A composite current collector, its preparation method, electrode and battery

By depositing a metal oxide or non-metal oxide interface layer on the pore walls of the polymer base film and combining it with a surface metal layer, the problem of poor interface state inside the pores of the perforated base film is solved, and the interface inside the pores is strengthened and the surface metal layer is firmly attached, thereby improving the stability and conductivity of the composite current collector.

CN123120751APending Publication Date: 2026-11-17JIANGSU ENPACK COMPOSITE CURRENT COLLECTORS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611541230.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the interface state inside the pores of the perforated base film is poor, and the adhesion of the surface metal layer to the inner wall of the pore is insufficient. This causes the composite current collector to easily peel off and fall off during processing and cycling, affecting its conductivity and cycle life.

Method used

A metal oxide or non-metal oxide interface layer is deposited on the pore walls of a polymer-based film. An atomic layer deposition process is used to form the pore wall oxide interface layer, which is combined with the surface metal layer to form a chemically bonded and mechanically interlocked interface structure, thereby improving the interfacial strength within the pores.

Benefits of technology

It improves the interface state within the pores, enhances the adhesion of the surface metal layer, improves the long-term stability and conductivity of the composite current collector, and reduces the risk of failure during processing and battery cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120751A_ABST
    Figure CN123120751A_ABST
Patent Text Reader

Abstract

This invention relates to a composite current collector, its preparation method, an electrode, and a battery. The composite current collector comprises a polymer base film, a pore wall oxide interface layer, and a surface metal layer. The pore wall oxide interface layer is disposed on the pore wall of the through-hole, and the pore wall oxide interface layer comprises a metal oxide or a non-metal oxide. The surface metal layer is disposed on opposite sides of the polymer base film. The surface metal layer is formed and adhered in the orifice region of the through-hole, and contacts and bonds with the pore wall oxide interface layer, connecting the surface metal layers on opposite sides of the polymer base film through the pore wall oxide interface layer. This invention also provides an electrode comprising the composite current collector and a battery comprising the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a composite current collector, its preparation method, electrode, and battery. Background Technology

[0002] Composite current collectors typically use polymer films (such as PET and PP) as the base film, with conductive metal layers formed on opposite sides to replace traditional metal foils. This type of structure offers significant advantages in reducing weight, increasing battery energy density, improving flexibility, and limiting needle-puncture short circuits. However, the conductive metal layer and the polymer base film are two different materials, and an interfacial bonding problem remains. This means the interfacial adhesion between the surface metal layer and the base film needs further improvement, making it prone to peeling and detachment during subsequent processing or battery cycling, severely affecting the conductivity and cycle life of the composite current collector.

[0003] To address the need for further improvement in the interfacial adhesion between the surface metal layer and the base film, existing technologies have employed methods such as corona treatment, plasma activation, or coating with organic adhesive layers to modify the base film surface, aiming to enhance the interfacial bonding strength between the surface metal layer and the polymer base film. However, with the continuous development of composite current collector technology, the industry's demand for weight reduction in composite current collectors has increased to further reduce their weight and improve battery energy density, leading to the industry's exploration of perforated base films.

[0004] While the introduction of perforated substrate films further reduces the weight of composite current collectors, it also presents a significant challenge to the deposition of surface metal layers. The perforated substrate films possess complex three-dimensional microporous structures with limited internal space. Current mainstream processes for preparing surface metal layers (such as vacuum evaporation and magnetron sputtering) struggle to allow metal to effectively penetrate and uniformly cover the micropore walls of the substrate film. This results in conventional processes causing the surface metal layer to remain primarily on the outer surface of the substrate film, failing to form effective deposition on the pore walls. Even if a very small amount of metal enters the pores, the lack of chemical bonding sites on the polymer pore walls prevents the surface metal layer from firmly adhering to the pore walls.

[0005] Therefore, how to improve the interface state within the pores of the perforated substrate film, strengthen the interface within the pores, and enhance the adhesion of the metal layer on the substrate film surface has become a pressing technical problem to be solved in this field. The above content is only for assisting in understanding the technical solution of this invention and does not imply an admission that the above content is prior art. Summary of the Invention

[0006] The main objective of this invention is to provide a composite current collector, its preparation method, electrode, and battery, aiming to solve the aforementioned technical problems in the prior art.

[0007] To achieve the above objectives, the present invention provides a composite current collector, the composite current collector comprising: Polymer-based film, with through-holes throughout; A pore wall oxide interface layer is disposed on the pore wall of the through hole, and the pore wall oxide interface layer comprises metal oxide or non-metal oxide; A surface metal layer is disposed on opposite sides of the polymer base film; The surface metal layer is formed and attached in the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall, thereby connecting the surface metal layers on opposite sides of the polymer base film through the oxide interface layer of the hole wall.

[0008] Preferably, in the composite current collector, the pore wall oxide interface layer comprises Al2O3 or SiO2, and the thickness of the pore wall oxide interface layer is L1, 3nm≤L1≤8nm; And / or, The surface metal layer has a single-sided thickness of 0.5~2μm, and the surface metal layer includes aluminum or its alloy; And / or, The diameter of the through hole is D, and the hole spacing is H, where 8μm≤D≤20μm and 50μm≤H≤200μm.

[0009] Preferably, in the composite current collector, an outer surface oxide layer is further provided between the polymer base film and the surface metal layer, and the thickness of the outer surface oxide layer is 1~3nm.

[0010] To achieve the above objectives, the present invention also provides a method for preparing the above-mentioned composite current collector, comprising: A through-hole is formed in the polymer base film; Metal oxides or non-metal oxides are deposited on the pore walls of the through-hole using atomic deposition technology to form an oxide interface layer on the pore walls; Metal is deposited on opposite sides of the polymer base film to form a surface metal layer. The surface metal layer adheres to the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall. The surface metal layers on opposite sides of the polymer base film are connected through the oxide interface layer of the hole wall.

[0011] Preferably, in the method for preparing the composite current collector, the step of depositing a metal oxide or non-metal oxide on the pore wall of the through-hole using atomic deposition to form a pore wall oxide interface layer includes: The polymer-based film with the aforementioned through-holes is introduced into the atomic layer deposition cavity; Using trimethylaluminum and water as precursors for alternating pulses, atomic layer deposition is performed on the pore walls of the through-holes, allowing metal oxides or non-metal oxides to nucleate and grow in a conformal manner on the pore walls; The number of atomic layer deposition cycles is controlled to make the thickness of the pore wall oxide interface layer 3~8nm.

[0012] Preferably, in the method for preparing the composite current collector, before the step of forming a through-hole in the polymer base film, the method further includes: The polymer base film is surface activated to introduce oxygen-containing functional groups onto its surface, and an organic passivation layer is formed on the outer surface of the activated polymer base film. The thickness of the organic passivation layer is L2, where 200 nm ≤ L2 ≤ 1 μm.

[0013] Preferably, in the method for preparing the composite current collector, after depositing metal oxide or non-metal oxide on the pore wall of the through-hole using atomic deposition to form a pore wall oxide interface layer, and before depositing a surface metal layer on opposite sides of the polymer base film, the method further includes: The outer surface of the polymer base film is treated to remove the organic passivation layer and / or the outer surface oxide layer.

[0014] Preferably, in the method for preparing the composite current collector, forming a through-hole in the polymer base film includes: A pulsed laser is used to punch holes in the polymer base film, forming through holes in the polymer base film. The pulsed laser has a wavelength of 355nm, a pulse width of 10~50ps, a single pulse energy of 1~20μJ, 1~5 pulses per aperture, and a repetition frequency of 0.5~5MHz.

[0015] Preferably, in the method for preparing the composite current collector, after depositing metal oxides or non-metal oxides on the pore walls of the through-hole using atomic deposition to form a pore wall oxide interface layer, and before depositing metals on opposite sides of the polymer base film to form a surface metal layer, the method further includes: The outer surface of the polymer base film is treated to remove the organic passivation layer and / or the outer surface oxide layer.

[0016] Preferably, in the method for preparing the composite current collector, the deposition of surface metal layers on opposite sides of the polymer base film, wherein the surface metal layers adhere to and bond with the oxide interface layer of the pore wall in the orifice region of the through-hole, and the surface metal layers on opposite sides of the polymer base film are connected through the oxide interface layer of the pore wall, includes: A base layer is deposited on both sides of the polymer base film by magnetron sputtering. The base layer forms an adhesion in the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall. A thickened layer is deposited on the substrate by vacuum evaporation, so that the single-sided thickness of the surface metal layer reaches 0.5~2μm, and the surface metal layers on opposite sides of the polymer base film are connected through the orifice area of ​​the through hole. The surface metal layer includes aluminum or its alloy.

[0017] Furthermore, the present invention also provides an electrode sheet comprising any of the above-described composite current collectors or a composite current collector prepared by the above-described preparation method.

[0018] Furthermore, the present invention also provides a battery comprising the aforementioned electrode sheets.

[0019] The present invention has at least the following beneficial effects: The composite current collector provided by this invention includes a polymer base film, a pore wall oxide interface layer, and a surface metal layer. The polymer base film has through-holes; the pore wall oxide interface layer is disposed on the pore wall of the through-holes, and the pore wall oxide interface layer comprises metal oxides or non-metal oxides; the surface metal layer is disposed on opposite sides of the polymer base film; wherein the surface metal layer adheres to the pore opening region of the through-hole and contacts and bonds with the pore wall oxide interface layer, connecting the surface metal layers on opposite sides of the polymer base film through the pore wall oxide interface layer. This improves the intrapore interface state of the perforated base film, strengthens the intrapore interface, and enhances the adhesion of the surface metal layer of the base film.

[0020] Furthermore, due to the complex three-dimensional micropore structure of the perforated substrate film and the narrow space within the pores, conventional metallization processes such as vacuum evaporation and magnetron sputtering are insufficient to allow metal to effectively enter and uniformly cover the inner walls of the pores. The metal layer essentially remains only on the outer surface of the substrate film. Even if a very small amount of metal enters the pores, the lack of chemical bonding sites on the inner walls of the polymer pores makes it difficult for the metal layer to adhere firmly. Taking the Al2O3-containing oxide interface layer on the pore wall as an example, this invention sets an Al2O3-containing oxide interface layer on the pore wall of the perforation. This oxide interface layer can form Al-OC-like bonds with the oxygen-containing functional groups on the surface of the polymer pore wall, and provides compositional gradients and mechanical interlocking through the organic-inorganic hybrid transition region formed by the near-surface penetration of the precursor, thereby forming a synergistic interface structure of chemical bonding and mechanical interlocking on the pore wall. After the surface metal layer forms an adhesion in the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall, the Al2O3 at the edge of the orifice becomes an anchor point connecting the polymer base film and the surface metal layer. This allows the surface metal layer to form a firm bond with the base film through the oxide interface layer of the hole wall, thereby improving the internal interface state of the perforated base film, strengthening the internal interface and enhancing the surface metal layer of the base film, without having to rely on the metal layer penetrating deep into the micropores to achieve internal connection.

[0021] Furthermore, by controlling the cycle number, selective deposition lifetime and process stability are ensured. As the ALD cycle number increases, the physical adsorption of trimethylaluminum on the outer surface may gradually form new nucleation sites, leading to increased leakage growth on the outer surface and a gradual decrease in selectivity. This invention uses the ALD cycle number as a process control item, ensuring that the Al2O3 thickness on the pore wall reaches 3-8 nm while controlling the residual Al2O3 on the outer surface to 1-3 nm, and in principle not exceeding 5 nm. This allows for the deposition of the pore wall interface layer within the selectivity window, avoiding an increase in the outer surface contact resistance due to excessively high cycle numbers, thereby ensuring the consistency and reliability of selective deposition on the pore wall in mass production.

[0022] Furthermore, by controlling the upper limit of the oxide thickness on the pore walls, a balance is achieved between interfacial strengthening and mechanical reliability. Excessive Al2O3 thickness may cause the interfacial structure to change from a "metal-polymer bonding" to a "metal-brittle oxide-polymer" structure, thereby reducing peel resistance and bending resistance. This invention preferably controls the Al2O3 thickness on the pore walls to 3-8 nm, with an upper limit not exceeding 10 nm, allowing Al2O3 to function as a transition layer for chemical bonding sites and mechanical interlocking, rather than allowing the brittle oxide layer to dominate the interfacial mechanical response. This improves interfacial bonding while avoiding bending cracking and interfacial embrittlement caused by excessive oxide thickness, ensuring the mechanical reliability of the composite current collector under winding, bending, and thermal cycling conditions.

[0023] Furthermore, by controlling the carbonization of the pore walls, the interface of the pore walls is ensured to have low carbonization and a continuous morphology. During laser drilling, carbonization may occur in the pore wall region of the base film, with a small amount of oxygen-containing carbon or sp... 2 Carbon promotes initial nucleation, but thick carbonized layers can absorb water, weaken subsequent interfaces, and potentially introduce side reactions. This invention aims to maintain a low degree of carbonization on the pore walls, ensuring "low carbonization and continuous morphology." This exposes the polymer surface rich in reactive functional groups after laser depassivation, while avoiding the negative impact of thick carbonized layers on Al2O3 nucleation and interfacial bonding. This promotes uniform nucleation and shape-preserving growth of Al2O3 on the pore walls, improving the bonding quality between the oxide interfacial layer and the polymer pore walls. Attached Figure Description

[0024] Figure 1 A cross-sectional view of the composite current collector provided by the present invention; Figure 2 A flowchart of the method for preparing the composite current collector provided by the present invention in the first embodiment; Figure 3 A flowchart of the method for preparing the composite current collector provided by the present invention in a second embodiment; Figure 4 The flowchart of the method for preparing the composite current collector provided by the present invention in the third embodiment.

[0025] 1-Polymer base film, 11-Through pores, 2-Pore wall oxide interface layer, 3-Surface metal layer.

[0026] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0027] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The present invention will be described in detail below with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features in the embodiments of the present invention can be combined with each other.

[0028] In this embodiment of the invention, the term "and / or" describes the relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. The character " / " generally indicates that the preceding and following associated objects have an "or" relationship.

[0029] It should be noted that the terms "first," "second," etc., in the specification, claims, and drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.

[0030] In this embodiment of the invention, the term "multiple" refers to two or more, and other quantifiers are similar.

[0031] In this invention, unless otherwise stated, directional terms such as "upper," "lower," "top," and "bottom" are generally used in relation to the direction shown in the accompanying drawings, or in relation to the vertical, perpendicular, or gravitational direction of the component itself; similarly, for ease of understanding and description, "inner" and "outer" refer to the inner and outer contours of each component itself, but the above directional terms are not intended to limit this invention.

[0032] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the various embodiments of the present invention will be described in detail below with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details are presented in the embodiments of the present invention to facilitate a better understanding of the invention. However, the technical solutions claimed in the present invention can be implemented even without these technical details and various variations and modifications based on the following embodiments. The division of the following embodiments is for ease of description and should not constitute any limitation on the specific implementation of the present invention. The various embodiments can be combined with and referenced by each other without contradiction.

[0033] The pores in perforated substrate films have a significant characteristic: small pore size (micrometer scale). Although vacuum evaporation and magnetron sputtering are currently the mainstream processes for metallizing composite current collectors, their deposition mechanisms make it difficult for them to form an effective coating on the inner walls of deep pores.

[0034] Vacuum evaporation relies on the condensation of metal vapor on the surface of a substrate to form a film. During the evaporation process, the metal vapor is transported from the evaporation source to the substrate surface in an almost linear trajectory. When there are large micropores on the substrate surface, the vapor molecules are blocked at the pore openings, and only a very small number of vapor molecules incident at a certain angle can enter the pores. After entering the pores, the vapor molecules rapidly lose energy during collisions with the pore walls, making it difficult to form continuous deposition deep within the pore walls. Therefore, the evaporated metal can only remain on the outer surface of the substrate, and the inner walls of the pores are almost not effectively covered.

[0035] Magnetron sputtering relies on high-energy ions in plasma bombarding the target material, causing target atoms to be sputtered out at high energy and deposited on the surface of the base film. Sputtered atoms have higher energy than vapor-deposited atoms and possess a certain diffraction capability, making them easier to penetrate shallow holes or aperture regions than vapor-deposited atoms. However, when facing larger micropores, the transport of sputtered atoms within the pore is still limited by both geometric obstruction and collisions with the pore walls. Sputtered atoms can form a certain coverage in the aperture region, but the deposition flux decays faster the deeper into the pore. Therefore, although sputtering can improve the coverage in the aperture region, it is still difficult to form a continuous and uniform surface metal layer in the middle of the aperture wall and at the bottom of the aperture.

[0036] More importantly, even if a small amount of metal enters the pores, the inner walls of the polymer pores themselves lack active sites that can form chemical bonds with the metal. The adhesion of metal to the polymer surface mainly relies on physical effects such as van der Waals forces, resulting in limited interfacial bonding strength. During subsequent processing or battery cycling, the metal inside the pores is easily peeled off from the pore walls, making it difficult to form a stable and reliable intrapore interface.

[0037] Therefore, for perforated base films, the state of the interface inside the holes and the adhesion reliability of the metal layer in the hole area still need to be improved, especially the interface inside the holes and the adhesion of the metal layer on the surface of the base film need to be strengthened.

[0038] To address this issue, the present invention provides a composite current collector comprising a polymer base film 1, a pore wall oxide interface layer 2, and a surface metal layer 3. The polymer base film 1 has a through-hole 11 extending through it; the pore wall oxide interface layer 2 is disposed on the pore wall of the through-hole 11, and the pore wall oxide interface layer 2 comprises a metal oxide or a non-metal oxide; the surface metal layer 3 is disposed on opposite sides of the polymer base film 1; wherein the surface metal layer 3 is formed and adhered in the orifice region of the through-hole 11 and contacts and bonds with the pore wall oxide interface layer 2, connecting the surface metal layers 3 on opposite sides of the polymer base film 1 through the pore wall oxide interface layer 2.

[0039] It should be noted that the polymer base film 1 can be, but is not limited to, PET or PPS, and can also be extended to PI or PEN, with a preferred thickness of 4~12μm. The pore wall oxide interface layer 2 can, but is not limited to, contain Al2O3 or SiO2. The surface metal layer can, but is not limited to, contain aluminum or its alloys.

[0040] The present invention first deposits a layer of metal oxide or non-metal oxide (i.e., pore wall oxide interface layer 2) on the pore wall. The pore wall oxide interface layer 2 undertakes the functions of strengthening the interface inside the pore and fixing the pore opening. Then, the surface metal layer 3 is allowed to contact and bond with this oxide layer in the pore opening area.

[0041] Furthermore, before metallization, this invention first constructs a nanoscale metal oxide or non-metal oxide interface layer on the pore wall of the through-hole 11, transforming the weak bonding interface within the pore from a "polymer-metal" interface to a strong bonding interface of "polymer-metal oxide or non-metal oxide-metal". Since the base film after perforation has a large three-dimensional microporous structure, the interface state of the pore wall and the bonding reliability of the pore opening region significantly affect the long-term stability of the composite current collector. Therefore, by pre-constructing a continuous pore wall oxide interface layer, a stable bonding interface and pore opening anchoring structure are provided for the subsequent surface metal layer 3, which is beneficial for strengthening the pore interface and improving the adhesion of the metal layer 3 on the base film surface.

[0042] Furthermore, an atomic layer deposition (ALD) process is used to form a metal oxide or non-metal oxide interface layer on the pore walls. ALD involves alternating pulses of gaseous precursors into the pores. These precursor molecules are small in size and have strong diffusion capabilities, allowing them to reach the middle and bottom of the pore walls. Through self-limiting surface chemical reactions, metal oxides or non-metal oxides grow layer by layer. Therefore, even in confined pore spaces, a conformal, continuous nanoscale oxide layer can be formed on the pore walls. This metal oxide or non-metal oxide layer itself does not provide electrical conductivity but instead provides chemical bonding sites and pore-hole fixing structures for the subsequent surface metal layer 3. This improves the pore interface state of the perforated substrate film, enhances pore interface stability, and increases the adhesion of the surface metal layer 3.

[0043] Taking the Al2O3-containing oxide interface layer on the pore wall as an example, from the perspective of interface bonding principle, Al2O3 can form Al-OC-like bonds with oxygen-containing functional groups on the surface of the polymer pore wall. At the same time, the organic-inorganic hybrid transition region formed by the near-surface infiltration of the precursor provides compositional gradation and mechanical interlocking. In this way, the pore wall interface is upgraded from the original physical adhesion to a synergistic effect of chemical bonding and mechanical interlocking. The surface metal layer 3 is attached to the orifice region of the through hole 11 and contacts and bonds with the pore wall oxide interface layer 2. The pore wall oxide interface layer 2 connects the surface metal layers 3 on opposite sides of the polymer base film 1. At the same time, the Al2O3 at the edge of the orifice forms a reliable anchoring structure with the surface metal layer 3, thereby reducing the risk of peeling and detachment of the outer surface metal layer 3 during subsequent processing or battery cycling.

[0044] Furthermore, the metal oxide or non-metal oxide on the pore wall coats and passivates the heat-affected zone and orifice region formed by laser drilling, which can inhibit thermal shrinkage, pore collapse, and crack propagation in the pore area, and delay the erosion of the polymer on the pore wall by water, oxygen, and electrolyte, thus improving the stability of the pore interface under long-term immersion and circulation conditions. Therefore, this invention achieves pore interface strengthening and orifice fixation through the metal oxide or non-metal oxide interface layer on the pore wall, thereby improving the interfacial bonding strength and long-term reliability of the drilled composite current collector.

[0045] The aperture of the through-hole 11 is D, and the aperture spacing is H, where 8μm≤D≤20μm and 50μm≤H≤200μm. Aperture D refers to the opening size of the through-hole 11 on the surface of the polymer base film 1. When the aperture is too large, for example, significantly exceeding 20μm, although laser drilling is easier and the internal space of the hole is relatively spacious, a single through-hole 11 occupies too much base film area, which weakens the continuity of the base film in that area. The coverage span of the surface metal layer 3 at the edge of the aperture increases, and the surface metal layer 3 is prone to being suspended or incompletely covered in the aperture area. It also reduces the number of through-holes 11 that can be arranged per unit area, which is not conducive to achieving uniform weight reduction under the same aperture ratio. When the pore size is too small, for example, significantly less than 8 μm, although it is beneficial to maintain the continuity of the base film, the internal space of the pores is further reduced, making the diffusion and residence of atomic layer deposition precursors within the pores more difficult. This increases the difficulty of conformal deposition of metal oxides or non-metal oxides on the pore walls and reduces the thickness uniformity between the pore bottom and the pore opening. Simultaneously, the increased precision requirements of laser drilling make it more difficult to control burrs, residues, and carbonization at the pore opening, and also affects the adhesion of the surface metal layer 3 in the pore opening region and the reliability of the connection between the pore wall oxide interface layer 2 and the surface metal layers 3 on both sides. Therefore, controlling the pore size D within the range of 8 μm to 20 μm is the preferred range, balancing weight reduction and process stability, while ensuring conformal deposition of metal oxides or non-metal oxides on the pore walls, reliable coverage of the pore opening surface metal layer 3, and contact and bonding with the pore wall oxide interface layer 2.

[0046] The aperture spacing H refers to the center distance between two adjacent through holes 11. The aperture spacing needs to be set in conjunction with the aperture diameter to jointly determine the porosity and the uniformity of the pore area distribution. When the aperture spacing is too large, for example, significantly exceeding 200 μm, the number of through holes 11 per unit area decreases, resulting in a lower porosity. Although the continuity of the base film is better and the loss of mechanical properties is smaller, the weight reduction effect is limited, making it difficult to meet the requirements for further increasing the energy density of the battery. At the same time, the number of pore openings that contact and bond with the oxide interface layer 2 of the pore wall is reduced, which is not conducive to the stable connection of the metal layers 3 on both sides through the oxide interface layer 2 of the pore wall. When the aperture spacing is too small, for example, significantly less than 50 μm, the base film spacing between adjacent vias 11 is too narrow, the polymer wall thickness between the aperture regions is insufficient, and stress concentration easily forms in the base film within the aperture region. This can lead to the propagation of inter-aperture cracks or aperture collapse during subsequent processing or battery cycling. Simultaneously, if the distance between adjacent apertures is too close, the surface metal layer 3 is prone to mutual interference when covering the aperture region. Furthermore, the diffusion and purging of the precursor within the dense aperture group during atomic layer deposition (ALD) is more difficult to achieve uniformity, and the thickness uniformity of Al2O3 on the aperture walls decreases. Therefore, controlling the aperture spacing H within the range of 50 μm to 200 μm is the preferred range, balancing weight reduction, base film integrity, and ALD process uniformity, while ensuring uniform aperture distribution, reliable aperture contact, and reliable connection between the surface metal layers on both sides.

[0047] The thickness of the pore wall oxide interface layer 2 is L1, where 3nm ≤ L1 ≤ 8nm. If the thickness of the pore wall oxide interface layer 2 is too small, Al2O3 cannot form a continuous and complete coverage on the pore wall, resulting in locally exposed polymer areas or pinhole defects. These defective areas cannot form effective Al-OC bonds with the subsequent surface metal layer 3, and the pore wall interface remains primarily physically attached. After bending, thermal cycling, or electrolyte immersion, these areas are prone to becoming the starting point of interface failure. Simultaneously, if the thickness is too thin, the Al2O3's coating and passivation effect on the laser heat-affected zone and pore burrs is insufficient, significantly reducing the improvement effect on the thermomechanical stability and electrolyte erosion resistance of the pore area. The pore pore area may still become the starting point of subsequent failure. If the thickness of the pore wall oxide interface layer 2 is too large, the interface will change from a "metal-polymer bonding" structure to a "metal-brittle oxide-polymer" structure. The brittleness of the Al2O3 layer itself will become a stress concentration area during bending and thermal cycling, leading to a decrease in the interface's peel resistance and bending resistance. Meanwhile, excessively thick Al2O3 significantly increases the brittleness of the pore walls, easily leading to microcracks in the pore opening region, which in turn reduces the bonding reliability between the metal layer 3 on the pore opening surface and the pore wall oxide. Furthermore, excessively thick Al2O3 also increases the ALD cycle number, affecting the production cycle time, and may weaken the selective deposition effect due to the missed growth of the precursor on the outer surface. Therefore, controlling the thickness L1 of the pore wall oxide interface layer 2 within 3~8 nm strikes a balance between "sufficient interfacial chemical bonding" and "controllable interfacial brittleness." Below 3 nm, the interface coverage is incomplete, chemical bonding sites are insufficient, and the passivation effect is limited; above 8 nm, interfacial brittleness increases, bending and peel resistance decreases, and the production cycle time and selectivity control become more difficult. By setting 3 nm ≤ L1 ≤ 8 nm, Al2O3 can form sufficient Al-OC bonding and an organic-inorganic hybrid transition region with the polymer pore walls without introducing the risk of brittle failure due to excessive thickness, thus achieving a superior overall performance between pore wall interface strengthening, pore opening fixation, and long-term stability.

[0048] This invention provides a method for preparing a composite current collector. Examples of this method include the examples of the composite current collector described above, and the beneficial effects of the composite current collector can be applied to the method for preparing the composite current collector. Similarly, examples of the composite current collector described above include examples of the method for preparing the composite current collector, and the beneficial effects of the method for preparing the composite current collector can be applied to the composite current collector.

[0049] like Figure 2 As shown, the preparation method of the composite current collector includes steps S3000, S4000, and S6000.

[0050] In step S3000, a through hole 11 is formed in the polymer base film 1, penetrating the polymer base film 1.

[0051] It should be noted that the polymer base film 1 can be, but is not limited to, PET or PPS, and can also be extended to PI or PEN, with a thickness preferably of 4~12μm.

[0052] Specifically, step S3000 includes step S3100.

[0053] Step S3100 uses a pulsed laser to punch holes in the polymer base film 1, forming through holes 11 that penetrate the polymer base film 1. The pulsed laser has a wavelength of 355 nm, a pulse width of 10-50 ps, ​​a single pulse energy of 1-20 μJ, 1-5 pulses per hole, and a repetition frequency of 0.5-5 MHz. Pulsed lasers are used instead of mechanical punching or chemical etching because laser drilling offers high precision, controllable heat-affected zones, and ease of integration with roll-to-roll production lines. Furthermore, ultrashort pulsed lasers reduce burrs, residue, and carbonization at the hole opening, ensuring a favorable hole morphology for subsequent formation of the surface metal layer 3 in the hole opening region and its contact and bonding with the oxide interface layer 2 on the hole wall.

[0054] The wavelength of 355nm belongs to the ultraviolet band. Polymer materials have a high absorption rate for lasers in this band, and the energy is mainly concentrated on the surface of the material, which is conducive to achieving fine drilling and reducing the spread of the heat-affected zone to the area around the hole.

[0055] The ps-level pulse width falls within the ultra-short pulse range, with an extremely short single-pulse duration. This allows for ablation and removal of material before significant thermal diffusion occurs, thereby reducing the heat-affected zone at the orifice opening and minimizing carbonization and burrs. Excessive pulse width, such as in the nanosecond (ns) level, increases thermal diffusion time, making the area around the orifice prone to melting, recasting, carbonization, and burrs, affecting the uniform nucleation of Al2O3 on the orifice wall and the coverage of the surface metal layer 3 at the orifice opening. Conversely, insufficient pulse width, such as in the fs level, while resulting in a smaller heat-affected zone, increases equipment costs and production cycle pressure, and places higher demands on roll-to-roll tape stability. Therefore, the optimal pulse width for this invention is 10-50 ps.

[0056] The single-pulse energy determines whether a single pulse can effectively remove the base film material and form a through-hole. If the energy is too low, a single pulse is insufficient to penetrate the base film, requiring an increase in the number of pulses or the repetition frequency, leading to decreased drilling efficiency and potentially irregular hole morphology. If the energy is too high, the heat-affected zone around the hole expands, easily forming burrs, residues, and carbonization, and may even cause deformation of the base film around the hole, affecting the uniformity of subsequent ALD deposition and the reliability of the surface metal layer 3. A single-pulse energy of 1~20μJ represents the optimal range for minimizing thermal damage at the hole opening while ensuring effective removal of the base film material by a single pulse.

[0057] The combination of the above laser parameters results in the through hole 11 having regular hole shape, low burrs and carbonization degree, and small heat-affected zone during the formation process. This is beneficial for the subsequent uniform nucleation and shape-preserving growth of Al2O3 by the ALD precursor on the hole wall, and also for the surface metal layer 3 to form a continuous coverage in the hole opening area and reliably contact and bond with the Al2O3 on the hole wall.

[0058] The through-hole 11 can be, but is not limited to, a straight through-hole 11 or a bidirectional oblique hole. Inert gas purging and vacuum chip removal are used during processing to reduce residue, burrs, and carbonization at the hole opening. The dimensions of the through-hole 11 can be referenced in the above embodiments and will not be repeated here.

[0059] In step S4000, metal oxides or non-metal oxides are deposited on the hole wall of the through hole 11 using an atomic deposition process to form a hole wall oxide interface layer 2.

[0060] It should be noted that atomic layer deposition involves the alternating pulses of gaseous precursors into the pores. These precursor molecules are small in size and have strong diffusion capabilities, enabling them to reach the middle and bottom of the pore walls. Through self-limiting surface chemical reactions, they grow layer by layer of metal oxides or non-metal oxides (such as Al₂O₃ or SiO₂). Therefore, even in confined spaces, a conformal and continuous nanoscale oxide layer can be formed on the pore walls. By forming a layer of nanoscale metal oxides or non-metal oxides on the pore walls of through-hole 11, the pore interface is transformed from a weak "polymer-metal" interface to a strong "polymer-metal oxide or non-metal oxide-metal" interface.

[0061] Specifically, step S4000 includes steps S4100 to S4300.

[0062] Step S4100 involves introducing the polymer-based film 1 with the through-holes 11 into the atomic layer deposition chamber.

[0063] In step S4200, trimethylaluminum and water are used as precursors for alternating pulses to perform atomic layer deposition on the hole wall of the through hole 11, so that metal oxides or non-metal oxides (e.g., Al2O3 or SiO2) nucleate and grow in a conformal manner on the hole wall.

[0064] It should be noted that by alternating pulses of trimethylaluminum and water, a self-limiting surface chemical reaction is carried out on the pore wall, enabling the nucleation and shape-preserving growth of metal oxides or non-metal oxides (such as Al2O3 or SiO2) on the pore wall.

[0065] Taking Al2O3 as an example of an oxide interface layer on the pore wall, trimethylaluminum molecules are small in size and highly reactive, allowing them to diffuse into the micropores and react with oxygen-containing functional groups such as hydroxyl groups on the pore wall surface to form Al-O bonds. Water, acting as an oxygen source, reacts with the surface Al-CH3 groups, restoring the surface hydroxyl groups and releasing methane, completing one cycle. Due to the self-limiting nature of atomic layer deposition, each cycle deposits only a nominal thickness of about 0.1~0.13 nm. Therefore, even in a small pore space, a conformal and continuous Al2O3 layer can be formed in the middle of the pore wall and at the bottom of the pore, unlike vacuum evaporation or magnetron sputtering which are limited by shadowing effects and scattering losses.

[0066] The process temperature can be 60~120℃, with PET and PPS preferably not exceeding 100℃ and PEN preferably not exceeding 110℃. This is because excessively high process temperatures may cause thermal deformation or thermal degradation of the polymer base film 1, affecting the dimensional stability and pore integrity of the base film; excessively low temperatures may lead to insufficient precursor reactivity, a decrease in Al2O3 growth rate, and a reduction in nucleation density. A single cycle can use a TMA pulse of 0.1~0.5s, a purge of 5~20s, and an H2O pulse of 0.1~0.5s, followed by a purge of 5~20s. For higher through-holes 11, the precursor residence and purge times can be extended to ensure conformal coverage of the middle and bottom of the pore walls.

[0067] Step S4300 controls the number of cycles of atomic layer deposition so that the thickness of the pore wall oxide interface layer 2 is 3~8nm.

[0068] It should be noted that, for ease of explanation, the following description uses an Al2O3-containing oxide interface layer on the pore wall as an example, but it does not mean that the pore wall oxide interface layer is limited to containing Al2O3. By controlling the ALD cycle number, the thickness of the Al2O3 on the pore wall is controlled within the range of 3-8 nm. Since Al2O3 needs to reach a certain thickness to form a continuous and complete interface layer, providing sufficient chemical bonding sites and pore fixation for the subsequent surface metal layer 3; if the thickness is too small, for example, below 3 nm, the Al2O3 on the pore wall may be discontinuous, with insufficient nucleation density, resulting in limited interface strengthening effect. On the other hand, the Al2O3 thickness should not be too large. For example, when the Al2O3 thickness on the pore wall exceeds approximately 10 nm, it means that more Al2O3 will be deposited on the base film surface, and an excessively thick oxide layer will affect the conductivity of the entire current collector.

[0069] The optimal number of ALD cycles is 30-100, while for mass production lines it can be 50-80.

[0070] In addition, in some embodiments, an outer surface oxide layer of about 1-3 nm exists between the polymer base film 1 and the surface metal layer 3. The outer surface oxide layer contains Al2O3 and is in principle no more than 5 nm. In this way, while it is insufficient to form a continuous insulating barrier layer and has a limited impact on the contact resistance between the surface metal layer 3 and the base film, it can serve as a metal nucleation and wetting promotion layer, improving the adhesion and coverage of subsequent sputtering underlayers.

[0071] In step S6000, metal is deposited on both sides of the polymer base film 1 to form a surface metal layer 3. The surface metal layer 3 is attached to the orifice region of the through hole 11 and contacts and bonds with the oxide interface layer 2 of the hole wall, so that the surface metal layer 3 on both sides of the polymer base film 1 is connected to the oxide interface layer 2 of the hole wall.

[0072] It should be noted that the surface metal layer 3 includes, but is not limited to, aluminum or its alloy.

[0073] A surface metal layer 3 is formed on both sides of the polymer base film 1 to enable the composite current collector to conduct electricity. The surface metal layer 3 is mainly formed on the outer surface of the base film and the orifice region. The orifice region of the through hole 11 is the junction between the outer surface of the base film and the hole wall, and it is also the position where the surface metal layer 3 can contact and bond with the Al2O3 interface layer of the hole wall. If the surface metal layer 3 does not completely cover the orifice region, it is difficult to form an effective contact between the surface metal layer 3 and the Al2O3 of the hole wall. Therefore, the surface metal layer 3 forms a cover in the orifice region and contacts and bonds with the oxide interface layer 2 of the hole wall.

[0074] The Al2O3 interface layer on the pore wall forms a chemical bond with the polymer pore wall through Al-OC bonding, while the organic-inorganic hybrid transition region formed by the near-surface infiltration of the precursor provides mechanical interlocking. After the surface metal layer 3 contacts and bonds with the Al2O3 on the pore wall in the pore opening region, the Al2O3 at the pore opening edge becomes an "anchor point" connecting the polymer base film 1 and the surface metal layer 3, allowing the surface metal layer 3 to form a firm bond with the base film through the Al2O3 interface layer, rather than being directly attached to the polymer surface lacking chemical bonding sites. In this way, even if the surface metal layer 3 does not penetrate deep into the micropores, it can obtain reliable interfacial bonding through the Al2O3 in the pore opening region, avoiding peeling and detachment during subsequent processing or battery cycling.

[0075] After the surface metal layer 3 forms a cover in the orifice region of the through hole 11, the two surface metal layers 3 form a bonding interface through the metal cover in the orifice region and the Al2O3 interface layer of the orifice wall. Specifically, one side of the surface metal layer 3 covers the orifice region and contacts the Al2O3 of the orifice wall, and the other side of the surface metal layer 3 also covers the orifice region and contacts the Al2O3 of the orifice wall. The two surface metal layers 3 are connected through the metal cover layer in the orifice region.

[0076] Specifically, step S6000 includes steps S6100 and S6200.

[0077] In step S6100, magnetron sputtering is used to deposit a substrate layer on both sides of the polymer base film 1. The substrate layer forms a cover in the orifice region of the through hole 11 and contacts and bonds with the oxide interface layer 2 of the hole wall.

[0078] It should be noted that sputtered particles have higher energy and offer better step coverage and interface adhesion compared to simple vapor deposition. In the orifice region, since the Al2O3 interface layer has already formed on the orifice wall, sputtered particles can contact and deposit on the Al2O3 surface when they reach the orifice edge, forming a continuous coating layer that bonds with the oxide interface layer 2 on the orifice wall. If the underlayer coating is discontinuous, poor contact may occur between the surface metal layer 3 and the Al2O3 on the orifice wall in the orifice region, affecting the reliability of subsequent bonding performance. The preferred underlayer is an aluminum underlayer with a thickness of 5–20 nm.

[0079] If the underlayer thickness is too small, it is difficult to form a continuous and complete cover layer on both sides of the polymer base film 1. In the initial stage of magnetron sputtering, metal atoms nucleate in an island-like manner on the surface of the base film. A certain thickness is required for the island-like growth to transform into a continuous film. If the underlayer thickness is too thin, for example, less than 5 nm, local uncovered or discontinuous coverage areas may appear on the outer surface of the base film and in the orifice area. If the underlayer thickness is too large, it will lead to an increase in the metal coverage span and suspended section in the orifice area, excessive coverage of the orifice morphology and stress concentration, while increasing the weight of the composite current collector, weakening the weight reduction advantage and slowing down the mass production cycle of magnetron sputtering. Therefore, in this embodiment, the underlayer thickness is 5~20 nm.

[0080] In step S6200, a thickened layer is deposited on the substrate by vacuum evaporation, so that the single-sided thickness of the surface metal layer 3 reaches 0.5~2μm, and the surface metal layers 3 on opposite sides of the polymer base film 1 are connected through the orifice area of ​​the through hole 11.

[0081] It should be noted that the underlayer has already formed a continuous coverage in the orifice area through magnetron sputtering and has contacted and bonded with the Al2O3 of the orifice wall. The vapor-deposited thickening layer continues to grow on the underlayer, so that the overall surface metal layer 3 reaches the required thickness. The single-sided thickness of 0.5~2μm is set with the following limits: the lower limit is to ensure that the surface metal layer 3 has sufficient conductive cross-sectional area to meet the sheet resistance and via resistance requirements of the composite current collector; the upper limit is to avoid the surface metal layer 3 being too thick, which would increase the weight of the composite current collector and weaken the weight reduction advantage, while also avoiding excessively long vapor deposition cycles that would affect mass production efficiency. Through the cooperation of the underlayer and the thickening layer, the surface metal layer 3 contacts and bonds with the Al2O3 of the orifice wall in the orifice area. The Al2O3 at the edge of the orifice forms a reliable anchoring and bonding interface with the surface metal layer 3, thereby preventing the outer surface metal layer 3 from peeling or falling off during subsequent processing or battery cycling.

[0082] like Figure 3 As shown, in some embodiments, step S1000 is included before step S3000.

[0083] Step S1000 involves surface activation of the polymer base film 1, thereby introducing oxygen-containing functional groups onto the surface of the polymer base film 1.

[0084] It should be noted that before drilling and ALD deposition, the surface of the polymer base film 1 is activated to introduce oxygen-containing functional groups such as hydroxyl, carboxyl, and carbonyl groups, providing a chemical basis for the subsequent formation of the organic passivation layer and the nucleation of Al2O3 in the pore walls. Specifically, plasma treatment or corona treatment can be used.

[0085] Correspondingly, after step S1000 and before step S3000, the method further includes step S2000.

[0086] In step S2000, an organic passivation layer is formed on the outer surface of the activated polymer base film 1. The thickness of the organic passivation layer is L2, and 200nm≤L2≤1μm.

[0087] It should be noted that an organic passivation layer is formed on the outer surface of the polymer base film 1 to inhibit the chemical adsorption, physical adsorption and diffusion of subsequent ALD precursors (such as trimethylaluminum) into the polymer matrix on the outer surface, thus establishing a chemical reaction difference and physical barrier for "pore wall selective growth and outer surface inhibited growth".

[0088] In some embodiments, the organic passivation layer uses phosphonate self-assembled molecules, such as octadecylphosphonic acid (ODPA); for surfaces that have undergone sufficient oxidation treatment and have a suitable hydroxyl density, fluorosilane materials can also be used. These molecules can chemically bond with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface of the activated base film through their active end groups, forming an organic passivation layer covering the outer surface, thus depriving the outer surface of active sites that can react with TMA.

[0089] Because TMA is highly reactive and readily penetrates the polymer matrix through physical adsorption and diffusion at relatively low temperatures, if the organic passivation layer is too thin, such as a self-assembled monolayer of only 3-5 nm, it mainly relies on consuming surface reaction sites to achieve chemical passivation, with limited physical barrier capabilities. TMA can still penetrate into the matrix through intermolecular gaps, defects, or pinholes, leading to increased leakage growth on the outer surface and decreased selectivity. This invention controls the thickness of the organic passivation layer to 200 nm-1 μm. The organic passivation layer not only covers the oxygen-containing functional groups on the outer surface, reducing the chemical adsorption activity of TMA on the outer surface, but also forms an effective physical diffusion barrier layer due to its thickness and density, inhibiting the penetration of TMA into the polymer matrix. This ensures that Al2O3 preferentially nucleates and grows on the pore walls during ALD deposition, with virtually no or only a very small amount of deposition on the outer surface. When the organic passivation layer is too thick, the removal difficulty increases significantly. The organic passivation layer on the outer surface needs to be removed subsequently using methods such as UV-O3, plasma, or solvent cleaning. If the thickness is too large, the removal time will be prolonged, and the removal process may damage the Al2O3 on the pore walls or the pore morphology. It may also affect the contact resistance between the surface metal layer 3 and the base film due to residual organic matter. In addition, an excessively thick organic passivation layer will increase material costs and film formation time, affecting mass production cycle time. Therefore, controlling the thickness of the organic passivation layer to 200nm~1μm is the preferred range that balances removal feasibility, contact resistance, and mass production efficiency while ensuring effective physical barrier and chemical passivation.

[0090] like Figure 4 As shown, in some embodiments, before step S6000 and after step S4000, the method further includes step S5000.

[0091] Step S5000 processes the outer surface of the polymer base film 1 to remove the organic passivation layer and / or the outer surface oxide layer on the outer surface of the polymer base film 1.

[0092] It should be noted that by treating the outer surface to remove the organic passivation layer and / or the ultrathin oxide layer formed on the outer surface during the ALD process, a low-resistance window is formed on the outer surface of the base film, ensuring that the subsequent surface metal layer 3 has an acceptable contact resistance with the outer surface of the base film.

[0093] While the organic passivation layer inhibits the chemisorption and nucleation of TMA on the outer surface during ALD deposition, it is itself an insulating organic material. Simultaneously, a very thin Al2O3 layer may form on the outer surface during ALD due to a small amount of leak growth. If these organic residues and / or ultrathin oxides are not removed before metallization, they will be trapped between the outer surface of the base film and the surface metal layer 3, creating additional contact resistance and affecting the sheet resistance of the composite current collector, the resistance of the via 11, and the post-soldering resistance. Therefore, a low-resistance window needs to be formed on the outer surface to allow the surface metal layer 3 to form a reliable conductive contact with the Al2O3 on the outer surface of the base film or the hole wall in the orifice region.

[0094] In some embodiments, the present invention also provides an electrode comprising any of the aforementioned composite current collectors.

[0095] In some embodiments, the present invention also provides a battery comprising the aforementioned electrode plates.

[0096] To further verify the beneficial effects of the present invention, the following examples and comparative examples are used for further illustration.

[0097] Example 1

[0098] S1. A PET base film with a thickness of 6.0 μm is selected, and the surface of the PET base film to be treated is activated by plasma treatment to introduce oxygen-containing functional groups into the polymer surface.

[0099] S2, an organic passivation layer with a thickness of 200 nm is formed on the outer surface of the activated PET base film. The material is octadecylphosphonic acid (ODPA). The thickness of the organic passivation layer L2 is 200 nm, which is used to suppress the chemical adsorption and nucleation of the subsequent TMA precursor on the outer surface.

[0100] S3 uses a pulsed laser to form through-holes 11 on the base film. The hole diameter is 12μm, the hole spacing is 100μm, and the aperture ratio is 1.13%. The corresponding laser processing wavelength is 355nm, the focused spot size is 10μm, the pulse width is 30ps, the single pulse energy is 10μJ, 3 pulses per hole, and the repetition frequency is 2MHz. The hole diameter is 12μm, the hole spacing is 100μm, the aperture ratio is 1.1%, and the hole type is a straight through-hole 11. Inert gas purging and vacuum chip removal are used in conjunction with the processing.

[0101] In step S4, the perforated base film is introduced into the ALD chamber, and alternating pulses of trimethylaluminum (TMA) and water are used at a process temperature of 100℃. A single cycle consists of a 0.2s TMA pulse, a 10s purge, a 0.2s H2O pulse, and a 10s purge; the ALD cycle count is 60 times. Due to the inhibition of the outer surface passivation layer, Al2O3 preferentially nucleates and grows on the pore walls. The Al2O3 interface layer thickness L1 on the pore walls is 6nm, and the Al2O3 thickness on the outer surface is 2nm.

[0102] S5, with outer surface treatment and low-resistance window formation, removes the outer surface passivation layer and ultrathin oxide in the tab welding area (2mm wide) by masked oxygen plasma treatment.

[0103] S6, metallization is performed sequentially on both sides of the base film. First, 10nm of aluminum is sputtered on both sides to form a continuous base layer, and then the aluminum coating layer is thickened to 1μm on both sides by double-sided vacuum evaporation.

[0104] Example 2

[0105] The difference between this embodiment and Embodiment 1 is that: In S1, the polymer base film 1 is replaced with a PEN base film with a thickness of 4.5 μm; In S4, the ALD process temperature is 110℃, the ALD cycle number is adjusted to 30, and the corresponding L1 is reduced to 3nm.

[0106] Example 3

[0107] The difference between this embodiment and Embodiment 1 is that: In S1, the polymer base film 1 is replaced with a PPS base film with a thickness of 6.0 μm; In S4, the ALD process temperature is 80℃, the ALD cycle number is adjusted to 80, and the corresponding L1 is increased to 8nm.

[0108] Example 4

[0109] The difference between this embodiment and Embodiment 1 is that: In S3, the through-hole diameter is 10μm, the hole spacing is 60μm, and the aperture ratio is 2.18%. The corresponding laser focusing spot size is adjusted to 8μm. In S6, double-sided vacuum evaporation is used to thicken aluminum layers to 0.5 μm on each side.

[0110] Example 5

[0111] The difference between this embodiment and Embodiment 1 is that: In S2, the thickness L2 of the organic passivation layer is 1 μm; In S3, the through-hole diameter is 20μm, the hole spacing is 150μm, and the aperture ratio is 1.40%. The corresponding laser focusing spot size is adjusted to 15μm, the single-pulse energy is 20μJ, and there are 5 pulses per hole. In S5, the outer surface passivation layer and ultrathin oxide are removed by mask-fluorine-based plasma treatment; In S6, double-sided vacuum evaporation is used to thicken aluminum layers to 2.0 μm on each side.

[0112] Example 6

[0113] The difference between this embodiment and Embodiment 1 is that: In S6, the thickness of the continuous underlayer of double-sided magnetron sputtering is adjusted to 100nm on each side to achieve the connection of the metal coatings on the A and B sides within the channel.

[0114] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that after drilling, Al2O3 ALD deposition (atomic deposition) is not performed, and double-sided metallization is directly completed (the thickness of double-sided metallization is 1.0 μm on each side).

[0115] Comparative Example 2 The difference between Comparative Example 1 and Example 4 is that after drilling, Al2O3 ALD deposition (atomic deposition) is not performed, and double-sided metallization is directly completed (the thickness of double-sided metallization is 0.5 μm on each side).

[0116] Comparative Example 3 The difference between Comparative Example 1 and Example 5 is that after drilling, Al2O3 ALD deposition (atomic deposition) is not performed, and double-sided metallization is directly completed (the thickness of double-sided metallization is 2.0 μm on each side).

[0117] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that after drilling holes in the base film, a 100nm layer of Al2O3 was formed on the entire outer surface of the base film before metallization, without the use of an organic passivation layer and selective deposition.

[0118] Test case The physical bonding force (mechanical peel test) before and after stretching and the sheet resistance after immersion in electrolyte before and after stretching of the current collectors prepared in the above embodiments and comparative examples were tested.

[0119] Tensile pretreatment: Each sample was cut into strips 15 mm wide and at least 150 mm long. At least 5 parallel samples were set up in each group. The samples were stretched on a tensile testing machine at a speed of 1 mm / min to simulate the dynamic stretching of a battery until the elongation reached 30%. The stretching was repeated 10 times. At the same time, 5 control samples without stretching were also set up in each group.

[0120] Mechanical peel test: A universal testing machine was used to peel the material at a speed of 100 mm / min and at a 180° peel angle. The peel strength values ​​before and after each stretching were tested, and the unit was kN / m.

[0121] Sheet resistance test after electrolyte immersion: The pre-treated tensile samples and control strip samples were immersed in an electrolyte solution (1.0 mol / L LiPF6, solvent EC:DEC:EMC volume ratio 1:1:1, plus 1% VC) in an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm) and kept at 65℃ for 48 h. After removal, they were rinsed with ethanol and dried under vacuum at 60℃. Subsequently, a four-probe method was used, with at least 5 locations selected on both sides of each sample for testing and the average value taken, in mΩ / □.

[0122] Table 1. Experimental results of the examples and comparative examples.

[0123] Note: " / " indicates no reading, meaning the sheet resistance exceeds the instrument's detection limit of 2000Ω / □.

[0124] Based on the data in Table 1, the following can be determined through testing: Constructing an oxide interface layer on the pore walls of a perforated polymer-based film can effectively improve the interfacial state within the pores, enhancing the adhesion stability and electrolyte resistance of the surface metal layer. Specifically, Example 1, using moderate process parameters, exhibits relatively balanced overall performance, with a slight decrease in interfacial peel strength after stretching and a relatively gradual change in sheet resistance after electrolyte immersion. Example 2, with reduced oxide thickness on the pore walls, maintains a good level of interfacial peel strength, but the increase in sheet resistance after electrolyte immersion is greater, indicating that a thinner oxide layer weakens the corrosion resistance of the coating. Example 3, with increased oxide thickness on the pore walls, shows a certain improvement in initial peel strength, but the decrease in peel strength after stretching is more significant, and the increase in sheet resistance after electrolyte immersion is also greater, reflecting that excessively thick oxide layers tend to increase interfacial brittleness, which is detrimental to the overall performance balance. Example 4, with increased pore density and thinner metal layer, achieves relatively higher initial interfacial peel strength, good stretch retention and electrolyte resistance, and although a thinner metal layer affects the initial sheet resistance, the overall performance degradation is at a relatively optimal level. Example 5, which involves thickening the organic passivation layer, enlarging the pore size, and thickening the metal layer, exhibits a relatively low initial peel strength, which decreases more significantly after stretching. The sheet resistance increases considerably after immersion in the electrolyte, and the anchoring ability of the thick metal layer combined with the large-pore structure is significantly reduced. Example 6, which uses a through-hole structure with a suitable oxide layer, shows the least decrease in peel strength after stretching, the most gradual increase in sheet resistance after immersion in the electrolyte, and relatively superior resistance to electrochemical corrosion.

[0125] The comparative examples without a pore wall oxide interface layer all showed weaker overall performance than the corresponding embodiments. Specifically, Comparative Example 1, using a medium-thickness metal layer, exhibited a significant decrease in peel strength after stretching, and a sharp increase in sheet resistance after electrolyte immersion. This reflects that the adhesion and tensile strength of the metal layer are affected by the lack of pore interface reinforcement. Comparative Example 2, using a thin metal layer, performed slightly better than the comparative examples without a pore wall oxide interface layer, but its performance retention after stretching was still significantly weaker than the corresponding embodiment, and the increase in sheet resistance after electrolyte immersion was also greater. Comparative Example 3, using a thick metal layer, had a low initial peel strength, the most significant loss in peel strength after stretching, and the largest increase in sheet resistance after electrolyte immersion. The combined stress of the thick metal layer and the weak interface resulted in the worst overall performance.

[0126] Comparative Example 4, which forms a thick oxide layer on the entire outer surface of the base film, has extremely low initial peel strength. After stretching, the peel strength is almost lost, and the conductivity is also severely affected. This indicates that the thick oxide layer has a much greater effect on the embrittlement of the current collector interface than on the bonding effect on the coating.

[0127] In summary, selectively constructing an oxide interface layer of appropriate thickness on the pore wall is an effective way to improve the overall performance of perforated composite current collectors. By rationally matching the parameters of the pore structure, metal layer and oxide layer, an optimized balance of performance can be achieved.

[0128] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A composite current collector, characterized in that, include: Polymer-based film, with through-holes throughout; A pore wall oxide interface layer is disposed on the pore wall of the through hole, and the pore wall oxide interface layer comprises metal oxide or non-metal oxide; A surface metal layer is disposed on opposite sides of the polymer base film; The surface metal layer is formed and attached in the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall, thereby connecting the surface metal layers on opposite sides of the polymer base film through the oxide interface layer of the hole wall.

2. The composite current collector as described in claim 1, characterized in that, The pore wall oxide interface layer contains Al2O3 or SiO2, and the thickness of the pore wall oxide interface layer is L1, 3nm≤L1≤8nm. And / or, The surface metal layer has a single-sided thickness of 0.5~2μm, and the surface metal layer includes aluminum or its alloy; And / or, The diameter of the through hole is D, and the hole spacing is H, where 8μm≤D≤20μm and 50μm≤H≤200μm.

3. The composite current collector as described in claim 1, characterized in that, The polymer base film and the surface metal layer are further provided with an outer surface oxide layer, the outer surface oxide layer containing Al2O3, and the thickness of the outer surface oxide layer is 1~3nm.

4. A method for preparing a composite current collector as described in any one of claims 1 to 3, characterized in that, include: A through-hole is formed in the polymer base film; Metal oxides or non-metal oxides are deposited on the pore walls of the through-hole using atomic deposition technology to form an oxide interface layer on the pore walls; Metal is deposited on opposite sides of the polymer base film to form a surface metal layer. The surface metal layer adheres to the orifice region of the through hole and contacts and bonds with the oxide interface layer of the hole wall. The surface metal layers on opposite sides of the polymer base film are connected through the oxide interface layer of the hole wall.

5. The method for preparing the composite current collector as described in claim 4, characterized in that, The step of depositing metal oxides or non-metal oxides on the hole walls of the through-hole using atomic deposition technology to form a hole wall oxide interface layer includes: The polymer-based film with the aforementioned through-holes is introduced into the atomic layer deposition cavity; Using trimethylaluminum and water as precursors for alternating pulses, atomic layer deposition is performed on the pore walls of the through-holes, allowing metal oxides or non-metal oxides to nucleate and grow in a conformal manner on the pore walls; The number of atomic layer deposition cycles is controlled to make the thickness of the pore wall oxide interface layer 3~8nm.

6. The method for preparing the composite current collector as described in claim 4, characterized in that, Prior to the step of forming a through-hole in the polymer base film, the method further includes: The polymer base film is surface activated to introduce oxygen-containing functional groups onto its surface, and an organic passivation layer is formed on the outer surface of the activated polymer base film. The thickness of the organic passivation layer is L2, where 200 nm ≤ L2 ≤ 1 μm.

7. The method for preparing the composite current collector as described in claim 6, characterized in that, After depositing metal oxides or non-metal oxides on the pore walls of the through-hole using atomic deposition technology to form a pore wall oxide interface layer, and before depositing metals on opposite sides of the polymer base film to form a surface metal layer, the method further includes: The outer surface of the polymer base film is treated to remove the organic passivation layer and / or the outer surface oxide layer.

8. The method for preparing the composite current collector as described in claim 4, characterized in that, The method of forming a through-hole in the polymer base film includes: A pulsed laser is used to punch holes in the polymer base film, forming through holes in the polymer base film. The pulsed laser has a wavelength of 355nm, a pulse width of 10~50ps, a single pulse energy of 1~20μJ, 1~5 pulses per aperture, and a repetition frequency of 0.5~5MHz.

9. An electrode sheet, characterized in that, The composite current collector includes the composite current collector as described in any one of claims 1 to 3 or the composite current collector prepared by any one of claims 4 to 8.

10. A battery, characterized in that, It includes the electrode sheet as described in claim 9.