, and irreversible positive electrode additives, are formed by mixing and spray drying to improve their charge/discharge capacity and efficiency at high voltages, low-temperature discharge capacity and cycle life characteristics, and increase capacity per volume.
It improves the charge/discharge capacity and efficiency of rechargeable lithium batteries, enhances low-temperature discharge capacity and cycle life characteristics, increases capacity per volume, and maintains price competitiveness.
Smart Images

Figure CN123120715A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to composite positive electrode active materials, methods for preparing them, and rechargeable lithium batteries. Background Technology
[0002] Portable information devices (such as cellular phones, laptops, and smartphones) or electric vehicles already use rechargeable lithium batteries with high energy density as their power source. Recently, research has been actively conducted to use rechargeable lithium batteries with high energy density as a power source or energy storage source for hybrid or electric vehicles.
[0003] Furthermore, the increasing demand for high-performance, safe, and reliable novel positive electrode active materials is driven by the expansion and large-scale production of rechargeable lithium batteries. Lithium iron phosphate (LiFePO4)-based positive electrode active materials are attracting attention due to their structural stability, high heat resistance, and abundant raw material availability, making them cost-effective.
[0004] However, lithium iron phosphate-based positive electrode active materials exhibit a degradation in cycle life characteristics of rechargeable lithium batteries at high voltages, thus limiting the operating voltage of rechargeable lithium batteries. They also suffer from low capacity and energy density in rechargeable lithium batteries. Summary of the Invention
[0005] This disclosure provides composite positive electrode active materials, methods for preparing composite positive electrode active materials, and rechargeable lithium batteries that ensure price competitiveness for rechargeable lithium batteries, increase average voltage, improve charge / discharge capacity and efficiency, low-temperature discharge capacity and cycle life characteristics, and improve powder properties to increase particle density and significantly increase capacity per volume.
[0006] According to some embodiments of this disclosure, the composite positive electrode active material includes: a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of multiple primary particles; a second positive electrode active material comprising a lithium manganese-based oxide and in the form of multiple primary particles; and an irreversible positive electrode additive in the form of multiple primary particles. The composite positive electrode active material may have a particulate form comprising multiple primary particles of the first positive electrode active material, multiple primary particles of the second positive electrode active material, and multiple primary particles of the irreversible positive electrode additive.
[0007] In some embodiments, the lithium iron phosphate-based compound may include a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof. Formula 1 may be as follows:
[0008] [Chemical Formula 1]
[0009] Li a1 Fe (1-x1) M 1 x1 PO4,
[0010] Where 0.9 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4. M 1 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Chemical formula 2 can be as follows:
[0011] [Chemical Formula 2]
[0012] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4,
[0013] Where 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, and x² + y² < 1. M 2 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof.
[0014] In some embodiments, based on the total metals other than lithium in the lithium iron phosphate-based compound, the lithium iron phosphate-based compound may include Al, Mg, Ti, V or combinations thereof in an amount from about 0.1 mol% to about 0.5 mol%.
[0015] In some embodiments, the arithmetic mean size of the primary particles of the first positive electrode active material may be less than or equal to about 200 nm. The standard deviation of the arithmetic mean size of the primary particles of the first positive electrode active material may be less than or equal to about 100 nm.
[0016] In some embodiments, lithium manganese-based oxides may be represented as follows:
[0017] Li a3 Mn x3 M 3 y3 O 4-b3 X b3 ,
[0018] Where 0.9 ≤ a³ ≤ 1.8, 1.7 ≤ x³ ≤ 2, 0 ≤ y³ ≤ 0.3, 1.9 ≤ x³ + y³ ≤ 2.1, and 0 ≤ b³ ≤ 0.1. M 3X can be Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr, or combinations thereof. X can be F, P, S, or combinations thereof.
[0019] In some embodiments, the average particle size of the primary particles of the second positive electrode active material can be from about 2 μm to about 10 μm.
[0020] In some embodiments, the irreversible positive electrode additive may include lithium iron-based oxides, lithium cobalt-based oxides, lithium nickel-based oxides, or combinations thereof.
[0021] In some embodiments, the average particle size of the primary particles of the irreversible positive electrode additive can be from about 2 μm to about 10 μm.
[0022] In some embodiments, the composite positive electrode active material is in the form of multiple secondary particles, and the average particle size of the secondary particles of the composite positive electrode active material can be from about 3 μm to about 20 μm.
[0023] In some embodiments, based on 100% by weight of the first and second positive electrode active materials, the composite positive electrode active material may include the first positive electrode active material in an amount from about 50% to about 99% by weight. Based on 100% by weight of the first and second positive electrode active materials, the composite positive electrode active material may include the second positive electrode active material in an amount from about 1% to about 50% by weight.
[0024] In some embodiments, based on 100 parts by weight of the first positive electrode active material and the second positive electrode active material, the composite positive electrode active material may include an irreversible positive electrode additive in an amount of about 0.1 parts by weight to about 10 parts by weight.
[0025] In some embodiments, the particles of the composite positive electrode active material may include pores, and the porosity, expressed as the ratio of the area occupied by the pores to the cross-sectional area of the particles of the composite positive electrode active material, may be from about 10% to about 50%.
[0026] A method for preparing a composite positive electrode active material according to some embodiments of the present disclosure includes: preparing a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; preparing a second positive electrode active material comprising a lithium manganese-based oxide in the form of secondary particles wherein a plurality of primary particles are agglomerated; mixing the first positive electrode active material, the second positive electrode active material and an irreversible positive electrode additive in the form of primary particles and wet milling to prepare a first slurry; and adding the first slurry to a spray dryer and spray drying the first slurry to prepare a first dried product.
[0027] In some embodiments, the method may further include: after preparing a first dried product, subjecting the first dried product to firing to prepare a first fired product.
[0028] A rechargeable lithium battery according to some embodiments of this disclosure may include a positive electrode, a negative electrode, and an electrolyte. The positive electrode may include a positive electrode current collector; and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer including the aforementioned composite positive electrode active material.
[0029] Composite positive electrode active materials according to some embodiments can ensure price competitiveness while improving the charge / discharge capacity and efficiency, low-temperature discharge capacity and cycle life characteristics of rechargeable lithium batteries, and can improve powder characteristics to improve particle density and significantly increase the capacity per volume of rechargeable lithium batteries. Attached Figure Description
[0030] Figure 1 A schematic perspective view showing portions of a cylindrical rechargeable lithium battery according to some embodiments of the present disclosure.
[0031] Figure 2 A cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure is shown schematically.
[0032] Figure 3 and 4 Schematic exploded perspective views of pouch-type rechargeable lithium batteries according to some embodiments of the present disclosure.
[0033] Figure 5 This is a scanning electron microscope image of the cross-section of the composite positive electrode active material prepared in Example 2. Detailed Implementation
[0034] Specific embodiments will be described in detail below so that those skilled in the art can readily implement them. However, this disclosure may be embodied in many different forms and is not to be construed as limited to the embodiments set forth herein.
[0035] The terminology used herein is for describing implementation methods and is not intended to limit the invention. Unless the context clearly specifies otherwise, singular expressions include plural expressions.
[0036] The term "combination" refers to a mixture, laminate, complex, copolymer, alloy, blend, or reaction product of the constituent elements.
[0037] Terms such as “comprising,” “including,” or “having” are intended to indicate the presence of features, quantities, steps, elements, or combinations thereof embodied, but those terms do not preclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.
[0038] In the accompanying drawings, for clarity, the thickness of layers, films, panels, or regions is exaggerated, and throughout the specification, the same reference numerals denote the same elements. It will be understood that when an element, such as a layer, film, region, or substrate, is referred to as being "on" another element, it may be directly on said other element, or there may be intermediate elements present. Conversely, when an element is referred to as being "directly on" another element, there are no intermediate elements present.
[0039] In addition, the term "layer" in this article includes not only the geometry formed on the entire surface when viewed from a plan view, but also the geometry formed on a portion of the surface.
[0040] The average particle size can be measured, for example, by a particle size analyzer, or by transmission electron microscopy (TEM) or scanning electron microscopy (SEM) images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles in each size range, and calculating accordingly. In this disclosure, unless otherwise defined, the average particle size D... 50 This can mean the diameter of particles representing 50% of the cumulative volume in the particle size distribution, where the particles are considered (assumed) to be spherical. In this disclosure, unless otherwise defined, the average particle size refers to a value obtained by measuring the dimensions of approximately 20 randomly selected particles from scanning electron microscopy (SEM) images and calculating the arithmetic mean of the dimensions of approximately 20 randomly selected particles, where the size of each particle is defined as the diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles.
[0041] The word "or" is not interpreted as exclusive; for example, "A or B" is interpreted as including A, B, or A+B.
[0042] The term "metal" is interpreted to include the concepts of common metals, transition metals, and metalloids (semi-metals). As used herein, the term "metalloid" refers to an element that has properties intermediate between those of metals and nonmetals. Examples of metalloids include, but are not limited to, boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te).
[0043] As used herein, the term “vacuum” refers to a pressure in the range of 0.1 mbar to 10 mbar, as measured using a vacuum gauge in a processing chamber.
[0044] As used herein, the term "primary particle" refers to the smallest unit particle identified as an agglomeration (cluster) of individual particles when observed using a scanning electron microscope (SEM) of the positive electrode active material, where grain boundaries are not clearly distinguishable or are substantially (substantially) unobservable. Primary particles are the basic units constituting secondary particles formed by the aggregation of tens to hundreds of particles, and can exist individually or in a state where a small number (e.g., 20 or fewer) of primary particles are in contact with each other.
[0045] As used herein, the term "secondary particle" refers to an aggregate of primary particles of a given material, and may also be referred to as an assembly (assembly, collection) in this disclosure. Secondary particles have a structure in which primary particles are combined into individual particle forms (rather than a simple physical mixture) through interparticle contact and bonding. When observed using a scanning electron microscope (SEM), secondary particles can be identified as individual particle forms in which multiple primary particles are aggregated. Such secondary particles are distinguished from simple mixtures in which the corresponding particles are independently dispersed. Secondary particles can be formed by processes such as spray drying.
[0046] Composite positive electrode active material
[0047] According to some embodiments, a composite positive electrode active material includes: a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; a second positive electrode active material comprising a lithium manganese-based oxide and in the form of primary particles; and an irreversible positive electrode additive in the form of primary particles. The composite positive electrode active material has a particulate form comprising a plurality of primary particles of the first positive electrode active material, a plurality of primary particles of the second positive electrode active material, and a plurality of primary particles of the irreversible positive electrode additive.
[0048] Lithium iron phosphate (LFP) compounds, exhibiting excellent structural stability, high heat resistance, and competitive pricing, are attracting attention. However, despite offering superior cycle life characteristics, these characteristics deteriorate when used at high voltages, thus limiting their usable voltage.
[0049] Therefore, an attempt was made to simply mix and use lithium manganese-based oxides, which are low-cost materials with high average voltage. Although the average voltage is improved, the initial charge / discharge efficiency, discharge capacity at low temperatures (e.g., -20°C), cycle life characteristics, and high-temperature storage characteristics may deteriorate for rechargeable lithium batteries.
[0050] According to some embodiments, the composite positive electrode active material includes a lithium iron phosphate-based compound to ensure price competitiveness, and includes a lithium manganese-based oxide that can be used at high voltages and is relatively inexpensive compared to the lithium iron phosphate-based compound. It further includes an irreversible positive electrode additive in the form of primary particles, such that the composite positive electrode active material has a particulate form comprising primary particles of the lithium iron phosphate-based compound, primary particles of the lithium manganese-based oxide, and primary particles of the irreversible positive electrode additive. Specifically, the particulate form comprising primary particles of the lithium iron phosphate-based compound, primary particles of the lithium manganese-based oxide, and primary particles of the irreversible positive electrode additive can be in the form of individual secondary particles in which the primary particles of the lithium iron phosphate-based compound, primary particles of the lithium manganese-based oxide, and primary particles of the irreversible positive electrode additive are agglomerated together, and more specifically, in an assembly (assembly, aggregation) form, thereby improving the charge / discharge capacity and efficiency at high voltages, low-temperature discharge capacity and cycle life characteristics for rechargeable lithium batteries, and improving powder characteristics, thereby improving particle density, and simultaneously, significantly increasing the capacity per volume for rechargeable lithium batteries.
[0051] First positive electrode active material
[0052] The first positive electrode active material includes a lithium iron phosphate-based compound. By including a lithium iron phosphate-based compound as the first positive electrode active material, the composite positive electrode active material can ensure price competitiveness while also exhibiting excellent structural and thermal stability.
[0053] Lithium iron phosphate-based compounds may include, for example, compounds represented by Chemical Formula 1, compounds represented by Chemical Formula 2, or combinations thereof. Chemical Formula 1 is as follows:
[0054] [Chemical Formula 1]
[0055] Li a1 Fe (1-x1) M 1 x1 PO4.
[0056] In chemical formula 1, 0.9 ≤ a1 ≤ 1.5, 0 ≤ x1 ≤ 0.4, and M 1 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a1 ≤ 1.5, for example, 0.90 ≤ a1 ≤ 1.2, or 0.95 ≤ a1 ≤ 1.1. Additionally, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0.001 ≤ x1 ≤ 0.05.
[0057] Chemical formula 2 is as follows:
[0058] [Chemical Formula 2]
[0059] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4.
[0060] In chemical formula 2, 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, x² + y² < 1, and M 2 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a² ≤ 1.5, for example, 0.90 ≤ a² ≤ 1.2, or 0.95 ≤ a² ≤ 1.1. Additionally, 0.1 ≤ x² ≤ 0.9, 0.3 ≤ x² ≤ 0.9, or 0.4 ≤ x² ≤ 0.8 and 0 ≤ y² ≤ 0.4, 0 ≤ y² ≤ 0.3, 0 ≤ y² ≤ 0.2, 0 ≤ y² ≤ 0.1, or 0 ≤ y² ≤ 0.05.
[0061] Lithium iron phosphate-based compounds may include LiFePO4 and LiMn. 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof, but lithium iron phosphate-based compounds are not limited to these.
[0062] Lithium iron phosphate-based compounds may include Al, Mg, Ti, V, or combinations thereof as doping elements, and may include Al, Mg, Ti, V, or combinations thereof in amounts of about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol% or about 0.4 mol% based on the total metals other than lithium.
[0063] Lithium iron phosphate-based compounds may include Ti, Al, or a combination thereof as doping elements, wherein the amount of Ti may be from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%, based on the total metals excluding lithium, and the amount of Al may be from about 0.1 mol% to about 0.5 mol%, based on the total metals excluding lithium. This can improve rate performance and cycle life characteristics for rechargeable lithium batteries.
[0064] For example, M of chemical formula 11 And M of chemical formula 2 2 The active material may include Al, Mg, Ti, V, or combinations thereof, which in this case can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In Formulas 1 and 2, based on the total metals excluding lithium, Al, Mg, Ti, V, or combinations thereof may be included in amounts from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol% or about 0.4 mol%, and these amounts can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In chemical formula 1, 0.001≤x1≤0.005, 0.002≤x1≤0.005, 0.003≤x1≤0.005, or x1=0.004, and in chemical formula 2, 0.001≤x2≤0.005, 0.002≤x2≤0.005, 0.003≤x2≤0.005, or x2=0.004, which improves the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries.
[0065] The first positive electrode active material is in the form of primary particles, and the average particle size of the primary particles of the first positive electrode active material may be less than about 2 μm. The average particle size of the primary particles of the first positive electrode active material may be, for example, greater than or equal to about 0.1 μm and less than about 2 μm, about 0.1 μm to about 1.8 μm, about 0.1 μm to about 1.6 μm, about 0.1 μm to about 1.4 μm, about 0.1 μm to about 1.2 μm, about 0.1 μm to about 1 μm, about 0.1 μm to about 0.8 μm, about 0.2 μm to about 0.8 μm, about 0.3 μm to about 0.7 μm, or about 0.5 μm. The average particle size of the primary particles of the first positive electrode active material can be obtained by measuring the size of approximately 20 primary particles of the first positive electrode active material in an electron microscope image of the surface or cross-section of the composite positive electrode active material in the form of secondary particles, and calculating the arithmetic mean of the size of each particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. The average particle size of the primary particles of the first positive electrode active material may be smaller than the average particle size of the primary particles of the second positive electrode active material described below.
[0066] According to some embodiments, the first positive electrode active material may have small and uniform primary particles. Therefore, the composite positive electrode active material exhibits high charge / discharge capacity and excellent cycle life characteristics.
[0067] Furthermore, as measured by SEM images of the cross-section of the composite positive electrode active material, the arithmetic mean size of the primary particles of the first positive electrode active material constituting the composite positive electrode active material can be less than or equal to about 200 nm, about 50 nm to about 200 nm, or about 100 nm to about 200 nm, and the standard deviation of the arithmetic mean size can be less than or equal to about 100 nm, less than or equal to about 50 nm, or less than or equal to about 30 nm and can be greater than or equal to about 5 nm, greater than or equal to about 10 nm, or greater than or equal to about 12 nm. The arithmetic mean size and standard deviation of the primary particles of the first positive electrode active material can be obtained by measuring the size of about 20 random primary particles of the first positive electrode active material in an SEM image of the surface or cross-section of the composite positive electrode active material and calculating the arithmetic mean and the standard deviation of the arithmetic mean, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0068] The first positive electrode active material may further include a carbon coating layer on the surface of the primary particles. The carbon coating layer can improve the electrical conductivity of the first positive electrode active material and reduce the resistance of the positive electrode.
[0069] The carbon coating may include amorphous carbon and may be formed from, for example, glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, asphalt resins, tar resins, or combinations thereof.
[0070] Specifically, the carbon coating layer can be formed by: placing carbon raw material on the surface of the first positive electrode active material particles, and then performing a firing process. Alternatively, the carbon raw material and primary particles can be mixed and fired to form a carbon coating layer on the surface of the primary particles, or the carbon raw material and secondary particles can be mixed and fired to form a carbon coating layer on the surface of the secondary particles, and then pulverized to prepare primary particles with the carbon coating layer.
[0071] Based on 100% by weight of the first positive electrode active material, a carbon coating layer may be included in an amount from about 0.1% by weight to about 3.9% by weight, for example, from about 0.5% by weight to about 3.9% by weight, from about 1% by weight to about 3.9% by weight, from about 1.5% by weight to about 3.9% by weight, or from about 1.7% by weight to about 3.9% by weight. Based on 100% by weight of the first positive electrode active material, the amount of the carbon coating layer may be greater than or equal to about 1.5% by weight, greater than about 1.5% by weight, greater than or equal to about 1.6% by weight, greater than or equal to about 1.7% by weight, or greater than or equal to about 1.8% by weight. The amount of the carbon coating layer can be determined by completely burning the first positive electrode active material at a high temperature of about 1200°C to about 1400°C in an oxygen atmosphere to convert the carbon and sulfur in the first positive electrode active material into CO2 (or CO) and SO2, respectively. The amount of the carbon coating layer may be based on the amount of carbon in 100% by weight of the first positive electrode active material.
[0072] The first positive electrode active material can be manufactured by known methods or is a commercially available product. For example, the first positive electrode active material can be obtained by pulverizing secondary particles formed by the aggregation of multiple primary particles and includes lithium iron phosphate-based compounds.
[0073] Second positive electrode active material
[0074] The second positive electrode active material includes a lithium manganese-based composite oxide. The lithium manganese-based oxide included in the second positive electrode active material may have a spinel structure. Lithium manganese-based oxides with a spinel structure have a cubic crystal structure, and because they have a three-dimensional crystal structure, the lithium ion migration path is short, the ionic conductivity is high, and the overall structure of the lithium manganese-based oxide does not collapse when lithium ions are removed, making the structure very stable.
[0075] The lithium manganese-based oxide can be, for example, a spinel structure having LiMn2O4 as its basic composition. In addition to manganese, the lithium manganese-based oxide may further contain aluminum, magnesium, yttrium, or combinations thereof, and may contain no cobalt or may contain very small amounts of cobalt. For example, based on 100 mol% of metals other than lithium, the cobalt content in the lithium manganese-based oxide may be 5 wt% or less, 3 wt% or less, or 1 wt% or less, and may be 0 wt% or more.
[0076] Lithium manganese-based oxides can be represented by the following chemical formula 3:
[0077] [Chemical Formula 3]
[0078] Li a3 Mn x3 M 3 y3 O 4-b3 Xb3 .
[0079] In Chemical Formula 3, 0.9≤a3≤1.8, 1.7≤x3≤2, 0≤y3≤0.3, 1.9≤x3+y3≤2.1, and 0≤b3≤0.1, M 3 is Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
[0080] In Chemical Formula 3, 1.8≤x3≤2 and 0≤y3≤0.2, 1.9≤x3≤2 and 0≤y3≤0.1, or 1.7≤x3<2 and 0<y3≤0.3.
[0081] The lithium manganese-based oxide may be represented by the following Chemical Formula 4:
[0082] [Chemical Formula 4]
[0083] Li a4 Mn x4 Al y4 Mg z4 M 4 w4 O 4-b4 X b4 .
[0084] In Chemical Formula 4, 0.9≤a4≤1.8, 1.7≤x4<2.0, 0<y4≤0.015, 0<z4≤0.010, 0≤w4<0.3, 1.9≤x4+y4+z4+w4≤2.1, and 0≤b4≤0.1, M 4 is B, Ba, Ca, Ce, Cr, Fe, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
[0085] The second positive electrode active material is in the form of primary particles, and the average particle size of the primary particles of the second positive electrode active material can be greater than or equal to about 2 μm. For example, the average particle size of the primary particles of the second positive electrode active material can be about 2 μm to about 10 μm, about 2 μm to about 9.5 μm, about 2 μm to about 9 μm, about 2.5 μm to about 9 μm, about 3 μm to about 9 μm, about 3 μm to about 7 μm, or about 3 μm to about 5 μm. The average particle size of the second positive electrode active material can be larger than the average particle size of the first positive electrode active material described above. That is, the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material within the secondary particles can be distinguished based on particle size. The average particle size can be obtained by measuring the size of about 20 random primary particles of the second positive electrode active material in a scanning electron microscope image of the composite positive electrode active material and calculating its arithmetic mean, where the particle size is defined as the diameter in the case of spherical particles and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. Furthermore, the second positive electrode active material and the irreversible positive electrode additive can be distinguished based on differences in particle morphology in electron microscope images and elemental distribution according to energy-dispersive X-ray spectroscopy (EDX). Specifically, cross-sectional or surface images of the composite positive electrode active material are obtained using scanning electron microscopy (SEM), and EDX analysis is performed on the same field of view to map (plot) the elemental distribution. In this case, the second positive electrode active material is a lithium manganese-based oxide containing Mn as the main transition metal element and forming a homogeneous oxide phase, while the irreversible positive electrode additive may exist as a separate phase with different elemental compositions, such as metal oxides or lithium metal oxides containing Fe, Ni, Co, etc. Moreover, even when the particle size is similar, the two components can be distinguished based on the presence or absence of Mn distribution in the EDX mapping results or the spatial differences between the distribution of Mn and other transition metal elements. If desired, the Mn concentration distribution on the particle surface and inside can be further confirmed by STEM-EDS line scan analysis.
[0086] The second positive electrode active material may further include a coating layer on the surface of the primary particles. The coating layer may include compounds comprising the elements Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, S, or combinations thereof. When a coating layer comprising said compounds is formed on the surface of the second positive electrode active material, contact between the lithium manganese-based oxide and the electrolyte is blocked, thereby suppressing gas generation during charging and discharging and suppressing manganese elution at high temperatures. The coating layer may include ZnO, Al₂O₃, TiO₂, WO₃, etc. 3、MgO, CaO, B2O3, NbO2, SrO, CrO, Mo2O5, Bi2O3, SiO2, or combinations thereof. The coating layer may exist discontinuously or continuously.
[0087] The second positive electrode active material can be manufactured by known methods or is a commercially available product.
[0088] The second positive electrode active material can be prepared by solid-state reaction methods, etc. For example, a lithium precursor and a manganese precursor can be mixed in a predetermined molar ratio and then heat-treated in an oxygen atmosphere.
[0089] Examples of lithium precursors may include Li2CO3, LiOH and LiNO3, and examples of manganese precursors may include Mn2O3, MnO2 and Mn3O4.
[0090] Mixing can be carried out by dry or wet mixing methods, and can be performed using methods such as ball milling. The mixture can then be calcined in an oxygen or air atmosphere at a temperature of about 600°C to about 1000°C to form a spinel-structured lithium manganese oxide. If necessary, further pulverization, grading, or sieving can be performed.
[0091] The second positive electrode active material can be prepared in the form of secondary particles from which primary particles aggregate, and the secondary particles can subsequently be separated into primary particles during a wet milling process to form an assembly of composite positive electrode active materials.
[0092] Irreversible positive electrode additive
[0093] The composite positive electrode active material includes the first positive electrode active material comprising a lithium iron phosphate-based compound and the second positive electrode active material comprising a lithium manganese-based oxide, together with an irreversible positive electrode additive.
[0094] Irreversible positive electrode additives are compounds that act as sacrificial positive electrodes, compensating for irreversible lithium conversion that no longer participates in the charging / discharging reaction by participating in the formation of an SEI (solid electrolyte interphase) film on the surface of the negative electrode during charging / discharging. Irreversible positive electrode additives are compounds that decompose during the formation process (i.e., SEI film formation) to provide Li and do not participate in subsequent charging / discharging processes. By adding such irreversible positive electrode additives, consumed lithium can be replenished, thereby compensating for lithium loss and improving the energy density, cycle life, and stability of rechargeable lithium batteries.
[0095] Some of the lithium included in the positive electrode active material participates in irreversible reactions in the negative electrode and in the formation of the SEI film during charging and discharging, and this lithium is converted into irreversible lithium that no longer participates in charging and discharging reactions. This can cause a reduction in capacity, but this problem can be solved by including irreversible positive electrode additives. Furthermore, for rechargeable lithium batteries, discharge capacity at low temperatures (-20°C) can be improved, and particle density can be improved due to improved powder properties.
[0096] Irreversible positive electrode additives include lithium iron-based oxides, lithium cobalt-based oxides, lithium nickel-based oxides, or combinations thereof.
[0097] The lithium iron-based oxide can be Li5FeO4, LiFeO2, LiFe5O8 or a combination thereof, and among these, the use of Li5FeO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and therefore, this can greatly produce the effect of an irreversible positive electrode additive.
[0098] The lithium cobalt-based oxide can be Li6CoO4, and the use of Li6CoO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and therefore, can greatly produce the effect of an irreversible positive electrode additive.
[0099] The lithium nickel-based oxide can be Li2NiO2, and the use of Li2NiO2 can provide a large amount of lithium during the formation process, which can thus compensate for a large amount of irreversible lithium, and therefore, this can greatly produce the effect of an irreversible positive electrode additive.
[0100] The irreversible positive electrode additive is in the form of primary particles, and the average particle size of the primary particles of the irreversible positive electrode additive can be from about 2 μm to about 10 μm, for example, from about 2 μm to about 8 μm, from about 2 μm to about 6 μm, or from about 2 μm to about 5 μm. Furthermore, the second positive electrode active material and the irreversible positive electrode additive can be distinguished based on differences in particle morphology in electron microscope images and elemental distribution according to energy-dispersive X-ray spectroscopy (EDX). Specifically, cross-sectional or surface images of the composite positive electrode active material are obtained using scanning electron microscopy (SEM), and EDX analysis is performed on the same field of view to map (plot) the elemental distribution. In this case, the second positive electrode active material is a lithium manganese-based oxide containing Mn as the main transition metal element and forming a uniform oxide phase, while the irreversible positive electrode additive can exist as a separate phase with different elemental compositions, such as a metal oxide or lithium metal oxide containing Co. Moreover, even when the particle sizes are similar, the two components can be distinguished based on the presence or absence of Mn distribution in the EDX mapping results or the spatial differences between the distribution of Mn and other transition metal elements. If necessary, the Mn concentration distribution on the particle surface and inside can be further confirmed by STEM-EDS line scanning analysis. The average particle size can be obtained by measuring the size of approximately 20 particles in a scanning electron microscope image and calculating their arithmetic mean, where particle size is defined as diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles. If the average particle size of the irreversible positive electrode additive is within the above range, the agglomerate density can be improved, and a large amount of lithium can be provided during formation to compensate for the large amount of irreversible lithium. Furthermore, if the average particle size of the irreversible positive electrode additive is larger than the above range, it becomes difficult to properly perform the spray drying process described below, and even if spray drying is performed, it becomes difficult to form assemblies as in some embodiments.
[0101] Composite positive electrode active material
[0102] The composite positive electrode active material has the form of secondary particles comprising multiple primary particles of a first positive electrode active material, multiple primary particles of a second positive electrode active material, and multiple primary particles of an irreversible positive electrode additive. In this disclosure, the composite positive electrode active material can be in the form of secondary particles or an assembly, wherein the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the multiple primary particles of the irreversible positive electrode additive are aggregated. The secondary particles of the composite positive electrode active material may contain primary particles of the first positive electrode active material, primary particles of the second positive electrode active material, and primary particles of the irreversible positive electrode additive. The composite positive electrode active material particles are formed by the aggregation of multiple primary particles, and some of the primary particles are primary particles of the first positive electrode active material, some are primary particles of the second positive electrode active material, and the remaining primary particles are primary particles of the irreversible positive electrode additive. This structure differs from a core-shell structure with a shell structure, wherein the primary particles of the first positive electrode active material and / or the primary particles of the irreversible positive electrode additive surround the surface of a core of the second positive electrode active material particles. In this disclosure, the particulate form of the composite positive electrode active material may be referred to as the form of secondary particles or the form of an assembly, and particles described as being in the form of secondary particles or the form of an assembly should be understood to refer to the particles of the composite positive electrode active material.
[0103] The particle form of the composite positive electrode active material according to some embodiments differs from the conventional form of a mixture of lithium iron phosphate-based compounds, lithium manganese-based oxides, and irreversible positive electrode additives. When lithium iron phosphate-based compounds, lithium manganese-based oxides, and irreversible positive electrode additives are conventionally mixed and used as positive electrode active materials, the following problem exists: after the formation of the electrode plate, with repeated charging and discharging, the high-temperature storage characteristics deteriorate for secondary batteries due to the generation of spaces (gap) between the particles of the lithium iron phosphate-based compound, the particles of the lithium manganese-based composite oxide, and the particles of the irreversible positive electrode additive. However, the composite positive electrode active material according to some embodiments can solve the above problem by having a particle form comprising: primary particles of a first positive electrode active material comprising a lithium iron phosphate-based compound, primary particles of a second positive electrode active material comprising a lithium manganese-based composite oxide, and primary particles of the irreversible positive electrode additive. Specifically, the composite positive electrode active material may comprise particles in the form of individual secondary particles in which the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the primary particles of the irreversible positive electrode additive are agglomerated together, and more specifically, may comprise particles in the form of assemblies.
[0104] The composite positive electrode active material particles can have a spherical or ellipsoidal geometry by tightly agglomerating the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the primary particles of the irreversible positive electrode additive. The average particle size of the composite positive electrode active material particles can be, for example, about 3 μm to about 20 μm, about 6 μm to about 20 μm, or about 6 μm to about 15 μm. The average particle size of the composite positive electrode active material particles can be obtained, for example, by randomly selecting about 20 secondary particles from an electron microscope image of the composite positive electrode active material, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0105] The composite positive electrode active material may include an excessive amount of the first positive electrode active material and the second positive electrode active material. Based on 100% by weight of the composite positive electrode active material, the total weight of the first positive electrode active material and the second positive electrode active material may be greater than or equal to about 90% by weight, greater than or equal to about 92% by weight, greater than or equal to about 94% by weight, greater than or equal to about 95% by weight, or greater than or equal to about 96% by weight.
[0106] Based on the total weight of 100% by weight of the first and second positive electrode active materials, the amounts of the first and second positive electrode active materials can be appropriately adjusted. Based on 100% by weight of the first and second positive electrode active materials, the first positive electrode active material may be included in an amount of approximately 50% to approximately 99% by weight, approximately 55% to approximately 95% by weight, or approximately 60% to approximately 90% by weight. And based on 100% by weight of the first and second positive electrode active materials, the second positive electrode active material may be included in an amount of approximately 1% to approximately 50% by weight, approximately 5% to approximately 45% by weight, or approximately 10% to approximately 40% by weight. If the first and second positive electrode active materials are included in 100% by weight to satisfy the above ranges, the battery can operate at high voltages, and for rechargeable lithium batteries, overall battery performance (including initial charge / discharge capacity, efficiency, discharge capacity at low temperatures, and high-temperature storage characteristics) can be improved.
[0107] The irreversible positive electrode additive may be included in an amount equal to the weight percent of the weight of the first and second positive electrode active materials removed from 100% by weight of the composite positive electrode active material. Furthermore, based on 100 parts by weight of the first and second positive electrode active materials, the irreversible positive electrode additive may be included in amounts from about 0.1 parts by weight to about 10 parts by weight, for example from about 0.5 parts by weight to about 8 parts by weight, from about 1 part by weight to about 6 parts by weight, from about 1 part by weight to about 5 parts by weight, or from about 1 part by weight to about 4.5 parts by weight. If the amount of the irreversible positive electrode additive meets the above ranges, the capacity per volume can be increased, and furthermore, the discharge capacity at low temperatures can be improved, and powder characteristics can be improved, thereby improving particle density.
[0108] The composite positive electrode active material may further include a carbon coating layer on the surface of the composite positive electrode active material particles. The carbon coating layer can improve the electrical conductivity of the composite positive electrode active material and thereby reduce the resistance of the positive electrode comprising it. The carbon coating layer may be the same as the carbon coating layer on the surface of the primary particles of the first positive electrode active material of the composite positive electrode active material described above, and therefore a description of the carbon coating layer is omitted in this section.
[0109] The total number of primary particles of the second positive electrode active material and primary particles of the irreversible positive electrode additive in the particles of the composite positive electrode active material can be 10 or less, for example 9 or less, 8 or less, 7 or less, or 6 or less, and can be greater than zero, 1 or more, 2 or more, or 3 or more. For example, the total number of primary particles of the second positive electrode active material and primary particles of the irreversible positive electrode additive in the particles of the composite positive electrode active material can be in the range of 1 to 10, 2 to 10, 3 to 10, 3 to 9, 3 to 8, 3 to 7, or 3 to 6. The number of primary particles of the second positive electrode active material and primary particles of the irreversible positive electrode additive in the particles of the composite positive electrode active material can be determined by counting the number of particles with a particle size greater than or equal to about 2 μm within a single composite positive electrode active material particle, where particle size refers to diameter in the case of spherical particles and the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. Here, the total number of primary particles of the second positive electrode active material and the primary particles of the irreversible positive electrode additive can be the average of the total number of primary particles of the second positive electrode active material and the primary particles of the irreversible positive electrode additive in each of the multiple composite positive electrode active material particles.
[0110] The ratio of primary particles of the second positive electrode active material to primary particles of the irreversible positive electrode additive in the composite positive electrode active material can be in the range of about 10:1 to about 60:1, for example about 10:1 to about 40:1, about 15:1 to about 40:1, about 15:1 to about 60:1 or about 40:1 to about 60:1.
[0111] The composite positive electrode active material particles may include pores, and the porosity (which is the ratio of the area occupied by the pores to the cross-sectional area of the composite positive electrode active material particle) may be from about 10% to about 50%, for example from about 10% to about 40%, from about 10% to about 30%, or from about 15% to about 20%. The porosity can be obtained by cutting the composite positive electrode active material particles using a focused ion beam (FIB) to obtain a cross-section, and by measuring the ratio of the area occupied by the pores to the cross-sectional area of the composite positive electrode active material particle within the cross-section using an image analysis program such as ImageJ via scanning electron microscopy. The cross-section of the composite positive electrode active material can be obtained by cutting the composite positive electrode active material using a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be acquired, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or a consistent threshold setting method equally applied to all samples. The porosity of the composite positive electrode active material can be the average of the porosities measured for multiple composite positive electrode active materials, and can be obtained, for example, by measuring the porosity of at least 20 individual composite positive electrode active materials and calculating the average porosity of at least 20 individual composite positive electrode active materials. If the porosity in the composite positive electrode active material particles meets the above range, during positive electrode compression, primary particles can fill the spaces between the pores in secondary particles, thereby improving the aggregate density or positive electrode density, and thus improving the capacity characteristics and energy density of the rechargeable lithium battery.
[0112] The agglomerate density of the composite positive electrode active material can be greater than or equal to about 2.4 g / cc and can be about 2.4 g / cc to about 3 g / cc, about 2.45 g / cc to about 2.9 g / cc, about 2.5 g / cc to about 2.8 g / cc, about 2.5 g / cc to about 2.7 g / cc, or about 2.55 g / cc to about 2.65 g / cc. The agglomerate density of the composite positive electrode active material can be measured as follows: 3 g of the composite positive electrode active material is placed in a mold, and the material is held in the mold at 25°C for 30 seconds at a temperature of 4 tonnes. The thickness of the agglomerates is measured, and the agglomerate volume is calculated using the agglomerate thickness and the diameter of the mold. The mass of the composite positive electrode active material is then divided by the calculated volume. If the agglomerate density of the composite positive electrode active material meets the above range, the powder properties can be improved, thereby improving the capacity properties. When the porosity of the composite positive electrode active material particles meets the above range, the agglomeration density of the composite positive electrode active material can be improved when the particles fill the spaces between the pores once during compression.
[0113] Method for preparing composite positive electrode active materials
[0114] A method for preparing a composite positive electrode active material according to some embodiments includes: preparing a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; mixing and wet-milling the first positive electrode active material, a second positive electrode active material comprising a lithium manganese-based oxide in the form of secondary particles from which a plurality of primary particles are agglomerated, and an irreversible positive electrode additive in the form of primary particles to prepare a first slurry; and adding the first slurry to a spray dryer and spray-drying it to prepare a first dried product.
[0115] In some embodiments, the first positive electrode active material comprises a low-cost lithium iron phosphate compound to ensure price competitiveness, and is further comprised of a lithium manganese-based oxide that can be used at high voltages and is relatively low-cost compared to lithium iron phosphate-based compounds. Furthermore, an irreversible positive electrode additive in the form of primary particles is further comprised, such that the primary particles of the lithium iron phosphate compound, the primary particles of the lithium manganese-based oxide, and the primary particles of the irreversible positive electrode additive agglomerate to form a single secondary particle (a type of assembly form). This improves charge / discharge capacity and efficiency at high voltages, low-temperature discharge capacity, and cycle life characteristics for rechargeable lithium batteries, and improves particle density due to improved powder properties, and can significantly increase capacity per volume.
[0116] In the following preparation methods, terms using "first" and "second," other than the first positive electrode active material and the second positive electrode active material, are used to respectively identify (indicate) the process of preparing a composite positive electrode active material using the first positive electrode active material and the process of preparing the first positive electrode active material. In the process of preparing a composite positive electrode active material using the first positive electrode active material and the second positive electrode active material, the corresponding use of "slurry" may be indicated by "first slurry"; while in the process of preparing the first positive electrode active material, the corresponding use of "slurry" may be indicated by "second slurry".
[0117] For convenience, following the order described in the claims, the process of preparing the composite positive electrode active material using the first positive electrode active material and the second positive electrode active material is referred to as "first," and the process of preparing the first positive electrode active material is referred to as "second." However, it should be understood that "first" and "second" do not indicate their order.
[0118] Preparation of the first positive electrode active material
[0119] The preparation (processing) of the first positive electrode active material includes a process for preparing (processing) a first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles. The first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles can be prepared according to the methods described below, or a commercially available product can be obtained and used.
[0120] The preparation of a first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles may include: wet milling an iron iron phosphate-based precursor, a lithium raw material, and a carbon raw material mixed in a second solvent to prepare a second slurry; adding the wet-milled second slurry to a spray dryer and spray-drying the second slurry to prepare a second dried product; calcining the second dried product to prepare a second calcined product; and pulverizing the second calcined product. The steps for preparing the first positive electrode active material are described sequentially below.
[0121] First, the second slurry can be prepared by mixing an iron phosphate-based precursor, a lithium raw material, and a carbon raw material in a second solvent and wet milling the mixture. The preparation of the second slurry may include: mixing the iron phosphate-based precursor and the lithium raw material to prepare a raw material mixture; preparing the carbon raw material; and mixing the raw material mixture and the carbon raw material, adding the second solvent, and wet milling to prepare the second slurry. The weight ratio of the raw material mixture to the carbon raw material is not particularly limited, but may be, for example, about 5:5 to about 99:1, about 6:4 to about 99:1, about 7:3 to about 99:1, about 8:2 to about 99:1, or about 9:1 to about 99:1.
[0122] Ferric phosphate precursors can be ferric phosphate precursors such as ferric phosphate (FePO4) and ferric phosphate (II) (Fe3(PO4)2), or they can be formed by adding phosphoric acid precursors such as phosphoric acid (H3PO4), ammonium dihydrogen phosphate (NH4H2PO4), diammonium hydrogen phosphate ((NH4)2HPO4), or sodium orthophosphate (Na3PO4) to ferric raw materials such as ferric oxide (Fe2O3), ferric oxalate (FeC2O4), or ferric hydroxide (Fe(OH)3). Alternatively, ferric phosphate precursors can be manganese phosphate precursors formed by adding manganese raw materials such as manganese oxide, manganese carbonate, manganese sulfate, or manganese nitrate to ferric phosphate precursors. There are no limitations on the use of ferric phosphate precursors, as long as they are known materials used in solid-phase reactions.
[0123] Lithium raw materials may be, for example, Li2CO3, LiOH, their hydrates, or combinations thereof.
[0124] Carbon raw materials may include glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, pitch resins, tar resins, or combinations thereof. For example, a mixture of glucose and polyethylene glycol may be used as a carbon raw material, and the mixing ratio by weight is not particularly limited, but may be, for example, about 10:90 to about 90:10, about 20:80 to about 80:20, about 30:70 to about 70:30, about 40:60 to about 60:40, or about 50:50.
[0125] Wet milling can be performed by adding a second solvent, which can be any one of ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), tetraethylene glycol (TTEG), propylene glycol (PG), polyethylene glycol (PEG), polypropylene glycol (PPG), ethanol, water, and acetone. The second solvent can be a polyol solvent that induces a reducing atmosphere, either alone or as a mixture of the polyol solvent with water, acetone, ethanol, or a combination thereof.
[0126] Wet grinding can be performed using bead mills, ball mills, vibratory mills, or colloid mills. For example, in some embodiments, wet grinding can be performed using ball milling with zirconia balls, wherein the wet grinding can be performed by rotating the grinding vessel at a speed of about 50 rpm to about 2000 rpm for about 1 hour to about 10 hours.
[0127] In the preparation of the second slurry by wet milling, raw materials including Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof may be further added to the slurry. Raw materials including Al, Mg, Mn, Ti, V, or combinations thereof may be added. Raw materials including Al, Mg, Ti, V, or combinations thereof may be added as dopant elements, and based on the total metals other than lithium in the lithium iron phosphate-based compound of the first positive electrode active material, Al, Mg, Ti, V, or combinations thereof may be added in amounts of about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%. The Ti-containing raw material can be further added to the second slurry, and based on the total metals other than lithium in the first positive electrode active material, the amount of Ti added can be up to about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%. Therefore, the rate characteristics and cycle life characteristics of rechargeable lithium batteries can be improved.
[0128] Next, the wet-milled second slurry can be added to a spray dryer and spray-dried to produce a second dried product.
[0129] A second slurry, which has been wet-milled, can be injected into a spray dryer and sprayed to produce droplets (droplets) containing the desired uniform composition. The formed droplets can then be dried to produce a second dried product.
[0130] Spray dryers may include ultrasonic spray devices, single-fluid and dual-fluid air nozzle spray devices, ultrasonic nozzle spray devices, filter expansion droplet generators (FEAG), and disc droplet generators. Any known spray dryer may be used.
[0131] The amount of the second slurry added may vary depending on the spray dryer, but can be appropriately adjusted. In some embodiments, drying occurs at a blower speed of about 50 Hz and an addition pressure of about 0.5 MPa, and the addition rate of the second slurry may be less than or equal to about 1 kg / min, for example less than about 1 kg / min, less than or equal to about 0.9 kg / min, less than or equal to about 0.8 kg / min, less than or equal to about 0.7 kg / min, less than or equal to about 0.6 kg / min, or less than or equal to about 0.5 kg / min and greater than or equal to about 0.01 kg / min, greater than or equal to about 0.05 kg / min, greater than or equal to about 0.1 kg / min, greater than or equal to about 0.15 kg / min, greater than or equal to about 0.2 kg / min, greater than or equal to about 0.3 kg / min, or greater than or equal to about 0.4 kg / min. The addition rate of the second slurry is a value converted based on the solid content (solids) and is defined as the amount of second slurry supplied per minute (min) based on the mass of the solid content in the slurry. When the addition rate of the second slurry added to the spray dryer meets the above range, secondary particles of uniform size composed of primary particles can be produced, and the average size of the primary particles can be adjusted to be less than or equal to about 200 nm, and the size of the secondary particles can be uniformly controlled.
[0132] Spray drying can be carried out at a temperature greater than or equal to about 100°C, for example at about 150°C to about 400°C, about 150°C to about 300°C, or about 200°C to about 250°C, to dry the components and evaporate the solvent.
[0133] Next, the second dried product can be fired to produce a second fired product.
[0134] In the preparation of the second calcined product, calcination can be carried out under vacuum or an inert gas and at a temperature of about 700°C to about 1000°C, for example about 725°C to about 900°C or about 750°C to about 800°C. The inert gas can be argon or nitrogen.
[0135] The second calcined product may include a lithium iron phosphate-based compound and may be in the form of secondary particles in which multiple primary particles are aggregated. The secondary particles may also be represented as assemblies. More specifically, the secondary particles of the second calcined product may have a spherical or ellipsoidal geometry because the primary particles are tightly aggregated together. The average particle size of the secondary particles may be, for example, about 3 μm to about 20 μm, about 5 μm to about 18 μm, or about 7 μm to about 15 μm. The average particle size of the secondary particles can be obtained by randomly selecting about 20 secondary particles from an electron microscope image of the second calcined product, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0136] The secondary particles of the second calcined product may include pores, and the porosity may be from about 10% to about 50%, for example from about 10% to about 40%, or from about 10% to about 30%. Porosity can be the ratio of the area occupied by pores in the secondary particles to the cross-sectional area of the secondary particles, measured using an image analysis program such as ImageJ in a scanning electron microscope image of the cross-section of the secondary particles of the second calcined product. The cross-section of the secondary particles can be obtained by cutting the second calcined product using a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be acquired, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or a consistent threshold setting method equally applied to all samples. The porosity of the second fired product can be the average of the porosities measured for multiple second fired products, and can be obtained, for example, by measuring the porosity of at least 20 individual second fired products and calculating the average of the porosities of at least 20 individual second fired products.
[0137] The second calcined product may further include a carbon coating layer on the surface of the secondary particles, the surface of the primary particles constituting the secondary particles, or both. If the second calcined product is subsequently pulverized to prepare the first positive electrode active material of the primary particles, the carbon coating layer can improve the electrical conductivity of the first positive electrode active material and reduce the resistance of the positive electrode. The carbon coating layer can be formed through the above-described calcination process of the carbon raw materials.
[0138] Next, the second fired product can be crushed.
[0139] Crushing can be carried out using equipment such as a jet mill, ball mill, bead mill, or sand mill.
[0140] There are no particular limitations on the pulverization speed during the aforementioned pulverization process, as long as the second calcined product in the form of an assembly is separated into primary particles constituting the assembly. For example, the pulverization speed can exceed approximately 2000 rpm, or it can be carried out at a pulverization speed of approximately 3000 rpm to approximately 6000 rpm, or approximately 4000 rpm to approximately 6000 rpm. The pulverization speed of the second calcined product can be carried out under conditions in which the secondary particles can be pulverized and separated into multiple primary particles. If the pulverization speed is less than 2000 rpm, the secondary particles may not be pulverized and may exist in the form of an assembly. If the pulverization speed is greater than approximately 6000 rpm, the pulverized and separated primary particles may be damaged.
[0141] A first positive electrode active material comprising lithium iron phosphate-based compounds and in the form of primary particles can be prepared by pulverizing the second calcined product. In the above steps, the first positive electrode active material prepared according to the above method can be used.
[0142] The first positive electrode active material includes a lithium iron phosphate-based compound. Since the details of the first positive electrode active material can be described in the same manner as the description of the composite positive electrode active material above, the description of the first positive electrode active material is omitted below.
[0143] Preparation of the first slurry
[0144] The preparation of the first slurry includes a process of mixing and wet milling a first positive electrode active material, a second positive electrode active material comprising lithium manganese-based oxide in the form of secondary particles from which a plurality of primary particles are agglomerated, and an irreversible positive electrode additive in the form of primary particles.
[0145] The second positive electrode active material can be in the form of secondary particles from which multiple primary particles aggregate, and the average particle size of the secondary particles of the second positive electrode active material can be 2 μm to 10 μm, 3 μm to 10 μm, 4 μm to 10 μm, 5 μm to 10 μm, 6 μm to 10 μm, 7 μm to 10 μm, or 8 μm to 10 μm. The average particle size of the secondary particles of the second positive electrode active material can be obtained, for example, by measuring the size of approximately 20 particles in a scanning electron microscope image of the secondary particles of the second positive electrode active material and calculating their arithmetic mean, wherein the particle size is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0146] The details of the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive may be the same as those described above, and therefore, the descriptions of the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive are omitted in this section.
[0147] There are no particular limitations on the method of mixing the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive, and for example, a mixer can be used.
[0148] The weight ratio of the first positive electrode active material to the second positive electrode active material can be from about 50:50 to about 99:1, from about 55:45 to about 95:5, or from about 60:40 to about 90:10. When the weight ratio of the first positive electrode active material to the second positive electrode active material meets the above ranges, it is possible to operate at high voltage while ensuring price competitiveness, and it can improve charge / discharge efficiency, low-temperature discharge capacity, cycle life characteristics, and high-temperature storage characteristics, and improve powder characteristics, thereby improving particle density. Furthermore, when including a large amount of material with a relatively large average particle size D... 50 When the second positive electrode active material is spray-dried, it is difficult to properly spray-dry it, and even if spray-drying is performed, it is difficult to form an assembly as in some embodiments.
[0149] Based on 100 parts by weight of the first and second positive electrode active materials, an irreversible positive electrode additive may be added in amounts from about 0.1 parts by weight to about 10 parts by weight, for example from about 0.5 parts by weight to about 8 parts by weight, from about 1 part by weight to about 6 parts by weight, from about 1 part by weight to about 5 parts by weight, or from about 1 part by weight to about 4.5 parts by weight. When the amount of the irreversible positive electrode additive meets the above ranges, the capacity per volume can be increased, and furthermore, for rechargeable lithium batteries, the discharge capacity at low temperatures can be improved, and powder characteristics can be improved, thereby improving particle density.
[0150] A first slurry can be prepared by adding a first solvent to a first positive electrode active material, a second positive electrode active material, and an irreversible positive electrode additive during wet milling, and the specific type of the first solvent is as described for the second solvent. Wet milling can be performed using methods such as ultrasonic dispersion, stirred dispersion, using a homogenizer, using a high-shear mixer, using a jet mill, ball milling, or bead milling, and the methods are not particularly limited, as long as they are used for wet milling of the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive. For example, in some embodiments, mixing can be performed using zirconia balls via ball milling, and in this case, it can be carried out by rotating the milling vessel at a speed of about 10 rpm to about 100 rpm for about 10 minutes to about 3 hours.
[0151] In this process, the secondary particles of the second positive electrode active material can be separated into primary particles and can constitute a composite positive electrode active material prepared according to the spray drying process described below. Since the average particle size of the primary particles of the second positive electrode active material constituting the composite positive electrode active material is as described above, its repeated description will be omitted below.
[0152] Preparation of the first dried product
[0153] The preparation of the first dried product includes adding a first slurry to a spray dryer and spray drying the first slurry.
[0154] A first slurry can be added to a spray dryer and sprayed to produce droplets comprising a uniform composition. The droplets can then be dried to prepare a first dried product. The solvent in the droplets evaporates, and the remaining solids can be dried into granular form.
[0155] Spray dryers may include ultrasonic spray devices, single-fluid and dual-fluid air nozzle spray devices, ultrasonic nozzle spray devices, filtration expansion droplet generators (FEAG), and disc droplet generators. Any known spray dryer may be used.
[0156] The amount of the first slurry added may vary depending on the spray dryer, but can be adjusted appropriately. The addition rate of the first slurry may be less than or equal to about 1 kg / min, for example, less than or equal to about 1 kg / min, less than or equal to about 0.9 kg / min, less than or equal to about 0.8 kg / min, less than or equal to about 0.7 kg / min, less than or equal to about 0.6 kg / min, or less than or equal to about 0.5 kg / min and greater than or equal to about 0.01 kg / min, greater than or equal to about 0.05 kg / min, greater than or equal to about 0.1 kg / min, greater than or equal to about 0.15 kg / min, greater than or equal to about 0.2 kg / min, greater than or equal to about 0.3 kg / min, or greater than or equal to about 0.4 kg / min. Here, the feed rate of the first slurry is a value based on the solids content (solids) conversion and is defined as the amount fed per minute (min) based on the mass of the solids content in the first slurry. If the addition rate of the first slurry to the spray dryer meets the above range, the drying efficiency can be improved, a powder with a narrow particle size distribution and a relatively uniform geometry can be formed, and clogging and contamination inside the dryer can be prevented.
[0157] Spray drying can be carried out at temperatures greater than or equal to about 100°C, for example about 150°C to about 400°C, about 150°C to about 300°C, or about 200°C to about 250°C to dry the components and evaporate the solvent.
[0158] The first dried product obtained according to the above steps may have a particulate form comprising primary particles of a first positive electrode active material, primary particles of a second positive electrode active material, and primary particles of an irreversible positive electrode additive. It may also have a secondary particle form in which the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the primary particles of the irreversible positive electrode additive are agglomerated, and the secondary particles may be represented as an assembly. The first dried product may correspond to or be the same as the composite positive electrode active material in this specification.
[0159] The method for preparing composite positive electrode active materials may further include: after adding a first slurry to a spray dryer and spray-drying the first slurry to prepare a first dried product, calcining the first dried product to prepare a first calcined product. The preparation of the first calcined product may be referred to as a first calcination step to distinguish the preparation of the first dried product from the spray drying and calcination of a second slurry. The composite positive electrode active material can be further strengthened by performing a first calcination step after spray drying, thereby further stabilizing the crystal structure of the composite positive electrode active material and significantly improving its electrochemical properties, mechanical strength, and cycle life stability.
[0160] The first firing step can be carried out under vacuum or an inert gas and at a temperature of about 300°C to about 1000°C, for example, about 300°C to about 500°C or about 350°C to about 450°C. The inert gas can be argon or nitrogen. If the above firing temperature meets the above range, the electrochemical properties, mechanical strength and cycle life stability of the composite positive electrode active material can be greatly improved.
[0161] The first positive electrode active material may be in particulate form comprising primary particles of the first positive electrode active material, primary particles of the second positive electrode active material, and primary particles of the irreversible positive electrode additive, and may also be in the form of secondary particles or assemblies in which, for example, the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the primary particles of the irreversible positive electrode additive are agglomerated. The first calcined product may also correspond to the composite positive electrode active material in this specification, or may be the same as the composite positive electrode active material.
[0162] In the case of a composite positive electrode active material prepared according to a method for preparing a composite positive electrode active material according to one embodiment, the overall battery performance is superior compared to conventional simple mixtures, and the high-temperature storage characteristics are improved.
[0163] Rechargeable lithium batteries
[0164] A rechargeable lithium battery according to some embodiments includes: a positive electrode comprising a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and comprising the aforementioned composite positive electrode active material; a negative electrode; and an electrolyte. The rechargeable lithium battery may include a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte.
[0165] According to some embodiments, rechargeable lithium batteries can have overall improved battery performance by including the aforementioned composite positive electrode active material, and specifically, can have improved charge / discharge capacity and efficiency, low-temperature discharge capacity and cycle life characteristics, while ensuring price competitiveness and increasing average voltage, and can have improved powder characteristics, thereby improving particle density and significantly increasing capacity per volume.
[0166] Rechargeable lithium batteries can be categorized into cylindrical, prismatic, pouch-shaped, or coin-shaped geometric shapes. Figure 1 This is a schematic diagram showing a cross-section of a cylindrical rechargeable lithium battery cut along a vertical axis according to some embodiments of the present disclosure and an electrode assembly 40 extending from the cylindrical rechargeable lithium battery. Figure 2 This is a cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure. Figure 3 and 4 Each of the following is a schematic exploded perspective view of a pouch-type rechargeable lithium battery according to some embodiments of the present disclosure. The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown).
[0167] The rechargeable lithium battery 100 may include a seal 60 of the sealed housing 50, such as Figure 1 As shown. Additionally, in Figure 2 The rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. The rechargeable lithium battery 100 may include electrode connectors 70, which serve as electrical paths for conducting current generated in the electrode assembly 40 to the outside. The electrode connectors 70 may be as follows: Figure 4 They can be arranged in the same direction as in the middle, or the positive electrode terminal 71 and the negative electrode terminal 72 can be arranged as follows: Figure 3 It is set in the opposite direction as in the middle.
[0168] positive electrode
[0169] There are no particular restrictions on the positive electrode current collector, as long as it is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be an aluminum foil or stainless steel foil with a thickness of about 10 μm to about 15 μm.
[0170] The positive electrode active material layer includes the aforementioned composite positive electrode active material. Specific details of the composite positive electrode active material may be the same as those described above, and therefore, a description of the composite positive electrode active material is omitted in this section.
[0171] The amount of composite positive electrode active material may be about 60% to about 99.9% by weight, about 70% to about 99.8% by weight, about 80% to about 99% by weight, or about 90% to about 98% by weight, based on a 100% by weight positive electrode active material layer.
[0172] The positive electrode active material layer may optionally further include a binder, a conductive material, or a combination thereof.
[0173] The binder can be used to ensure good adhesion between composite positive electrode active material particles and to ensure good adhesion of the composite positive electrode active material to the positive electrode current collector. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide (polymers containing ethylene oxide), polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, or nylon, but the binder is not limited to these.
[0174] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes in the battery. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0175] In the positive electrode active material layer, based on 100% by weight of the positive electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the positive electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0176] In addition to the components described above, the positive electrode active material layer may further include other positive electrode active materials to the extent that they do not impair the purpose of this disclosure.
[0177] In addition to the aforementioned composite positive electrode active material, the positive electrode active material layer may further include a positive electrode active material having primary particle form and comprising the aforementioned lithium iron phosphate-based compound (hereinafter, "third positive electrode active material") and / or a positive electrode active material having primary particle form and comprising the aforementioned lithium manganese-based composite oxide (hereinafter, "fourth positive electrode active material"). Here, the third positive electrode active material and / or the fourth positive electrode active material may each be independently those of the first positive electrode active material and / or the second positive electrode active material included in the composite positive electrode active material, which exist in an unassembled and separated state. In this case, the average particle size of the primary particles of the third positive electrode active material may be the same as described above for the first positive electrode active material, and the average particle size of the primary particles of the fourth positive electrode active material may be the same as described above for the second positive electrode active material. Here, the third positive electrode active material and / or the fourth positive electrode active material exist in a non-aggregated, separated state, and do not agglomerate with the aforementioned composite positive electrode active material to form an assembled structure.
[0178] If, in addition to the composite positive electrode active material, the positive electrode active material layer further comprises a third positive electrode active material and / or a fourth positive electrode active material, the weight ratio of the composite positive electrode active material to the third positive electrode active material, the fourth positive electrode active material, or a combination thereof may be from about 1:9 to about 9:1, and may be added appropriately depending on the purpose. The third positive electrode active material may further comprise the aforementioned carbon coating layer on the surface of the primary particles, and since the specific details of the carbon coating layer are the same as those described above, a description of the carbon coating layer is omitted in this section.
[0179] negative electrode
[0180] The negative electrode for a rechargeable lithium battery includes a negative electrode current collector and a layer of negative electrode active material on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material and may optionally further include a binder, a conductive material, or a combination thereof.
[0181] There are no particular restrictions on the negative electrode current collector, as long as the negative electrode current collector is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be a copper foil with a thickness of about 10 μm to about 15 μm.
[0182] Negative electrode active materials include materials capable of reversibly inserting / deintercalating lithium ions, lithium metal, lithium metal alloys, materials capable of doping and dedoping lithium, or transition metal oxides.
[0183] The material capable of reversibly intercalating / deintercalating lithium ions may be a carbon-based negative electrode active material, such as crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be in the form of irregular, flaky, scaly, spherical or fibrous natural graphite or artificial graphite. The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonized product, or calcined coke.
[0184] As the alloy of lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn may be used.
[0185] The material capable of doping and dedoping lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements [excluding Si], Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and may for example be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO₂, a Sn alloy, or a combination thereof.
[0186] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter D of the silicon-carbon composite particles 50 may be, for example, from about 0.5 μm to about 20 μm. According to some embodiments, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surfaces of the silicon particles. The silicon-carbon composite may include secondary particles (core) in which silicon primary particles are assembled (aggregated) and an amorphous carbon coating layer (shell) on the surfaces of the secondary particles. Amorphous carbon may also be present between the silicon primary particles; the silicon primary particles may be coated with amorphous carbon. The secondary particles may be present dispersed in an amorphous carbon matrix.
[0187] The silicon-carbon composite may further include crystalline carbon. The silicon-carbon composite may include: a core including crystalline carbon and silicon particles, and an amorphous carbon coating layer on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon or hard carbon, a mesophase pitch carbonized product, or calcined coke.
[0188] When the silicon-carbon composite includes silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be about 10 wt% to about 50 wt%, and the amount of amorphous carbon may be about 50 wt% to about 90 wt%. In addition, when the composite includes silicon, amorphous carbon and crystalline carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be about 10 wt% to about 70 wt%, the amount of crystalline carbon may be about 1 wt% to about 60 wt%, and the amount of amorphous carbon may be about 15 wt% to about 50 wt%.
[0189] In addition, the thickness of the amorphous carbon coating layer may be about 5 nm to about 100 nm. The average particle diameter D of the silicon particles (primary particles) 50 may be about 10 nm to about 1 μm or about 10 nm to about 200 nm. In the present disclosure, when no additional definition is provided, the average particle diameter D 50 represents the diameter of particles having a cumulative volume of about 50 vol% in the particle size distribution. The silicon particles may exist as elemental silicon, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon may be represented as SiO x (0<x≤2). The atomic ratio of Si:O indicating the oxidation degree may be about 99:1 to about 33:67.
[0190] The Si-based negative electrode active material or Sn-based negative electrode active material may be mixed with the carbon-based negative electrode active material. When a mixture of the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material is used, the mixing ratio may be about 1:99 to about 90:10 by weight.
[0191] Based on 100 wt% of the negative electrode active material layer, the negative electrode active material may be included in an amount of about 90 wt% to about 99.8 wt% or about 94 wt% to about 99 wt%.
[0192] The binder is used to make the negative electrode active material particles adhere well to each other, and is also used to adhere the negative electrode active material to the negative electrode current collector. The binder may be a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0193] The non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0194] Waterborne adhesives may include styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepoxygenated alcohol, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or combinations thereof.
[0195] When an aqueous binder is used as the negative electrode binder, it may further include a cellulose-based compound capable of imparting viscosity. As a cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or their alkali metal salts may be mixed and used. The alkali metal may be Na, K, or Li.
[0196] Dry adhesives can be polymeric materials that can be turned into fibers and can be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.
[0197] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used unless it causes undesirable chemical changes. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0198] Based on 100% by weight of the negative electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the negative electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0199] electrolytes
[0200] The electrolyte used in rechargeable lithium batteries is an electrolyte solution and includes a non-aqueous organic solvent and a lithium salt.
[0201] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of a battery. Non-aqueous organic solvents can be carbonate (carbonate-based) solvents, ester (ester-based) solvents, ether (ether-based) solvents, ketone (ketone-based) solvents, alcohol (alcohol-based) solvents, aprotic solvents, or combinations thereof.
[0202] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butyl carbonate (BC). Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, or caprolactone. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, or tetrahydrofuran. Ketone solvents may include cyclohexanone. Alcohol solvents may include ethanol or isopropanol, and aprotic solvents may include nitriles such as R-CN (where R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups); amides such as dimethylformamide; dioxolane such as 1,3-dioxolane or 1,4-dioxolane; or sulfolane.
[0203] Non-aqueous organic solvents can be used alone or in combination of two or more non-aqueous organic solvents, and when two or more non-aqueous organic solvents are used in combination, the mixing ratio can be appropriately adjusted depending on the expected battery performance, as is widely understood by those skilled in the art.
[0204] When using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.
[0205] Non-aqueous organic solvents may further include aromatic hydrocarbon organic solvents. Carbonate solvents and aromatic hydrocarbon organic solvents may be mixed and used in a volume ratio of about 1:1 to about 30:1.
[0206] The electrolyte solution may further include vinylene carbonate, vinylene carbonate, or ethylene carbonate compounds to improve the cycle life of the rechargeable lithium battery.
[0207] Examples of ethylene carbonate compounds may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0208] Lithium salts dissolved in non-aqueous organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts may include at least one of the following: LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).
[0209] The concentration of lithium salt can range from about 0.1 M to about 2.0 M. When the concentration of lithium salt is within this range, the electrolyte solution has suitable ionic conductivity and viscosity. Therefore, excellent performance can be achieved, and lithium ions can move efficiently.
[0210] diaphragm
[0211] Depending on the type of rechargeable lithium battery, a separator may be present between the positive and negative electrodes. The separator may be made of polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer membrane of two or more layers, and may of course be a hybrid multilayer membrane such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polypropylene three-layer separator, or a polypropylene / polypropylene / polypropylene three-layer separator.
[0212] The diaphragm may include a porous substrate and a coating on one or both surfaces of the porous substrate, comprising organic materials, inorganic materials, or combinations thereof.
[0213] The porous substrate may be a polymer film formed from any of the following polymers: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene ether; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; polytetrafluoroethylene (e.g., Teflon). ® (TEFLON ® Porous substrates may include glass fibers, or composite films comprising polymers and glass fibers.
[0214] The porous substrate may have a thickness of about 1 μm to about 40 μm, for example, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm.
[0215] Organic materials may include (meth)acrylic acid copolymers, which include a first structural unit and a second structural unit derived from (meth)acrylamide, wherein the second structural unit includes at least one structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.
[0216] Inorganic materials may include the following inorganic particles: Al₂O₃, SiO₂, TiO₂, SnO₂, CeO₂, MgO, NiO, CaO, GaO, ZnO, ZrO₂, Y₂O₃, SrTiO₃, BaTiO₃, Mg(OH)₂, boehmite, and combinations thereof, but inorganic materials are not limited to these. The average particle size D of the inorganic particles... 50 It can be about 1 nm to about 2000 nm, for example about 100 nm to about 1000 nm or about 100 nm to about 700 nm.
[0217] Organic and inorganic materials can be mixed in a coating, or coatings containing organic materials and coatings containing inorganic materials can be stacked.
[0218] The coating thickness can be from about 0.5 μm to about 20 μm, for example from about 1 μm to about 10 μm or from about 1 μm to about 5 μm.
[0219] In the following sections, embodiments and comparative examples of the present invention are described. However, the embodiments described below are merely some implementations of the present invention, and the present invention is not limited to the embodiments described below.
[0220] Example 1
[0221] (1) Preparation of composite positive electrode active material
[0222] (Preparation of the active material for the first positive electrode)
[0223] A raw material mixture was prepared by mixing FePO4, as an iron phosphate-based precursor, and Li2CO3, as a lithium raw material, in a molar ratio of 2:1. A carbon raw material was prepared by mixing glucose and polyethylene glycol in a weight ratio of 5:5. Furthermore, 90 wt% of the raw material mixture and 10 wt% of the carbon raw material were mixed to produce a mixture, and distilled water, as a second solvent, was added to the mixture, followed by wet milling to prepare a second slurry. Wet milling was performed using a ball mill. Specifically, approximately 90 wt% of the raw material mixture and approximately 10 wt% of the carbon source material were introduced into a milling vessel with a capacity of approximately 5 L, along with approximately 3 kg of zirconia balls and approximately 2 kg of water, and wet milling was performed by rotating the vessel at approximately 100 rpm for approximately 3 hours. Here, TiO2, as a Ti raw material, was added to the mixture during wet milling, and the amount was adjusted such that Ti accounted for 0.4 mol%, based on the total metals other than lithium in the final lithium iron phosphate-based compound.
[0224] A wet-milled slurry was added to a spray dryer (Büchi Mini SprayDryer B-290) at a rate of 0.5 kg / min and then spray-dried at 200°C to obtain a second dried product. This second dried product was calcined at 750°C for 8 hours to obtain a second calcined product, which was then pulverized into primary particles at 6000 rpm using an air-jet mill to obtain a first positive electrode active material. Through a pulverization process, the second calcined product, comprising lithium iron phosphate-based compounds, was pulverized into a first positive electrode active material in the form of secondary particles from which multiple primary particles agglomerated, instead of agglomerating. The first positive electrode active material has an average particle size of 0.5 μm and LiFe... 0.996 Ti 0.004 PO4 is composed of primary particles.
[0225] (Preparation of the active material for the second positive electrode)
[0226] Li₂CO₃ and Mn₂O₃ were mixed in a molar ratio of 1.02:2.0, and then heated from 25°C to 820°C at a heating rate of 5°C / min under an oxygen atmosphere, and held at 820°C for 8 hours to obtain a calcined product. The obtained calcined product was then sieved through a 325-mesh sieve to prepare the second positive electrode active material. At this point, the second positive electrode active material was in the form of secondary particles formed by the agglomeration of multiple primary particles, with an average particle size of 9 μm, and its composition was Li₂CO₃. 1.02Mn2O4. The secondary particles of the second positive electrode active material are separated into primary particles by a wet milling process performed during the preparation of the composite positive electrode active material as described later, and the separated primary particles subsequently constitute the secondary particles of the composite positive electrode active material prepared by a spray drying process.
[0227] (Preparation of irreversible positive electrode additives)
[0228] As an irreversible positive electrode additive, a lithium iron-based oxide (IZ-2L, manufactured by Dynanonic) was prepared, which has a primary particle form, an average particle size of 5 μm for primary particles, and a composition of Li5FeO4.
[0229] (Preparation of composite positive electrode active material)
[0230] The first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive were mixed at 15 rpm for 30 minutes using a mixer (L5M-A) to produce a mixture. This mixture was then wet-dispersed in ethanol as the first solvent to prepare a first slurry, which was added at 0.5 kg / min to a spray dryer (Büchi Mini Spray Dryer B-290) and then spray-dried at 200°C to obtain a first dried product. Wet milling was then performed using a ball mill. Specifically, approximately 3 kg of zirconia balls, approximately 2 kg of ethanol, and approximately 2 kg of a mixture of the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive were introduced into a milling vessel with a capacity of approximately 5 L, and the vessel was rotated at approximately 50 rpm for approximately 1 hour. During this process, the second positive electrode active material, in the form of secondary particles, separated into primary particles. The first dried product is a composite positive electrode active material in the form of secondary particles, wherein primary particles of the first positive electrode active material, primary particles of the second positive electrode active material, and primary particles of the irreversible positive electrode additive are agglomerated. The first slurry is prepared by mixing the first and second positive electrode active materials at a weight ratio of 80:20, and then adding an irreversible positive electrode additive in an amount of 1.01 parts by weight based on 100 parts by weight of the first and second positive electrode active materials.
[0231] (2) Manufacturing of the positive electrode
[0232] A composite positive electrode active material was prepared by mixing polyvinylidene fluoride as a binder and carbon nanotubes as a conductive material at a weight ratio of 96:2:2 (positive electrode active material: binder: conductive material). This composition was dispersed in N-methylpyrrolidone solvent to prepare a positive electrode active material slurry, which was then coated onto a 15 μm thick Al foil, dried, and compressed to fabricate the positive electrode.
[0233] (3) Manufacturing of rechargeable lithium battery cells
[0234] A negative electrode active material slurry was prepared by dispersing 97.5% by weight graphite as the negative electrode active material, 1.5% by weight carboxymethyl cellulose and 1% by weight styrene-butadiene rubber as binders in distilled water. This slurry was coated onto a 10 μm thick Cu foil, then dried and compressed to fabricate the negative electrode.
[0235] A 10 μm thick polyethylene separator is placed between the positive and negative electrodes to fabricate an electrode assembly, which is then inserted into a housing. An electrolyte is injected into the housing to fabricate a rechargeable lithium-ion battery cell (a pouch cell at the 100 mAh level). The electrolyte is prepared by mixing EC (ethylene carbonate): EMC (ethyl methyl carbonate): DMC (dimethyl carbonate) at a volume ratio of 2:4:4 and dissolving 1.15 M LiPF6 in the mixed solvent.
[0236] Examples 2 to 4
[0237] The composite positive electrode active material, positive electrode and rechargeable lithium battery cell according to Examples 2 to 4 were manufactured in the same manner as in Example 1, except that: in part “(1) Preparation of composite positive electrode active material”, an irreversible positive electrode additive was added to prepare a first slurry based on 100 parts by weight of the first positive electrode active material and the second positive electrode active material in the amount shown in Table 1 (instead of 1.01 parts by weight).
[0238] In Table 1, the amount of irreversible positive electrode additive is calculated based on 100 parts by weight of the first positive electrode active material and the second positive electrode active material, and then rounded to two decimal places.
[0239] Table 1:
[0240]
[0241] Example 5
[0242] The composite positive electrode active material, positive electrode, and rechargeable lithium battery cell according to Example 5 were manufactured in the same manner as in Example 3, except that: in part “(1) Preparation of composite positive electrode active material” of Example 3, a first slurry was added to a spray dryer and then spray dried to obtain a first dried product, which was additionally calcined at 400°C for 8 hours under a nitrogen atmosphere to obtain a first calcined product, and the first calcined product was used as the composite positive electrode active material in part “(2) Manufacturing of positive electrode”.
[0243] The composite positive electrode active material can be referred to as the first product after firing.
[0244] Comparative Example 1
[0245] The positive electrode and rechargeable lithium battery cell were manufactured in the same manner as in Example 1, except that: the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive prepared in part “(1) Preparation of composite positive electrode active material” were simply mixed for 30 minutes at 15 rpm using a mixer (L5M-A), and then used as the positive electrode active material in part “(2) Manufacturing of positive electrode” of Example 1. The first positive electrode active material and the second positive electrode active material were mixed at a weight ratio of 80:20, and the irreversible positive electrode additive was added in an amount of 1.01 parts by weight based on 100 parts by weight of the first positive electrode active material and the second positive electrode active material.
[0246] Evaluation Example 1: Evaluation of Composite Positive Electrode Active Materials
[0247] (1) Porosity evaluation
[0248] The porosity of the composite positive electrode active materials of Examples 1 to 5 was measured, and the results are shown in Table 2. The porosity was obtained by taking scanning electron microscope images of the cross-section of the secondary particles to measure the ratio of the area of the pores in the cross-section of the secondary particles to the cross-sectional area of the secondary particles of each composite positive electrode active material, and the results are shown in Table 2.
[0249] (2) Particle analysis
[0250] The composite positive electrode active material of Example 2 was imaged using a scanning electron microscope image of its cross-section. Figure 5 A scanning electron microscope image showing the cross-section of the composite positive electrode active material of Example 2.
[0251] exist Figure 5In the diagram, within a single composite positive electrode active material particle, black indicates internal pores, and gray indicates the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive. Among those marked in gray, the second positive electrode active material and the irreversible positive electrode additive are particles with a particle size of approximately 2 μm or larger, where particle size refers to the diameter in the case of spherical particles and the square root of the product of the major and minor axes in the case of non-spherical particles, and the first positive electrode active material corresponds to the remaining particles with a particle size of less than approximately 2 μm according to the same standard.
[0252] Reference Figure 5 Multiple first positive electrode active material particles, second positive electrode active material particles, and irreversible positive electrode additive particles agglomerate to form an assembly.
[0253] Similar to Example 2, scanning electron microscope images of the cross-sections of the composite positive electrode active materials of Examples 1 and 3 to 5 were taken. Using the images, the average particle size of the secondary particles, the average particle size of the primary particles of the first positive electrode active material, the arithmetic mean size of the first positive electrode active material, the standard deviation of the first positive electrode active material, and the average particle size of the second positive electrode active material were measured and are shown in Table 2.
[0254] Specifically, the average particle size of the secondary particles was determined as follows: approximately 20 secondary particles were randomly selected from the scanning electron microscope (SEM) image of the composite positive electrode active material, and their particle size (the square root of the product of the diameter in the case of spherical particles and the product of the major and minor axis lengths in the case of non-spherical particles) was measured, and their arithmetic mean was calculated. Furthermore, the average particle size of the primary particles of the first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive was determined as follows: the particle size (the square root of the product of the diameter in the case of spherical particles and the product of the major and minor axis lengths in the case of non-spherical particles) of approximately 20 randomly selected primary particles from the SEM image of the composite positive electrode active material was measured, and their arithmetic mean was calculated. In this case, among the particles in the composite positive electrode active material, particles with a particle size of less than approximately 2 μm were considered as primary particles of the first positive electrode active material as described above, and their arithmetic mean was calculated by measuring their particle size. Meanwhile, particles with a size of 2 μm or larger are considered primary particles of the second positive electrode active material and primary particles of the irreversible positive electrode additive. Their respective particle sizes are measured and their arithmetic mean is calculated by distinguishing particles based on electron microscopy images and energy-dispersive X-ray spectroscopy (EDX) analysis results. Specifically, after obtaining cross-sectional or surface images of the positive electrode using scanning electron microscopy (SEM), EDX analysis is performed on the same field of view. The morphology and diameter of each particle are measured using SEM images, and the distribution of elements such as Mn is identified through EDX analysis. Particles in which Mn is predominantly distributed are identified as primary particles of the second positive electrode active material, while particles in which Mn is not detected or Co is predominantly detected are identified as primary particles of the irreversible positive electrode additive.
[0255] The arithmetic mean size and standard deviation of the first positive electrode active material were calculated as follows: the size of approximately 20 arbitrary particles of the first positive electrode active material was measured from the SEM image of the cross-section of the composite positive electrode active material (the diameter in the case of spherical particles and the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles), and then the arithmetic mean and its standard deviation were calculated.
[0256] (Unlike Examples 1 to 5, in which they were spray-dried to produce a dried product and then fired into an assembly form), Comparative Example 1, in which the first positive electrode active material, the second positive electrode active material and the irreversible positive electrode additive were simply mixed, exhibited the first positive electrode active material, the second positive electrode active material and the irreversible positive electrode additive in a dispersed state, so that the evaluation shown in Table 2 was not necessary.
[0257] Table 2:
[0258]
[0259] Referring to Table 2, it is confirmed that for the composite positive electrode active materials of Examples 1 to 5, the first positive electrode active material is prepared such that it has relatively small and uniform primary particles, and the primary particles together with the primary particles of the second positive electrode active material and the primary particles of the irreversible positive electrode additive form an assembly.
[0260] Evaluation Example 2: Particle Density Evaluation
[0261] The agglomerate density of the (composite) positive electrode active material of Examples 1 to 5 and Comparative Example 1 was determined as follows: 3 g of the (composite) positive electrode active material was placed in a mold, and the (composite) positive electrode active material was held in the mold at 25°C for 30 seconds. The thickness of the agglomerate was measured, and the agglomerate volume was calculated using the agglomerate thickness and the diameter of the mold. The mass of the (composite) positive electrode active material was divided by the calculated volume.
[0262] Evaluation Example 3: Evaluation of Battery Performance
[0263] (1) Evaluation of initial charge / discharge capacity and efficiency
[0264] The rechargeable lithium-ion battery cells of Examples 1 to 5 and Comparative Example 1 were charged at 25°C at a rate of 0.2 C to a battery voltage of 4.45 V and discharged at a rate of 0.2 C to a cutoff voltage of 3.0 V to measure the initial charge / discharge capacity, which was used to calculate the initial efficiency according to Equation 1. The results are shown in Table 3.
[0265] Equation 1 is as follows:
[0266] [Equation 1]
[0267] Initial efficiency [%] = [Discharge capacity in the first cycle / Charge capacity in the first cycle] × 100.
[0268] (2) Average voltage
[0269] The average voltage of the rechargeable lithium battery cells according to Examples 1 to 5 and Comparative Example 1 was measured at 50% SOC (State of Charge) during the initial discharge period, and the results are shown in Table 3.
[0270] (3) Low-temperature capacity evaluation
[0271] The rechargeable lithium-ion battery cells of Examples 1 to 5 and Comparative Example 1 were fully charged to a battery voltage of 4.3 V at a rate of 0.2 C, and then discharged to 3.0 V at a rate of 0.2 C in an atmosphere set to -20°C to measure the low-temperature discharge capacity. The results are shown in Table 3.
[0272] (4) Cyclic life characteristic evaluation
[0273] After initial charging and discharging, the rechargeable lithium battery cells of Examples 1 to 5 and Comparative Example 1 were repeatedly charged at a rate of 0.2 C to a battery voltage of 4.3 V, and then discharged at a rate of 0.2 C to a cutoff voltage of 3.0 V 50 times. The ratio of the discharge capacity of the 50th cycle to the initial discharge capacity was calculated according to Equation 2 below, and the results are shown in Table 3.
[0274] Equation 2 is as follows:
[0275] [Equation 2]
[0276] Cycle lifetime [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100.
[0277] (5) Evaluation of high temperature storage characteristics
[0278] The rechargeable lithium battery cells of Examples 1 to 5 and Comparative Example 1 were charged to 98% SOC at a rate of 0.2 C, and then left to stand at 45°C for 7 days in a high-temperature room to measure capacity retention. The results are shown in Table 3.
[0279] (6) Capacity evaluation per volume
[0280] The capacity per volume of the rechargeable lithium battery cells of Examples 1 to 5 and Comparative Example 1 was measured by multiplying the density by the capacity, and the results are shown in Table 3.
[0281] Table 3:
[0282]
[0283] Referring to Table 3, compared to the rechargeable lithium battery cell of Comparative Example 1 (whose positive electrode active material was prepared by simply mixing a first positive electrode active material, a second positive electrode active material, and an irreversible positive electrode additive), the rechargeable lithium battery cell of Example 1 (whose positive electrode active material was prepared by mixing a first positive electrode active material and a second positive electrode active material in the same weight ratio to generate a mixture and adding an irreversible positive electrode additive to the mixture in an assembled form) showed significantly superior aggregate density, initial discharge capacity, low-temperature discharge capacity, cycle life characteristics, and high-temperature capacity retention. The rechargeable lithium battery cell of Comparative Example 1, which includes a positive electrode active material prepared by simply mixing a first positive electrode active material, a second positive electrode active material, and an irreversible positive electrode additive, lacks sufficient electrochemical reaction between these heterogeneous particles, resulting in particle isolation. This leads to physical connection problems between the heterogeneous particles, resulting in overall deteriorated battery performance and particularly significantly deteriorated high-temperature storage characteristics. Meanwhile, Examples 1 to 4 (whose positive electrode active materials were prepared by adding irreversible positive electrode additives to the mixture in different amounts while maintaining a fixed weight ratio of the first and second positive electrode active materials) showed that as the amount of irreversible positive electrode additives increased, the initial discharge capacity, low-temperature discharge capacity, and capacity per volume improved, although cycle life and high-temperature capacity retention slightly deteriorated. Therefore, Examples 1 to 4 exhibited excellent battery performance.
[0284] Furthermore, compared to Example 3, the rechargeable lithium-ion battery cell including the positive electrode active material of Example 5 (wherein the dried product in the manufacturing process of the composite positive electrode active material of Example 3 was additionally calcined) has been shown to exhibit improved battery performance for rechargeable lithium-ion batteries. The calcined product obtained by additionally calcining the dried product in the assembly formation process is used as the positive electrode active material to further strengthen the bonding between the primary particles of the first positive electrode active material, the primary particles of the second positive electrode active material, and the primary particles of the irreversible positive electrode additive in the dried product, thereby further stabilizing their crystal structure and thus improving the electrochemical characteristics of the composite positive electrode active material for rechargeable lithium-ion batteries.
[0285] Although the invention has been described with respect to what are now considered practical embodiments, this disclosure is not limited to the embodiments described above.
[0286] <Description of representative figure labels>
[0287] 100: Rechargeable lithium battery; 10: Positive electrode
[0288] 11: Positive electrode lead connector 12: Positive electrode terminal
[0289] 20: Negative electrode 21: Negative electrode lead connector
[0290] 22: Negative electrode terminal; 30: Diaphragm
[0291] 40: Electrode assembly; 50: Housing
[0292] 60: Seal 70: Electrode terminal
[0293] 71: Positive electrode connector; 72: Negative electrode connector
Claims
1. A composite positive electrode active material, which is in particulate form, said composite positive electrode active material comprising: The first positive electrode active material includes lithium iron phosphate-based compounds and is in the form of multiple primary particles; The second positive electrode active material includes lithium manganese-based oxide and is in the form of multiple primary particles; and Irreversible positive electrode additives in the form of multiple primary particles. The composite positive electrode active material is in particulate form, which includes the plurality of primary particles of the first positive electrode active material, the plurality of primary particles of the second positive electrode active material, and the plurality of primary particles of the irreversible positive electrode additive.
2. The composite positive electrode active material according to claim 1, wherein the lithium iron phosphate-based compound comprises a compound represented by chemical formula 1, a compound represented by chemical formula 2, or a combination thereof: [Chemical Formula 1] Li a1 Fe (1-x1) M 1 x1 PO4, Where 0.9≤a1≤1.5, 0≤x1≤0.4, and M 1 Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof; and [Chemical Formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4, Where 0.9≤a²≤1.5, 0.1≤x²≤0.9, 0≤y²<0.9, x²+y²<1, and M 2 It is Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.
3. The composite positive electrode active material according to claim 1, wherein, based on the total metals other than lithium in the lithium iron phosphate-based compound, the lithium iron phosphate-based compound comprises Al, Mg, Ti, V or combinations thereof in an amount of 0.1 mol% to 0.5 mol%.
4. The composite positive electrode active material according to claim 1, wherein the arithmetic mean size of the primary particles of the first positive electrode active material is less than or equal to 200 nm, and The standard deviation of the arithmetic mean size of the primary particles of the first positive electrode active material is less than or equal to 100 nm.
5. The composite positive electrode active material according to claim 1, wherein the lithium manganese-based oxide is represented by the following: Li a3 Mn x3 M 3 y3 O 4-b3 X b3 , Where 0.9 ≤ a³ ≤ 1.8, 1.7 ≤ x³ ≤ 2, 0 ≤ y³ ≤ 0.3, 1.9 ≤ x³ + y³ ≤ 2.1, and 0 ≤ b³ ≤ 0.1, M 3 X is Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zr or a combination thereof, and X is F, P, S or a combination thereof.
6. The composite positive electrode active material according to claim 1, wherein the average particle size of the primary particles of the second positive electrode active material is 2 μm to 10 μm.
7. The composite positive electrode active material according to claim 1, wherein the irreversible positive electrode additive comprises lithium iron-based oxide, lithium cobalt-based oxide, lithium nickel-based oxide, or a combination thereof.
8. The composite positive electrode active material according to claim 1, wherein the average particle size of the primary particles of the irreversible positive electrode additive is 2 μm to 10 μm.
9. The composite positive electrode active material according to claim 1, wherein the composite positive electrode active material is in the form of a plurality of secondary particles, and the average particle size of the secondary particles of the composite positive electrode active material is 3 μm to 20 μm.
10. The composite positive electrode active material according to claim 1, wherein, based on 100% by weight of the first positive electrode active material and the second positive electrode active material, the composite positive electrode active material comprises the first positive electrode active material in an amount of 50% by weight to 99% by weight, and The composite positive electrode active material comprises 100% by weight of the first positive electrode active material and the second positive electrode active material, and includes the second positive electrode active material in an amount of 1% to 50% by weight.
11. The composite positive electrode active material according to claim 1, wherein the composite positive electrode active material comprises the irreversible positive electrode additive in an amount of 0.1 parts by weight to 10 parts by weight, based on 100 parts by weight of the first positive electrode active material and the second positive electrode active material.
12. The composite positive electrode active material according to claim 1, wherein the particles of the composite positive electrode active material include pores, and the porosity, expressed as the ratio of the area occupied by the pores to the cross-sectional area of the particles of the composite positive electrode active material, is 10% to 50%.
13. A method for preparing the composite positive electrode active material according to any one of claims 1 to 12, the method comprising: Prepare a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; Prepare a second positive electrode active material, including lithium manganese-based oxides, in the form of secondary particles from which multiple primary particles agglomerate. The first positive electrode active material, the second positive electrode active material, and the irreversible positive electrode additive in the form of primary particles are mixed and wet-milled to prepare a first slurry; as well as The first slurry is added to a spray dryer and the first slurry is spray-dried to prepare a first dried product.
14. The method of claim 13, further comprising, after preparing the first dried product, subjecting the first dried product to firing to prepare a first fired product.
15. A rechargeable lithium battery, including: Positive electrode; negative electrode; and Electrolytes, The positive electrode includes: Positive electrode current collector; and A positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer comprising the composite positive electrode active material according to any one of claims 1 to 12.