A sodium battery self-generated negative electrode ladder coating and a preparation method thereof

By employing a stepped coating design in the self-generated negative electrode of sodium-ion batteries, the problems of uncontrollable sodium dendrite growth and high volume expansion stress are solved, thereby improving the safety and cycle life of sodium-ion batteries and enhancing their energy density and kinetic performance.

CN123120737APending Publication Date: 2026-11-17SUZHOU YIDONG XINNENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611497493.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Sodium-ion batteries suffer from problems such as uncontrollable sodium dendrite growth, high volume expansion stress leading to coating detachment, and high interfacial impedance, which affect battery safety and cycle life.

Method used

The stepped coating design includes a bottom sodium-loving sodium-storing conductive layer, a middle porous/mesoporous buffer layer, and a top sodium-loving protective layer. Through multi-layer co-extrusion coating technology and heat treatment, a through-hole microporous structure is formed. Combined with specific binders and fast ion conductors, the uniformity of sodium deposition and the safety performance of the battery are synergistically improved.

Benefits of technology

It significantly suppressed the risk of sodium dendrite puncture, reduced the interfacial charge transfer impedance, improved the battery's safety performance and cycle stability, and increased the battery's energy density and kinetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application relates to the technical field of sodium ion battery negative electrode materials, and particularly discloses a ladder type coating of a sodium battery self-generated negative electrode and a preparation method thereof. The ladder type coating is sequentially arranged on the surface of a current collector from bottom to top as a bottom sodium-attracting sodium-storing conductive layer, a middle porous / mesoporous buffer layer and a top sodium-attracting protective layer. The application uses a microporous aluminum foil with superfine pore diameter and large specific surface area as a current collector, forms a composite layer containing sodium-attracting inorganic particles and a protective interface on the outermost layer, provides large specific surface area and rich sodium-attracting active sites, guides sodium to realize uniform and dense deposition when entering from the outer layer, reserves sufficient volume expansion space to ensure free access, cooperates with a three-dimensional porous / mesoporous buffer network formed by in-situ pyrolysis of a pore-forming agent in the middle layer, and cooperates with conductive materials and three-dimensional copolymer binders to effectively release internal mechanical stress, and the application significantly improves the safety performance and cycle life of the negative electrode-free sodium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery anode material technology, specifically to a stepped coating for sodium-ion battery self-generating anode and its preparation method. Background Technology

[0002] In recent years, sodium-ion batteries have shown great application potential in energy storage and low-speed electric vehicles due to their abundant resources and low cost. Among them, self-generating negative electrode (or low-negative electrode, negative electrode-free) sodium-ion batteries do not contain negative electrode materials during initial assembly. Instead, they rely on sodium ions released from the positive electrode during the first charge to directly deposit on the current collector. This design eliminates most of the hard carbon, significantly improving the battery's energy density.

[0003] However, self-generated negative electrodes face the following technical drawbacks in practical applications: First, sodium metal easily forms dendritic sodium dendrites when deposited on the current collector surface, which can pierce the separator and cause a short circuit in the battery, posing a serious safety hazard. Second, the deposition and stripping of sodium ions are accompanied by significant volume expansion and contraction, leading to huge internal stress in conventional surface coatings, resulting in cracking, pulverization, and detachment. Third, uneven deposition causes a sharp increase in local interfacial impedance, reducing the battery's coulombic efficiency and cycle life. Fourth, the lack of use of microporous current collectors with ultra-high specific surface area results in a very limited coating areal loading. The current collector itself has a very small capacity, forcing a relatively thick coating to match the capacity of the positive electrode, resulting in a low energy density.

[0004] Existing modification methods mostly involve coating the current collector surface with a single layer of conductive carbon or a single layer of metalophilic layer. However, these homogeneous coatings cannot simultaneously resolve the physical contradictions of induced deposition, dendrite suppression, and accommodation of expansion stress. Based on the above, this invention proposes a stepped coating for the self-generating negative electrode of sodium-ion batteries and its preparation method. Summary of the Invention

[0005] To address the technical problems of uncontrollable sodium dendrite growth, high volume expansion stress leading to coating detachment, and high interfacial impedance in existing sodium-electric self-generated negative electrodes, this invention proposes a stepped coating for sodium-electric self-generated negative electrodes and its preparation method.

[0006] In a first aspect, the present invention provides a stepped coating for sodium-electric self-generated negative electrode, employing the following technical solution: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 3-5 parts of sodium-loving nucleating agent, 10-25 parts of conductive carbon skeleton, and 8-10 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 20-40 parts of porous carbon material, 5-20 parts of pore-forming agent, and 5-8 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 15-35 parts of fast ion conductor, 10-20 parts of sodium-loving inorganic particles, and 10-12 parts of a third binder.

[0007] Preferably, the sodium-loving nucleating agent is one or more of nano-silver, nano-zinc, nano-bismuth, nano-tin, nano-zinc oxide, porous micron-sized zinc oxide, titanium nitride, or carbon nitride, and the D50 particle size of the sodium-loving nucleating agent is 30-80 nm.

[0008] Preferably, the conductive carbon skeleton is carbon nanotubes, graphene, or high specific surface area conductive carbon black.

[0009] Preferably, the first adhesive is polyethyleneimine.

[0010] Preferably, the porous carbon material is one or more of mesoporous hard carbon, carbon nanotubes, hollow carbon spheres, or porous carbon nanofibers; and the specific surface area of ​​the porous carbon material is 20-500 m². 2 / g.

[0011] Preferably, the pore-forming agent is polypropylene carbonate.

[0012] Preferably, the second adhesive is a butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer, prepared by the following method: Solvent was added to the reactor, and after argon gas was passed through to remove oxygen, butyl acrylate, maleic anhydride and acrylonitrile were added in sequence. After stirring evenly, an initiator was added, and the reaction system was heated to 70-80℃. After reacting at a constant temperature for 10-14 hours, the product was dropped into a large amount of deionized water to precipitate, filtered, washed and vacuum dried to obtain a butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0013] This invention synthesizes a three-dimensional copolymer of butyl acrylate, maleic anhydride, and acrylonitrile through a specific monomer mass ratio. The butyl acrylate provides the flexibility of the polymer long chain to buffer mechanical deformation, the maleic anhydride provides polar functional groups to enhance the interfacial bonding force with carbon materials and current collectors, and the acrylonitrile imparts good resistance to electrolyte swelling and electrochemical stability to the polymer.

[0014] Preferably, the solvent is anhydrous N,N-dimethylformamide.

[0015] Preferably, the mass ratio of butyl acrylate, maleic anhydride and acrylonitrile is 4-6:2-4:1-3.

[0016] Preferably, the amount of solvent used is 4-6 times the total mass of butyl acrylate, maleic anhydride and acrylonitrile.

[0017] Preferably, the initiator is azobisisobutyronitrile.

[0018] Preferably, the amount of the initiator is 0.4-0.6% of the total mass of butyl acrylate, maleic anhydride and acrylonitrile.

[0019] Preferably, the washing refers to washing with anhydrous ethanol 3-5 times.

[0020] Preferably, the vacuum drying temperature is 50-70℃ and the vacuum drying time is 18-24h.

[0021] Preferably, the fast ion conductor is one or more of the following: NASICON-type solid electrolyte, halide solid electrolyte, anti-perovskite solid electrolyte, or polymer-based solid electrolyte.

[0022] Preferably, the current collector is a microporous aluminum foil, consisting of one or a superposition of disordered and ordered pores, with a porosity of 30-70, an average pore diameter of 21 μm for disordered pores and 50 μm for ordered pores, and a thickness of 15-30 μm for the microporous aluminum foil.

[0023] Preferably, the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0024] Preferably, the stepped coating has a full-layer sodium-loving structure, and the top layer forms a composite layer interface containing sodium-loving inorganic particles, which synergistically guides sodium deposition.

[0025] Secondly, the present invention provides a method for preparing the above-mentioned stepped coating for sodium-ion self-generated negative electrode, using the following technical solution: A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. The raw materials of the bottom sodium-loving sodium-storing conductive component, the middle porous / mesoporous buffer component, and the top sodium-loving protective component are mixed with solvents and dispersed evenly to obtain the bottom slurry, the middle slurry, and the top slurry. S2. Using multi-layer co-extrusion coating technology or sequential layer-by-layer coating technology, the bottom layer slurry, the middle layer slurry, and the top layer slurry are coated on the surface of the current collector in sequence. S3. The coated current collector is subjected to gradient drying, followed by heat treatment under a protective atmosphere to generate a through-hole microporous structure inside the coating, resulting in a stepped coating that generates a sodium electrode.

[0026] Preferably, in step S1, the solvent for preparing the bottom layer slurry and the middle layer slurry is tetrahydrofuran, and the solvent for preparing the top layer slurry is anhydrous xylene.

[0027] Preferably, in step S1, the solid content of the bottom layer slurry is 8-12%, the solid content of the middle layer slurry is 20-30%, and the solid content of the top layer slurry is 15-25%.

[0028] Preferably, in step S3, the gradient drying parameters are: controlling the linear speed at 50-80 m / min, and performing roll-to-roll dynamic drying sequentially at temperatures of 60-80℃ and 60-120℃.

[0029] Preferably, in step S3, the heat treatment parameters are: dynamic heat treatment is performed on a roll-to-roll production line by passing through a heat treatment zone with a set temperature of 150-180℃ at a linear speed of 50-80m / min.

[0030] This invention limits the heat treatment parameters in the preparation method; the specific heat treatment temperature range not only ensures that the pore-forming agent can be decomposed by heat to generate gas and form pores, but also avoids the thermal degradation of the polymer binder in the coating due to excessive temperature, thereby maintaining the mechanical stability of the stepped coating while realizing the construction of a porous network.

[0031] In summary, the present invention has the following beneficial effects: This invention utilizes the strong sodium-affinity nucleation sites in the bottom layer and the top layer, which also possesses sodium-affinity properties, in synergy. The top layer does not reject sodium, and through methods such as composite sodium-affinity inorganic particles, a composite layer interface containing sodium-affinity inorganic particles is directly formed on the outermost layer. This interface not only provides a large specific surface area and a sufficient number of active sites to accommodate sodium deposition, allowing for uniform and dense sodium deposition, but also, with the fast ion conductor and microporous structure, it provides ample expansion space, ensuring free access channels and fundamentally suppressing the risk of surface sodium dendrite puncture, thus improving the battery's safety performance.

[0032] The present invention achieves microporous coating by in-situ pyrolysis of the pore-forming agent, forming a three-dimensional ion transport channel that runs through the entire structure. This structure significantly increases the effective contact area between the coating and the electrolyte, reduces the local real exchange current density, thereby significantly reducing the interfacial charge transfer impedance and improving the kinetic performance of charging and discharging.

[0033] This invention, by controlling the thickness of the middle layer to be maximized and rich in microporous networks, reserves sufficient buffer space for the drastic volume expansion caused by sodium deposition, effectively releasing internal mechanical stress; thereby ensuring the uniformity and density of the sodium deposition layer, avoiding coating powdering and peeling, and thus endowing the sodium-generated negative electrode with excellent long-term cycling stability.

[0034] In this invention, a three-dimensional copolymer of butyl acrylate, maleic anhydride, and acrylonitrile is used as the second binder in the middle layer. The butyl acrylate segments provide excellent flexibility, effectively accommodating volume expansion during charge and discharge. The maleic anhydride segments are rich in polar functional groups, significantly enhancing adhesion between porous carbon skeletons and between the coating and adjacent layers. The acrylonitrile segments provide excellent resistance to electrolyte swelling and electrochemical stability. The synergistic effect of these three components ensures the structural integrity of the porous / mesoporous buffer layer during long-term cycling, preventing powdering and detachment caused by stress accumulation within the coating, and greatly extending the battery's cycle life.

[0035] This invention employs a gradient drying and heat treatment process. Gradient drying enables the smooth evaporation of water and a small amount of solvent from the multilayer coating structure, avoiding macroscopic cracking caused by the rapid escape of each coating layer and ensuring consistency. Heat treatment at a suitable temperature ensures the compatibility between the decomposition of the pore-forming agent and the stable structure of the binder, guaranteeing the uniformity of the three-dimensional pore structure. Detailed Implementation

[0036] The present invention will be further described in detail below with reference to the embodiments.

[0037] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0038] Among them, the conductive carbon black is Super P, with a particle size of 30nm, brand name Baochi, and purchased from Tianjin Baochi Chemical Technology Co., Ltd.

[0039] Polyethyleneimine: 50% content (molecular weight 7w), purchased from Wuhan Camic Technology Co., Ltd.

[0040] Styrene-ethylene-butene-styrene block copolymer: SEBS 6159, purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd.

[0041] Polyvinylidene fluoride: Grade 1100, brand: Kureha, Japan, purchased from Shanghai Xincheng Hongtai Plastics Technology Co., Ltd.

[0042] Examples 1-3 provide a stepped coating for sodium-ion self-generated negative electrode and its preparation method.

[0043] Example 1 A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0044] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0045] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0046] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 5:3:2. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a three-dimensional copolymer of butyl acrylate-maleic anhydride-acrylonitrile.

[0047] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0048] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 20%, a middle slurry with a solid content of 25%, and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0049] Example 2 A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 15 parts of sodium-loving nucleating agent, 25 parts of conductive carbon skeleton, and 8 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 40 parts of porous carbon material, 20 parts of pore-forming agent, and 10 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 35 parts of fast ion conductor, 20 parts of sodium-loving inorganic particles, and 18 parts of a third binder.

[0050] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 50nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0051] Porous carbon materials have a specific surface area of ​​500 m². 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0052] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 6:4:3. The amount of anhydrous N,N-dimethylformamide was 6 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 600 rpm for 20 min until homogeneous. Then, azobisisobutyronitrile (0.6% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 80℃ and reacted at a constant temperature for 10 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed 5 times with anhydrous ethanol, and dried under vacuum at 70℃ for 18 h to obtain a butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0053] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 65%, an average pore size of 50 μm, and a thickness of 30 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0054] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 25%, a middle slurry with a solid content of 30%, and a top slurry with a solid content of 25%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 80 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 80°C and 120°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 180°C at a linear speed of 80 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0055] Example 3 A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 5 parts of sodium-loving nucleating agent, 10 parts of conductive carbon skeleton, and 2 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 20 parts of porous carbon material, 5 parts of pore-forming agent, and 3 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 15 parts of fast ion conductor, 10 parts of sodium-loving inorganic particles, and 3 parts of a third binder.

[0056] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 20μm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0057] Porous carbon materials have a specific surface area of ​​20 m². 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0058] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 4:2:1. The amount of anhydrous N,N-dimethylformamide was 4 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 400 rpm for 40 min until homogeneous. Then, azobisisobutyronitrile (0.4% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 70℃ and reacted at a constant temperature for 14 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed three times with anhydrous ethanol, and dried under vacuum at 50℃ for 24 h to obtain a three-dimensional copolymer of butyl acrylate-maleic anhydride-acrylonitrile.

[0059] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 40%, an average pore size of 30 μm, and a thickness of 16 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0060] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 15%, a middle slurry with a solid content of 20%, and a top slurry with a solid content of 15%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a linear speed of 50 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 60°C and 100°C. Then, under an argon atmosphere, it is dynamically heat-treated in a heat treatment zone at a set temperature of 150°C at a linear speed of 50 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0061] To verify the comprehensive performance of the stepped coating for the sodium-ion self-generated negative electrode prepared in Examples 1-3 of this invention, Comparative Examples 1-8 were set up, wherein: Comparative Example 1 Comparative Example 1 is the same as Example 1, except that it does not involve layered coating. Details are as follows: A coating comprising, by relative mass parts of each component, 4 parts of a sodium-loving nucleating agent, 18 parts of a conductive carbon skeleton, 9 parts of a first binder, 30 parts of a porous carbon material, 12 parts of a pore-forming agent, 6.5 parts of a second binder, 25 parts of a fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0062] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0063] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0064] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 5:3:2. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a three-dimensional copolymer of butyl acrylate-maleic anhydride-acrylonitrile.

[0065] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4).12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0066] A method for preparing a coating includes the following steps: S1. Using the same amount as in the previous example, all raw materials are mixed with tetrahydrofuran and anhydrous xylene, and dispersed evenly to obtain a mixed slurry; S2. Apply the mixed slurry to the surface of the current collector; S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min, thereby generating a permeable microporous structure within the coating to obtain the coating.

[0067] Comparative Example 2 Comparative Example 2 is the same as Example 1, except that it lacks the underlying sodium-loving, sodium-storing, and conductive layer. Specifically: A stepped coating for sodium-electric self-generated negative electrode, wherein the stepped coating consists of a middle porous / mesoporous buffer layer and a top sodium-loving protective layer from bottom to top on the current collector surface. Based on the relative mass parts of each component, the intermediate porous / mesoporous buffer layer is prepared from an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder; The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0068] Among them, the porous carbon material has a specific surface area of ​​260 m². 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0069] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 5:3:2. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a three-dimensional copolymer of butyl acrylate-maleic anhydride-acrylonitrile.

[0070] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0071] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw material of the middle layer porous / mesoporous buffer component with tetrahydrofuran, and mix the raw material of the top layer sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a middle layer slurry with a solid content of 25% and a top layer slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the middle layer slurry and the top layer slurry are applied sequentially to the surface of the current collector; S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0072] Comparative Example 3 Comparative Example 3 is the same as Example 1, except that it lacks a middle porous / mesoporous buffer layer. Specifically: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0073] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0074] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0075] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving and sodium-storing conductive component with tetrahydrofuran, and mix the raw materials of the top sodium-loving protective component with anhydrous xylene. Disperse them evenly to obtain a bottom slurry with a solid content of 20% and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry and the top layer slurry are applied sequentially to the surface of the current collector. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0076] Comparative Example 4 Comparative Example 4 is the same as Example 1, except that it lacks a top sodium-loving protective layer. Details are as follows: A stepped coating for sodium-electric self-generated negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer and a middle porous / mesoporous buffer layer on the surface of the current collector, from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder.

[0077] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0078] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

[0079] The butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile was controlled at 5:3:2. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate, maleic anhydride, and acrylonitrile were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a three-dimensional copolymer of butyl acrylate-maleic anhydride-acrylonitrile.

[0080] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. The raw materials of the bottom sodium-loving and sodium-storing conductive component and the middle porous / mesoporous buffer component are respectively mixed with tetrahydrofuran and dispersed evenly to obtain a bottom slurry with a solid content of 20% and a middle slurry with a solid content of 25%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry and the middle layer slurry are coated on the surface of the current collector in sequence; S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0081] Comparative Example 5 Comparative Example 5 is the same as Example 1, except that the second adhesive used is polyvinylidene fluoride. Details are as follows: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 0 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0082] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0083] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is polyvinylidene fluoride.

[0084] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0085] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 20%, a middle slurry with a solid content of 25%, and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0086] Comparative Example 6 Comparative Example 6 is the same as Example 1, except that the second binder is a butyl acrylate-maleic anhydride two-dimensional copolymer. Details are as follows: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0087] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0088] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-maleic anhydride two-dimensional copolymer.

[0089] The butyl acrylate-maleic anhydride two-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate to maleic anhydride was controlled at 5:3. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate and maleic anhydride. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate and maleic anhydride were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate and maleic anhydride) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain the butyl acrylate-maleic anhydride two-dimensional copolymer.

[0090] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0091] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 20%, a middle slurry with a solid content of 25%, and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0092] Comparative Example 7 Comparative Example 7 is the same as Example 1, except that the second binder is a styrene-maleic anhydride two-dimensional copolymer. Details are as follows: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0093] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0094] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is styrene-maleic anhydride two-dimensional copolymer.

[0095] The styrene-maleic anhydride two-dimensional copolymer is prepared by the following method: The mass ratio of styrene to maleic anhydride was controlled at 5:3. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of styrene and maleic anhydride. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, styrene and maleic anhydride were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of styrene and maleic anhydride) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a styrene-maleic anhydride two-dimensional copolymer.

[0096] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0097] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 20%, a middle slurry with a solid content of 25%, and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0098] Comparative Example 8 Comparative Example 8 is the same as Example 1, except that the second adhesive is a butyl acrylate-acrylonitrile two-dimensional copolymer. Details are as follows: A stepped coating for sodium-electric self-generating negative electrode, wherein the stepped coating consists of a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface from bottom to top. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 4 parts of sodium-loving nucleating agent, 18 parts of conductive carbon skeleton, and 9 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 30 parts of porous carbon material, 12 parts of pore-forming agent, and 6.5 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 25 parts of fast ion conductor, 15 parts of sodium-loving inorganic particles, and 11 parts of a third binder.

[0099] Among them, the sodium-loving nucleating agent is nano-zinc with a D50 particle size of 30nm; the conductive carbon skeleton is conductive carbon black; and the first binder is polyethyleneimine.

[0100] Porous carbon material with a specific surface area of ​​260 m² 2 / g porous carbon nanofibers; the pore-forming agent is polypropylene carbonate; the second binder is butyl acrylate-acrylonitrile two-dimensional copolymer.

[0101] The butyl acrylate-acrylonitrile two-dimensional copolymer is prepared by the following method: The mass ratio of butyl acrylate to acrylonitrile was controlled at 5:2. The amount of anhydrous N,N-dimethylformamide was 5 times the total mass of butyl acrylate and acrylonitrile. Anhydrous N,N-dimethylformamide was added to the reactor, and after purging with argon gas for 30 min to remove oxygen, butyl acrylate and acrylonitrile were added sequentially. The mixture was stirred at 500 rpm for 30 min until homogeneous. Then, azobisisobutyronitrile (0.5% of the total mass of butyl acrylate and acrylonitrile) was added. The reaction system was heated to 75℃ and reacted at a constant temperature for 12 h. The product was then dropped into a large amount of deionized water to precipitate, filtered, washed four times with anhydrous ethanol, and dried under vacuum at 60℃ for 21 h to obtain a two-dimensional copolymer of butyl acrylate and acrylonitrile.

[0102] The fast ion conductor is a NASICON-type solid electrolyte (Na3Zr2Si2PO4). 12 The current collector is a microporous aluminum foil with a porosity of 52%, an average pore size of 21 μm, and a thickness of 22 μm; the third binder is a styrene-ethylene-butene-styrene block copolymer.

[0103] A method for preparing a stepped coating for sodium-ion self-generated negative electrode includes the following steps: S1. Mix the raw materials of the bottom sodium-loving sodium-storing conductive component and the middle porous / mesoporous buffer component with tetrahydrofuran respectively, and mix the raw material of the top sodium-loving protective component with anhydrous xylene. Disperse evenly to obtain a bottom slurry with a solid content of 20%, a middle slurry with a solid content of 25%, and a top slurry with a solid content of 20%. S2. Using a sequential layer-by-layer coating technique, the bottom layer slurry, the middle layer slurry, and the top layer slurry are applied to the surface of the current collector in sequence. S3. With a controlled linear speed of 65 m / min, the coated current collector is dynamically dried in roll-to-roll configuration at temperatures of 70°C and 110°C. Subsequently, under an argon atmosphere, it undergoes dynamic heat treatment by passing through a heat treatment zone at a set temperature of 165°C at a linear speed of 65 m / min. This process generates a permeable microporous structure within the coating, resulting in a stepped coating that allows the sodium electrode to generate its own negative electrode.

[0104] The comprehensive performance of the stepped coatings for sodium-ion self-generated negative electrodes prepared in Examples 1-3 and Comparative Examples 1-8 of this invention was tested respectively.

[0105] All electrochemical tests were conducted using aluminum foil with a stepped coating as the working electrode and CR2032 coin cell half-cells or full cells assembled with sodium metal sheet as the counter electrode. The electrolyte used in the test cells consisted of 1.0M NaPF6 dissolved in a 1:1 volume ratio mixture of ethylene carbonate (EC) and diethyl carbonate (DEC), with 5wt% fluoroethylene carbonate (FEC) added as an additive.

[0106] 1. Contact area ratio: The specific surface area and porosity analyzer was used to test the specific surface area of ​​the electrode coating at liquid nitrogen temperature (77K) in accordance with the national standard GB / T19587-2017 "Determination of specific surface area of ​​solid materials by gas adsorption BET method". The test results were then calculated as a ratio to the geometric area of ​​the aluminum foil. 2. Interfacial Impedance (Rct, Ω): An electrochemical workstation was used to perform AC impedance spectroscopy measurements after the assembled half-cell had been left to stand for 24 hours. The test frequency range was set from 100 kHz to 10 mHz, and the AC amplitude was set to 5 mV. The charge transfer impedance value was obtained by fitting an equivalent circuit. 3. Deposition volume expansion rate (%): For assembled sodium-coated half-cells, at 1 mA / cm²... 2 Deposition at current density of 3mAh / cm 2 Sodium metal. The battery was disassembled in an argon glove box. After cleaning and drying the electrodes, the electrode cross-section was cut using a cross-linked ion beam. The percentage change in electrode coating thickness before and after charging and discharging was measured by field emission scanning electron microscopy. 4. Coulombic efficiency (%) at 50th cycle: Assembled sodium-coated half-cell, at 1 mA / cm² 2 At a current density of 1 mAh / cm, a 1 mAh / cm² deposit was made on the working electrode. 2 The sodium metal was then charged to 1V for sodium removal, and the coulombic efficiency of the 50th charge-discharge cycle was recorded. 5. Long-term cycle stability: The test was conducted in accordance with the national standard GB / T 31484-2015 "Cycle Life Requirements and Test Methods for Power Batteries for Electric Vehicles," using sodium vanadium phosphate (Na3V2(PO4)3) as the positive electrode. Under constant temperature conditions of 25℃, the voltage test range was set to 2.5 to 3.8V, and constant current charge-discharge tests were performed at a constant rate of 5C. The discharge capacity of the 1000th cycle was recorded and compared with the discharge capacity of the first cycle to calculate the cycle capacity retention rate (%).

[0107] The test results are shown in Table 1: Table 1: Note: Data marked with a number indicates that the battery experienced significant dendritic short-circuit failure in the later stages of cycling.

[0108] As shown in Table 1, the stepped coatings for sodium-ion batteries that generate their own negative electrodes in Examples 1-3 of this invention exhibit excellent and balanced comprehensive performance in terms of increasing specific surface area, reducing interfacial impedance, suppressing deposition volume expansion, improving coulombic efficiency, and enhancing long-term cycling stability, which are significantly better than those in Comparative Examples 1-8.

[0109] As can be seen from Example 1 and Comparative Example 1, after the stepped structure was replaced with a homogeneous coating, the coating lost the driving force for directional nucleation and the porous space to accommodate it, resulting in a significant increase in interfacial impedance, a significant increase in volume expansion rate, and the inability to suppress sodium dendrite growth, ultimately leading to short-circuit failure of the battery.

[0110] As can be seen from Example 1 and Comparative Example 2, when the underlying sodium-loving sodium-storing conductive layer is missing, the bottom of the coating lacks sufficient electron and sodium-loving sites. Sodium tends to be deposited locally in the top or middle layers, causing increased volume expansion and easy penetration of the coating to form dendrites, resulting in short-circuit failure.

[0111] As can be seen from Example 1 and Comparative Example 3, the absence of a middle porous / mesoporous buffer layer leads to a complete loss of buffer space in the system, a surge in the deposition volume expansion rate, and coating peeling resulting in extremely low cycle retention rate.

[0112] As can be seen from Example 1 and Comparative Example 4, the absence of the top sodium-loving protective layer results in the surface being directly exposed to the electrolyte. This leads to the loss of the composite layer interface formed by sodium-loving inorganic particles on the outermost layer, which provides a large specific surface area, sodium-loving active deposition sites, and reserved expansion space. Consequently, it is impossible to smoothly guide the uniform entry and dense deposition of sodium ions. Sodium tends to grow rapidly on the surface as dendrites, causing short circuits.

[0113] As can be seen from Example 1 and Comparative Example 5, after replacing the second adhesive in the middle layer with polyvinylidene fluoride, the adhesive lacks sufficient flexibility and polar functional group adhesion, and cannot effectively resist the accumulation of small volume deformation stress during long-term cycling, resulting in the gradual powdering of the coating interior and a significant decrease in cycle capacity retention.

[0114] As can be seen from Example 1 and Comparative Example 6, after replacing the middle layer binder with butyl acrylate-maleic anhydride two-dimensional copolymer, the acrylonitrile segment is missing, the coating's resistance to electrolyte swelling decreases, and side reactions are prone to occur when immersed in electrolyte for a long time, resulting in increased interfacial impedance and reduced cycle capacity retention.

[0115] As can be seen from Example 1 and Comparative Example 7, replacing the middle layer binder with a styrene-maleic anhydride two-dimensional copolymer, which lacks butyl acrylate and acrylonitrile segments, results in insufficient binder flexibility, making it unable to effectively buffer the volume expansion stress during charge and discharge, thus causing microcracks in the coating. On the other hand, the coating's resistance to electrolyte swelling decreases, and long-term immersion in electrolyte can easily trigger side reactions, leading to increased interfacial impedance and a significant decrease in cycle stability.

[0116] As can be seen from Example 1 and Comparative Example 8, after replacing the middle layer adhesive with butyl acrylate-acrylonitrile two-dimensional copolymer, the maleic anhydride fragment is missing, the polar functional groups in the adhesive molecule are reduced, the adhesion between the porous carbon skeleton and between the coating and the current collector is weakened, resulting in the coating peeling off during charge-discharge cycles, causing local sodium dendrite growth and internal short circuit failure.

[0117] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A stepped coating for sodium-ion self-generated negative electrode, characterized in that, The stepped coating consists of, from bottom to top, a bottom sodium-loving sodium-storing conductive layer, a middle porous / mesoporous buffer layer, and a top sodium-loving protective layer on the current collector surface. Based on the relative mass parts of each component, the bottom sodium-loving sodium-storing conductive layer is made from the bottom sodium-loving sodium-storing conductive component, which includes 3-5 parts of sodium-loving nucleating agent, 10-25 parts of conductive carbon skeleton, and 8-10 parts of first binder. The intermediate porous / mesoporous buffer layer is made of an intermediate porous / mesoporous buffer component, which includes 20-40 parts of porous carbon material, 5-20 parts of pore-forming agent, and 5-8 parts of second binder. The top sodium-loving protective layer is made from a top sodium-loving protective component, which includes 15-35 parts of fast ion conductor, 10-20 parts of sodium-loving inorganic particles, and 10-12 parts of a third binder.

2. The stepped coating for sodium-electric self-generated negative electrode according to claim 1, characterized in that, The sodium-loving nucleating agent is one or more of nano-silver, nano-zinc, nano-bismuth, nano-tin, nano-zinc oxide, porous micron-sized zinc oxide, titanium nitride, or carbon nitride, and the D50 particle size of the sodium-loving nucleating agent is 30-80 nm; the conductive carbon framework is carbon nanotubes, expanded graphite, graphene, or high specific surface area conductive carbon black; the first binder is polyethyleneimine.

3. The stepped coating for sodium-ion self-generated negative electrode according to claim 1, characterized in that, The porous carbon material is one or more of mesoporous hard carbon, carbon nanotubes, hollow carbon spheres, or porous carbon nanofibers; and the specific surface area of ​​the porous carbon material is 20-500 m². 2 / g; the pore-forming agent is polypropylene carbonate.

4. The stepped coating for sodium-electric self-generated negative electrode according to claim 1, characterized in that, The second adhesive is a three-dimensional copolymer of butyl acrylate, maleic anhydride, and acrylonitrile, prepared by the following method: Solvent was added to the reactor, and after argon gas was passed through to remove oxygen, butyl acrylate, maleic anhydride and acrylonitrile were added in sequence. After stirring evenly, an initiator was added, and the reaction system was heated to 70-80℃. After reacting at a constant temperature for 10-14 hours, the product was dropped into a large amount of deionized water to precipitate, filtered, washed and vacuum dried to obtain a butyl acrylate-maleic anhydride-acrylonitrile three-dimensional copolymer.

5. The stepped coating for sodium-electric self-generated negative electrode according to claim 4, characterized in that, The mass ratio of butyl acrylate, maleic anhydride, and acrylonitrile is 4-6:2-4:1-3; the amount of solvent used is 4-6 times the total mass of butyl acrylate, maleic anhydride, and acrylonitrile; and the amount of initiator used is 0.4-0.6% of the total mass of butyl acrylate, maleic anhydride, and acrylonitrile.

6. The stepped coating for sodium-electric self-generated negative electrode according to claim 1, characterized in that, The fast ion conductor is one or more of the following: NASICON-type solid electrolyte, halide solid electrolyte, anti-perovskite solid electrolyte, or polymer-based solid electrolyte; the current collector is a microporous aluminum foil, consisting of one or a superposition of disordered and ordered pores, with a porosity of 30-70, an average pore diameter of 21 μm for disordered pores and 50 μm for ordered pores, and a thickness of 15-30 μm for the microporous aluminum foil; the third binder is a styrene-ethylene-butene-styrene block copolymer.

7. A method for preparing a stepped coating for a sodium-ion self-generated negative electrode as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. The raw materials of the bottom sodium-loving sodium-storing conductive component, the middle porous / mesoporous buffer component, and the top sodium-loving protective component are mixed with solvents and dispersed evenly to obtain the bottom slurry, the middle slurry, and the top slurry. S2. Using multi-layer co-extrusion coating technology or sequential layer-by-layer coating technology, the bottom layer slurry, the middle layer slurry, and the top layer slurry are coated on the surface of the current collector in sequence. S3. The coated current collector is subjected to gradient drying, followed by heat treatment under a protective atmosphere to generate a through-hole microporous structure inside the coating, resulting in a stepped coating that generates a sodium electrode.

8. The method for preparing the stepped coating for sodium-ion self-generated negative electrode according to claim 7, characterized in that, In step S1, the solid content of the bottom layer slurry is 8-12%, the solid content of the middle layer slurry is 20-30%, and the solid content of the top layer slurry is 15-25%.

9. The method for preparing the stepped coating for sodium-ion self-generated negative electrode according to claim 7, characterized in that, In step S3, the gradient drying parameters are: controlling the linear speed at 50-80 m / min, and performing roll-to-roll dynamic drying at temperatures of 60-80℃ and 100-120℃ respectively.

10. The method for preparing the stepped coating of the sodium-electric self-generated negative electrode according to claim 7, characterized in that, In step S3, the heat treatment parameters are as follows: on the roll-to-roll production line, dynamic heat treatment is performed by passing through a heat treatment zone with a set temperature of 60-120℃ at a linear speed of 50-80m / min.