Composite conductive agents and their preparation methods, electrodes, solid-state batteries and electrical devices
By introducing a SAM anchoring layer and a multilayer coating structure of polyindole conductive polymer on the surface of the conductive agent core, the incompatibility problem between carbon-based conductive agents and sulfide electrolytes was solved, significantly improving the electrochemical performance of all-solid-state batteries.
Patent Information
- Application Number
- CN202611246131.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
The incompatibility between carbon-based conductive agents and sulfide electrolytes in composite electrodes leads to electrochemical instability in all-solid-state batteries, including electron channel effects, defects in amorphous carbon layers, thermodynamic stability defects of sulfide electrolytes, and structural flexibility issues, resulting in accelerated side reactions and increased interfacial impedance.
By introducing a self-assembled monolayer (SAM) to the surface of the conductive agent core to assist in the coating of polyindole conductive polymer, a multi-layered ordered coating structure of conductive agent core + SAM anchoring layer + polymer functional layer is formed, which isolates the conductive agent from direct contact with the sulfide electrolyte and enhances the interfacial stability.
It significantly improves the electrochemical performance of sulfide all-solid-state batteries, including higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
Smart Images

Figure CN123120733A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of solid-state battery technology, specifically relating to a composite conductive agent and its preparation method, an electrode, a solid-state battery, and an electrical device. Background Technology
[0002] The incompatibility between carbon-based conductive agents and sulfide electrolytes in composite electrodes poses a significant challenge to all-solid-state batteries. Sulfide solid-state electrolytes (such as Li6PS5Cl, Li3PS4, Li...) 10 GeP2S 12 The side reactions between sulfide electrolytes and carbon-based conductive agents (such as SuperP, acetylene black, and graphite) are essentially the result of the coupling between electrochemical instability and electronic conductivity networks. According to DFT calculations and experimental verification, sulfide electrolytes have a narrower electrochemical stability window, approximately 1.6–2.3 V vs. Li. + / Li. When the electron percolation network constructed by the carbon conductive agent comes into direct contact with the electrolyte, it significantly accelerates the decomposition of the electrolyte. Oxidation side: The electrolyte is oxidized at the high charging potential, generating S, P2S5, LiCl, and polysulfides (Li2S). n On the reduction side, the electrolyte is reduced at low discharge potential, producing products such as Li3P, Li2S, and LiCl. These decomposition products, especially Li2S and Li3P, have extremely low ionic conductivity, forming a high-resistivity layer at the interface, hindering the absorption of LiCl. + Transmit and increase interface resistance.
[0003] The drawbacks of carbon-based conductive agents are as follows: First, the electron channel effect. The core problem with carbon-based conductive agents lies in the fatal combination of their high electronic conductivity and the narrow electrochemical window of sulfide electrolytes. As an electron "highway," the carbon conductive agent effectively transfers the redox potential of the electrode to the electrolyte surface, causing the electrolyte to decompose in the thermodynamically unstable potential range. This electron-induced decomposition is particularly severe in composite cathodes because carbon, electrolyte, and active materials form a three-phase interface with short electron transfer paths and rapid kinetics. Second, the amorphous carbon layer defect. Studies have shown that a 5 nm to 7 nm thick amorphous carbon layer inevitably exists on the surface of commercial graphite and carbon black. This layer forms during the synthesis of carbon materials, covering the highly crystalline graphite surface. The harmful mechanism of the amorphous carbon layer includes: ① structural defects, sp 2 / sp 3 Hybridized carbon atoms are randomly arranged, containing numerous dangling bonds, vacancies, and edge sites, providing highly active reaction sites and lowering the activation energy of the reaction; ② Oxygen-containing functional groups, such as –OH, –COOH, and C=O surface functional groups, directly interact with PS4. 3-Nucleophilic reactions occur, triggering electrolyte decomposition; ③ High specific surface area, nanoscale pores and rough surfaces increase the effective contact area, accelerating side reaction kinetics; ④ Electronic state differences, the Fermi level of amorphous carbon is different from that of crystalline graphite, changing the interfacial electron transfer energy barrier and promoting redox reactions.
[0004] The drawbacks of sulfide electrolytes are: first, their intrinsic electrochemical window is narrow, stemming from their poor thermodynamic stability. For example, Li6PS5Cl has an oxidation limit of approximately ~2.3 V vs. Li. + / Li, reduction limit approximately ~1.7 V vs. Li + / Li. When matched with a high-voltage positive electrode such as NMC or LCO with an operating potential of 3.0~4.3 V, or a low-potential negative electrode such as metallic lithium with a potential of approximately 0 V, the electrolyte will be in a thermodynamically unstable state. Second, the defect of mixed ionic-electron conductivity. An ideal interface should satisfy ionic conductivity and electronic insulation, allowing Li + By preventing electron leakage, a passivated SEI is formed. Actual sulfide decomposition products are Li₂S (band gap ~3.5 eV, insulator), Li₃P (semiconductor), P₂S₅ (insulator), etc. If the decomposition products have mixed ionic-electron conductivity, an effective passivation layer cannot be formed, and the electrolyte will continue to decompose. The presence of carbon conductive agents provides electron channels, allowing the decomposition reaction to self-catalyze and continue. Third, structural flexibility and lattice defects. Sulfide electrolytes have soft lattice characteristics, S… 2- PS4 has a large ionic radius, high polarizability, and low lattice distortion energy. It is prone to structural rearrangement under electric fields and mechanical stress. 3- During oxidation, the tetrahedron undergoes distortion, forming SS bonds and ultimately generating P2S5 and Li2S. This structural instability is amplified at the carbon / electrolyte interface because the local electric field and chemisorption on the carbon surface further lower the reaction energy barrier. Fourth, sensitivity to reactive oxygen species (ROS). In high-voltage cathode systems, the carbon conductive agent surface not only reacts directly with the electrolyte but also catalyzes the release of reactive oxygen species, such as O2, from the cathode. 2- Singlet oxygen 1 O2. ROS attacks PS4 3- Unit, resulting in S 2- Oxidized to SO3 2- SO4 2- This generates insulating sulfates, which severely hinder ion transport. Summary of the Invention
[0005] This application aims to at least partially address one of the technical problems in related technologies. Therefore, the purpose of this application is to provide a composite conductive agent and its preparation method, an electrode, a solid-state battery, and an electrical device. This application effectively isolates the direct contact between the conductive agent and the sulfide electrolyte by coating the surface of the conductive agent core with a self-assembled monolayer (SAM) assisted coating of a polyindole-based conductive polymer, thereby effectively enhancing the interfacial stability between the conductive agent and the sulfide electrolyte, suppressing side reactions between the conductive agent and the sulfide electrolyte, and thus significantly improving the electrochemical performance of the sulfide solid-state battery.
[0006] In one aspect of this application, a composite conductive agent is provided. According to an embodiment of this application, the composite conductive agent comprises: Conductive core; SAM anchoring layer, the SAM anchoring layer being disposed on at least a portion of the surface of the conductive agent core; A polymer functional layer disposed on at least a portion of the surface of the SAM anchoring layer away from the conductive core; The polymer functional layer includes at least one of polyindole and polyindole derivatives.
[0007] According to embodiments of this application, the composite conductive agent involves a self-assembled monolayer (SAM) assisted coating of a polyindole conductive polymer onto the surface of the conductive agent core. This effectively isolates the direct contact between the conductive agent and the sulfide electrolyte, thereby significantly enhancing the interfacial stability between the conductive agent and the sulfide electrolyte. This effectively mitigates the decomposition of the sulfide electrolyte and suppresses side reactions between the conductive agent and the sulfide electrolyte, thereby significantly improving the electrochemical performance of the sulfide all-solid-state battery, including higher initial discharge capacity, superior cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
[0008] In addition, the composite conductive agent according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the conductive agent core includes at least one of fibrous conductive agent core and granular conductive agent core, wherein the fibrous conductive agent has an average diameter of 10 nm to 500 nm and an average length of 1 μm to 50 μm, and the granular conductive agent has an average particle size of 20 nm to 500 nm; and / or, the conductive agent core includes at least one of vapor-grown carbon fiber, carbon nanotube, acetylene black, conductive graphite, graphene, and superconducting carbon black.
[0009] In some embodiments of this application, the thickness of the SAM anchoring layer is 1 nm to 100 nm; and / or, the SAM anchoring layer comprises at least one of a head-segment-tail compound, wherein the head group is selected from at least one of silyl, mercapto, phosphate, and carboxyl groups, and the segment is selected from C2 to C3. 18 The SAM anchoring layer comprises at least one of the following: a straight-chain or branched alkylene chain, a polyethylene glycol chain, or an oligosiloxane chain; wherein the tail group is selected from at least one of an amino group, an epoxy group, an isocyanate group, a maleimide group, an aldehyde group, an acyl chloride group, or a carboxyl group; and / or, the SAM anchoring layer comprises at least one of 3-aminopropyltriethoxysilane, 3-glycidyl etheroxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 11-bromoundecyltrichlorosilane, 11-mercaptoundecanoic acid, 16-mercaptohexadecanoic acid, cysteine, 12-phosphododecanoic acid, phosphate-O-(2-aminoethyl) ester, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0010] In some embodiments of this application, the thickness of the polymer functional layer is 1 nm to 100 nm; and / or, the indole structural units of the polyindole derivative are repeatedly linked by 2,3-carbon-carbon bonds, 2,2-carbon-carbon bonds, 3,3-carbon-carbon bonds or 1,3-carbon-nitrogen bonds to form a main chain conjugated structure, and the benzene ring on the indole structural unit is unsubstituted or substituted by at least one substituent, wherein the substituent is selected from at least one of alkyl, alkoxy, halogen, hydroxyl, amino, nitro, cyano, carboxyl, ester, amide and sulfonic acid groups.
[0011] In a second aspect, this application provides a method for preparing the composite conductive agent described in the above embodiments. According to an embodiment of this application, the method includes: (1) Surface activation of the conductive agent core; (2) The activated conductive core, SAM molecules and the first solvent are mixed to obtain the first solution, stirred and post-treated to obtain the SAM-modified conductive core; (3) The SAM-modified conductive agent core, indole-containing monomer, oxidant and second solvent are mixed to obtain a second solution, and graft polymerization reaction is carried out. After post-treatment, the composite conductive agent is obtained. Alternatively, the SAM-modified conductive agent core can be used as the working electrode and placed in an electrolyte containing indole monomers and supporting electrolytes for electrochemical oxidation polymerization to obtain the composite conductive agent.
[0012] The method for preparing composite conductive agents according to embodiments of this application involves first introducing a SAM anchoring layer onto the surface of the conductive agent core, and then introducing a polymer functional layer using the chemical bonding between the terminal active groups of SAM and the polymer. This constructs a multi-layered ordered coating structure consisting of a conductive agent core, a SAM anchoring layer, and a polymer functional layer, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge. This achieves multifunctional synergy in interfacial bonding, electronic conductivity, and chemical stability, effectively isolating the conductive agent from direct contact with the sulfide electrolyte, thereby effectively enhancing the interfacial stability between the conductive agent and the sulfide electrolyte. It also effectively alleviates the decomposition of the sulfide electrolyte and suppresses side reactions between the conductive agent and the sulfide electrolyte. This significantly improves the electrochemical performance of sulfide all-solid-state batteries, including higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
[0013] In addition, the method according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, in step (1), the conductive agent core is dispersed in concentrated H2SO4 / HNO3 mixed acid, ultrasonically treated at 60℃~80℃ for 2 h~12 h, washed, and the activated conductive agent core is obtained; and / or, in step (2), stirring is performed for 2 h~24 h; and / or, in step (2), the concentration of the SAM molecule in the first solution is 1 mM~50 mM; and / or, in step (3), the temperature of the graft polymerization reaction is 20℃~60℃, and the time is 6 h~48 h; and / or, in step (3), the oxidant includes at least one of anhydrous FeCl3, ammonium persulfate, benzoyl peroxide, and iodine; and / or, in step (3), the molar ratio of the oxidant to the indole monomer is (1:1)~(4:1); and / or, in step (3), the concentration of the indole monomer in the second solution is 0.01 mol / L~0.5 mol / L; and / or, in step (3), the concentration of the indole monomer in the electrolyte is 0.01 mol / L to 0.2 mol / L; and / or, in step (3), the supporting electrolyte is LiClO4 or Bu4NPF6; and / or, in step (3), the concentration of the supporting electrolyte in the electrolyte is 0.1 mol / L to 1 mol / L; and / or, in step (3), the conditions for the electrochemical oxidation polymerization are: constant potential 0.7 V to 1.2 V, polymerization time 10 min to 120 min; or cyclic voltammetry scan 0 V to 1.5 V, 10 to 50 cycles.
[0014] In a third aspect, this application proposes an electrode. According to embodiments of this application, the electrode comprises a composite conductive agent as described in the first aspect or a composite conductive agent prepared by the method of the second aspect. Thus, the electrode of this application employs a multi-layered ordered coating structure of a conductive agent core + SAM anchoring layer + polymer functional layer. Relying on the chemical bonding between the active groups at the ends of the SAM anchoring molecules and the polymer, a high-density, ordered, strongly bonded, and highly stable interfacial bridge is constructed within the electrode, achieving a multi-functional synergy of interfacial bonding force, electronic conductivity, and chemical stability. This effectively isolates the direct contact between the conductive agent and the sulfide electrolyte within the electrode, significantly enhancing the interfacial stability between the conductive agent and the sulfide electrolyte, effectively mitigating the decomposition of the sulfide electrolyte, and suppressing side reactions between the conductive agent and the sulfide electrolyte within the electrode. This significantly improves the overall electrochemical performance of the sulfide all-solid-state battery, enabling the battery to possess higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and superior rate performance.
[0015] In addition, the electrode sheet according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the electrode also includes a sulfide electrolyte.
[0016] In a fourth aspect, this application proposes a solid-state battery. According to embodiments of this application, the solid-state battery includes the composite conductive agent described in the first aspect, a composite conductive agent prepared by the method described in the second aspect, or an electrode described in the third aspect. This significantly improves the electrochemical performance of the solid-state battery, including higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
[0017] A fifth aspect of this application discloses an electrical device. According to an embodiment of this application, the electrical device includes a solid-state battery as described in the fourth aspect. The features and advantages described above for the solid-state battery also apply to this electrical device, and will not be repeated here.
[0018] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0019] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a scanning electron microscope (SEM) image of the unmodified VGCF in Example 1; Figure 2This is a scanning electron microscope (SEM) image of APTES@polyindole-coated VGCF in Example 1; Figure 3 This is a transmission electron microscope (TEM) image of APTES@polyindole-coated VGCF in Example 1; Figure 4 This is a comparison of the Fourier Transform Infrared (FTIR) spectra of APTES@polyindole-coated VGCF in Example 1; Figure 5 This is a comparison of XRD patterns of APTES@polyindole-coated VGCF in Example 1; Figure 6 The photon spectrum of APTES@polyindole-coated VGCF in Example 1 is shown. Detailed Implementation
[0020] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application.
[0021] In one aspect of this application, a composite conductive agent is proposed. According to an embodiment of this application, the composite conductive agent comprises: a conductive agent core; a SAM anchoring layer disposed on at least a portion of the surface of the conductive agent core; and a polymer functional layer disposed on at least a portion of the surface of the SAM anchoring layer away from the conductive agent core; the polymer functional layer comprises at least one of polyindole and polyindole derivatives.
[0022] The beneficial effects achievable by the composite conductive agent proposed in this application will be described in detail below: This application constructs a multi-layered ordered coating structure consisting of a conductive agent core, a SAM anchoring layer, and a polymer functional layer by first introducing a SAM anchoring layer on the surface of the conductive agent core and then introducing a polymer functional layer using the chemical bonding between the terminal active groups of SAM and the polymer. SAM acts as a "molecular glue," with one end tightly bonded to the surface of the conductive agent core and the other end firmly connected to the polymer layer, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge. This achieves multi-functional synergy of interfacial bonding force, electronic conductivity, and chemical stability, solving the problems of easy hydrogen bond breakage, coating layer detachment, and continuous interfacial side reactions of existing modified conductive agents under high-temperature solid-state battery operating conditions.
[0023] SAMs possess self-assembly and ordered molecular arrangement. During self-assembly, SAM molecules connect to the conductive agent core via chemical bonds, forming a highly ordered molecular layer. Since SAM growth proceeds from disorder to order (entropy reduction), the compensation from the increasing entropy of the environment makes it a thermodynamically spontaneous process. This results in SAM modification typically requiring low energy consumption and achieving high interfacial coverage. Polymers, used as coating materials, leverage their unique NH hydrogen bond donors and benzopyrrole conjugated structure to enhance interfacial compatibility and chemical stability with sulfide electrolytes while maintaining high electronic conductivity.
[0024] On the surface of the conductive agent core, a self-assembled monolayer (SAM) is used to coat a polyindole-based conductive polymer, effectively isolating the conductive agent from direct contact with the sulfide electrolyte, thereby significantly enhancing the interfacial stability between the conductive agent and the sulfide electrolyte. This effectively mitigates the decomposition of the sulfide electrolyte and suppresses side reactions between the conductive agent and the sulfide electrolyte. It significantly improves the electrochemical performance of the sulfide all-solid-state battery, including higher initial discharge capacity, superior cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance. Specifically, the discharge capacity at 1C exceeds 175 mAh / g, and the cycle life is improved by more than 30%.
[0025] Compared with the prior art, the present invention has the following significant advantages: First, dense molecular-level coverage. SAM molecules self-assemble on the surface of the conductive agent core to form a dense and ordered monolayer, with a coverage density of up to 10. 14 ~10 15 mol / cm 2 The functional group density is much higher than that of conventional oxidation treatment (10 12 ~10 13 mol / cm 2 This fundamentally eliminates the direct contact between conductive carbon and sulfide electrolytes, improving interfacial chemical stability by an order of magnitude.
[0026] Second, ordered interface bridges. SAM segments provide regular molecular spacers, and their tails provide directional reactive sites, enabling the polyindole layers to graft and grow in an ordered manner, forming a highly ordered coating structure, avoiding the disordered aggregation of physical mixing and the random reactions of in-situ bonding.
[0027] Third, multiple bonding mechanisms. The head group of SAM forms covalent bonds with the conductive agent core (e.g., Si-OC, CS, etc.), and its tail group forms covalent bonds with polyindole (e.g., amide bonds, N-alkylation bonds, Michael addition, etc.) or strong physical interactions (e.g., hydrogen bonds, π-π stacking, electrostatic interactions, etc.), constructing a multi-stable interface system of "covalent bonds + hydrogen bonds + π-π stacking + electrostatic interactions", which eliminates the risk of hydrogen bond breakage under high-temperature operating conditions.
[0028] Fourth, stress buffering and flexible adaptation. The alkylene segments of SAM are flexible and stretchable, which can buffer the volume expansion / contraction of the active material during charging and discharging, with strain reaching 20%~30%, preventing the coating layer from cracking and falling off, significantly improving cycle stability, with a retention rate of >95% after 100 cycles.
[0029] Fifth, the unique advantages of polyindole polymers. The conjugated backbone of polyindole polymers provides electron conduction channels, and the NH groups provide hydrogen bond donor sites, enabling weak hydrogen bond interactions with sulfide ions in sulfide electrolytes, thus enhancing interfacial compatibility. The benzopyrrole conjugated structure of polyindole polymers provides additional π-π stacking capacity, forming multiple π-π stacks with the phenylene segments of SAM or the graphite structure of the conductive core, enhancing interfacial bonding. The electron-rich nature of the indole 3-position carbon makes it prone to electrophilic reactions such as Michael addition, expanding the range of selectable SAM tail reaction mechanisms. The functional layer of polyindole polymers is tightly bound to the anchoring layer through the directional reaction of the SAM tail, forming a synergistic structure of "SAM bridging + polyindole functionalization".
[0030] Sixth, high retention of electronic conductivity. The conductivity retention rate of the modified conductive agent after coating is >75%, which is far superior to the coating of electronic insulating polymers. Coating of PVDF, PEO, etc. will lead to a decrease in conductivity of >90%.
[0031] Seventh, the coating thickness is precisely controllable. This is achieved through the control of SAM segment length (C2-C). 18 Adjustable) and polyindole polymerization degree control enable precise control of coating thickness in the range of 3 nm to 50 nm, with extremely high coating uniformity and thickness deviation of <±10%.
[0032] In the embodiments of this application, the specific type of conductive agent core is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific embodiments, the conductive agent core is a carbon-based material with good electronic conductivity, selected from at least one of vapor-grown carbon fiber (VGCF), carbon nanotubes (CNTs, including single-walled and multi-walled), acetylene black, conductive graphite, graphene, superconducting carbon black, etc. Preferably, the conductive agent core is a common conductive agent used in lithium batteries, such as vapor-grown carbon fiber (VGCF), carbon nanotubes (CNTs), or acetylene black.
[0033] According to some specific embodiments of this application, the conductive agent core includes at least one of fibrous conductive agent core and granular conductive agent core. The average diameter of the fibrous conductive agent is 10 nm to 500 nm (e.g., it can be 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.), and the average length is 1 μm to 50 μm (e.g., it can be 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, etc.). The average particle size of the granular conductive agent is 20 nm to 500 nm (e.g., it can be 20 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.).
[0034] In the embodiments of this application, the conductive core can be surface activated before use to introduce oxygen-containing functional groups (-OH, -COOH) to provide active sites for SAM anchoring.
[0035] According to further specific embodiments of this application, the aforementioned SAM anchoring layer is coated on at least a portion of the surface of the conductive agent core, forming a dense and ordered monolayer with a thickness of 1 nm to 100 nm (e.g., 1 nm, 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, etc.). This further ensures that the SAM anchoring layer acts as a "molecular glue," with one end tightly bonded to the surface of the conductive agent core and the other end firmly connected to the polymer layer, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge. Preferably, the thickness is 1 nm to 50 nm.
[0036] According to some specific embodiments of this application, the SAM molecules in the above-mentioned SAM anchoring layer have a three-segment structure of head group-chain segment-tail group. The head group is selected from at least one of silyl group (-Si(OR)3, where R is methyl or ethyl), mercapto group (-SH), phosphate group (-PO(OH)2), and carboxyl group (-COOH), used to react with the -OH / -COOH functional groups on the surface of the conductive agent core to form a strong chemical bond (Si-OC, CS, POC, etc.). The chain segment is selected from C2~C... 18 Straight-chain or branched alkylene chains (-(CH2)) n- n is selected from 2 to 18), polyethylene glycol chain (-(CH2CH2O) m-The m group is selected from at least one of 2-10 oligosiloxane chains, providing molecular spacing, flexibility, and steric hindrance regulation. The tail group is selected from at least one of amino (-NH2), epoxy (-C2H3O), isocyanate (-NCO), maleimide (-C4H2NO2), aldehyde (-CHO), acyl chloride (-COCl), and carboxyl (-COOH), used to form chemical bonds or strong physical interactions with polyindole. This further ensures that the SAM anchoring layer acts as a "molecular glue," with the head group forming covalent bonds with the conductive core and the tail group forming covalent bonds or strong physical interactions with polyindole, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge.
[0037] In some preferred embodiments, the SAM molecules in the SAM anchoring layer are selected from at least one of silane SAM molecules, thiol SAM molecules, phosphoric acid SAM molecules, and bifunctional SAM molecules. Specifically, the silane SAM molecules are selected from 3-aminopropyltriethoxysilane (APTES, H2N-(CH2)3-Si(OC2H5)3), 3-glycidyl etheroxypropyltrimethoxysilane (GPTMS, C2H3O-(CH2)3-Si(OCH3)3), 3-mercaptopropyltrimethoxysilane (MPTMS, HS-(CH2)3-Si(OCH3)3), and 11-bromoundecyltrichlorosilane (Br-(CH2)3). 11 At least one of the following: (-SiCl3). Thiol SAM molecules are selected from 11-mercaptoundecanoic acid (HS-(CH2)). 10 -COOH), 16-mercaptohexadecanoic acid (HS-(CH2) 15 At least one of the following: -COOH, cysteine (HS-(CH2)2-NH2), etc. Phosphophosphate SAM molecules are selected from 12-phosphododecanoic acid ((HO)2P(O)-(CH2)). 11 At least one of the following: -COOH, phosphate-O-(2-aminoethyl) ester, etc. Bifunctional SAM molecules include N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AEAPTMS, H2N-(CH2)2-NH-(CH2)3-Si(OCH3)3), which has two amino terminals and can simultaneously anchor two polymer layers. This further ensures that the SAM anchoring layer acts as a "molecular glue," with the head group forming a covalent bond with the conductive core and the tail group forming a covalent bond or strong physical interaction with polyindole, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge.
[0038] According to some specific embodiments of this application, the thickness of the polymer functional layer is 1 nm to 100 nm, for example, it can be 1 nm, 10 nm, 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, etc. This further effectively isolates the direct contact between the conductive agent and the sulfide electrolyte, thereby further enhancing the interfacial stability between the conductive agent and the sulfide electrolyte, effectively mitigating the decomposition of the sulfide electrolyte, and effectively suppressing side reactions between the conductive agent and the sulfide electrolyte. Preferably, it is 5 nm to 50 nm.
[0039] In the embodiments of this application, the above-mentioned polyindole has the following structural features: the main chain is a benzopyrrole conjugated structure, the indole units are connected by 3,3'-carbon-carbon bonds to form a linear polymer chain, and NH groups are retained on the molecular chain.
[0040] According to some specific embodiments of this application, the indole structural units of the above-mentioned polyindole derivatives are repeatedly linked through 2,3-position carbon-carbon bonds, 2,2-position carbon-carbon bonds, 3,3-position carbon-carbon bonds or 1,3-position carbon-nitrogen bonds to form a main chain conjugated structure. The benzene ring on the indole structural unit is not substituted or is substituted by at least one substituent. The substituent is selected from at least one of alkyl, alkoxy, halogen, hydroxy, amino, nitro, cyano, carboxyl, ester, amide and sulfonic acid groups.
[0041] According to some specific embodiments of this application, the number average molecular weight (Mn) of the above-mentioned polyindole is 2000~50000, preferably 5000~20000; and / or, the number average molecular weight (Mn) of the polyindole derivative is 2000~50000, preferably 5000~20000.
[0042] In the embodiments of this application, the conjugated backbone of the aforementioned polyindole and its related derivatives provides electronic conduction channels, and the NH group provides hydrogen bond donor sites, which can form weak hydrogen bond interactions with sulfide ions in the sulfide electrolyte, enhancing interfacial compatibility. The benzo[a]cyclic structure of the aforementioned polyindole and its related derivatives provides additional π-π stacking capability, forming multiple π-π stacks with the phenylene segments of SAM or the graphite structure of the conductive core, enhancing interfacial bonding. The functional layer of the aforementioned polyindole and its related derivatives is tightly bonded to the anchoring layer through the directional reaction of the SAM tail group, forming a synergistic structure of "SAM bridging + polyindole functionalization".
[0043] In a second aspect of this application, a method for preparing the composite conductive agent of the above embodiments is provided. According to an embodiment of this application, the method includes: S100: surface activation of the conductive agent core; S200: dispersing the activated conductive agent core in a first solution containing SAM molecules, stirring, and post-processing to obtain a SAM-modified conductive agent core; S300: dispersing the SAM-modified conductive agent core in a second solution containing indole monomer and oxidant, performing a graft polymerization reaction, and post-processing to obtain a composite conductive agent; or, using the SAM-modified conductive agent core as a working electrode, placing it in an electrolyte containing indole monomer and supporting electrolyte, and performing electrochemical oxidative polymerization to obtain a composite conductive agent.
[0044] The method for preparing composite conductive agents according to embodiments of this application involves first introducing a SAM anchoring layer onto the surface of the conductive agent core, and then introducing a polymer functional layer using the chemical bonding between the terminal active groups of SAM and the polymer. This constructs a multi-layered ordered coating structure consisting of a conductive agent core, a SAM anchoring layer, and a polymer functional layer, forming a high-density, ordered, strongly bonded, and highly stable interfacial bridge. This achieves multifunctional synergy in interfacial bonding, electronic conductivity, and chemical stability, effectively isolating the conductive agent from direct contact with the sulfide electrolyte, thereby effectively enhancing the interfacial stability between the conductive agent and the sulfide electrolyte. It also effectively alleviates the decomposition of the sulfide electrolyte and suppresses side reactions between the conductive agent and the sulfide electrolyte. This significantly improves the electrochemical performance of sulfide all-solid-state batteries, including higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
[0045] The core innovation of this invention lies in using self-assembled monolayers (SAMs) as "molecular glue" to assist in the coating of polyindole conductive polymers. This method is completely different from the in-situ bonding coating, physical mixing coating, and MLD deposition in existing technologies. Its principle is as follows: SAM self-assembly principle: In solution, SAM molecules undergo chemical reactions with the -OH / -COOH functional groups on the surface of the conductive agent core through head groups (such as hydrolysis and condensation of silane groups, coordination of thiol groups with metals, and coordination of phosphate groups with oxides). Simultaneously, they spontaneously align themselves to form a dense and ordered monolayer through intermolecular van der Waals forces and hydrophobic interactions. This process is self-limiting; once the surface is completely covered, the reaction automatically stops, ensuring precise control over the monolayer thickness.
[0046] Polyindole polymerization mechanism: Under oxidative conditions, the carbon atom at the 3-position of the indole monomer undergoes electrophilic substitution or oxidative coupling, forming a polymer chain linked by 3,3'-carbon-carbon bonds. The NH group remains on the polymer backbone, providing hydrogen bond donor sites. Polymerization can be achieved through chemical oxidation (FeCl3, etc.) or electrochemical oxidation (anodic oxidation).
[0047] As a specific example, the reaction equation is:
[0048] Specifically, the above method includes the following steps: S100: Surface activation of the conductive agent core; In this step, the conductive agent core undergoes surface activation treatment to introduce oxygen-containing functional groups (-OH, -COOH), providing active sites for SAM anchoring.
[0049] According to some specific embodiments of this application, the conductive agent core is dispersed in a concentrated H2SO4 / HNO3 mixed acid, ultrasonically treated at 60℃~80℃ for 2 h~12 h, washed with deionized water until neutral, and dried to obtain an activated conductive agent core with a surface rich in -OH / -COOH functional groups. As a specific embodiment, the volume ratio of H2SO4 to HNO3 is 3:1.
[0050] S200: The activated conductive core, SAM molecules and the first solvent are mixed to obtain the first solution, stirred and post-treated to obtain the SAM-modified conductive core; In this step, the activated conductive agent core, SAM molecules and a first solvent are mixed to obtain a first solution, which is stirred to allow SAM molecules to self-assemble on the surface of the conductive agent to form a dense and ordered monolayer; after post-processing, a SAM-modified conductive agent core is obtained.
[0051] According to some specific embodiments of this application, in step S200, the stirring is carried out for 2 h to 24 h, for example, 2 h, 5 h, 10 h, 15 h, 20 h, 24 h, etc., thereby further ensuring that SAM molecules self-assemble on the surface of the conductive agent to form a dense and ordered monolayer.
[0052] According to some specific embodiments of this application, the concentration of the SAM molecules in the first solution is 1 mM to 50 mM, for example, 1 mM, 10 mM, 20 mM, 30 mM, 40 mM, 50 mM, etc., thereby further ensuring that the SAM molecules self-assemble on the surface of the conductive agent to form a dense and ordered monolayer. Preferably, it is 5 mM to 20 mM.
[0053] In the embodiments of this application, the specific type of the first solvent is not particularly limited. Those skilled in the art can select it according to actual needs. As some specific embodiments, the first solvent is selected from at least one of anhydrous toluene, anhydrous ethanol, anhydrous acetone, and anhydrous acetonitrile.
[0054] According to some specific embodiments of this application, in step S200, the post-processing includes: washing 3-5 times with a corresponding solvent to remove excess physically adsorbed SAM molecules, and vacuum drying at 60℃~100℃ for 2 h~6 h.
[0055] S300: A second solution is obtained by mixing a SAM-modified conductive agent core, an indole-containing monomer, an oxidant, and a second solvent. Graft polymerization is then carried out, followed by post-treatment to obtain a composite conductive agent. In this step, a chemical oxidative grafting polymerization method is used. The SAM-modified conductive core, indole monomer, oxidant and second solvent are mixed to obtain a second solution, and a grafting polymerization reaction is carried out. Under the action of the oxidant, the indole monomer initiates polymerization at the active site of the SAM tail group to form a polyindole functional layer.
[0056] According to some specific embodiments of this application, the temperature of the above-mentioned graft polymerization reaction is 20℃~60℃ (e.g., 20℃, 30℃, 40℃, 50℃, 60℃, etc.), and the time is 6 h~48 h (e.g., 6 h, 10 h, 20 h, 30 h, 40 h, 48 h, etc.). This can further ensure that the indole monomer initiates polymerization at the active site of the SAM tail group to form a polyindole functional layer of suitable thickness.
[0057] In the embodiments of this application, the specific type of oxidant is not particularly limited. Those skilled in the art can select it according to actual needs. As some specific embodiments, the oxidant includes at least one of anhydrous FeCl3, ammonium persulfate (APS), benzoyl peroxide (BPO), and iodine (I2).
[0058] According to further specific embodiments of this application, the concentration of indole monomer in the second solution is 0.01 mol / L to 0.5 mol / L, for example, 0.01 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, etc. This further ensures that the indole monomer initiates polymerization at the active site of the SAM tail group, forming a polyindole functional layer of suitable thickness. Preferably, the concentration is 0.05 mol / L to 0.2 mol / L.
[0059] According to some specific embodiments of this application, the molar ratio of oxidant to indole monomer is (1:1) to (4:1); for example, it can be 1:1, 2:1, 3:1, 4:1, etc., thereby further ensuring that under the action of oxidant, indole monomer initiates polymerization at the active site of SAM tail group to form polyindole functional layer.
[0060] In the embodiments of this application, the specific type of the second solvent is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific embodiments, the second solvent includes at least one of chloroform, dichloromethane, toluene, acetonitrile, and N-methylpyrrolidone (NMP).
[0061] As some specific examples, in step S300, the above post-processing includes: washing with an organic solvent 3-5 times to remove homopolymer and residual monomers, and vacuum drying at 80°C to 120°C for 12 h to 24 h.
[0062] Alternatively, S300': Using a SAM-modified conductive agent core as the working electrode, it is placed in an electrolyte containing indole monomers and supporting electrolytes for electrochemical oxidation polymerization to obtain a composite conductive agent.
[0063] In this step, the SAM-modified conductive core is used as the working electrode and placed in an electrolyte containing indole monomers and supporting electrolytes. Polyindole is directly grown on the SAM tail through electrochemical oxidative polymerization to form a polyindole functional layer.
[0064] According to some specific embodiments of this application, in step S300', the concentration of indole monomer in the electrolyte is 0.01 mol / L to 0.2 mol / L, for example, it can be 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, etc., thereby further ensuring that polyindole is directly grown on the SAM tail by electrochemical oxidative polymerization to form a polyindole functional layer of suitable thickness.
[0065] In the embodiments of this application, the specific type of supporting electrolyte is not particularly limited. Those skilled in the art can choose according to actual needs. As some specific embodiments, the supporting electrolyte is LiClO4 or Bu4NPF6.
[0066] According to some specific embodiments of this application, in step S300', the concentration of the electrolyte in the electrolyte solution is supported to be 0.1 mol / L to 1 mol / L. This further ensures that polyindole is directly grown on the SAM tail by electrochemical oxidative polymerization to form a polyindole functional layer of suitable thickness.
[0067] According to some specific embodiments of this application, in step S300', the conditions for electrochemical oxidative polymerization are: constant potential of 0.7 V to 1.2 V, polymerization time of 10 min to 120 min; or cyclic voltammetry scan of 0 V to 1.5 V, for 10 to 50 cycles. This further ensures that polyindole is directly grown on the SAM tail via electrochemical oxidative polymerization, forming a polyindole functional layer of suitable thickness.
[0068] In a third aspect, this application proposes an electrode. According to embodiments of this application, the electrode comprises a composite conductive agent as described in the first aspect or a composite conductive agent prepared by the method of the second aspect. Thus, the electrode of this application employs a multi-layered ordered coating structure of a conductive agent core + SAM anchoring layer + polymer functional layer. Relying on the chemical bonding between the active groups at the ends of the SAM anchoring molecules and the polymer, a high-density, ordered, strongly bonded, and highly stable interfacial bridge is constructed within the electrode, achieving a multi-functional synergy of interfacial bonding force, electronic conductivity, and chemical stability. This effectively isolates the direct contact between the conductive agent and the sulfide electrolyte within the electrode, significantly enhancing the interfacial stability between the conductive agent and the sulfide electrolyte, effectively mitigating the decomposition of the sulfide electrolyte, and suppressing side reactions between the conductive agent and the sulfide electrolyte within the electrode. This significantly improves the overall electrochemical performance of the sulfide all-solid-state battery, enabling the battery to possess higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and superior rate performance.
[0069] According to some specific embodiments of this application, the electrode further includes a sulfide electrolyte. The sulfide electrolyte exhibits severe side reactions with conventional carbon-based conductive agents, and its decomposition products, particularly Li₂S and Li₃P, have extremely low ionic conductivity, forming a high-resistivity layer at the interface and hindering the flow of Li₂. + This application utilizes a composite conductive agent with a multi-layered ordered coating structure consisting of a conductive agent core, a SAM anchoring layer, and a polymer functional layer within the electrode. This effectively isolates the direct contact between the conductive agent and the sulfide electrolyte within the electrode, significantly enhancing the interfacial stability between the conductive agent and the sulfide electrolyte, effectively mitigating the decomposition of the sulfide electrolyte, and suppressing side reactions between the conductive agent and the sulfide electrolyte within the electrode.
[0070] In the embodiments of this application, the aforementioned composite conductive agent can be applied to both the positive and negative electrode sheets. Whether applied to the positive or negative electrode sheet, the composite conductive agent achieves the aforementioned technical effects.
[0071] According to some specific embodiments of this application, the above-mentioned electrode is a positive electrode. The positive electrode includes a positive current collector and a positive active material layer. The positive active material layer is disposed on at least one side of the positive current collector. The positive active material layer includes a positive active substance, a positive binder, a composite conductive agent, and a sulfide electrolyte.
[0072] In the embodiments of this application, the material of the positive current collector is not particularly limited. As some preferred options, the positive current collector includes at least one of aluminum foil, aluminum foam, carbon-coated aluminum foil, carbon mesh, and carbon cloth.
[0073] In the embodiments of the present application, the specific type of the above-mentioned positive electrode active material is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred solutions, the above-mentioned positive electrode active material includes lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium iron phosphate (LiFePO4), lithium cobalt phosphate (LiCoPO4), lithium manganese phosphate (LiMnPO4), lithium nickel phosphate (LiNiPO4), lithium manganate (LiMnO2), binary material LiNi x A (1-x) O2 (wherein A is selected from one of Co and Mn, 0<x<1), ternary material LiNi m B n C (1-m-n) O2 (wherein B and C are independently selected from at least one of Co, Al and Mn, B and C are different, 0<m<1, 0<n<1).
[0074] In the embodiments of the present application, the specific type of the above-mentioned positive electrode binder is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred solutions, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polyamide (PA), polyacrylonitrile (PAN), polyacrylate, polyvinyl ether, polymethyl methacrylate (PMMA), polyhexafluoropropylene and styrene-butadiene rubber (SBR).
[0075] In the embodiments of the present application, the specific type of the above-mentioned sulfide electrolyte is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific embodiments, the above-mentioned sulfide electrolyte includes at least one of Li6PS5Cl, Li3PS4, and Li 10 GeP2S 12 .
[0076] In some embodiments of the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, and the negative electrode active material layer contains a negative electrode active material, a negative electrode binder, a composite conductive agent and a sulfide electrolyte.
[0077] In some embodiments of the present application, the negative electrode current collector may adopt a metal foil or a composite current collector. For example, as the metal foil, copper foil, stainless steel foil, or titanium foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).
[0078] In some embodiments of this application, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium metal, etc. Silicon-based materials may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include at least one of elemental tin, tin oxide compounds, and tin alloys.
[0079] In some embodiments of this application, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), polyurethane (PU), and carboxymethyl chitosan (CMCS).
[0080] In some embodiments of this application, the negative electrode active layer may optionally include other additives, such as thickeners and plasticizers, including at least one of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol diethyl ether, 1,3-dioxolane, 1,4-dioxane, propylene carbonate, ethylene carbonate, diethyl carbonate or dimethyl carbonate, succinate, and adiponitrile.
[0081] In a fourth aspect, this application proposes a solid-state battery. According to embodiments of this application, the solid-state battery includes the composite conductive agent described in the first aspect, a composite conductive agent prepared by the method described in the second aspect, or an electrode described in the third aspect. This significantly improves the electrochemical performance of the solid-state battery, including higher initial discharge capacity, better cycle stability, optimized average discharge potential, lower voltage polarization, and significantly improved rate performance.
[0082] In some embodiments of this application, the solid-state battery includes a positive electrode, a negative electrode, and a polymer solid-state electrolyte membrane. During the charging and discharging process of the solid-state battery, active ions repeatedly insert and extract between the positive and negative electrode. The polymer solid-state electrolyte membrane acts as a conductor of ions between the positive and negative electrode.
[0083] The aforementioned solid-state batteries can be in the form of individual battery cells, battery modules, and battery packs. In some embodiments, individual battery cells can be assembled into battery modules, and the number of battery cells contained in a battery module can be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery module. In some embodiments, battery modules can also be assembled into battery packs, and the number of battery modules contained in a battery pack can be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0084] A fifth aspect of this application discloses an electrical device. According to an embodiment of this application, the electrical device includes a solid-state battery as described in the fourth aspect. The features and advantages described above for the solid-state battery also apply to this electrical device, and will not be repeated here.
[0085] Solid-state battery cells, solid-state battery modules, and solid-state battery packs can be used as power sources for electrical devices or as energy storage units for electrical devices. Electrical devices can include, but are not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0086] As electrical equipment, solid-state battery cells, solid-state battery modules, or solid-state battery packs can be selected according to their usage requirements.
[0087] As one example, the electrical device can be a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the electrical device for solid-state batteries, solid-state battery packs or solid-state battery modules can be used.
[0088] Another example of the device could be a mobile phone, tablet computer, laptop computer, etc. Such devices typically require a thin and light design and can use solid-state battery cells as a power source.
[0089] It should be noted that the features and advantages described above for solid-state batteries also apply to this electrical device, and will not be repeated here.
[0090] The embodiments of this application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. In addition, unless otherwise specified, all reagents used in the following embodiments are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also readily available to those skilled in the art.
[0091] Example 1 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid-phase acidification method: 1 g of conductive agent VGCF (fibrous, 150 nm in diameter, 5 μm in length) was placed in concentrated H2SO4:HNO3 = 3:1 (volume ratio) at 65 °C and ultrasonically treated for 6 h to introduce -OH / -COOH groups. The filtrate was washed with deionized water until the pH was >6, and then vacuum dried at 80 °C for 12 h to obtain activated VGCF.
[0092] 2) APTES-SAM self-assembly: 0.5 g of activated VGCF was dispersed in 100 mL of anhydrous toluene, and 10 mM of 3-aminopropyltriethoxysilane (APTES) was added. The mixture was stirred under nitrogen protection at room temperature (25 °C) for 4 h. After the reaction was completed, the mixture was washed 5 times with anhydrous toluene and 2 times with anhydrous ethanol, dried under nitrogen, and vacuum dried at 80 °C for 4 h to obtain APTES-SAM modified VGCF. The thickness of the SAM anchoring layer (i.e., APTES-SAM) was approximately 100 nm.
[0093] 3) Polyindole grafting growth: 0.2 g of APTES-SAM modified VGCF was dispersed in 50 mL of anhydrous chloroform, and 0.01 mol of indole and 0.03 mol of anhydrous FeCl3 were added. The reaction was carried out under nitrogen protection with stirring at room temperature for 24 h. After the reaction, the mixture was washed 5 times with chloroform and 3 times with methanol to remove residual FeCl3 and homopolymer. The mixture was then vacuum dried at 80 °C for 12 h to obtain APTES-SAM-assisted polyindole-coated VGCF. Indole underwent coupling polymerization at the 3-position under FeCl3 oxidation, while NH was retained and formed hydrogen bonds with -NH2 of APTES. Some NH underwent N-alkylation with -NH2 under alkaline post-treatment conditions to form covalent bonds. Finally, APTES-SAM-assisted polyindole-coated VGCF conductive material (i.e., APTES@polyindole-coated VGCF) was obtained, in which the polyindole layer thickness was approximately 100 nm.
[0094] 4) Solid-state cell preparation: 88 wt% of positive electrode active material NCM811 and 11.4 wt% of silver-germanium sulfide type solid electrolyte (Li) are used. 5.5 PS 4.5 Cl 1.5 A positive electrode slurry was prepared by mixing 0.2 wt% isobutyl isobutyrate binder, 0.3 wt% SAM-assisted polyindole-coated VGCF conductive material, and 0.1 wt% dispersant with isobutyl isobutyrate (IBIB) solvent. The slurry was then coated onto a current collector and dried to prepare the positive electrode sheet.
[0095] Hydrogenated styrene-butadiene block copolymer binder is dissolved in xylene, and then sulfide-germanium ore type solid electrolyte (Li 5.5 PS4.5 Cl 1.5 Add the above mixture to the mixture and mix. While mixing, add solvent to adjust the viscosity to 1500~2000 mPa·s. Coat the slurry onto a release film and remove most of the solvent at room temperature, then bake at 80°C for 4 h to form a solid electrolyte membrane.
[0096] The negative electrode active material is 89 wt% and the solid electrolyte is 10 wt% silver-germanium sulfide (Li) 5.5 PS 4.5 Cl 1.5 A negative electrode active material composition was prepared by mixing 0.5 wt% isobutyl isobutyrate binder, 0.4 wt% SAM-assisted polyindole-coated VGCF conductive material, and 0.1 wt% dispersant with isobutyl isobutyrate solvent. This composition was then coated onto a negative electrode current collector and dried to prepare the negative electrode sheet.
[0097] The positive electrode, solid electrolyte membrane, and negative electrode are stacked sequentially. The stacked cell is then sealed and subjected to warm isostatic pressing (WIP) at 500 MPa for 30 minutes at high temperature to obtain an all-solid-state battery cell. The pouch cell is then placed at room temperature and activated at 0.05 C, followed by 1 C cycle testing.
[0098] Example 2 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid phase acidification method: The conductive agent VGCF is fibrous with a diameter of 500nm and a length of 50μm. Other contents are the same as in Example 1.
[0099] 2) GPTMS-SAM self-assembly: 0.5 g of activated VGCF (fibrous, 500 nm in diameter, 50 μm in length) was dispersed in 100 mL of anhydrous toluene, and 10 mM of 3-glycidyl etheroxypropyltrimethoxysilane (GPTMS) was added. The mixture was stirred under nitrogen protection at room temperature for 4 h. The post-treatment was the same as in Example 1, resulting in GPTMS-SAM modified VGCF with a SAM anchoring layer (i.e., GPTMS-SAM) thickness of approximately 2 nm.
[0100] 3) Polyindole grafting growth: 0.2 g of GPTMS-SAM modified VGCF was dispersed in 50 mL of anhydrous chloroform, and 0.01 mol of indole and 0.03 mol of anhydrous FeCl3 were added. The reaction was carried out under nitrogen protection with stirring at room temperature for 24 h. The NH group of indole attacked the epoxy group of GPTMS, forming an N-CH2-CH(OH)-O-etheramine structure. At the same time, the polyindole chain grew from the 3-position under the oxidation of FeCl3. The post-treatment was the same as in Example 1 to obtain GPTMS-SAM-assisted polyindole-coated VGCF conductive material, wherein the polyindole layer thickness was approximately 50 nm.
[0101] 4) Solid-state cell preparation: Same as in Example 1.
[0102] Example 3 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid phase acidification method: The conductive agent VGCF is fibrous, with a diameter of 10nm and a length of 1μm. Other contents are the same as in Example 1.
[0103] 2) MPTMS-SAM self-assembly: 0.5 g of activated VGCF (fibrous, 10 nm in diameter, 1 μm in length) was dispersed in 100 mL of anhydrous ethanol, and 10 mM of 3-mercaptopropyltrimethoxysilane (MPTMS) was added. The mixture was stirred under nitrogen protection at room temperature for 6 h. The post-treatment was the same as in Example 1 to obtain MPTMS-SAM modified VGCF.
[0104] 3) SAM tailing conversion: MPTMS-SAM modified VGCF was dispersed in 30 mL of anhydrous THF, and 0.01 mol of N-(2-bromoethyl)maleimide and 0.01 mol of triethylamine were added. The mixture was stirred at room temperature for 12 h to allow the thiol group to undergo Michael addition with the maleimide, resulting in maleimide tailing SAM modified VGCF. The thickness of the SAM anchoring layer (i.e., maleimide tailing SAM) was approximately 50 nm.
[0105] 4) Polyindole Michael addition grafting: 0.2 g of maleimide-tailed SAM-modified VGCF was dispersed in 50 mL of anhydrous chloroform, and 0.01 mol of indole and 0.03 mol of anhydrous FeCl3 were added. The reaction was carried out under nitrogen protection at room temperature with stirring for 6 h. The 3-position carbon of the polyindole undergoes Michael addition with the electron-deficient double bond of the maleimide to form a stable C-C bond. The post-treatment was the same as in Example 1 to obtain MPTMS-SAM-assisted polyindole-coated VGCF, wherein the polyindole layer thickness was approximately 10 nm.
[0106] 5) Solid-state cell preparation: Same as in Example 1.
[0107] Example 4 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid phase acidification method: Same as in Example 1.
[0108] 2) SAM self-assembly: 0.5 g of activated VGCF (fibrous, 150 nm in diameter, 5 μm in length) was dispersed in 100 mL of anhydrous toluene, and 10 mM of 11-chloroformylundecyltrichlorosilane (ClCO-(CH2)) was added. 10-SiCl3), stirred under nitrogen protection at room temperature for 2 h. Post-treatment was the same as in Example 1 to obtain VGCF modified with acyl chloride tail SAM, wherein the thickness of the SAM anchoring layer (i.e., acyl chloride tail SAM) is approximately 2 nm.
[0109] 3) Polyindole amide bond grafting: 0.2 g of SAM-modified VGCF with an acyl chloride tail was dispersed in 30 mL of anhydrous pyridine, and 0.1 mol of indole was added. The mixture was stirred at room temperature for 12 h. The NH group of the indole reacted with the acyl chloride to form an amide bond (-CO-N<). Subsequently, 0.1 mol of anhydrous FeCl3 was added, and the mixture was stirred at room temperature for another 12 h to polymerize the indole. The post-treatment was the same as in Example 1 to obtain SAM-assisted polyindole-coated VGCF with an acyl chloride tail, wherein the polyindole layer thickness was approximately 20 nm.
[0110] 4) Solid-state cell preparation: Same as in Example 1.
[0111] Example 5 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid phase acidification method: Same as in Example 1.
[0112] 2) AEAPTMS-SAM self-assembly: 0.5 g of activated VGCF (fibrous, 150 nm in diameter, 5 μm in length) was dispersed in 100 mL of anhydrous toluene, and 10 mM of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AEAPTMS) was added. The mixture was stirred under nitrogen protection at room temperature for 4 h. The post-treatment was the same as in Example 1 to obtain AEAPTMS-SAM modified VGCF, wherein the thickness of the SAM anchoring layer (i.e., AEAPTMS) was approximately 1 nm.
[0113] 3) Polyindole grafting: 0.2 g of AEAPTMS-SAM modified VGCF was reacted with 0.1 mol indole and 0.4 mol FeCl3 in 30 mL of chloroform at room temperature for 12 h. Polyindole grafting was initiated by surface amino groups to obtain AEAPTMS-SAM-assisted polyindole-coated VGCF conductive material, wherein the thickness of the polyindole layer was approximately 5 nm.
[0114] 4) Solid-state cell preparation: Same as in Example 1.
[0115] Example 6 This embodiment provides a solid-state battery, the preparation method of which includes the following steps: 1) Liquid phase acidification method: Same as in Example 1.
[0116] 2) APTES-SAM self-assembly: Same as Example 1.
[0117] 3) Electrochemical polymerization of polyindole: APTES-SAM modified VGCF (fibrous, 150 nm in diameter, 5 μm in length) was coated onto a platinum sheet as the working electrode and placed in an electrolyte containing 0.05 mol / L indole and 0.1 mol / L LiClO4 in acetonitrile / dichloromethane (volume ratio 1:1). A platinum wire was used as the counter electrode. Ag / Ag + This serves as the reference electrode. At +0.9 V (vs Ag / Ag) + Polymerization was carried out at a constant potential for 60 min with a charge of 180 mC. Indole underwent anodic oxidation, resulting in coupling polymerization of the carbon at the 3-position, while NH4+ formed hydrogen bonds with the -NH2 group of APTES. Post-treatment: washing three times with acetonitrile, twice with chloroform, and vacuum drying at 80 °C for 12 h yielded APTES-SAM-assisted polyindole-coated VGCF conductive material, with a polyindole layer thickness of approximately 1 nm.
[0118] 4) Solid-state cell preparation: Same as in Example 1.
[0119] Example 7 This embodiment provides a solid-state battery, the preparation method of which is basically the same as that in Embodiment 1, except that: In Example 1, the conductive agent core was replaced with multi-walled carbon nanotubes (MWCNTs, fibrous, 75 nm in diameter, 2 μm in length) at a dosage of 0.5 g. The SAM self-assembly and polyindole grafting conditions were the same as in Example 1. Due to the larger specific surface area of CNTs, the SAM coverage density was higher, resulting in a more uniform polyindole coating layer. In the preparation of the all-solid-state battery, the conductive agent in both the positive and negative electrode plates was replaced with SAM-assisted polyindole-coated CNTs, while the remaining components remained the same as in Example 1.
[0120] Example 8 This embodiment provides a solid-state battery, the preparation method of which is basically the same as that in Embodiment 1, except that: In Example 1, the conductive agent core was replaced with acetylene black (granular, 40 nm particle size) at a dosage of 0.5 g. Due to the small size of the acetylene black particles, ultrasonic-assisted SAM self-assembly was used with an ultrasonic power of 100 W for 30 min to ensure uniform SAM coverage. The polyindole grafting conditions were the same as in Example 1. In the preparation of the all-solid-state battery, the conductive agent in both the positive and negative electrode plates was replaced with SAM-assisted polyindole-coated acetylene black, with the dosage adjusted accordingly. The remaining components were the same as in Example 1.
[0121] Example 9 This embodiment provides a solid-state battery, the preparation method of which is basically the same as that in Embodiment 1, except that: In Example 1, the conductive agent core was replaced with reduced graphene oxide (rGO, granular, 100 nm in diameter) at a dosage of 0.3 g. Due to the relatively few defect sites on the graphene surface, it was pretreated in oxygen plasma for 5 min before SAM self-assembly to introduce more -OH groups. The SAM self-assembly and polyindole grafting conditions were the same as in Example 1. In the preparation of the all-solid-state battery, the conductive agent in both the positive and negative electrode plates was replaced with SAM-assisted polyindole-coated graphene at a dosage of 0.2 wt%, with the remaining components being the same as in Example 1.
[0122] Example 10 This embodiment provides a solid-state battery, the preparation method of which is basically the same as that in Embodiment 1, except that: The indole monomer in Example 1 was replaced with 3-methylindole (0.01 mol). The 3-methyl substitution caused the polymerization to mainly occur at the 2-NC coupling and the 1,3-coupling, forming different linkage modes, but the NH group was still retained. The remaining steps were the same as in Example 1. Through hyperbranching, a special group was introduced to obtain a polyindole derivative, which enhanced the interfacial stability with the sulfide electrolyte.
[0123] Comparative Example 1 This comparative example provides a solid-state battery that uses unmodified VGCF as a conductive agent.
[0124] The positive electrode active material (NCM811) and the solid electrolyte (Li) are composed of 88 wt% positive electrode active material and 11.4 wt% silver-germanium sulfide type solid electrolyte (Li). 5.5 PS 4.5 Cl 1.5 A positive electrode slurry was prepared by mixing 0.2 wt% isobutyl butyrate (IBIB) binder, 0.3 wt% vapor-grown carbon fiber (VGCF, 150 nm in diameter and 5 μm in length) conductive material, and 0.1 wt% dispersant with isobutyl butyrate (IBIB) solvent. The slurry was then coated onto a current collector and dried to prepare the positive electrode sheet.
[0125] Hydrogenated styrene-butadiene block copolymer binder is dissolved in xylene, and then sulfide-germanium ore type solid electrolyte (Li 5.5 PS 4.5 Cl 1.5 Add the above mixture to the mixture. While mixing, add solvent to adjust the viscosity to 1500~2000 mPa·s. Coat the slurry onto the release film and remove most of the solvent at room temperature, then bake at 80°C for 4 h to form a solid electrolyte membrane.
[0126] The negative electrode active material is 89.1 wt% and the solid electrolyte is 10 wt% silver-germanium sulfide (Li) 5.5 PS 4.5 Cl1.5 A negative electrode active material composition was prepared by mixing 0.5 wt% isobutyl isobutyrate (IBIB) binder, 0.3 wt% vapor-grown carbon fiber (VGCF, 150 nm in diameter and 5 μm in length) conductive material, and 0.1 wt% dispersant with isobutyl isobutyrate (IBIB) solvent. This composition was then coated onto a negative electrode current collector and dried to prepare the negative electrode sheet.
[0127] The positive electrode, solid electrolyte membrane, and negative electrode are stacked sequentially. The stacked cell is then sealed and subjected to warm isostatic pressing (WIP) at 500 MPa for 30 minutes at high temperature to obtain an all-solid-state battery cell. The pouch cell is then placed at room temperature and activated at 0.05 C, followed by 1 C cycle testing.
[0128] Comparative Example 2 This comparative example provides a solid-state battery that uses physically mixed polyindole-coated VGCF as a conductive agent.
[0129] 0.1 g of commercial polyindole (Mn=10000) was dissolved in 10 mL of NMP, and 1 g of VGCF (150 nm in diameter and 5 μm in length) was added. The mixture was ultrasonically dispersed for 2 h and then stirred at room temperature for 12 h. The mixture was then dried in a forced-air oven at 60 °C for 6 h, and then baked under vacuum at 100 °C for 24 h to obtain a physically mixed polyindole / VGCF. The all-solid-state battery preparation was the same as in Comparative Example 1.
[0130] Comparative Example 3 This comparative example provides a solid-state battery that uses SAM-free direct polyindole-grafted VGCF as a conductive agent.
[0131] Activated VGCF (150 nm in diameter and 5 μm in length) was reacted directly with indole and FeCl3 in chloroform (same as step 3 in Example 1, but omitting the SAM self-assembly step). The all-solid-state battery was prepared in the same manner as in Comparative Example 1.
[0132] The solid-state batteries of Examples 1-10 and Comparative Examples 1-3 were tested for 1C discharge capacity and capacity retention after 100 cycles at room temperature (25°C). The results are shown in Table 1.
[0133] Table 1
[0134] As can be seen from Table 1, compared with Comparative Examples 1-3, the 1C discharge capacity and 100-cycle capacity retention of Examples 1-10 are effectively improved. It can be seen that by coating the surface of the conductive core with a self-assembled monolayer (SAM) assisted polyindole conductive polymer, the 1C discharge capacity and 100-cycle capacity retention of the solid-state battery can be effectively improved.
[0135] Figure 1 The image shown is a scanning electron microscope (SEM) image of the unmodified VGCF in Example 1. It can be seen that the surface of the unmodified VGCF carbon fiber is smooth and the diameter is about 150 nm.
[0136] Figure 2 The image shown is a scanning electron microscope (SEM) image of APTES@polyindole-coated VGCF in Example 1, which shows a clear "core-SAM-shell" three-layer structure with a diameter of about 400 nm.
[0137] Figure 3 The image shown is a transmission electron microscope (TEM) image of APTES@polyindole-coated VGCF in Example 1. A clear "core-SAM-shell" three-layer structure can be seen, with the SAM layer being approximately 100 nm and the polyindole layer being approximately 100 nm.
[0138] Figure 4 This is a comparison of the Fourier Transform Infrared (FTIR) spectra of APTES@polyindole-coated VGCF in Example 1, at 3400 cm⁻¹. -1 For NH stretching, 1080 cm -1 It is a Si-O-Si stretching vibration, 1100 cm. -1 ~1600 cm -1 It is a characteristic peak of the benzene ring, 740 cm⁻¹ -1 It is a characteristic peak of out-of-plane bending of the CH group of the benzene ring.
[0139] Figure 5 The image shows a comparison of the XRD patterns of APTES@polyindole-coated VGCF in Example 1. The characteristic peaks of the conductive agent are still visible before and after coating.
[0140] Figure 6 The above is the 1H NMR spectrum of APTES@polyindole-coated VGCF in Example 1. 7.03, 7.05, 7.10, and 7.54 are all aryl hydrogens of the indole ring, 4.16 is a methylene group (N-CH2) adjacent to the indole nitrogen, 3.83 is a methylene group (O-CH2) of ethoxysilane, 2.19 and 2.26 are methyl groups on the indole ring, 1.52 is a methylene group (CH2), 1.21 is a methyl group (CH3) of ethoxysilane, and 0.56 is a methylene group (Si-CH2) attached to silicon.
[0141] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0142] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A composite conductive agent, characterized in that, include: Conductive core; SAM anchoring layer, the SAM anchoring layer being disposed on at least a portion of the surface of the conductive agent core; A polymer functional layer disposed on at least a portion of the surface of the SAM anchoring layer away from the conductive core; The polymer functional layer includes at least one of polyindole and polyindole derivatives.
2. The composite conductive agent according to claim 1, characterized in that, The conductive agent core includes at least one of fibrous conductive agent core and granular conductive agent core. The fibrous conductive agent has an average diameter of 10 nm to 500 nm and an average length of 1 μm to 50 μm. The granular conductive agent has an average particle size of 20 nm to 500 nm. And / or, the conductive core includes at least one of vapor-grown carbon fiber, carbon nanotubes, acetylene black, conductive graphite, graphene, and superconducting carbon black.
3. The composite conductive agent according to claim 1, characterized in that, The thickness of the SAM anchoring layer is 1 nm to 100 nm; And / or, the SAM anchoring layer comprises at least one of a head-segment-tail compound, wherein the head group is selected from at least one of silyl, mercapto, phosphate, and carboxyl groups, and the segment is selected from C2~C3. 18 The chain may contain at least one of straight or branched alkylene chains, polyethylene glycol chains, or oligosiloxane chains, wherein the tail group is selected from at least one of amino, epoxy, isocyanate, maleimide, aldehyde, acyl chloride, or carboxyl groups. And / or, the SAM anchoring layer comprises at least one of 3-aminopropyltriethoxysilane, 3-glycidyl etheroxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 11-bromoundecyltrichlorosilane, 11-mercaptoundecanoic acid, 16-mercaptohexadecanoic acid, cysteine, 12-phosphododecanoic acid, phosphate-O-(2-aminoethyl) ester, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
4. The composite conductive agent according to any one of claims 1 to 3, characterized in that, The thickness of the polymer functional layer is 1 nm to 100 nm; And / or, the indole structural units of the polyindole derivative are repeatedly linked by 2,3-carbon-carbon bonds, 2,2-carbon-carbon bonds, 3,3-carbon-carbon bonds or 1,3-carbon-nitrogen bonds to form a main chain conjugated structure, wherein the benzene ring on the indole structural unit is unsubstituted or substituted by at least one substituent selected from at least one of alkyl, alkoxy, halogen, hydroxy, amino, nitro, cyano, carboxyl, ester, amide and sulfonic acid groups.
5. A method for preparing the composite conductive agent according to any one of claims 1 to 4, comprising: (1) Surface activation of the conductive agent core; (2) The activated conductive core, SAM molecules and the first solvent are mixed to obtain the first solution, stirred and post-treated to obtain the SAM-modified conductive core; (3) The SAM-modified conductive agent core, indole-containing monomer, oxidant and second solvent are mixed to obtain a second solution, and graft polymerization reaction is carried out. After post-treatment, the composite conductive agent is obtained. Alternatively, the SAM-modified conductive agent core can be used as the working electrode and placed in an electrolyte containing indole monomers and supporting electrolytes for electrochemical oxidation polymerization to obtain the composite conductive agent.
6. The method according to claim 5, characterized in that, In step (1), the conductive agent core is dispersed in concentrated H2SO4 / HNO3 mixed acid, ultrasonically treated at 60℃~80℃ for 2 h~12 h, and washed to obtain the activated conductive agent core; And / or, in step (2), stir for 2 h to 24 h; And / or, in step (2), the concentration of the SAM molecules in the first solution is 1 mM to 50 mM; And / or, in step (3), the temperature of the graft polymerization reaction is 20℃~60℃ and the time is 6 h~48 h; And / or, in step (3), the oxidant includes at least one of anhydrous FeCl3, ammonium persulfate, benzoyl peroxide, and iodine; And / or, in step (3), the molar ratio of the oxidant to the indole monomer is (1:1) to (4:1); And / or, in step (3), the concentration of the indole monomer in the second solution is 0.01 mol / L to 0.5 mol / L; And / or, in step (3), the concentration of the indole monomer in the electrolyte is 0.01 mol / L to 0.2 mol / L; And / or, in step (3), the supporting electrolyte is LiClO4 or Bu4NPF6; And / or, in step (3), the concentration of the supporting electrolyte in the electrolyte is 0.1 mol / L to 1 mol / L; And / or, in step (3), the conditions for the electrochemical oxidation polymerization are: constant potential 0.7 V~1.2 V, polymerization time 10 min~120 min; or cyclic voltammetry scan 0 V~1.5 V, 10~50 cycles.
7. An electrode sheet, characterized in that, The composite conductive agent includes any one of claims 1 to 4 or the composite conductive agent prepared by the method described in any one of claims 5 to 6.
8. The electrode sheet according to claim 7, characterized in that, Also includes: Sulfide electrolytes.
9. A solid-state battery, characterized in that, It includes the composite conductive agent according to any one of claims 1 to 4, the composite conductive agent prepared by the method according to any one of claims 5 to 6, or the electrode according to any one of claims 7 to 8.
10. An electrical appliance, characterized in that, It has the solid-state battery as described in claim 9.