Positive electrode active material, method for preparing positive electrode active material, positive electrode slurry and rechargeable lithium battery

By controlling the shape of secondary particles and adding a carbon coating, a lithium iron phosphate-based positive electrode active material with uniform size was synthesized, which solved the problems of insufficient electrical conductivity, energy density and low-temperature characteristics of existing lithium iron phosphate-based positive electrode active materials, and achieved high density, excellent capacity characteristics and cycle life characteristics.

CN123120716APending Publication Date: 2026-11-17SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610665877.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-04-23
Filing Date
2026-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium iron phosphate-based positive electrode active materials are inferior in terms of electrical conductivity, energy density, and low-temperature performance, and are not cost-effective.

Method used

By controlling the geometry of secondary particles, suppressing the growth of primary particle size, and adding a carbon coating, a uniformly sized positive electrode active material is synthesized, forming a secondary particle form in which multiple primary particles agglomerate, including a specific range of chromaticity parameters.

Benefits of technology

It improves the density characteristics, initial charge/discharge capacity and efficiency characteristics, rate capability, low temperature characteristics and cycle life characteristics of the positive electrode active material, while maintaining price competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120716A_ABST
    Figure CN123120716A_ABST
Patent Text Reader

Abstract

This disclosure discloses a positive electrode active material, a method for preparing the positive electrode active material, a positive electrode slurry, and a rechargeable lithium battery. According to some embodiments of this disclosure, the positive electrode active material may be in the form of secondary particles in which a plurality of primary particles can agglomerate, and the positive electrode active material includes a lithium iron phosphate-based compound. The positive electrode active material may have an L value less than or equal to about 30, an R value less than or equal to about 70, a G value less than or equal to about 70, and a B value less than or equal to about 70, as measured by a colorimeter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to positive electrode active materials, methods for preparing positive electrode active materials, positive electrode slurries, and rechargeable lithium batteries. Background Technology

[0002] Portable information devices (such as mobile phones, laptops, or smartphones) or electric vehicles already use rechargeable lithium batteries with high energy density as their power source. Recently, research has been actively underway to use rechargeable lithium batteries with high energy density as a power source or energy storage source for hybrid or electric vehicles.

[0003] To enable large-scale and mass production of rechargeable lithium-ion batteries, the demand for new positive electrode active materials with high performance, safety, and reliability is increasing. Lithium iron phosphate (LiFePO4)-based positive electrode active materials are attracting attention because they are structurally stable, have high heat resistance, and are abundant in terms of raw materials, making them cost-effective.

[0004] However, existing lithium iron phosphate-based positive electrode active materials are poor in terms of electrical conductivity, energy density, and low-temperature performance, and therefore, improvements are needed. Summary of the Invention

[0005] This disclosure provides positive electrode active materials, methods for preparing positive electrode active materials, positive electrode slurries, and rechargeable lithium batteries with improved density characteristics, initial charge / discharge capacity and efficiency characteristics, rate characteristics, low-temperature characteristics, and cycle life characteristics, and is price-competitive.

[0006] The positive electrode active material according to some embodiments of this disclosure may be in the form of secondary particles in which a plurality of primary particles can aggregate, and the positive electrode active material includes a lithium iron phosphate-based compound. The positive electrode active material may have an L value of less than or equal to about 30, an R value of less than or equal to about 70, a G value of less than or equal to about 70, and a B value of less than or equal to about 70, as measured by a colorimeter (colorimeter).

[0007] In some implementations, the L value ranges from about 2 to about 30, the R value ranges from about 20 to about 70, the G value ranges from about 45 to about 70, and the B value ranges from about 30 to about 70.

[0008] In some embodiments, the lithium iron phosphate-based compound may include a compound represented by Chemical Formula 1, a compound represented by Chemical Formula 2, or a combination thereof. Chemical Formula 1 may be as follows:

[0009] [Chemical Formula 1]

[0010] Lia1 Fe (1-x1) M 1 x1 PO4,

[0011] Where 0.9 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4. M 1 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Chemical formula 2 can be as follows:

[0012] [Chemical Formula 2]

[0013] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4,

[0014] Where 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, and x² + y² < 1. M 2 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.

[0015] In some embodiments, based on the total metals in the lithium iron phosphate-based compound excluding lithium, the lithium iron phosphate-based compound may include Al, Mg, Ti, V or combinations thereof in an amount from about 0.1 mol% to about 0.5 mol%.

[0016] In some embodiments, the average particle size of the secondary particles can be from about 3 μm to about 20 μm.

[0017] In some embodiments, the arithmetic mean size of the secondary particles can be from about 3 μm to about 20 μm. The standard deviation of the arithmetic mean size of the secondary particles can be less than or equal to about 2.1 μm.

[0018] In some embodiments, the arithmetic mean size of the primary particles constituting the secondary particles may be less than or equal to about 200 nm. The standard deviation of the arithmetic mean size of the primary particles may be less than or equal to about 100 nm.

[0019] In some embodiments, the secondary particles may include pores, and the porosity (which may be the ratio of the area occupied by pores in the cross-section of the secondary particle to the cross-sectional area of ​​the secondary particle) may be from about 10% to about 50%.

[0020] In some embodiments, the positive electrode active material may further include a carbon coating (coating) on ​​the surface of the secondary particles. Based on 100% by weight of the positive electrode active material, the amount of carbon coating in the positive electrode active material may be from about 1.55% by weight to about 2% by weight.

[0021] In some embodiments, the agglomerate (disc) density of the positive electrode active material may be from about 2.35 g / cc to about 2.5 g / cc.

[0022] A method for preparing a positive electrode active material according to some embodiments of the present disclosure may include: mixing an iron phosphate-based precursor, a lithium raw material, and a carbon raw material in a solvent, and wet-milling the iron phosphate-based precursor, the lithium raw material, and the carbon raw material to prepare a slurry; adding the slurry to a spray dryer and spray-drying the slurry to prepare a dried product; calcining the dried product to prepare a calcined product; and pulverizing the calcined product to obtain the positive electrode active material.

[0023] In some embodiments, adding slurry to a spray dryer may include adding slurry to the spray dryer at an addition rate of less than or equal to about 1 kg / min.

[0024] In some embodiments, spray drying of the slurry to prepare a dried product may include spray drying the slurry at a temperature of about 150°C to about 400°C.

[0025] In some embodiments, pulverizing the calcined product to obtain the positive electrode active material may include pulverizing the calcined product at a pulverization speed of less than or equal to about 2000 rpm.

[0026] In some embodiments, the obtained positive electrode active material may be in the form of secondary particles in which multiple primary particles can agglomerate, the obtained positive electrode active material may include lithium iron phosphate-based compounds, and the obtained positive electrode active material may have an L value of less than or equal to about 30, an R value of less than or equal to about 70, a G value of less than or equal to about 70 and a B value of less than or equal to about 70 as measured by a colorimeter.

[0027] Positive electrode slurries according to some embodiments of this disclosure may include: the positive electrode active material described above; and a solvent, wherein the positive electrode slurry may have a viscosity of less than or equal to about 8000 mPa·s.

[0028] A rechargeable lithium battery according to some embodiments of this disclosure may include a positive electrode, a negative electrode, and an electrolyte. The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the positive electrode active material as described above.

[0029] Positive electrode active materials according to some embodiments may be price-competitive and may have improved density characteristics, initial charge / discharge capacity and efficiency characteristics, rate characteristics, low-temperature characteristics and cycle life characteristics. Attached Figure Description

[0030] Figure 1 This is a schematic perspective view showing a portion of a cylindrical rechargeable lithium battery cut off according to some embodiments of this disclosure.

[0031] Figure 2 This is a cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure.

[0032] Figure 3 and 4 Schematic exploded perspective views of pouch-type rechargeable lithium batteries according to some embodiments of the present disclosure.

[0033] Figure 5 and 6 Each is a scanning electron microscope image of the surface of the positive electrode active material according to Example 1. Detailed Implementation

[0034] Specific embodiments will be described in detail below so that those skilled in the art can readily implement them. However, this disclosure may be embodied in many different forms and is not to be construed as limited to the embodiments set forth herein.

[0035] The terminology used herein is for describing implementation methods and is not intended to limit the invention. Unless the context clearly specifies otherwise, singular expressions include plural expressions.

[0036] As used herein, “combination of” refers to mixtures, laminates, complexes, copolymers, alloys, blends or reaction products of the constituent elements.

[0037] Terms such as “comprising,” “including,” or “having” are intended to specify the presence of the features, quantities, steps, elements, or combinations thereof embodied, but those terms do not preclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.

[0038] In the accompanying drawings, for clarity, the thickness of layers, films, panels, or regions is exaggerated, and the same reference numerals denote the same elements throughout the specification. It will be understood that when an element, such as a layer, film, region, or substrate, is referred to as being "on" another element, it may be directly on said other element, or there may be intermediate elements present. Conversely, when an element is referred to as being "directly on" another element, there are no intermediate elements present.

[0039] In addition, the term "layer" in this article includes not only the geometry formed on the entire surface when viewed from a plan view, but also the geometry formed on a portion of the surface.

[0040] The average particle size can be measured, for example, by a particle size analyzer or by transmission electron microscopy (TEM) or scanning electron microscopy (SEM) images. The average particle size value can also be obtained by measuring using a dynamic light scattering method, performing data analysis, counting the number of particles for each particle size range, and calculating accordingly. In this disclosure, unless otherwise defined, the average particle size D... 50 This can mean the diameter of particles that have a cumulative volume of 50% in the particle size distribution, where the particles are considered (assumed) to be spherical. As used herein, unless otherwise defined, the average particle size refers to a value obtained by measuring the size of approximately 20 randomly selected particles from scanning electron microscope (SEM) images and calculating the arithmetic mean of the sizes of approximately 20 randomly selected particles, where the size of each particle is defined as the diameter in the case of spherical particles and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.

[0041] "Or" will not be interpreted as having an exclusive meaning; for example, "A or B" will be interpreted as including A, B, and A+B.

[0042] The term "metal" is interpreted to include the concepts of common metals, transition metals, and metalloids (semi-metals). As used herein, a "metalloid" refers to an element that possesses properties intermediate between those of metals and nonmetals. Examples of metalloids include, but are not limited to, boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te).

[0043] As used herein, the term "primary particle" refers to the smallest unit particle that is identified as a single particle when observed using a scanning electron microscope (SEM) of the positive electrode active material, where grain boundaries are not clearly identifiable or are substantially not observed. Primary particles are the basic units that constitute secondary particles formed by the aggregation of tens to hundreds of particles, and can exist individually or in a state where a small number (e.g., 20 or fewer) of primary particles are in contact with each other.

[0044] As used herein, the term "secondary particle" refers to an aggregate of primary particles of a given substance (material), and may also be referred to as an assembly (assembly, collection) in this disclosure. Secondary particles have a structure in which primary particles are combined into individual particles (rather than simply physically mixed) through interparticle contact and bonding. When observed using a scanning electron microscope (SEM), secondary particles can be identified as individual particles in which multiple primary particles are aggregated. Such secondary particles are distinguished from simple mixtures in which the corresponding particles are independently dispersed. Secondary particles can be formed by processes such as spray drying.

[0045] Positive electrode active material

[0046] According to some embodiments, the positive electrode active material is in the form of secondary particles in which a plurality of primary particles are agglomerated, wherein the positive electrode active material comprises a lithium iron phosphate-based compound, and the positive electrode active material has an L value less than or equal to about 30, an R value less than or equal to about 70, a G value less than or equal to about 70, and a B value less than or equal to about 70, as measured by a colorimeter. The L, R, G, and B values ​​can be obtained, for example, by obtaining the L, a, and b values ​​in the CIE LAB color coordinates of the positive electrode active material using a commercially available, conventional colorimeter, and then calculating these values ​​using a program such as SpectraMagic. The L, R, G, and B values ​​of the positive electrode active material can be measured in powder form and can be determined based on the white point defined according to the D65 illuminant in the DCI-P3 color space.

[0047] Lithium iron phosphate (LFP)-based compounds, exhibiting excellent structural stability, high heat resistance, and competitive pricing, are attracting attention. However, existing LFP-based compounds suffer from poor electrical conductivity, energy density, and low-temperature performance.

[0048] Therefore, according to some embodiments, the positive electrode active material can improve capacity characteristics by controlling the geometry of secondary particles to suppress the growth of primary particle size and increase the amount of carbon, and by allowing primary particles to grow to a uniform size when the positive electrode active material is synthesized in the form of secondary particles, thereby improving cycle life characteristics. These positive electrode active materials have specific ranges of chromaticity parameter values, and with positive electrode active materials meeting these ranges, high density can be achieved, and for rechargeable lithium batteries, capacity characteristics, charge / discharge efficiency, rate performance, low-temperature performance, and cycle life characteristics can be improved.

[0049] The L value of the positive electrode active material, as measured by a colorimeter, may be less than or equal to about 29, less than or equal to about 28, or less than or equal to about 27, and may be greater than or equal to about 2, greater than or equal to about 5, greater than or equal to about 10, greater than or equal to about 15, greater than or equal to about 20, greater than or equal to about 22, or greater than or equal to about 23, and may, for example, be about 2 to about 30, about 5 to about 30, about 10 to about 30, about 20 to about 30, or about 23 to about 27.

[0050] The R value of the positive electrode active material, as measured by a colorimeter, may be less than or equal to about 69, less than or equal to about 68, less than or equal to about 67, less than or equal to about 66, or less than or equal to about 65, and may be greater than or equal to about 10, greater than or equal to about 20, greater than or equal to about 30, greater than or equal to about 40, greater than or equal to about 45, greater than or equal to about 50, or greater than or equal to about 55, and may, for example, be about 10 to about 70, about 20 to about 70, about 30 to about 70, about 40 to about 70, about 50 to about 70, or about 55 to about 65.

[0051] The G value of the positive electrode active material, as measured by a colorimeter, may be less than or equal to about 69, less than or equal to about 68, less than or equal to about 67, less than or equal to about 65, less than or equal to about 64, less than or equal to about 63, less than or equal to about 62, or less than or equal to about 61.5, and may be greater than or equal to about 10, greater than or equal to about 20, greater than or equal to about 30, greater than or equal to about 40, greater than or equal to about 45, greater than or equal to about 50, greater than or equal to about 55, greater than or equal to about 56, or greater than or equal to about 57, and may, for example, be about 40 to about 70, about 45 to about 65, about 50 to about 65, about 55 to about 65, about 55 to about 63, or about 57 to about 63.

[0052] The B value of the positive electrode active material, as measured by a colorimeter, may be less than or equal to about 69, less than or equal to about 68, less than or equal to about 67, less than or equal to about 65, less than or equal to about 64, less than or equal to about 63, less than or equal to about 62, less than or equal to about 61, less than or equal to about 60, less than or equal to about 59, or less than or equal to about 58, and may be greater than or equal to about 10, greater than or equal to about 20, greater than or equal to about 30, greater than or equal to about 35, greater than or equal to about 40, greater than or equal to about 45, greater than or equal to about 50, greater than or equal to about 51, greater than or equal to about 52, or greater than or equal to about 53, and may, for example, be about 30 to about 70, about 30 to about 65, about 40 to about 65, about 50 to about 65, about 50 to about 60, or about 53 to about 58.

[0053] The L, R, G, and B values ​​of the positive electrode active material, measured by a colorimeter, can be obtained as follows: The L, a, and b values ​​of the positive electrode active material are measured using a colorimeter with color coordinates in the CIE LAB color space, and the R, G, and B values ​​are calculated using these values. When the positive electrode active material has L, R, G, and B values ​​within the above ranges, it can exhibit excellent surface properties, high density, and improved capacity, efficiency, rate capability, low-temperature performance, and cycle life characteristics for rechargeable lithium batteries.

[0054] The positive electrode active material includes lithium iron phosphate-based compounds. Because the positive electrode active material includes lithium iron phosphate-based compounds, it ensures price competitiveness while also exhibiting excellent structural and thermal stability.

[0055] Lithium iron phosphate-based compounds may include, for example, compounds represented by Chemical Formula 1, compounds represented by Chemical Formula 2, or combinations thereof. Chemical Formula 1 is as follows:

[0056] [Chemical Formula 1]

[0057] Li a1 Fe (1-x1) M 1 x1 PO4.

[0058] In chemical formula 1, 0.9 ≤ a1 ≤ 1.5, 0 ≤ x1 ≤ 0.4, and M 1 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a1 ≤ 1.5; for example, 0.90 ≤ a1 ≤ 1.2 or 0.95 ≤ a1 ≤ 1.1. Additionally, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0.001 ≤ x1 ≤ 0.05.

[0059] Chemical formula 2 is as follows:

[0060] [Chemical Formula 2]

[0061] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4.

[0062] In chemical formula 2, 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, x² + y² < 1, and M 2The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a² ≤ 1.5; for example, 0.90 ≤ a² ≤ 1.2 or 0.95 ≤ a² ≤ 1.1. Additionally, 0.1 ≤ x² ≤ 0.9, 0.3 ≤ x² ≤ 0.9 or 0.4 ≤ x² ≤ 0.8, and 0 ≤ y² ≤ 0.4, 0 ≤ y² ≤ 0.3, 0 ≤ y² ≤ 0.2, 0 ≤ y² ≤ 0.1 or 0 ≤ y² ≤ 0.05.

[0063] Lithium iron phosphate-based compounds may include LiFePO4 and LiMn. 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof, but lithium iron phosphate-based compounds are not limited to these.

[0064] Lithium iron phosphate-based compounds may include Al, Mg, Ti, V, or combinations thereof as doping elements, and may include Al, Mg, Ti, V, or combinations thereof in amounts of about 0.1 mol% to about 0.5 mol%, about 0.1 mol% to about 0.4 mol%, about 0.1 mol% to about 0.3 mol% or about 0.2 mol% based on the total metal excluding lithium. In this case, the rate performance and cycle life characteristics of rechargeable lithium batteries can be improved.

[0065] Lithium iron phosphate-based compounds may include Ti, Al, or a combination thereof as doping elements, and based on the total metal excluding lithium, the amount of Ti may be from about 0.1 mol% to about 0.5 mol%, from about 0.1 mol% to about 0.4 mol%, from about 0.1 mol% to about 0.3 mol%, or about 0.2 mol%, and based on the total metal excluding lithium, the amount of Al may be from about 0.1 mol% to about 0.5 mol%. This can improve rate performance and cycle life characteristics for rechargeable lithium batteries.

[0066] M of chemical formula 1 1 And M of chemical formula 2 2The active material may include Al, Mg, Ti, V, or combinations thereof, which improves the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In Formulas 1 and 2, based on the total metal excluding lithium, Al, Mg, Ti, V, or combinations thereof may be included in amounts from about 0.1 mol% to about 0.5 mol%, from about 0.1 mol% to about 0.4 mol%, from about 0.1 mol% to about 0.3 mol%, or about 0.2 mol%, and this improves the cycle life characteristics of the lithium iron phosphate-based positive electrode active material. In chemical formula 1, the following conditions must be met: 0.001 ≤ x1 ≤ 0.005, 0.001 ≤ x1 ≤ 0.004, 0.001 ≤ x1 ≤ 0.003, or x1 = 0.002. Similarly, in chemical formula 2, the following conditions must be met: 0.001 ≤ x2 ≤ 0.005, 0.001 ≤ x2 ≤ 0.004, 0.001 ≤ x2 ≤ 0.003, or x2 = 0.002. Therefore, this can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material in rechargeable lithium batteries.

[0067] The positive electrode active material has a secondary particle form in which multiple primary particles are aggregated. Because the primary particles are tightly aggregated together, the secondary particles can have a spherical or ellipsoidal geometry. The secondary particles can be represented as assemblies. The average particle size of the secondary particles can be, for example, about 3 μm to about 20 μm, about 5 μm to about 18 μm, about 5 μm to about 15 μm, about 5 μm to about 12 μm, about 5 μm to about 10 μm, about 5 μm to about 9 μm, or about 7 μm to about 9 μm. The average particle size of the secondary particles can be obtained by randomly selecting about 20 secondary particles from an electron microscope image of the positive electrode active material, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.

[0068] According to some embodiments, the positive electrode active material may have secondary particles of uniform size, and the primary particles constituting the secondary particles may be small and uniform in size. Therefore, the positive electrode active material exhibits high charge / discharge capacity and excellent cycle life characteristics.

[0069] The arithmetic mean size of secondary particles, measured by SEM images of the surface of the positive electrode active material, can be about 3 µm to about 20 µm, about 5 µm to about 18 µm, about 5 µm to about 15 µm, about 5 µm to about 12 µm, about 5 µm to about 10 µm, about 5 µm to about 9 µm, or about 7 µm to about 9 µm. The standard deviation of the arithmetic mean size of the secondary particles can be less than or equal to about 2.1 μm, less than or equal to about 2.05 μm, less than or equal to about 2 μm, less than or equal to about 1.95 μm, or less than or equal to about 1.9 μm, and can be greater than or equal to about 0 μm, greater than or equal to about 0.5 μm, greater than or equal to about 1 μm, greater than or equal to about 1.5 μm, greater than or equal to about 1.7 μm, greater than or equal to about 1.9 μm, greater than or equal to about 1.95 μm, or greater than or equal to about 2 μm. Additionally, as measured by SEM images, the arithmetic mean size of the primary particles constituting the secondary particles may be less than or equal to about 200 nm, or may be about 10 nm to about 200 nm, about 50 nm to about 200 nm, about 60 nm to about 150 nm, about 70 nm to about 140 nm, about 80 nm to about 120 nm, or about 100 nm. The standard deviation of the arithmetic mean size of the primary particles may be less than or equal to about 100 nm, less than or equal to about 50 nm, or less than or equal to about 30 nm, and may be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 12 nm, greater than or equal to about 15 nm, greater than or equal to about 18 nm, greater than or equal to about 20 nm, greater than or equal to about 22 nm, or greater than or equal to about 24 nm. The arithmetic mean size and standard deviation of the secondary particles can be obtained as follows: Measure the size of approximately 20 random secondary particles in SEM or TEM images of the surface of the positive electrode active material, and calculate the arithmetic mean and standard deviation. The size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. The arithmetic mean size and standard deviation of the primary particles can be obtained as follows: Measure the size of approximately 20 random primary particles in SEM images of the surface of the secondary particles, and calculate the arithmetic mean and standard deviation. The size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. When the arithmetic mean size and standard deviation of both secondary and primary particles meet the above ranges, the positive electrode active material exhibits high uniformity in terms of both secondary and primary particle sizes, thereby improving the agglomeration density of the positive electrode active material and enabling the rechargeable lithium battery to exhibit high initial charge / discharge capacity and excellent cycle life characteristics.

[0070] Secondary particles may include pores, and the porosity (which is the ratio of the area occupied by pores to the cross-sectional area of ​​the secondary particle) may be from about 10% to about 50%, for example from about 10% to about 40%, from about 10% to about 30%, from about 20% to about 30%, or from about 25% to about 30%. Porosity can mean the ratio of the area occupied by pores to the cross-sectional area of ​​the secondary particle within its cross-sectional area. Porosity can be obtained, for example, by cutting the positive electrode active material particles using a focused ion beam (FIB) to obtain a cross-section, and measuring the ratio of the area occupied by pores to the cross-sectional area of ​​the secondary particle within the cross-section of the secondary particle from a scanning electron microscope image of the cross-section using an image analysis program (e.g., Image J). The cross-section of the secondary particle can be obtained by cutting the secondary particle using a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be obtained, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or consistent threshold setting method applied to all samples. The porosity of the secondary particles can be the average of the porosities measured for multiple secondary particles, and can be obtained, for example, by measuring the porosity of at least 20 individual secondary particles and calculating the average porosity of the at least 20 individual secondary particles. If the porosity within the secondary particles meets the above range, the primary particles can fill the spaces between the pores within the secondary particles during positive electrode compression, thereby improving the aggregate density or positive electrode density, and thus improving the capacity characteristics and energy density of the rechargeable lithium battery.

[0071] The positive electrode active material may further include a carbon coating on the surface of the secondary particles, the surface of the primary particles constituting the secondary particles, or both. The carbon coating can improve the electrical conductivity of the positive electrode active material and reduce the resistance of the positive electrode.

[0072] The carbon coating may include amorphous carbon and may be formed using, for example, glucose, sucrose, lactose, starch, oligosaccharides, poly-oligosaccharides (polyoligosaccharides), fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, bitumen-based resins, tar-based resins, or combinations thereof.

[0073] Carbon coatings can be formed by placing carbon raw materials on the surface of positive electrode active material particles and then performing a firing process. Alternatively, carbon raw materials and primary particles can be mixed and fired to form a carbon coating on the surface of the primary particles, and then secondary particles from which the primary particles agglomerate can be prepared through post-processing. Or, carbon raw materials and secondary particles can be mixed and fired to form a carbon coating on the surface of the secondary particles.

[0074] The amount of carbon coating can be greater than or equal to about 1.55% by weight, for example greater than or equal to about 1.6% by weight, greater than or equal to about 1.65% by weight, greater than or equal to about 1.7% by weight, greater than or equal to about 1.75% by weight, or greater than or equal to about 1.8% by weight, based on 100% by weight of the positive electrode active material. There is no particular upper limit to the amount of carbon coating, but it can be, for example, less than or equal to about 2% by weight. The amount of carbon coating can be from about 1.55% by weight to about 2% by weight, from about 1.6% by weight to about 2% by weight, from about 1.65% by weight to about 2% by weight, from about 1.7% by weight to about 2% by weight, from about 1.75% by weight to about 2% by weight, or from about 1.8% by weight to about 2% by weight, based on 100% by weight of the positive electrode active material. The amount of carbon coating can be analyzed, for example, by completely burning the positive electrode active material at a high temperature of about 1200°C to about 1400°C in an oxygen atmosphere to convert the carbon and sulfur in the positive electrode active material into CO2 (or CO) and SO2, respectively. The positive electrode active material is in the form of secondary particles, which are assemblies of primary particles. The secondary particles and the primary particles that constitute them grow uniformly, which reduces the contact area due to the external atmosphere during the firing process. As a result, carbon loss is reduced, and thus the carbon coating (coating) amount can be increased compared to existing lithium iron phosphate-based compounds in the form of single particles.

[0075] The agglomerate density of the positive electrode active material can be greater than or equal to about 2.1 g / cc and can be about 2.1 g / cc to about 2.6 g / cc, about 2.35 g / cc to about 2.5 g / cc, about 2.35 g / cc to about 2.46 g / cc, or about 2.43 g / cc to about 2.46 g / cc. The agglomerate density of the positive electrode active material can be measured as follows: 3 g of the positive electrode active material is placed in a mold, and the positive electrode active material is held in the mold at 25°C for 30 seconds. The thickness of the resulting agglomerates is measured, and the agglomerate volume is calculated using the agglomerate thickness and the diameter of the mold. The mass of the positive electrode active material is then divided by the calculated volume. If the agglomerate density of the positive electrode active material meets the above range, the powder properties can be improved, thereby improving the capacity properties. When the porosity within the secondary particles of the positive electrode active material meets the above range, the agglomerate density of the positive electrode active material can be improved, allowing the primary particles to fill the pores during compression.

[0076] Methods for preparing positive electrode active materials

[0077] A method for preparing a positive electrode active material according to some embodiments includes: mixing an iron phosphate-based precursor, a lithium raw material, and a carbon raw material in a solvent and wet-milling them to prepare a slurry; adding the wet-milled slurry to a spray dryer and spray-drying the wet-milled slurry to prepare a dried product; calcining the dried product to prepare a calcined product; and pulverizing the calcined product to obtain a positive electrode active material.

[0078] Positive electrode active materials, including lithium iron phosphate-based compounds, can be prepared primarily through liquid-phase and solid-phase methods. Liquid-phase methods refer to methods for preparing lithium iron phosphate-based compounds through chemical reactions in a solution phase, such as hydrothermal synthesis, sol-gel methods, and co-precipitation methods. Typically, lithium iron phosphate-based compounds prepared by liquid-phase methods have advantages such as: complete crystal structure, absence of impurity peaks, uniform particle size, and uniform carbon coating on the particle surface. However, liquid-phase methods have problems such as: complex preparation processes, high consumption of lithium raw materials, high cost, and low reaction temperatures for preparing lithium iron phosphate (which easily leads to antisite defects in the material lattice), and difficulty in preparing the final product in the form of secondary particles or assemblies where multiple primary particles agglomerate, such as the positive electrode active materials according to some embodiments. Another disadvantage is that the preparation process does not include a spray drying process, making it impossible to synthesize materials in the form of secondary particles.

[0079] However, according to some embodiments, the positive electrode active material is prepared by a type of solid-phase method that reacts the raw materials in a solid state, and by applying the above preparation method, it has the form of secondary particles in which a plurality of primary particles agglomerate and can meet the range of the above-mentioned colorimetric parameters, and the primary particles grow to a uniform size, and the size of the secondary particles can also be controlled to be uniform.

[0080] Preparation of slurry

[0081] A method for preparing a positive electrode active material may include a process of mixing an iron phosphate-based precursor, a lithium raw material, and a carbon raw material in a solvent and wet-milling the iron phosphate-based precursor, lithium raw material, and carbon raw material in the solvent to prepare a slurry. The preparation of the slurry may include: mixing the iron phosphate-based precursor and the lithium raw material to prepare a raw material mixture; preparing the carbon raw material; mixing the raw material mixture and the carbon raw material; adding a solvent; and wet-milling to prepare the slurry. The weight ratio of the raw material mixture to the carbon raw material is not particularly limited, but may be, for example, about 5:5 to about 99:1, about 6:4 to about 99:1, about 7:3 to about 99:1, about 8:2 to about 99:1, or about 9:1 to about 99:1.

[0082] Ferric phosphate precursors can be ferric phosphate precursors such as ferric phosphate (FePO4) and ferric phosphate (II) (Fe3(PO4)2), formed by adding phosphoric raw materials such as phosphoric acid (H3PO4), ammonium dihydrogen phosphate (NH4H2PO4), diammonium hydrogen phosphate ((NH4)2HPO4), or trisodium phosphate (Na3PO4) to iron raw materials such as ferric oxide (Fe2O3), ferric oxalate (FeC2O4), or ferric hydroxide (Fe(OH)3). Alternatively, they can be ferric manganese phosphate precursors formed by further adding manganese raw materials such as manganese oxide (manganese oxide), manganese carbonate, manganese sulfate, or manganese nitrate to ferric phosphate precursors. Ferric phosphate precursors can be used without limitation, provided that the ferric phosphate precursor is a known material for solid-phase reactions.

[0083] Lithium raw materials may be, for example, Li2CO3, LiOH, their hydrates, their hydrides, or combinations thereof.

[0084] Carbon raw materials may include glucose, sucrose, lactose, starch, oligosaccharides, poly-oligosaccharides, fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, pitch resins, tar resins, or combinations thereof. For example, a mixture of glucose and polyethylene glycol may be used as a carbon raw material, and there is no specific limitation on the mixing weight ratio, but it may be, for example, about 10:90 to about 90:10, about 20:80 to about 80:20, about 30:70 to about 70:30, about 40:60 to about 60:40, or about 50:50.

[0085] Wet milling is performed by adding and mixing a solvent, and any one of ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), tetraethylene glycol (TetraEG), propylene glycol (PG), polyethylene glycol (PEG), polypropylene glycol (PPG), ethanol, water, and acetone can be used as a solvent. Alternatively, polyol solvents that induce a reducing atmosphere can be used alone or in mixtures with water, acetone, or ethanol.

[0086] Wet grinding can be performed using bead mills, ball mills, vibratory mills, or colloid mills. In some embodiments, wet grinding can be performed using a ball milling method utilizing zirconia balls, wherein wet grinding is carried out by rotating the grinding vessel at a rotational speed of about 50 rpm to about 2000 rpm for about 1 hour to about 10 hours.

[0087] When preparing the slurry by wet milling, raw materials including Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof may be further added to the slurry. Raw materials including Al, Mg, Mn, Ti, V, or combinations thereof may be added. Raw materials including Al, Mg, Ti, V, or combinations thereof as doping elements may be further added, and based on the total metal excluding lithium in the lithium iron phosphate-based compound of the final positive electrode active material, Al, Mg, Ti, V, or combinations thereof may be added in amounts of about 0.1 mol% to about 0.5 mol%, about 0.1 mol% to about 0.4 mol%, about 0.1 mol% to about 0.3 mol% or about 0.2 mol%. Ti-containing raw materials can be further added to the slurry, and the amount of Ti can be added to about 0.1 mol% to about 0.5 mol%, about 0.1 mol% to about 0.4 mol%, about 0.1 mol% to about 0.3 mol% or about 0.2 mol% based on the total metal excluding lithium in the final positive electrode active material. Therefore, rate performance and cycle life characteristics can be improved for rechargeable lithium batteries.

[0088] Preparation of dried products

[0089] Methods for preparing positive electrode active materials may include a process of adding a wet-milled slurry to a spray dryer and spray-drying the wet-milled slurry to prepare a dried product.

[0090] A wet-milled slurry can be injected into a spray dryer and sprayed to produce droplets (droplets) containing a uniform desired composition. The formed droplets can then be dried to produce a dried product.

[0091] Spray dryers may include ultrasonic spray devices, single-fluid and dual-fluid air nozzle spray devices, ultrasonic nozzle spray devices, filter expansion droplet generators (FEAG), and disc droplet generators, or any known spray dryer may be used without limitation. Dual-fluid air nozzle spray devices may be used in spray dryers.

[0092] The amount of slurry added may vary depending on the spray dryer, but can be adjusted appropriately. For example, at a blower speed of about 50 Hz and an addition pressure of about 0.5 MPa, the slurry addition rate may be less than or equal to about 1 kg / min, for example less than about 1 kg / min, less than or equal to about 0.9 kg / min, less than or equal to about 0.8 kg / min, less than or equal to about 0.7 kg / min, less than or equal to about 0.6 kg / min, or less than or equal to about 0.5 kg / min, and greater than or equal to about 0.01 kg / min, greater than or equal to about 0.05 kg / min, greater than or equal to about 0.1 kg / min, greater than or equal to about 0.15 kg / min, greater than or equal to about 0.2 kg / min, greater than or equal to about 0.3 kg / min, or greater than or equal to about 0.4 kg / min. The slurry addition rate is a value converted based on the solid content (solid contents) and is defined as the amount of slurry supplied per minute (min) based on the mass of the solid content (solid contents) in the slurry. When the slurry addition rate to the spray dryer meets the above range, secondary particles consisting of primary particles of uniform size can be produced, and the average size of the primary particles can be adjusted to be less than or equal to about 200 nm. The size of the secondary particles can also be uniformly controlled, and positive electrode active materials exhibiting the above colorimetric values ​​can be prepared.

[0093] Spray drying can be carried out at a temperature greater than or equal to about 100°C, for example at about 150°C to about 400°C, about 150°C to about 300°C, about 200°C to about 300°C, or about 200°C to about 250°C to dry the components and evaporate the solvent.

[0094] Preparation of calcined products

[0095] Methods for preparing positive electrode active materials may include processes for preparing calcined products, which can be achieved by calcining dried products.

[0096] Firing can be carried out under vacuum or an inert gas and at temperatures of about 700°C to about 1000°C, for example, about 725°C to about 900°C or about 750°C to about 800°C. The inert gas can be argon or nitrogen. The calcined product can be in the form of secondary particles comprising agglomerates of multiple primary particles including a lithium iron phosphate-based compound, and the secondary particles may be non-uniform (e.g., in size) compared to the obtained positive electrode active material described later, but the characteristics of the primary particles included in the calcined product and the primary particles included in the positive electrode active material described later may be the same.

[0097] Obtaining positive electrode active material

[0098] Methods for preparing positive electrode active materials may include a process of pulverizing a calcined product to obtain the positive electrode active material. This pulverization process ensures that the secondary particles of the calcined product are uniform (e.g., in terms of size).

[0099] The grinding can be carried out using equipment such as a jet mill, ball mill, bead mill, or sand mill, and there are no restrictions on the use of known equipment.

[0100] During the above pulverization process, pulverization can be carried out under relatively mild conditions to ensure uniform secondary particle size (e.g., in terms of size) of the calcined product. For example, pulverization can be carried out at pulverization speeds of less than or equal to about 2000 rpm, such as less than or equal to about 1900 rpm, less than or equal to about 1800 rpm, less than or equal to about 1700 rpm, less than or equal to about 1600 rpm, or less than or equal to about 1500 rpm and greater than or equal to about 100 rpm, greater than or equal to about 300 rpm, greater than or equal to about 500 rpm, greater than or equal to about 700 rpm, greater than or equal to about 900 rpm, greater than or equal to about 1000 rpm, greater than or equal to about 1200 rpm, or greater than or equal to about 1400 rpm. Pulverization can also be carried out at pulverization speeds of, for example, about 100 rpm to about 2000 rpm, about 500 rpm to about 2000 rpm, or about 1000 rpm to about 2000 rpm. If the grinding speed meets the above range during grinding, a positive electrode active material in the form of secondary particles from which multiple primary particles agglomerate can be obtained, and a positive electrode active material in which the secondary particles have a uniform particle size can be obtained. If the grinding speed is greater than about 2000 rpm, the secondary particles can be ground and separated in the form of nanoparticles, rather than forming assemblies in the form of secondary particles from which multiple primary particles agglomerate. Therefore, the colorimetric parameter values ​​of the positive electrode active material described below may not be met, and even if the same amount of carbon raw material is added, the amount of carbon retained in the final positive electrode active material may be reduced.

[0101] The obtained positive electrode active material can be in the form of secondary particles formed by the agglomeration of multiple primary particles. The obtained positive electrode active material may include lithium iron phosphate-based compounds, and may have an L value of less than or equal to about 30, an R value of less than or equal to about 70, a G value of less than or equal to about 70, and a B value of less than or equal to about 70, as measured by a colorimeter. Depending on the pulverization process, the secondary particles may become more uniform. In the obtained positive electrode active material, the average particle size of the secondary particles may be from about 3 μm to about 20 μm. The obtained positive electrode active material can be described in the same manner as the positive electrode active material described above, and therefore the description of the obtained positive electrode active material is omitted below.

[0102] The positive electrode active material obtained by the above preparation method can ensure a rechargeable lithium battery with price competitiveness and improved density characteristics, initial charge / discharge capacity and efficiency characteristics, rate characteristics, low temperature characteristics and cycle life characteristics.

[0103] Positive electrode paste

[0104] Some embodiments provide a positive electrode slurry comprising the above-described positive electrode active material and a solvent, wherein the positive electrode slurry has a viscosity less than or equal to about 8000 mPa·s. The positive electrode slurry can be prepared by dispersing the positive electrode active material in a solvent, although the preparation method is not limited thereto.

[0105] The viscosity of the aforementioned positive electrode slurry may be, for example, less than or equal to about 7,500 mPa·s, less than or equal to about 7,000 mPa·s, less than or equal to about 6,500 mPa·s, less than or equal to about 6,000 mPa·s, less than or equal to about 5,500 mPa·s, less than or equal to about 5,000 mPa·s, or less than or equal to about 4,500 mPa·s, and may be greater than or equal to about 1,000 mPa·s, greater than or equal to about 2,000 mPa·s, greater than or equal to about 3,000 mPa·s, or greater than or equal to about 3,500 mPa·s. The viscosity of the positive electrode slurry can be approximately 1000 mPa·s to approximately 8000 mPa·s, approximately 2000 mPa·s to approximately 7000 mPa·s, approximately 3000 mPa·s to approximately 6000 mPa·s, approximately 3000 mPa·s to approximately 5000 mPa·s, or approximately 3500 mPa·s to approximately 4500 mPa·s. The viscosity of the positive electrode slurry can be measured at 25°C with a sample volume of 3 g using a Brookfield rotational viscometer at 20 rpm. If the viscosity of the positive electrode slurry meets the above range, the coating process can be more efficient and the stability and consistency of the process can be improved. Because the positive electrode active material can be described in the same way as described above, the description of the positive electrode active material is omitted below.

[0106] N-methylpyrrolidone (NMP), acetone, or water can be used as solvents, but the solvent is not limited to these. Known solvents can be used as solvents.

[0107] In addition to the positive electrode active material, the positive electrode paste may optionally further include a binder, a conductive material, or a combination thereof. Specific details regarding the binder and conductive material are described below for the positive electrode active material layer.

[0108] Rechargeable lithium batteries

[0109] A rechargeable lithium battery according to some embodiments includes: a positive electrode; a negative electrode; and an electrolyte, wherein the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the aforementioned positive electrode active material. A rechargeable lithium battery may include a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte.

[0110] According to some embodiments, rechargeable lithium batteries can have generally improved battery performance by including a positive electrode containing the aforementioned positive electrode active material, and specifically, can have improved low-temperature capacity and cycle life characteristics.

[0111] The rechargeable lithium batteries described above may have improved low-temperature capacity, such that the discharge capacity at low temperatures (e.g., about -20°C) is greater than or equal to about 80 mAh / g. The low-temperature discharge capacity of the rechargeable lithium batteries may be greater than or equal to about 85 mAh / g, greater than or equal to about 90 mAh / g, or greater than or equal to about 95 mAh / g. The low-temperature discharge capacity of the rechargeable lithium battery may refer to the ratio of the battery's initial discharge capacity to the weight of the positive electrode active material, and may be measured according to the methods described in the examples below.

[0112] Furthermore, when a rechargeable lithium-ion battery undergoes an initial charge / discharge cycle of charging and discharging at a 0.2C rate, followed by repeating this cycle 50 or more times at a 1C rate, and the ratio of the discharge capacity of the 50th cycle to the initial discharge capacity is calculated according to Equation 2 below (cycle life), the cycle life of the rechargeable lithium-ion battery can be improved to 98% or greater, indicating improved cycle life characteristics for rechargeable lithium-ion batteries. The cycle life of the rechargeable lithium-ion battery can be greater than or equal to approximately 98.5%, greater than or equal to approximately 98.7%, greater than or equal to approximately 98.9%, greater than or equal to approximately 99%, or greater than or equal to approximately 99.5%.

[0113] [Equation 2]

[0114] Cycle life [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100

[0115] Rechargeable lithium batteries can be categorized into cylindrical, prismatic, pouch, or coin-shaped geometries. Figure 1 This is a schematic diagram of a cylindrical rechargeable lithium battery cut along a vertical axis and an electrode assembly 40 extending from the cylindrical rechargeable lithium battery, according to some embodiments of the present disclosure. Figure 2 This is a cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure. Figure 3 and 4Each is a schematic exploded perspective view of a pouch-type rechargeable lithium battery. The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed in the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown).

[0116] The rechargeable lithium battery 100 may include a seal 60 of the sealed housing 50, such as Figure 1 As shown. Additionally, in Figure 2 The rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. The rechargeable lithium battery 100 may include electrode connectors 70, which serve as electrical paths for conducting current generated in the electrode assembly 40 to the outside. The electrode connectors 70 may be as follows: Figure 4 The positive electrode terminal 71 and the negative electrode terminal 72 can be set in the same direction as in the middle, or they can be set in the same direction as in the middle. Figure 3 It is set in the opposite direction as in the middle.

[0117] positive electrode

[0118] The positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the above-mentioned positive electrode active material. According to some embodiments, the positive electrode can ensure price competitiveness by including the above-mentioned positive electrode active material, and can have improved density characteristics, initial charge / discharge capacity and efficiency characteristics, rate performance, low temperature characteristics, and cycle life characteristics.

[0119] There are no particular restrictions on the positive electrode current collector, as long as it is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be an aluminum foil or stainless steel foil with a thickness of about 10 μm to about 15 μm.

[0120] The positive electrode active material layer includes the aforementioned positive electrode active material. Specific details of the positive electrode active material can be described in the same manner as described above, and therefore those details are omitted below.

[0121] Based on a 100% by weight positive electrode active material layer, the amount of positive electrode active material may be about 60% by weight to about 99.9% by weight, about 70% by weight to about 99.8% by weight, about 80% by weight to about 99% by weight, or about 90% by weight to about 98% by weight.

[0122] The positive electrode active material layer may optionally further include a binder, a conductive material, or a combination thereof.

[0123] The binder can be used to ensure good adhesion between positive electrode active material particles and also to ensure good adhesion of the positive electrode active material to the current collector. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide (polymers containing ethylene oxide), polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, or nylon, but the binder is not limited to these.

[0124] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes in the battery. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0125] In the positive electrode active material layer, based on 100% by weight of the positive electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the positive electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.

[0126] In addition to the components mentioned above, the positive electrode active material layer may further include other positive electrode active materials without prejudice to the purpose of this disclosure, or may further include irreversible positive electrode additives.

[0127] In addition to the aforementioned positive electrode active material, the positive electrode active material layer may further include a positive electrode active material in the form of primary particles comprising the aforementioned lithium iron phosphate-based compound. In this document, the primary particle form of the positive electrode active material comprising the lithium iron phosphate-based compound can refer to unassembled and separated primary particles of the lithium iron phosphate-based compound within the positive electrode active material, and the arithmetic mean size of the primary particles is as described above and will not be repeated here. The inclusion of the aforementioned primary particle form of the lithium iron phosphate-based compound in the positive electrode active material means that it does not exist in an assembled form by agglomeration with the aforementioned positive electrode active material, but rather exists in a non-agglomerated state by separation from each other.

[0128] When further comprising a positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles, the weight ratio of the positive electrode active material in the form of secondary particles to the positive electrode active material in the form of primary particles comprising a lithium iron phosphate-based compound can be from about 1:9 to about 9:1, and can be appropriately added depending on the purpose. The positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles may further comprise the aforementioned carbon coating on the surface of the primary particles, and since the specific details of the carbon coating are the same as described above, they are omitted below.

[0129] Irreversible positive electrode additives are compounds that act as sacrificial positive electrodes, compensating for the irreversible conversion of Li that no longer participates in the charging / discharging reaction by participating in the formation of an SEI (solid electrolyte interphase) film on the surface of the negative electrode during charging / discharging. Irreversible positive electrode additives are compounds that decompose during the formation process to provide Li and do not participate in subsequent charging / discharging processes. By adding such irreversible positive electrode additives, consumed lithium can be replenished, thereby compensating for lithium loss and improving the energy density, cycle life, and stability of rechargeable lithium batteries.

[0130] Irreversible positive electrode additives may include lithium iron-based oxides, lithium cobalt-based oxides, lithium nickel-based oxides, or combinations thereof.

[0131] The lithium iron-based oxide can be Li5FeO4, LiFeO2, LiFe5O8 or a combination thereof, and among these, the use of Li5FeO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and thus greatly achieve the effect of an irreversible positive electrode additive.

[0132] The lithium cobalt-based oxide can be Li6CoO4, and the use of Li6CoO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium and thus greatly achieve the effect of an irreversible positive electrode additive.

[0133] The lithium nickel-based oxide can be Li2NiO2, and the use of Li2NiO2 can provide a large amount of lithium during the formation process, which can compensate for a large amount of irreversible lithium and thus greatly achieve the effect of an irreversible positive electrode additive.

[0134] The average particle size D of the irreversible positive electrode additive 50 There are no particular limitations, but it can be, for example, about 0.5 μm to about 20 μm, about 0.5 μm to about 10 μm, about 0.5 μm to about 5 μm, or about 0.5 μm to about 3 μm.

[0135] negative electrode

[0136] A negative electrode for a rechargeable lithium battery includes a negative electrode current collector and a negative electrode active material layer on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, and may optionally further include a binder, a conductive material, or a combination thereof.

[0137] The negative electrode current collector is not particularly limited as long as it has electrical conductivity and does not cause undesired chemical changes in the rechargeable lithium battery, and may be a copper foil having a thickness of about 10 μm to about 15 μm.

[0138] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0139] The material capable of reversibly intercalating / deintercalating lithium ions may be a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon may be natural graphite or artificial graphite having an irregular, sheet, flake, spherical, or fibrous geometry. The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonized product, or calcined coke.

[0140] As the alloy of lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.

[0141] The material capable of doping and dedoping lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements [other than Si], Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and may for example be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO₂, a Sn alloy, or a combination thereof.

[0142] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter D of the silicon-carbon composite particles 50may be, for example, from about 0.5 μm to about 20 μm. According to some embodiments, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surfaces of the silicon particles. The silicon-carbon composite may include secondary particles (core) in which silicon primary particles are assembled (aggregated) and an amorphous carbon coating (shell) on the surfaces of the secondary particles. Amorphous carbon may also be present between the silicon primary particles, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be present dispersed in an amorphous carbon matrix.

[0143] The silicon-carbon composite may further include crystalline carbon. The silicon-carbon composite may include: a core comprising crystalline carbon and silicon particles, and an amorphous carbon coating on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon, hard carbon, mesophase pitch carbonized product, or calcined coke.

[0144] When the silicon-carbon composite includes silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be from about 10 wt% to about 50 wt%, and the amount of amorphous carbon may be from about 50 wt% to about 90 wt%. In addition, when the composite includes silicon, amorphous carbon and crystalline carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be from about 10 wt% to about 70 wt%, the amount of crystalline carbon may be from about 1 wt% to about 60 wt%, and the amount of amorphous carbon may be from about 15 wt% to about 50 wt%.

[0145] In addition, the thickness of the amorphous carbon coating may be from about 5 nm to about 100 nm. The average particle diameter D of the silicon particles (primary particles) 50 may be from about 10 nm to about 1 μm or from about 10 nm to about 200 nm. The silicon particles may exist as elemental silicon, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon may be represented as SiO x (0<x≤2). The atomic ratio of Si:O, which indicates the degree of oxidation, may be from about 99:1 to about 33:67. As used herein, when no other definition is provided, the average particle diameter D 50 refers to the diameter of particles at a cumulative volume of about 50 vol% in the particle size distribution, and this value may be calculated based on the assumption that the particles are spherical.

[0146] The Si-based negative electrode active material or Sn-based negative electrode active material may be mixed with the carbon-based negative electrode active material. When a mixture of the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material is used, the mixing ratio may be from about 1:99 to about 90:10 by weight.

[0147] The negative electrode active material may be included in an amount of about 90 wt% to about 99.8 wt% or about 94 wt% to about 99 wt%, based on 100 wt% of the negative electrode active material layer.

[0148] The binder is used to ensure good adhesion between the particles of the negative electrode active material, and also to ensure adhesion of the negative electrode active material to the negative electrode current collector. The binder may be a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.

[0149] Non-aqueous adhesives may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or combinations thereof.

[0150] Waterborne adhesives may include styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepoxygenated alcohol, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or combinations thereof.

[0151] When an aqueous binder is used as the negative electrode binder, it may further include a cellulose-based compound capable of imparting viscosity. As a cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or their alkali metal salts may be mixed and used. The alkali metal may be Na, K, or Li.

[0152] Dry adhesives can be polymeric materials that can be turned into fibers and can be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.

[0153] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used unless it causes undesirable chemical changes. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, or aluminum and silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0154] Based on 100% by weight of the negative electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the negative electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.

[0155] electrolytes

[0156] The electrolyte used in rechargeable lithium batteries is an electrolyte solution and includes a non-aqueous organic solvent and a lithium salt.

[0157] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of a battery. Non-aqueous organic solvents can be carbonate (carbonate-based) solvents, ester (ester-based) solvents, ether (ether-based) solvents, ketone (ketone-based) solvents, alcohol (alcohol-based) solvents, aprotic solvents, or combinations thereof.

[0158] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butyl carbonate (BC). Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, or caprolactone. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, or tetrahydrofuran. Ketone solvents may include cyclohexanone. Alcohol solvents may include ethanol or isopropanol, and aprotic solvents may include nitriles such as R-CN (where R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups); amides such as dimethylformamide; dioxolane such as 1,3-dioxolane or 1,4-dioxolane; or sulfolane.

[0159] Non-aqueous organic solvents can be used alone or in combination of two or more non-aqueous organic solvents, and when two or more non-aqueous organic solvents are used in combination, the mixing ratio can be appropriately adjusted depending on the expected battery performance, as is widely understood by those skilled in the art.

[0160] When using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.

[0161] Non-aqueous organic solvents may further include aromatic hydrocarbon organic solvents. Carbonate solvents and aromatic hydrocarbon organic solvents may be mixed and used in a volume ratio of about 1:1 to about 30:1.

[0162] The electrolyte solution may further include vinylene carbonate, vinylene carbonate, or ethylene carbonate compounds to improve the cycle life of rechargeable lithium batteries.

[0163] Examples of ethylene carbonate compounds may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.

[0164] Lithium salts dissolved in non-aqueous organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts may include at least one of the following: LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).

[0165] The concentration of lithium salt can range from about 0.1 M to about 2.0 M. When the concentration of lithium salt is within this range, the electrolyte solution has suitable ionic conductivity and viscosity. Therefore, excellent performance can be achieved, and lithium ions can move efficiently.

[0166] diaphragm

[0167] Depending on the type of rechargeable lithium battery, a separator may be present between the positive and negative electrodes. The separator may be made of polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer membrane of two or more layers, and may of course be a hybrid multilayer membrane such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polypropylene three-layer separator, or a polypropylene / polypropylene / polypropylene three-layer separator.

[0168] The diaphragm may include a porous substrate and a coating on one or both surfaces of the porous substrate, comprising organic materials, inorganic materials, or combinations thereof.

[0169] The porous substrate may be a polymer film formed from any of the following polymers: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene ether; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; polytetrafluoroethylene (e.g., Teflon). ® (TEFLON ® Porous substrates may include glass fibers or composite films of polymers and glass fibers.

[0170] The porous substrate may have a thickness of about 1 μm to about 40 μm, for example, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm.

[0171] Organic materials may include (meth)acrylic acid copolymers, which include a first structural unit and a second structural unit, wherein the first structural unit is derived from (meth)acrylamide, and the second structural unit includes at least one structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.

[0172] Inorganic materials may include the following inorganic particles: Al₂O₃, SiO₂, TiO₂, SnO₂, CeO₂, MgO, NiO, CaO, Ga₂O₃, ZnO, ZrO₂, Y₂O₃, SrTiO₃, BaTiO₃, Mg(OH)₂, boehmite, and combinations thereof, but inorganic materials are not limited to these. The average particle size D of the inorganic particles... 50 It can be about 1 nm to about 2000 nm, for example about 100 nm to about 1000 nm or about 100 nm to about 700 nm.

[0173] Organic and inorganic materials can be mixed in a coating, or coatings containing organic materials and coatings containing inorganic materials can be stacked.

[0174] The coating thickness can be from about 0.5 μm to about 20 μm, for example from about 1 μm to about 10 μm or from about 1 μm to about 5 μm.

[0175] The following describes embodiments and comparative examples of the present invention. However, the embodiments described below are merely some implementations of the present invention, and the present invention is not limited to the embodiments described below.

[0176] Example 1

[0177] (1) Preparation of positive electrode active material

[0178] A raw material mixture was prepared by mixing FePO4, as an iron phosphate-based precursor, and Li2CO3, as a lithium raw material, in a molar ratio of 2:1. A carbon raw material was prepared by mixing glucose and polyethylene glycol in a weight ratio of 5:5. Subsequently, 90 wt% of the raw material mixture and 10 wt% of the carbon raw material were mixed, and then wet-milled to prepare a slurry by adding water as a solvent to the mixture of the raw material mixture and the carbon raw material. Wet milling was carried out using a ball mill apparatus. Specifically, approximately 90 wt% of the raw material mixture and approximately 10 wt% of the carbon raw material mixture were introduced together with approximately 3 kg of zirconia balls and approximately 2 kg of water into a milling vessel with a capacity of approximately 5 L, and wet milling was performed by rotating the vessel at a rotational speed of approximately 100 rpm for approximately 3 hours. During wet milling, TiO2 was used as the Ti raw material, and its amount was adjusted such that Ti accounted for 0.2 mol% based on the total metal excluding lithium in the finally obtained lithium iron phosphate-based compound.

[0179] The wet-milled slurry was added at a rate of 0.5 kg / min to a spray dryer (Büchi Mini SprayDryer B-290) and then spray-dried at 200°C to form a dried product, which was then calcined at 750°C for 8 hours to obtain a calcined product. The calcined product comprises a lithium iron phosphate-based compound in the form of secondary particles from which multiple primary particles agglomerate.

[0180] The positive electrode active material was prepared by pulverizing the calcined product at 1500 rpm using an air jet mill. The positive electrode active material contained lithium iron phosphate-based compounds (LiFe) in the form of secondary particles consisting of multiple primary particle agglomerations. 0.998 Ti 0.002 PO4).

[0181] (2) Manufacturing of the positive electrode

[0182] A positive electrode active material composition was prepared by mixing polyvinylidene fluoride (PVDF) as a binder and carbon nanotubes as a conductive material at a weight ratio of 96:2:2 (positive electrode active material: binder: conductive material). This composition was dispersed in N-methylpyrrolidone solvent to prepare a positive electrode slurry, which was then coated onto a 15 μm thick Al foil, dried, and compressed to fabricate the positive electrode.

[0183] (3) Manufacturing of rechargeable lithium battery cells

[0184] A negative electrode active material slurry was prepared by dispersing 97.5% by weight graphite as the negative electrode active material, 1.5% by weight carboxymethyl cellulose and 1% by weight styrene-butadiene rubber as binders in distilled water. This slurry was coated onto a 10 μm thick Cu foil, then dried and compressed to fabricate the negative electrode.

[0185] An electrode assembly was fabricated by placing a 10 μm thick polyethylene separator between the positive and negative electrodes, inserting it into a housing, and injecting the electrolyte into the housing to fabricate a rechargeable lithium-ion battery cell (a pouch cell at the 100 mAh level). The electrolyte was prepared by mixing EC (ethylene carbonate): EMC (ethyl methyl carbonate): DMC (dimethyl carbonate) in a volume ratio of 2:4:4 and dissolving 1.15 M LiPF6 in the mixed solvent.

[0186] Examples 2 to 4 and Comparative Examples 1 to 4

[0187] The positive electrode active materials, positive electrodes, and rechargeable lithium battery cells of Examples 2 to 4 and Comparative Examples 1 to 4 were manufactured in essentially the same manner as in Example 1, except that in “(1) Preparation of Positive Electrode Active Material” of Example 1, the slurry addition rate and temperature during spray drying and the pulverization rate of the calcined product were varied as shown in Table 1. In Table 1, the slurry addition rate during spray drying is based on the amount of lithium iron phosphate-based compound, which is expressed as the weight (kg) of lithium iron phosphate-based compound added per minute.

[0188] Table 1:

[0189]

[0190] Referring to Table 1, Examples 1 to 4 have a pulverization speed of calcined products adjusted to 2000 rpm or less, and Comparative Examples 1 to 4 have a pulverization speed of calcined products adjusted to 8000 rpm.

[0191] Evaluation Example 1: Evaluation of Positive Electrode Active Material

[0192] (1) Porosity evaluation

[0193] The porosity of the positive electrode active materials according to Examples 1 to 4 and Comparative Examples 1 to 4 was measured, and the results are shown in Table 2. The porosity was obtained by measuring the ratio of the pore area to the cross-sectional area of ​​the secondary particles in scanning electron microscope images of the respective secondary particles of the positive electrode active materials using the image analysis program Image J, and the results are shown in Table 2.

[0194] (2) Particle analysis

[0195] Figure 5 and 6 Each is a scanning electron microscope image of the surface of the positive electrode active material according to Example 1. Figure 5 and 6 The scanning electron microscope images are taken at different magnifications of the surface of the positive electrode active material of Example 1.

[0196] refer to Figure 5 The positive electrode active material of Example 1 has multiple assemblies in the form of aggregated secondary particles in which multiple primary particles are agglomerated, and refers to Figure 6 When the surface of an assembly is magnified, primary particles exist relatively uniformly within the assembly.

[0197] Similar to the positive electrode active material in Example 1, scanning electron microscope images of the surface of the positive electrode active materials in Examples 2 to 4 were taken respectively, and with reference to the images, the average particle size of the secondary particles, the arithmetic mean size of the secondary particles, the standard deviation of the arithmetic mean size of the secondary particles, the arithmetic mean size of the primary particles, and the standard deviation of the arithmetic mean size of the primary particles were measured, and the results are shown in Table 2.

[0198] Specifically, the average particle size of the secondary particles is obtained as follows: approximately 20 secondary particles are randomly selected from the scanning electron microscope images of the positive electrode active materials, the size of each secondary particle is measured, and the arithmetic mean of the sizes of each secondary particle is calculated, wherein the size of each secondary particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.

[0199] The arithmetic mean size of the secondary particles, the standard deviation of the arithmetic mean size of the secondary particles, the arithmetic mean size of the primary particles, and the standard deviation of the arithmetic mean size of the primary particles were obtained as follows: the sizes of approximately 20 randomly selected secondary particles and approximately 20 randomly selected primary particles were measured from scanning electron microscope (SEM) images, and the arithmetic mean and its standard deviation were calculated, wherein the size of each particle was defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.

[0200] The positive electrode active materials of Comparative Examples 1 to 4 could not be evaluated according to Table 2 because when the calcined product in assembly form was pulverized at 8000 rpm (greater than 2000 rpm), the multiple primary particles of the positive electrode active material were in a dispersed state as the secondary particles did not maintain the assembly form but instead separated into multiple primary particles.

[0201] Table 2:

[0202]

[0203] Referring to Table 2, it is confirmed that the positive electrode active materials of Examples 1 to 4, in which the pulverization speed is adjusted to 2000 rpm or less, have uniformly formed secondary particles and uniformly formed primary particles.

[0204] (3) Evaluation of aggregate density

[0205] The agglomerate density of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 4 was measured, and the results are shown in Table 3. The agglomerate density was determined as follows: 3 g of each positive electrode active material was placed in a mold, and each positive electrode active material was held in the mold at 25°C for 30 seconds. The thickness of the resulting agglomerates was measured, and the agglomerate volume was calculated using the agglomerate thickness and the diameter of the mold. The mass of the positive electrode active material was then divided by the calculated volume.

[0206] (4) Measurement of the amount of carbon

[0207] The amount of carbon in the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 4 was measured, and the content is shown in Table 3. Specifically, the amount of carbon was analyzed by completely burning each of the positive electrode active materials at a high temperature of 1200°C to 1400°C in an oxygen atmosphere to convert the carbon and sulfur in the positive electrode active materials into CO2 (or CO) and SO2. In Table 3, the amount of carbon is based on 100% by weight of each positive electrode active material. The following amounts of carbon correspond to the amount of carbon coating based on 100% by weight of the positive electrode active material.

[0208] (5) Evaluation of colorimetric parameters

[0209] The chromaticity parameters, such as L, R, G, and B, of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 4 were evaluated as follows: the L, a, and b values ​​were measured using a colorimeter via color coordinates in the CIE LAB color space, and then processed using the "SpectraMagic" program. The results are shown in Table 3. The chromaticity parameters of the positive electrode active materials can be measured in powder form and based on the white point corresponding to the D65 illuminant in the DCI-P3 color space.

[0210] Table 3:

[0211]

[0212] Referring to Table 3, Examples 1 to 4, where the pulverization speed of the calcined product was adjusted to 2000 rpm or less, exhibited comparable or superior agglomerate densities to Comparative Examples 1 to 4. However, despite using the same amount of carbon raw material in Examples 1 to 4 and Comparative Examples 1 to 4, it was confirmed that Examples 1 to 4 exhibited significantly greater amounts of carbon than Comparative Examples 1 to 4. This indicates that when the pulverization speed of the calcined product is too high, the secondary particle assembly form does not remain in assembly form but rather separates into nanoparticles. The carbon is not effectively attached (adhered) to the surface of the positive electrode active material during the pulverization process, but is partially detached or lost, thus significantly reducing the measured amount. However, when the pulverization speed is within the appropriate range of 2000 rpm or less, the positive electrode active material retains its assembly form well, so that the carbon does not detach but instead is stably fixed on the surface and inside the positive electrode active material and is effectively retained even after the pulverization process. Furthermore, Examples 1 to 4, in which the grinding speed of the calcined product was adjusted to 2000 rpm or less, exhibited chromaticity parameters of 30 or less for L, 70 or less for R, 70 or less for G, and 70 or less for B. However, Comparative Examples 1 to 4, in which the grinding speed of the calcined product was adjusted to greater than 2000 rpm, exhibited values ​​that did not meet the same range as above.

[0213] Evaluation Example 2: Measurement of the viscosity of the positive electrode slurry

[0214] The viscosity of positive electrode slurries comprising the positive electrode active materials according to Examples 1 to 4 and Comparative Examples 1 to 4 was measured at 20 rpm for a sample amount of 3 g using a Brookfield rotational viscometer, and the results are shown in Table 4.

[0215] Evaluation Example 3: Evaluation of Battery Performance

[0216] (1) Evaluation of initial charge / discharge capacity and efficiency

[0217] The rechargeable lithium-ion battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were charged at 25°C at a rate of 0.2 C to 3.8 V, and then discharged at a rate of 0.2 C to a cutoff voltage of 3.0 V to measure the initial charge / discharge capacity. The initial efficiency was calculated using this capacity according to Equation 1. The results are shown in Table 4.

[0218] [Equation 1]

[0219] Initial efficiency [%] = [Discharge capacity at the first cycle / Charge capacity at the first cycle] × 100

[0220] (2) Low-temperature capacity evaluation

[0221] The rechargeable lithium-ion battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were fully charged to a battery voltage of 3.8V at a rate of 0.2C, and then discharged to 3.0V at a rate of 0.2C in a thermostat under an atmosphere set at -20°C to measure the low-temperature discharge capacity. The results are shown in Table 4.

[0222] (3) Cyclic life characteristic evaluation

[0223] The rechargeable lithium battery cells of Examples 1 to 4 and Comparative Examples 1 to 4 were repeatedly charged at a rate of 1.0 C to a battery voltage of 3.8 V and discharged at a rate of 1.0 C to a cutoff voltage of 3.0 V 50 times or more after initial charging and discharging. The ratio of the discharge capacity of the 50th cycle to the initial discharge capacity was calculated according to Equation 2, and the results are shown in Table 4.

[0224] [Equation 2]

[0225] Cycle life [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100

[0226] Table 4:

[0227]

[0228] Referring to Table 4, the positive electrode slurries comprising the positive electrode active materials of Examples 1 to 4 (all satisfying chromaticity parameters of 30 or less L, 70 or less R, 70 or less G, and 70 or less B) have a viscosity of 8000 mPa·s or less, and therefore exhibit ease of coating and improved process stability and consistency. However, the slurries of Comparative Examples 1 to 4 (which do not satisfy the chromaticity parameters of L, R, G, and B) exhibit a viscosity greater than 8000 mPa·s, and therefore do not exhibit ease of coating and exhibit deteriorated process stability and consistency. Furthermore, unlike those comprising the positive electrode active materials of Comparative Examples 1 to 4, the rechargeable lithium-ion battery cells prepared using the positive electrode slurries comprising the positive electrode active materials of Examples 1 to 4 (satisfying chromaticity parameters of 30 or less L, 70 or less R, 70 or less G, and 70 or less B) exhibit excellent initial charge and discharge efficiency, low-temperature discharge capacity, and cycle life characteristics. In particular, the rechargeable lithium-ion battery cells of Examples 1 to 4 meet a low-temperature discharge capacity of 90 mAh / g or greater, which is a remarkably excellent low-temperature discharge capacity. This indicates that the rechargeable lithium-ion battery cells comprising the positive electrode active materials of Examples 1 to 4 (in the form of assemblies having multiple primary particles agglomerated therein) exhibit interconnectivity between particles, thereby continuously forming conductive paths, and thus enabling smooth movement of electrons and lithium ions and exhibiting excellent discharge characteristics in low-temperature environments. However, the rechargeable lithium-ion battery cells comprising the positive electrode active materials of Comparative Examples 1 to 4, which are separated into nanoparticles, have relatively large contact resistance between particles and are prone to disrupting conductive paths, leading to rapid degradation of discharge efficiency under low-temperature conditions.

[0229] in conclusion

[0230] As shown in Table 1, the positive electrode active materials of Examples 1 to 4, in which the pulverization conditions of the calcined product were adjusted to 2000 rpm or less, were confirmed to have an assembly form in which multiple primary particles agglomerated into secondary particles, and the secondary particles were formed relatively uniformly. When measured with a colorimeter, the positive electrode active materials having such an assembly form met the conditions of 30 or less L, 70 or less R, 70 or less G, and 70 or less B, but the positive electrode active materials of Comparative Examples 1 to 4, which added the same carbon raw materials, showed a much smaller carbon coating amount.

[0231] Furthermore, the positive electrode active materials of Examples 1 to 4 maintain the assembly structure, which results in the primary particles constituting the assembly structure being filled into the pores of the assembly structure during subsequent compression of the positive electrode in their respective electrode plate manufacturing processes. This increases the aggregate density and controls the slurry viscosity within an appropriate range, thereby leading to excellent processability. It has been confirmed that these structural characteristics result in improved overall electrochemical performance of rechargeable lithium batteries, such as initial charge / discharge capacity, efficiency, low-temperature discharge capacity, and cycle life characteristics.

[0232] Meanwhile, the positive electrode active materials of Comparative Examples 1 to 4, in which the pulverization speed of the calcined product was adjusted to greater than 2000 rpm, did not maintain the assembled form of secondary particle structure; instead, the secondary particles were dispersed into nanoparticles. Therefore, the chromaticity parameters were unsatisfactory, and the amount of carbon was less than that of Examples 1 to 4. As a result, compared with Examples 1 to 4, the comparative examples exhibited poorer overall performance, such as initial charge / discharge capacity, efficiency, low-temperature discharge capacity, and cycle life characteristics, and in particular, the comparative examples exhibited significantly deteriorated low-temperature discharge capacity.

[0233] While the invention has been described in conjunction with what are now considered some embodiments, this disclosure is not limited to the embodiments described above. Rather, this disclosure covers various modifications and equivalent arrangements of the embodiments described above.

[0234] <Description of representative figure labels>

[0235] 100: Rechargeable lithium battery; 10: Positive electrode

[0236] 11: Positive electrode lead connector 12: Positive electrode terminal

[0237] 20: Negative electrode 21: Negative electrode lead connector

[0238] 22: Negative electrode terminal; 30: Diaphragm

[0239] 40: Electrode assembly; 50: Housing

[0240] 60: Seal 70: Electrode terminal

[0241] 71: Positive electrode connector; 72: Negative electrode connector

Claims

1. A positive electrode active material having the form of secondary particles in which multiple primary particles are aggregated, said positive electrode active material comprising a lithium iron phosphate-based compound. The positive electrode active material has an L value of less than or equal to 30, an R value of less than or equal to 70, a G value of less than or equal to 70, and a B value of less than or equal to 70 as measured by a colorimeter.

2. The positive electrode active material according to claim 1, wherein the L value ranges from 2 to 30, the R value ranges from 20 to 70, the G value ranges from 45 to 70, and the B value ranges from 30 to 70.

3. The positive electrode active material according to claim 1, wherein the lithium iron phosphate-based compound comprises a compound represented by chemical formula 1, a compound represented by chemical formula 2, or a combination thereof: [Chemical Formula 1] Li a1 Fe (1-x1) M 1 x1 PO4, Where 0.9 ≤ a1 ≤ 1.5, 0 ≤ x1 ≤ 0.4, and M 1 Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof; and [Chemical Formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4, Where 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, and x² + y² < 1, and M 2 It is Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.

4. The positive electrode active material according to claim 1, wherein, based on the total metals excluding lithium in the lithium iron phosphate-based compound, the lithium iron phosphate-based compound comprises Al, Mg, Ti, V or combinations thereof in an amount of 0.1 mol% to 0.5 mol%.

5. The positive electrode active material according to claim 1, wherein the average particle size of the secondary particles is 3 μm to 20 μm.

6. The positive electrode active material according to claim 1, wherein the arithmetic mean size of the secondary particles is 3 μm to 20 μm, and The standard deviation of the arithmetic mean size of the secondary particles is less than or equal to 2.1 μm.

7. The positive electrode active material according to claim 1, wherein the arithmetic mean size of the primary particles constituting the secondary particles is less than or equal to 200 nm, and The standard deviation of the arithmetic mean size of the primary particles is less than or equal to 100 nm.

8. The positive electrode active material according to claim 1, wherein the secondary particles comprise pores, and the porosity, which is the ratio of the area occupied by the pores in the cross-section of the secondary particles to the cross-sectional area of ​​the secondary particles, is 10% to 50%.

9. The positive electrode active material according to claim 1, wherein the positive electrode active material further comprises a carbon coating on the surface of the secondary particles, and The amount of carbon coating in the positive electrode active material is 1.55% to 2% by weight, based on 100% by weight of the positive electrode active material.

10. The positive electrode active material according to claim 1, wherein the particle density of the positive electrode active material is from 2.35 g / cc to 2.5 g / cc.

11. A method for preparing a positive electrode active material, the method comprising: A phosphate-based precursor, a lithium raw material, and a carbon raw material are mixed in a solvent, and the phosphate-based precursor, the lithium raw material, and the carbon raw material are wet-milled to prepare a slurry. The slurry is added to a spray dryer and the slurry is spray-dried to prepare a dried product; The dried product is calcined to prepare a calcined product; and The calcined product is pulverized to obtain the positive electrode active material.

12. The method of claim 11, wherein adding the slurry to the spray dryer comprises adding the slurry to the spray dryer at an addition rate of less than or equal to 1 kg / min.

13. The method of claim 11, wherein spray drying the slurry to prepare the dried product comprises spray drying the slurry at a temperature of 150°C to 400°C.

14. The method of claim 11, wherein pulverizing the calcined product to obtain the positive electrode active material comprises pulverizing the calcined product at a pulverization speed of less than or equal to 2000 rpm.

15. The method of claim 11, wherein the obtained positive electrode active material is in the form of secondary particles in which a plurality of primary particles are agglomerated, the obtained positive electrode active material comprises a lithium iron phosphate-based compound, and the obtained positive electrode active material has an L value of less than or equal to 30, an R value of less than or equal to 70, a G value of less than or equal to 70 and a B value of less than or equal to 70 as measured by a colorimeter.

16. Positive electrode paste, including: The positive electrode active material according to any one of claims 1 to 10; and solvent, The positive electrode slurry has a viscosity of less than or equal to 8000 mPa·s.

17. A rechargeable lithium battery, comprising: Positive electrode; negative electrode; and Electrolytes, The positive electrode includes: Positive electrode current collector; and A positive electrode active material layer is disposed on the positive electrode current collector and includes the positive electrode active material according to any one of claims 1 to 10.