Janus Asymmetric Interface Functionalized SPEEK Membrane, Its Preparation Method and Application in Flow Batteries
By constructing hydrophobic and hydrophilic functional layers on both sides of the SPEEK base film, the differentiated requirements of the positive and negative electrodes of alkaline all-iron flow batteries were addressed. This achieved efficient triethanolamine barrier and ferrocyanide ion transport, improving the coulombic efficiency and energy efficiency of the battery while maintaining long-term cycle stability.
Patent Information
- Application Number
- CN202611320747.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to meet the differentiated requirements of positive and negative electrodes in alkaline all-iron flow batteries. Traditional homogeneous films cannot simultaneously adapt to the chemical environments of positive and negative electrodes. Existing improvement solutions are limited in function and lack the functional design of Janus asymmetric interfaces.
A hydrophobic functional layer and a hydrophilic ion-conducting functional layer were constructed on both sides of the SPEEK base film. The hydrophobic functional layer was formed by covalently grafting fluorinated silane coupling agents and long-chain alkyl silane coupling agents, while the hydrophilic ion-conducting functional layer was formed by graft polymerization of polymerizable hydrophilic monomers containing sulfonic acid groups. The thickness of the two functional layers was precisely controlled between 0.3 and 1.5 μm, and the total thickness did not exceed 2 μm.
It achieves effective blocking of triethanolamine and efficient transport of ferrocyanide ions, reduces film surface resistance, improves battery coulombic efficiency and energy efficiency, and ensures long-term cycle stability.
Smart Images

Figure CN123120769A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery materials technology, and relates to SPEEK films, their preparation methods, and their applications in flow batteries. Background Technology
[0002] Alkaline all-iron flow batteries, using abundant, inexpensive, and environmentally friendly iron-based materials as active materials, are considered one of the important technological routes for large-scale, long-term energy storage. This battery utilizes ferrocyanide / ferricyanide ([Fe(CN)6)6) 4- / 3- The electrode uses a triethanolamine-iron complex (TEA-Fe) as the positive electrode redox couple and a triethanolamine-iron complex (TEA-Fe) as the negative electrode redox couple, with potassium hydroxide aqueous solution as the electrolyte matrix. The negative electrode side is a strongly alkaline environment (pH 12-14) containing the organic amine ligand triethanolamine (TEA), while the positive electrode side is a neutral to weakly alkaline environment containing ferrocyanide ions. As the core component separating the positive and negative electrodes and conducting charge carriers, the membrane must simultaneously cope with the vastly different chemical environments on both sides, imposing stringent and contradictory requirements on its interfacial properties. Sulfonated polyetheretherketone (SPEEK), with its excellent chemical stability, good mechanical properties, and adjustable ion exchange capacity (IEC), is considered a strong candidate material to replace perfluorosulfonic acid membranes (such as Nafion), demonstrating significant application value in novel energy storage systems such as alkaline all-iron flow batteries.
[0003] However, existing technologies are difficult to meet the above requirements, mainly due to the following problems: (1) Homogeneous membrane modification is inefficient: The chemical structures on both sides of the traditional homogeneous SPEEK membrane are exactly the same, making it difficult to adapt to the different needs of the positive and negative electrodes respectively. If both sides of the membrane are modified to be hydrophilic, although the ion conduction on the positive electrode side is improved, the permeation of triethanolamine (TEA) on the negative electrode side is aggravated, causing cross-contamination and capacity decay. If both sides are modified to be hydrophobic, although the permeation of triethanolamine (TEA) is inhibited, the ion transport on the positive electrode side is severely hindered, resulting in increased polarization and decreased efficiency. Homogeneous modification falls into a structural problem of inefficiency. Dilemmas; (2) Existing improvement schemes are single-function and still homogeneous on both sides: Current graphene oxide composite membranes, Nafion-based composite membranes and alkaline zinc-iron flow battery separators (publication number CN121905887A) are all only aimed at improving a single function and have not designed interfaces for the different chemical environments of the positive and negative electrodes; (3) Lack of Janus asymmetric interface functionalization schemes: There is no Janus asymmetric design for the different chemical environments of the positive and negative electrodes of alkaline all-iron flow batteries in the existing technology, nor is there any report on the independent interface functionalization of the two sides of the separator to adapt to the two electrode environments respectively. Summary of the Invention
[0004] To address the issues mentioned in the background art, such as the inability of traditional homogeneous membranes to meet the differentiated requirements of positive and negative electrodes in alkaline all-iron flow batteries, the limited functionality of existing improved solutions which are still bilaterally homogeneous, and the lack of Janus asymmetric interface functionalization solutions, this invention provides a Janus asymmetric interface functionalized SPEEK membrane, its preparation method, and its application in flow batteries. Interfacial functional layers with distinctly different chemical properties are constructed on both sides of the same SPEEK base membrane, making it particularly suitable for alkaline all-iron flow batteries where the chemical environments of the positive and negative electrodes differ significantly.
[0005] In a first aspect, the present invention provides a Janus asymmetric interface functionalized SPEEK membrane, comprising a SPEEK base membrane having a first surface facing the negative electrode of an alkaline all-iron flow battery and a second surface facing the positive electrode during use; the first surface is covalently grafted with a hydrophobic functional layer, and the water contact angle of the first surface is greater than or equal to 115°; the hydrophobic functional layer is formed by a hydrolysis-condensation reaction of a fluorinated silane coupling agent and / or a long-chain alkyl silane coupling agent on the surface of the SPEEK base membrane; the second surface is covalently grafted with a hydrophilic ion-conducting functional layer, and the water contact angle of the second surface is less than or equal to 22°; the hydrophilic ion-conducting functional layer is formed by graft polymerization of a polymerizable hydrophilic monomer containing sulfonic acid groups on the surface of the SPEEK base membrane; the thickness of the hydrophobic functional layer and the hydrophilic ion-conducting functional layer are each independently 0.3-1.5 μm, and the sum of the two does not exceed 2 μm.
[0006] It should be noted that the first and second surfaces of this invention are defined by the assembly orientation of the membrane in the battery: the first surface is the side facing the negative electrode during use, and the second surface is the side facing the positive electrode during use. The water contact angle is measured using the seated drop method, and the extreme differentiation of the water contact angles on both sides of the membrane (one side greater than or equal to 115°, and the other side less than or equal to 22°) is a direct criterion for the successful construction of the Janus asymmetric interface structure.
[0007] It should be noted that the thickness of the hydrophobic functional layer is 0.3-1.5 μm, the thickness of the hydrophilic ion-conducting functional layer is 0.3-1.5 μm, and the total thickness of the two functional layers does not exceed 2 μm. This thickness window is crucial: if the thickness of a single functional layer exceeds its upper limit of 1.5 μm, its intrinsic resistivity contributes significantly to the surface resistivity, and the film surface resistivity rises to 0.88 Ω·cm. 2If the thickness is too high, the energy efficiency drops to around 78.2%, leading to increased ohmic polarization and decreased energy efficiency. If the thickness is less than 0.3 μm, it is difficult to form a continuous and complete interfacial functional layer, resulting in insufficient hydrophobic or hydrophilic effects. This invention precisely controls the thickness of the functional layers on both sides within the above-mentioned range by controlling the temperature, time, and reactant concentration of the grafting reaction. This ensures that the total thickness of the functional layers on both sides (not exceeding 2 μm) is less than one-tenth of the thickness of the SPEEK base film (25-40 μm). The hydrophobic layer is a low-crosslink density siloxane network. Although its intrinsic resistivity is higher than that of the SPEEK bulk, its extremely thin thickness results in its contribution to the surface resistivity being less than 0.05 Ω·cm. 2 The hydrophilic layer is a highly hydrated sulfonic acid polymer with an ionic conductivity comparable to or even higher than that of the SPEEK bulk. Therefore, the overall sheet resistivity of the SPEEK membrane of this invention can be controlled within 0.50-0.65 Ω·cm. 2 Compared with unmodified SPEEK membrane (approximately 0.40 Ω·cm) 2 The interface functionality was introduced without sacrificing ohmic properties.
[0008] In summary, the Janus asymmetric interface functionalized SPEEK membrane of the present invention uses a single SPEEK base membrane as a common body, and introduces submicron to micron-level functional layers only on its two sides. The membrane body maintains a continuous and uniform structure and there is no material interface formed by multi-layer composite stacking. The functional layers on both sides perform the functions of repulsion and conduction for the chemical environment of the negative electrode side and the positive electrode side, respectively. From the structural design, it solves the dilemma of homogeneous membranes that cannot take care of one side.
[0009] Furthermore, the fluorinated silane coupling agent is selected from any one of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and perfluorooctylethyltrichlorosilane, and the long-chain alkylsilane coupling agent is octadecyltrimethoxysilane. After hydrolysis and condensation, the fluorinated segments of the fluorinated silane coupling agent impart extremely low surface energy (as low as 15-20 mN / m) to the membrane surface, which can form a hydrophobic barrier on the membrane surface; the long-chain alkylsilane reduces the membrane surface energy and repels organic amine molecules from approaching the membrane surface through the hydrophobic interaction of the long-chain alkyl groups.
[0010] The triethanolamine (TEA) blocking mechanism of the hydrophobic functional layer on the negative electrode side is as follows: Triethanolamine (TEA, chemical formula N(CH2CH2OH)3) is a moderately polar organic molecule containing three hydroxyethyl groups (molecular weight 149.19, pKa=7.77). In strongly alkaline electrolytes, it mainly exists in an unprotonated molecular state with a molecular size of approximately 0.6-0.8 nm, which is comparable to or smaller than the size of ferricyanide complex ions, and it is electrically neutral. Therefore, the blocking of triethanolamine (TEA) in this invention does not mainly rely on size sieving and electrostatic repulsion, but rather on the low surface energy interface formed by the hydrophobic functional layer: This dense organic-inorganic hybrid layer, through hydrophobic repulsion and interfacial energy barrier effects, significantly reduces the partition coefficient of triethanolamine (TEA) molecules at the membrane / electrolyte interface, significantly weakens the transmembrane permeation driving force and effective channels, and ultimately reduces the permeation coefficient of triethanolamine (TEA) by nearly an order of magnitude compared to the unmodified membrane.
[0011] Further, the polymerizable hydrophilic monomer containing sulfonic acid groups is selected from any one of sodium vinyl sulfonate, potassium 3-sulfonopropyl methacrylate (SPMA), and sulfonate betaine monomer (SBMA, chemically named [2-(methacryloyloxy)ethyl]dimethyl(3-sulfonopropyl)ammonium hydroxide inner salt); the surface sulfonic acid group density of the hydrophilic ion-conducting functional layer is 1.8-2.7 mmol / g (based on the dry weight of the functional layer, estimated by SEM thickness measurement of the combined membrane area and density or XPS surface quantitative calibration); preferably, the surface sulfonic acid group density is 2-2.7 mmol / g. In the sulfonic acid polymer formed by grafting, the sulfonic acid group (-SO3) - It maintains a high degree of dissociation in alkaline electrolyte, forming a high-density fixed negative charge interface.
[0012] The hydrophilic ion-conducting mechanism of the positive electrode side hydrophilic ion-conducting functional layer is as follows: the sulfonic acid polymer brush is fully hydrated in the alkaline electrolyte, forming a continuous water-rich interface layer on the membrane surface; the sulfonate anions fixed in the layer hinder the ferrocyanide anions ([Fe(CN)6)6) through the Donnan repulsion effect. 4- ) approaches and penetrates the membrane surface, while K + Equal charge carriers can be efficiently transported through hydrated ion channels in the water-rich interface layer, thus significantly reducing the interface resistance. Simultaneously, the electrostatic repulsion of ferrocyanide ions by the fixed negative charge reduces the adsorption and deposition of active species on the membrane surface, inhibiting interface passivation. It should be noted that for the grafted layer formed by zwitterionic monomers of SBMA, where sulfonate and quaternary ammonium groups coexist in equimolar amounts and the net surface charge is close to zero, the barrier and conduction functions mainly rely on a dense hydration layer formed by strong electrostatic hydration, which also imparts hydrophilicity to the interface and inhibits the adsorption and deposition of active species.
[0013] Furthermore, the SPEEK base film is a dense film with a sulfonation degree (the average number of sulfonic acid groups in each PEEK repeating unit) of 0.70-0.85 and a thickness of 25-40 μm. The selection of the sulfonation degree is based on the following: when the sulfonation degree is below 0.70, the density of sulfonic acid groups in the base film is insufficient, resulting in a significant decrease in bulk ionic conductivity, an increase in sheet resistance, and increased battery polarization; when the sulfonation degree is above 0.85, the swelling rate of the film in alkaline electrolyte increases sharply (exceeding 80%), resulting in decreased mechanical strength, poorer dimensional stability, and excessive swelling will expand the ion channels in the film, weakening the barrier ability against triethanolamine (TEA). The film thickness of 25-40 μm balances ion conduction and mechanical reliability: when the film is thinner than 25 μm, it is prone to puncture or tearing during stack assembly and long-term operation; when the film thickness is greater than 40 μm, the sheet resistance increases significantly, and the energy efficiency decreases.
[0014] Furthermore, the SPEEK base film is prepared by sulfonation of polyetheretherketone (PEEK) with a number average molecular weight of 80,000-200,000 using concentrated sulfuric acid. The concentrated sulfuric acid has a mass fraction of 95%-98%, the sulfonation temperature is 40-60 °C, and the sulfonation time is 1-8 hours. A number average molecular weight higher than 80,000 ensures that the sulfonated SPEEK maintains sufficient chain entanglement density and mechanical strength; when the molecular weight exceeds 200,000, the solubility of the resin in concentrated sulfuric acid decreases, and the uniformity of sulfonation declines. By controlling the sulfonation temperature and time, the degree of sulfonation of the SPEEK base film can be stably controlled within the target range of 0.70-0.85. The SPEEK base film can be prepared by solution casting: the sulfonation product is dissolved in a polar organic solvent such as N,N-dimethylformamide to prepare a casting solution with a mass fraction of 10%-20% (preferably 15%). After degassing, the solution is cast or coated to form a film, and then dried and cured in stages to obtain a SPEEK base film with uniform thickness and no pinhole defects.
[0015] Secondly, the present invention provides a method for preparing the Janus asymmetric interface functionalized SPEEK film described above, comprising the following steps: Step 1: Tightly protect the second surface of the SPEEK base film with solvent-resistant tape to isolate the second surface from the subsequent processing environment; Step 2: Expose the unprotected first surface to low-temperature plasma for activation treatment. The plasma power is 50-80 W and the treatment time is 3-6 minutes to generate active sites on the first surface. Step 3: Immerse the activated membrane in an organic solution containing a hydrophobic silane coupling agent, heat it under normal pressure to 70%-95% of the boiling point of the selected solvent, and react for 2-6 hours to form a hydrophobic functional layer on the first surface; the volume concentration of the hydrophobic silane coupling agent in the organic solution is 1%-5%. Step 4: Remove the solvent-resistant tape, wash and dry the membrane, and then tightly protect the first surface where the hydrophobic functional layer has been formed with new solvent-resistant tape. Step 5: Expose the unprotected second surface to low-temperature plasma for activation treatment. The plasma power is 50-80 W and the treatment time is 3-6 minutes to generate active sites on the second surface. Step 6: The membrane is then immersed in an aqueous solution containing hydrophilic monomers and persulfate initiators, and reacted at 60-80 °C for 1-4 hours under nitrogen protection to form a hydrophilic ion-conducting functional layer on the second surface; the mass concentration of the hydrophilic monomers in the aqueous solution is 5%-15%, and the mass concentration of the persulfate initiator is 0.05%-0.2%. Step 7: Remove the membrane, wash and dry it to obtain the Janus asymmetric interface functionalized SPEEK membrane.
[0016] The essence of the preparation method of this invention is to adopt a step-by-step process route of "single-sided protection - plasma activation - directional grafting": the surface on the side that is not to be treated is physically shielded using solvent-resistant tape, so that each round of plasma activation and grafting reaction only acts on the exposed single surface, and the modification on both sides is isolated from each other in time and space and does not interfere with each other. When the SPEEK base film surface is bombarded by low-temperature plasma, the high-energy particles break the polymer chain on the polymer surface and introduce active sites: among them, oxygen plasma is mainly used for oxidation reaction, generating oxygen-containing polar groups such as hydroxyl (-OH) and carboxyl (-COOH) on the surface; argon plasma or nitrogen plasma is mainly used for bond breaking, generating surface free radicals, which can be further converted into peroxy (-OOH) after being exposed to air. The aforementioned active groups serve as grafting anchors: on one hand, the alkoxy groups of the silane coupling agent hydrolyze to generate silanol groups (-Si-OH) through adsorbed water on the membrane surface or trace amounts of water in the environment, which then form Si-OC covalent bonds through a condensation reaction with the hydroxyl groups on the surface; on the other hand, surface peroxy groups or free radicals undergo free radical grafting polymerization with vinyl monomers under the action of free radicals generated by the persulfate initiator under heating, forming a polymer brush connected to the base membrane surface by CC bonds. Since both functional layers are firmly bonded to the SPEEK base membrane through covalent bonds, the functional layers are not easily detached or peeled off during long-term immersion in alkaline electrolyte and electrochemical cycling, ensuring the durability of the interfacial function.
[0017] Furthermore, in steps 2 and 5, the low-temperature plasma is selected from oxygen plasma, argon plasma, and nitrogen plasma. Steps 2 and 5 can use the same or different plasma types. When the plasma power is below 50 W or the processing time is too short, the surface activation is insufficient, the active site density is low, and the subsequent grafting density decreases accordingly. When the power is above 80 W or the processing time is too long, the etching effect of the plasma is enhanced, which may damage the surface structure of the SPEEK base film, and even lead to the removal or degradation of surface sulfonic acid groups.
[0018] Further, in step 3, the volume concentration of the hydrophobic silane coupling agent in the organic solution is 2%-3%, and the organic solvent used in the organic solution is toluene or n-hexane, with a reaction time of 3-5 hours. The reaction temperature matches the boiling point of the selected organic solvent: when the organic solvent is toluene, the reaction temperature is 80-100 °C (toluene's boiling point at room pressure is approximately 110.6 °C); when the organic solvent is n-hexane, the reaction temperature is its reflux temperature, i.e., 60-65 °C (n-hexane's boiling point at room pressure is approximately 69 °C). When the concentration of the silane coupling agent is below 2%, the adsorption density of silane molecules on the membrane surface is insufficient, making it difficult to form a continuous hydrophobic layer; when the concentration is above 3%, the self-polymerization tendency of silane molecules in the solution is enhanced, easily forming bulk polysiloxanes rather than surface grafted layers, resulting in a significant increase in membrane surface resistance. The organic solvent does not react with the silane coupling agent.
[0019] Further, in step 6, the mass concentration of the hydrophilic monomer in the aqueous solution is 8%-12%, the mass concentration of the persulfate initiator is 0.08%-0.15%, the reaction temperature is 65-75 ℃, and the reaction time is 1.5-2.5 hours; the persulfate initiator is selected from any one of potassium persulfate, ammonium persulfate, and sodium persulfate. The above-mentioned persulfate initiator thermally decomposes at the reaction temperature (65-75 ℃) in step 5 to generate sulfate free radicals (SO4). - The initiator (·) then initiates the free radical grafting polymerization of vinyl monomers on the activated surface. When the initiator dosage is less than 0.08%, the free radical generation rate is too low, resulting in poor grafting polymerization efficiency; when the dosage is higher than 0.15%, the homopolymerization reaction in the solution intensifies, the viscosity increases, hindering the diffusion of monomers to the membrane surface, and excessive initiator residue may accelerate membrane aging and degradation.
[0020] Further, in steps 1 and 4, the solvent-resistant tape is polyimide tape or polytetrafluoroethylene tape; when implementing protection, it should be ensured that the edge of the tape is completely adhered to the film surface to avoid solution leakage. The washing in step 4 is used to remove unreacted silane monomers and byproducts, and can be carried out sequentially with toluene, ethanol and deionized water; the washing in step 6 is used to remove unreacted hydrophilic monomers and homopolymers, and can be carried out with deionized water, supplemented by washing with ethanol if necessary; drying can be carried out by vacuum drying at 60 ℃.
[0021] Thirdly, the present invention provides an alkaline all-iron flow battery, comprising: Positive electrode electrolyte: Contains ferrocyanide and / or ferricyanide as positive electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the positive electrode electrolyte is 0.3-1.0 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; Negative electrode electrolyte: containing triethanolamine iron complex as the negative electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the negative electrode electrolyte is 0.3-1.2 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; Separator: The Janus asymmetric interface functionalized SPEEK membrane described above is assembled in the alkaline all-iron flow battery with its first surface facing the negative electrode and its second surface facing the positive electrode.
[0022] In the alkaline all-iron flow battery of this invention, the directional assembly of the SPEEK membrane ensures precise matching of the chemical environments of the functional layers on both sides of the membrane with the corresponding electrode sides: the hydrophobic functional layer on the negative electrode side continuously repels triethanolamine (TEA), inhibiting the transmembrane migration of TEA ligands from the negative electrode electrolyte to the positive electrode side and the resulting capacity decay; the hydrophilic ion-conducting functional layer on the positive electrode side maintains a low-resistance interfacial ion transport channel, reducing the impedance growth at the membrane-electrolyte interface during cycling. The synergistic effect of these two elements enables the battery to achieve high coulombic efficiency while maintaining high energy efficiency, and exhibits excellent long-term cycling stability: at 60 mA / cm²... 2 After 8000 constant current charge-discharge cycles at the current density, the capacity retention rate is still above 93%, which is significantly better than that of the unmodified homogeneous film and the double-sided homogeneous modified film.
[0023] Compared with the prior art, the present invention has the following advantages: (1) Overcoming the structural dilemma of homogeneous membranes: The positive and negative electrodes of alkaline all-iron flow batteries place contradictory requirements on the interfacial properties of the membrane: the negative electrode side is a strongly alkaline environment (pH 12-14) and contains the organic amine ligand triethanolamine (TEA), requiring a low surface energy hydrophobic interface to inhibit its permeation; the positive electrode side is an environment containing ferrocyanide ions, requiring a hydrophilic interface to ensure efficient carrier transport. The chemical structures on both sides of a traditional homogeneous membrane are completely identical, and whether it is hydrophilic or hydrophobic modification, it can only meet the needs of one side; the present invention covalently grafts a hydrophobic functional layer (water contact angle ≥115°) and a hydrophilic ion conduction functional layer (water contact angle ≤22°) onto the two sides of a single SPEEK base membrane, respectively. The functional layers on both sides perform the functions of repulsion and conduction for the chemical environments of the negative and positive electrodes, respectively, thus overcoming the dilemma of homogeneous membranes in terms of structural design; (2) Effectively suppress triethanolamine (TEA) cross-contamination and ensure battery capacity: Triethanolamine (TEA) is a small molecule organic amine, and its transmembrane permeation is difficult to be effectively blocked by conventional size sieving and electrostatic repulsion mechanisms. It is an important cause of cross-contamination and capacity decay in alkaline all-iron flow batteries. In this invention, a low surface energy hydrophobic functional layer formed by the reaction of hydrophobic silane coupling agent is constructed on the first surface facing the negative electrode. Through hydrophobic repulsion and interfacial energy barrier effect, the distribution of triethanolamine (TEA) at the membrane / electrolyte interface is reduced, and its transmembrane permeation driving force is weakened. This continuously suppresses the transmembrane migration of triethanolamine (TEA) ligands in the negative electrode electrolyte to the positive electrode side and the resulting capacity decay, thus ensuring the battery capacity. (3) Maintaining low surface resistivity and interface functionalization without sacrificing ohmic properties: The introduction of functional layers into the diaphragm is usually accompanied by an increase in resistance. This invention solves this contradiction by controlling the thickness: the thickness of the functional layers on both sides is controlled at 0.3-1.5 μm, and the total thickness does not exceed 2 μm, which is less than one-tenth of the thickness of the SPEEK base film (25-40 μm); among them, although the hydrophobic layer has a high intrinsic resistivity, its extremely thin thickness makes its contribution to the surface resistivity less than 0.05 Ω·cm. 2 The hydrophilic layer is a highly hydrated sulfonic acid polymer with an ionic conductivity comparable to or even higher than that of the SPEEK bulk. Therefore, the overall sheet resistance of the SPEEK membrane of this invention can be controlled within 0.50-0.65 Ω·cm. 2 Compared with unmodified SPEEK membrane (approximately 0.40 Ω·cm) 2 )near; (4) The functional layers are firmly covalently bonded and the interface functions are durable and stable: The functional layers on both sides are firmly bonded to the SPEEK base film through Si-OC covalent bonds (hydrophobic layer) and CC covalent bonds (hydrophilic layer), respectively, which is different from the weak bonding methods such as physical coating and electrostatic self-assembly. In the long-term immersion in alkaline electrolyte and electrochemical cycling, the covalently grafted functional layers are not easy to fall off or peel off, which ensures the durability of hydrophobic barrier and hydrophilic conduction functions, and provides structural support for the long-term cycle stability of the battery. (5) The preparation process is step-by-step and controllable, and easy to scale up: The present invention adopts a step-by-step process of "single-sided protection-plasma activation-directional grafting". Solvent-resistant tape is used to physically shield the surface of the side that is not being treated, so that each round of plasma activation and grafting reaction only acts on the exposed single surface. The modification on both sides is isolated from each other in time and space and does not interfere with each other. This process only requires conventional plasma treatment equipment and conventional reagents. The reaction conditions are mild and the parameters are highly controllable, which is convenient for industrial scale-up. (6) Excellent overall battery performance, combining high coulombic efficiency, high energy efficiency, and long-term cycle stability: The SPEEK membrane of this invention is oriented and assembled in an alkaline all-iron flow battery with its first surface facing the negative electrode and its second surface facing the positive electrode. The chemical environments of the functional layers on both sides are precisely matched with those of the corresponding electrode sides: the hydrophobic functional layer on the negative electrode side continuously repels triethanolamine (TEA) and inhibits cross-contamination; the hydrophilic ion conduction functional layer on the positive electrode side maintains a low-resistance interfacial ion transport channel, reducing the impedance growth of the membrane-electrolyte interface during cycling. The synergistic effect of these two factors enables the battery to achieve high coulombic efficiency while maintaining high energy efficiency, and exhibits excellent long-term cycle stability: at 60 mA / cm 2 After 8000 constant current charge-discharge cycles at the current density, the capacity retention rate is still above 93%, which is significantly better than that of the unmodified homogeneous film and the double-sided homogeneous modified film.
[0024] In summary, this invention covalently grafts a hydrophobic functional layer and a hydrophilic ion-conducting functional layer onto both sides of a SPEEK base film, forming a Janus interface with asymmetric wettability. This interface is fabricated using a single-sided protection-plasma activation-directional grafting process, and is assembled in an alkaline all-iron flow battery with the hydrophobic side facing the negative electrode and the hydrophilic side facing the positive electrode. This solution overcomes the dilemma of homogeneous membranes where one side is compromised: the hydrophobic layer inhibits triethanolamine (TEA) cross-contamination, the hydrophilic layer maintains low-resistance ion transport, and the covalently bonded functional layers are robust and durable. The battery exhibits high coulombic efficiency, high energy efficiency, and excellent long-cycle stability. Attached Figure Description
[0025] Figure 1This is a schematic diagram of the cross-sectional structure of the Janus asymmetric interface functionalized SPEEK membrane of the present invention, showing a three-layer asymmetric structure consisting of a hydrophobic functional layer on the first surface facing the negative electrode, a SPEEK base film, and a hydrophilic ion-conducting functional layer on the second surface facing the positive electrode.
[0026] Figure 2 Photographs and comparative bar charts of the water contact angle test results of the first and second surfaces of the SPEEK membrane prepared in Example 1 of the present invention.
[0027] Figure 3 This is a comparison of the polarization curves of the alkaline all-iron flow batteries assembled in Example 1 of the present invention with those of Comparative Examples 1 and 2.
[0028] Figure 4 The membranes of Example 1, Comparative Examples 1 and 2 of this invention were tested at 60 mA / cm. 2 Comparison of charge and discharge efficiencies at current densities.
[0029] Figure 5 The following are the long-cycle capacity retention curves (0-8000 cycles) of the membranes of Example 1, Comparative Examples 1 and 2 of this invention. Test conditions: current density 60 mA / cm². 2 Temperature 25±1℃.
[0030] Figure 6 The graph shows a comparison of sheet resistivity and TEA permeability coefficient of SPEEK base membranes with different degrees of sulfonation (DS=0.65, 0.70, 0.75, 0.80, 0.85, 0.90) after the same modification. The process parameters are the same as those in Example 1.
[0031] Figure 7 The graph shows a comparison of the water contact angle and surface resistivity of the first surface of the membrane modified with different concentrations of hydrophobic silane coupling agent (0.5 vol%, 1 vol%, 2 vol%, 3 vol%, 6 vol%). The modification of the second surface is uniformly performed under the conditions of Example 1.
[0032] Figure 8 The membrane of Example 1 of the present invention was tested at different current densities (40, 60, 80, 100 mA / cm²). 2 A comparison chart of charge and discharge efficiencies under different conditions. Detailed Implementation
[0033] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of this application.
[0034] In the following embodiments and comparative examples, the performance characteristics are characterized as follows: (1) Water contact angle test on both sides of the membrane: The water contact angle of the first surface (negative electrode side) and the second surface (positive electrode side) of the membrane was measured by the seat drop method using a contact angle measuring instrument (OCA 25, Dataphysics). The droplet volume was 2 μL, and at least 5 different positions were measured for each sample and the average value was taken. The test environment temperature was 25±1 ℃ and the relative humidity was 50±5%.
[0035] (2) Surface resistivity test: AC impedance spectroscopy (EIS) was used with an electrochemical workstation (Gamry Interface 1010E) at a frequency range of 10. 6 Hz to 10 -2 The surface resistivity of the membrane was measured in 1 mol / L KOH solution at a frequency of Hz and an amplitude of 5 mV, with an effective area of 1 cm². 2 Before testing, the membrane sample was soaked in 1 mol / L KOH solution for 24 hours to reach equilibrium; the sheet resistance R (Ω·cm) 2 )=Rm×A, where Rm is the measured resistance and A is the effective area.
[0036] (3) TEA permeability coefficient test: H-type diffusion cell (effective area 7.07 cm²) was used. 2 The supply chamber contained a mixed solution of 0.1 mol / L triethanolamine (TEA) and 1 mol / L KOH, while the receiving chamber contained a 1 mol / L KOH solution. The mixture was magnetically stirred (300 rpm) at room temperature (25 ℃), and 1 mL of sample was taken from the receiving chamber every 30 minutes for a total of 10 samplings. The concentration of triethanolamine (TEA) was measured at 280 nm using a UV-Vis spectrophotometer (UV-2600, Shimadzu). The permeability coefficient P was calculated according to Fick's first law: P = (Vd × L) / (A × t × (Cs - Cd(t))) × dCd / dt, where Vd is the volume of the receiving chamber, L is the membrane thickness, A is the effective area, t is time, Cs is the initial concentration in the supply chamber, and Cd(t) is the concentration in the receiving chamber at time t. A standard curve was plotted using a series of triethanolamine (TEA) standard solutions ranging from 0.001 to 0.05 mol / L, measured at 280 nm (R). 2 >0.999); Three parallel samples were set up for each group of experiments, and the average value was taken.
[0037] (4) Single cell performance test: effective membrane area 25 cm² 2The negative electrode electrolyte was a mixed solution of 0.5 mol / L TEA-Fe(III) and 3 mol / L KOH, and the positive electrode electrolyte was a mixed solution of 0.4 mol / L K3Fe(CN)6 / K4Fe(CN)6 (molar ratio 1:1) and 1 mol / L KOH, with each electrolyte having a volume of 50 mL. Constant current charge-discharge tests were performed using a flow battery testing system (LANDCT2001A), with a current density of 60 mA / cm² unless otherwise specified. 2 Cut-off voltage 0.5-1.5 V; Coulombic efficiency CE = discharge capacity / charge capacity × 100%, voltage efficiency VE = average discharge voltage / average charge voltage × 100%, energy efficiency EE = CE × VE.
[0038] (5) Long-term cycling stability test: at 60 mA / cm 2 Constant current charge-discharge cycles were performed at current density. The discharge capacity, coulombic efficiency, voltage efficiency, and energy efficiency were recorded every 100 cycles. The sheet resistance change of the film was tested using EIS every 500 cycles. The total number of cycles was 8000. Capacity retention rate = discharge capacity of the Nth cycle / discharge capacity of the 1st cycle × 100%.
[0039] (6) Modified layer thickness test: The cross-sectional morphology of the film was observed using a scanning electron microscope (SEM, Hitachi SU8010) with an accelerating voltage of 5 kV. The sample was subjected to liquid nitrogen embrittlement and then sputtered with gold. The thickness of the hydrophobic functional layer and the hydrophilic ion conduction functional layer was measured using ImageJ software. The average value was taken at 5 different locations for each sample.
[0040] (7) Determination of sulfonic acid group density: Using acid-base titration, accurately weigh approximately 0.5 g of the dried membrane sample and immerse it in 1 mol / L NaCl solution for 24 hours to allow the Na group to settle. + After thorough exchange with sulfonic acid protons, the released H+ was titrated with 0.01 mol / L NaOH standard solution using phenolphthalein as an indicator. + Sulfonic acid group density (mmol / g) = (VNaOH×CNaOH) / msample, where VNaOH is the volume of NaOH standard solution consumed (mL), CNaOH is the concentration of NaOH standard solution (mol / L), and msample is the dry weight of the membrane sample (g); each sample was measured 3 times and the average value was taken.
[0041] (8) Degree of sulfonation (DS): The degree of sulfonation refers to the average number of sulfonic acid groups in each PEEK repeating unit; it is determined by... 1 H nuclear magnetic resonance spectroscopy (H nuclear magnetic resonance spectroscopy) 1The SPEEK sample was dissolved in deuterated dimethyl sulfoxide (DMSO-d6) and tetramethylsilane was used as an internal standard. The degree of sulfonation was calculated by comparing the integral area ratio of the proton signals of sulfonated benzene rings and non-sulfonated benzene rings.
[0042] (9) Swelling rate determination: Cut the dry film sample into a square sample of 2 cm × 2 cm, measure its dry area, immerse it in 3 mol / L KOH solution, soak it at room temperature for 24 hours, take it out and quickly wipe off the residual liquid on the surface and measure the wet area. Swelling rate = (wet area - dry area) / dry area × 100%; each group of samples was measured in parallel 3 times and the average value was taken.
[0043] (10) Tensile strength test: The membrane was cut into dumbbell-shaped strips using a universal testing machine and the tensile strength was measured at room temperature; each group of samples was measured in parallel 3 times and the average value was taken.
[0044] In the following examples and comparative examples, the raw materials and reagents are as follows: Polyetheretherketone (PEEK): Victrex 450G brand, number average molecular weight approximately 160,000, or 770G brand, number average molecular weight approximately 120,000. Concentrated sulfuric acid: 95%-98% by mass, analytical grade. 1H,1H,2H,2H-Perfluorodecyltriethoxysilane (FAS, CAS: 101947-16-4): Purity ≥97%. Octadecyltrimethoxysilane (ODTS, CAS: 3069-42-9): Purity ≥95%. Perfluorooctylethyltrichlorosilane (CAS: 78560-45-9): Purity ≥97%. Potassium 3-Sulfopropylmethacrylate (SPMA, CAS: 31098-21-2): Purity ≥98%. Sodium vinylsulfonate (CAS: 3039-83-6): Purity ≥98%.
[0045] Sulfonate betaine monomer (SBMA) was synthesized as follows: 1,3-propanesulfonic acid lactone (10.0 g, 81.9 mmol) and dimethylaminoethyl methacrylate (13.0 g, 82.5 mmol) were dissolved in 50 mL of anhydrous acetonitrile, and the mixture was stirred at 60 °C for 24 hours under nitrogen protection. After the reaction was completed, the mixture was cooled to room temperature, filtered to collect the white precipitate, washed three times with acetonitrile, and dried under vacuum at 60 °C for 12 hours to obtain sulfonate betaine monomer in approximately 92% yield. 1 H NMR (400 MHz, D2O): δ6.10 (s, 1H), 5.65 (s, 1H), 4.30 (t, 2H), 3.80 (t, 2H), 3.50 (t, 2H), 3.20 (s, 6H), 2.90 (t, 2H), 1.90 (s, 3H).
[0046] Potassium persulfate (KPS, CAS: 7727-21-1), ammonium persulfate (APS, CAS: 7727-54-0): analytical grade. Triethanolamine (TEA, CAS: 102-71-6): analytical grade. Potassium ferrocyanide (K4Fe(CN)6·3H2O, CAS: 14459-95-1) and potassium ferrocyanide (K3Fe(CN)6, CAS: 13746-66-2): analytical grade. Potassium hydroxide (KOH, CAS: 1310-58-3): analytical grade. N,N-Dimethylformamide (DMF, CAS: 68-12-2): analytical grade. Toluene (CAS: 108-88-3), n-hexane (CAS: 110-54-3), ethanol (CAS: 64-17-5): analytical grade. Solvent-resistant tape: polyimide tape (0.05 mm thick) or polytetrafluoroethylene tape (0.08 mm thick).
[0047] Example 1 In this embodiment, a Janus asymmetric interface functionalized SPEEK membrane was prepared using FAS as a hydrophobic modifier and SPMA as a hydrophilic monomer, as detailed below.
[0048] Step 1: Preparation of SPEEK base film: Victrex 450G PEEK powder (number average molecular weight approximately 160,000) was added to 98% concentrated sulfuric acid and sulfonated at 50 °C for 5 hours. After the reaction, the reaction solution was slowly poured into an ice-water mixture to precipitate. The precipitate was filtered and repeatedly washed with deionized water until neutral. After drying, a SPEEK resin with a degree of sulfonation DS=0.75 was obtained. This SPEEK resin was dissolved in N,N-dimethylformamide (DMF) to prepare a 15% casting solution. After vacuum degassing for 2 hours, the solution was cast onto a clean glass plate and dried at 80 °C for 12 hours. Subsequently, the temperature was raised to 120 °C and vacuum dried for 4 hours to obtain a dense SPEEK base film with a thickness of approximately 30 μm.
[0049] Step 2: Hydrophobic modification of the first surface (negative electrode side): The second surface of the SPEEK base film was tightly protected with polyimide tape, ensuring that the tape edges were completely adhered to the film surface to prevent solution leakage. The unprotected first surface was exposed to oxygen plasma at a power of 50 W for 4 minutes to generate active sites on the surface. Subsequently, the film was immersed in a toluene solution containing 2 vol% 1H,1H,2H,2H-perfluorodecyltriethoxysilane (FAS) (toluene has a boiling point of approximately 110.6 °C at normal pressure; the reaction temperature should not exceed the boiling point of the selected solvent) at 80 °C for 4 hours. After removal, the film was washed three times each with toluene and ethanol, and then vacuum dried at 60 °C for 6 hours. SEM measurements showed that the thickness of the hydrophobic functional layer formed on the first surface was approximately 0.8 μm.
[0050] Step 3: Hydrophilic modification of the second surface (positive electrode side): Remove the tape from Step 2 and tightly protect the first surface, where the hydrophobic functional layer has been formed, with new polyimide tape. Expose the unprotected second surface to argon plasma at 80 W for 5 minutes to generate active sites on the surface. Subsequently, immerse the membrane in an aqueous solution containing 10 wt% potassium 3-sulfopropyl methacrylate (SPMA) and 0.1 wt% potassium persulfate (KPS) initiator, and react at 70 °C for 2 hours under nitrogen protection. After removal, wash thoroughly with deionized water until the washing solution is neutral, and vacuum dry at 60 °C for 6 hours to obtain the Janus asymmetric interface functionalized SPEEK membrane. SEM measurements show that the thickness of the hydrophilic ion-conducting functional layer formed on the second surface is approximately 0.6 μm.
[0051] In this embodiment, steps two and three use oxygen plasma and argon plasma respectively, verifying the process flexibility of the present invention, which allows for activation on both sides using the same or different plasma types.
[0052] Characterization results: such as Figure 1 As shown, the membrane in this embodiment consists of a three-layer asymmetric structure comprising a first surface hydrophobic functional layer, a SPEEK base film, and a second surface hydrophilic ion-conducting functional layer; as Figure 2 As shown, the water contact angle on the first surface (negative electrode side) is 128°, and the water contact angle on the second surface (positive electrode side) is 18°. The extreme divergence of the contact angles on both sides visually verifies the successful construction of the Janus asymmetric structure. The sheet resistivity of the membrane is 0.55 Ω·cm. 2 The TEA permeability coefficient is 0.8 × 10⁻⁶. -7 cm 2 / min, the density of sulfonic acid groups on the surface of the grafted layer is 2.3 mmol / g (based on the dry weight of the functional layer).
[0053] Battery performance testing: Assemble the battery according to the single-cell performance testing method described above, and test at 60 mA / cm². 2 At the given current density, the coulombic efficiency is 99.8%, the voltage efficiency is 85.3%, and the energy efficiency is 85.1%; for example... Figure 5 As shown, the capacity retention rate is 94.2% after 8000 long cycles, and the surface resistivity increases by only 3.5% every 500 cycles.
[0054] Example 2 This embodiment prepares a Janus asymmetric interface functionalized SPEEK membrane using ODTS as a hydrophobic modifier and sulfobetaine monomer as a hydrophilic monomer. The preparation of the SPEEK base membrane is the same as in Example 1; in the first surface hydrophobic modification, a toluene solution containing 3 vol% octadecyltrimethoxysilane (ODTS) is used, and the reaction is carried out at 85 °C for 4 hours; in the second surface hydrophilic modification, an aqueous solution containing 10 wt% sulfobetaine monomer (SBMA) and 0.1 wt% KPS is used, and the reaction is carried out at 70 °C for 2.5 hours; the remaining conditions are the same as in Example 1.
[0055] Test results show that the water contact angle of the first surface is 115°, and the water contact angle of the second surface is 22°; the surface resistivity is 0.60 Ω·cm. 2 The TEA permeability coefficient is 1.1 × 10⁻⁶. -7 cm 2 / min, sulfonic acid group density is 2.1 mmol / g. At 60 mA / cm 2 At current density, the coulombic efficiency is 99.7%, the voltage efficiency is 84.8%, and the energy efficiency is 84.5%; the capacity retention rate is 93.5% after 8000 long cycles.
[0056] It should be noted that SBMA is an amphoteric monomer. In its grafted layer, sulfonate and quaternary ammonium groups coexist in equal molar amounts, and the net surface charge is close to zero. Its barrier and conduction functions mainly rely on the dense hydration layer formed by strong electrostatic hydration. This embodiment verifies that this type of monomer can also construct an interfacial functional layer that combines hydrophilicity, barrier properties, and ionic conductivity.
[0057] Example 3 This embodiment prepares a Janus asymmetric interface functionalized SPEEK membrane using perfluorooctyl ethyl trichlorosilane as a hydrophobic modifier and sodium vinyl sulfonate as a hydrophilic monomer. The preparation of the SPEEK base membrane is the same as in Example 1; in the first surface hydrophobic modification, a hexane solution containing 2.5 vol% perfluorooctyl ethyl trichlorosilane was used (because chlorosilane is easily hydrolyzed, the humidity of the operating environment was controlled below 30%), and the reaction was carried out at 65 °C for 5 hours (the boiling point of hexane at normal pressure is about 69 °C, and the reaction temperature was taken near its reflux temperature and not higher than the boiling point of the selected solvent); in the second surface hydrophilic modification, an aqueous solution containing 12 wt% sodium vinyl sulfonate and 0.12 wt% ammonium persulfate (APS) was used, and the reaction was carried out at 65 °C for 2 hours; the remaining conditions are the same as in Example 1.
[0058] Test results show that the water contact angle of the first surface is 125° and the water contact angle of the second surface is 15°; the surface resistivity is 0.52 Ω·cm. 2 The TEA permeability coefficient is 0.9 × 10⁻⁶. -7 cm 2 / min, sulfonic acid group density is 2.5 mmol / g. At 60 mA / cm 2 At current density, the coulombic efficiency is 99.7%, the voltage efficiency is 85.5%, and the energy efficiency is 85.3%.
[0059] Example 4 This example investigates the effect of a base film with the lower limit of the sulfonation degree range (DS=0.70) on the performance of a SPEEK membrane. SPEEK with a sulfonation degree of DS=0.70 was prepared by sulfonating PEEK in concentrated sulfuric acid at 45 °C for 4 hours. A base film with a thickness of approximately 30 μm was then prepared and modified in the same manner as in Example 1. Test results show that the water contact angle of the first surface is 126°, and the water contact angle of the second surface is 19°; the sheet resistivity is 0.65 Ω·cm. 2 The TEA permeability coefficient is 0.7 × 10⁻⁶. -7 cm 2 / min. At 60 mA / cm 2 At current density, the coulombic efficiency is 99.7%, the voltage efficiency is 84.0%, and the energy efficiency is 83.7%; the capacity retention rate is 93.8% after 8000 long cycles.
[0060] Example 5 This example investigates the effect of a base film with a high degree of sulfonation (DS=0.80) on the performance of the SPEEK membrane. SPEEK with a sulfonation degree of DS=0.80 was prepared by sulfonating PEEK in concentrated sulfuric acid at 50 °C for 5.5 hours. A base film with a thickness of approximately 30 μm was then prepared according to the method in Example 1 and subjected to the same process. Modification. Test results show that the water contact angle of the first surface is 129°, and the water contact angle of the second surface is 17°; the surface resistivity is 0.50 Ω·cm. 2 The TEA permeability coefficient is 1.0 × 10⁻⁶. -7 cm 2 / min. At 60 mA / cm 2 At current density, the coulombic efficiency is 99.7%, the voltage efficiency is 85.0%, and the energy efficiency is 84.7%; the capacity retention rate is 93.9% after 8000 long cycles.
[0061] Example 6 This example investigates the effect of a lower hydrophobic silane concentration (1 vol%) on the performance of the SPEEK membrane to verify the necessity of a lower limit for the concentration of the hydrophobic silane coupling agent. The preparation process of Example 1 was repeated, except that the volume concentration of FAS in step two was changed to 1%, and the reaction time was extended to 5 hours. Test results show that the water contact angle of the first surface is 108°, the thickness of the hydrophobic functional layer is approximately 0.5 μm, and the sheet resistivity is 0.50 Ω·cm. 2The TEA permeability coefficient is 3.2 × 10⁻⁶. -7 cm 2 / min. At 60 mA / cm 2 At the current density, the coulombic efficiency is 99.6% and the energy efficiency is 84.0%. Compared with Example 1, the hydrophobic layer is discontinuous and thinner after the silane concentration is reduced, the first surface contact angle is less than 115° and the TEA permeability coefficient is significantly increased, confirming the necessity of the lower limit of the hydrophobic silane concentration range.
[0062] Example 7 This example investigates the effect of a lower hydrophilic monomer concentration (6 wt%) on the performance of the SPEEK membrane to verify the necessity of a lower limit for the hydrophilic monomer concentration. The preparation process of Example 1 was repeated, except that the mass concentration of SPMA in step three was changed to 6%, and the reaction time was extended to 3 hours. Test results show that the water contact angle of the second surface is 25°, the thickness of the hydrophilic ion-conducting functional layer is approximately 0.4 μm, and the sheet resistivity is 0.52 Ω·cm. 2 The density of the sulfonic acid group is 1.8 mmol / g. At 60 mA / cm²... 2 At the given current density, the coulombic efficiency was 99.7%, the voltage efficiency was 84.5%, and the energy efficiency was 84.2%. Compared to Example 1, the grafted layer was thinner after the monomer concentration was reduced, the surface sulfonic acid group density decreased to the lower limit of the range, and the second surface contact angle was slightly higher than 22°.
[0063] Example 8 This example investigates the effect of a higher hydrophilic monomer concentration (14 wt%) on the performance of the SPEEK membrane to verify the necessity of an upper limit for the hydrophilic monomer concentration. The preparation process of Example 1 was repeated, except that the mass concentration of SPMA in step three was changed to 14%, and the reaction time was shortened to 1.5 hours. Test results show that the water contact angle of the second surface is 16°, the thickness of the hydrophilic ion-conducting functional layer is approximately 1.2 μm, and the sheet resistivity is 0.58 Ω·cm. 2 The sulfonic acid group density is 2.7 mmol / g. At 60 mA / cm²... 2 At the given current density, the coulombic efficiency is 99.8%, the voltage efficiency is 84.9%, and the energy efficiency is 84.7%. In this embodiment, the hydrophobic layer is approximately 0.8 μm thick, the hydrophilic layer is approximately 1.2 μm thick, and the total thickness of the two layers is approximately 2.0 μm, which is exactly at the boundary of the total thickness limit (not exceeding 2 μm) specified in this invention. The battery performance is still good, further confirming the rationality of this upper limit of thickness.
[0064] Example 9 This embodiment examines the adaptability of the SPEEK membrane under different current densities. Single cells were assembled using the SPEEK membrane prepared in Example 1, and tested at current densities of 40, 60, 80, and 100 mA / cm².2 Constant current charge-discharge tests were conducted at the current density, with other test conditions the same as in Example 1. The test results are shown in Table 1.
[0065] Table 1. Charge-discharge performance of SPEEK film in Example 1 at different current densities. like Figure 8 As shown in Table 1, the SPEEK membrane of Example 1 operates at 40-100 mA / cm². 2 It maintains high coulombic efficiency (>99.5%) and energy efficiency (>80%) across a wide current density range, indicating that it has good adaptability to operating conditions.
[0066] Comparative Example 1 This comparative example is a homogeneous hydrophilic modified membrane with sulfonic acid groups grafted on both sides, used to demonstrate the necessity of a hydrophobic functional layer on the negative electrode side. The preparation of the SPEEK base membrane is the same as in Example 1, but without unilateral protection. The base membrane is exposed to argon plasma (power 80 W, 5 minutes) and then immersed in an aqueous solution containing 10 wt% SPMA and 0.1 wt% KPS. The reaction is carried out at 70 °C for 2 hours. After washing and drying, a hydrophilic modified membrane with both sides is obtained.
[0067] Test results show that the water contact angles on both sides of the membrane are 20° and 18°, respectively, indicating strong hydrophilicity on both sides; the sheet resistivity is 0.45 Ω·cm. 2 The TEA permeability coefficient is 7.5 × 10⁻⁶. -7 cm 2 / min, close to that of the unmodified membrane. At 60 mA / cm 2 At current density, the coulombic efficiency is 99.5% and the energy efficiency is 83.2%; the capacity retention rate is 88.1% after 8000 long cycles.
[0068] This comparative example shows that although hydrophilic modification on both sides can reduce sheet resistance, it cannot inhibit the transmembrane permeation of triethanolamine (TEA), and the long-term cycling capacity decay is significantly accelerated.
[0069] Comparative Example 2 This comparative example uses an unmodified SPEEK homogeneous membrane. The SPEEK base membrane (DS=0.75, thickness 30 μm) prepared in Example 1 was used directly without any surface modification.
[0070] Test results show that the water contact angle on both sides of the membrane is 65°; the sheet resistivity is 0.40 Ω·cm. 2 The TEA permeability coefficient is 8.2 × 10⁻⁶. -7 cm 2 / min. At 60 mA / cm 2At current density, the coulombic efficiency is 99.4% and the energy efficiency is 83.0%; after 8000 long cycles, the capacity retention is 86.5%.
[0071] Comparative Examples 3-8 This group comparatively investigated the performance of SPEEK base films with different degrees of sulfonation after the same modification to verify the rationality of the base film sulfonation degree range (DS=0.70-0.85). SPEEK base films with sulfonation degrees DS of 0.65, 0.70, 0.75, 0.80, 0.85, and 0.90 were prepared respectively: the film with DS=0.65 was prepared by sulfonating PEEK in concentrated sulfuric acid at 40 °C for 3 hours, the film with DS=0.85 was prepared by sulfonating at 55 °C for 6 hours, and the film with DS=0.90 was prepared by sulfonating at 60 °C for 8 hours. The base films with DS=0.70, 0.75, and 0.80 were the same as those in Examples 4, 1, and 5, respectively; the thickness of all base films was controlled to be approximately 30 μm. All sulfonated membranes were modified according to the method in Example 1 (sample data for DS=0.70, 0.75, and 0.80 were obtained from Examples 4, 1, and 5, respectively). The test results are shown in Table 2. The comparison between sheet resistivity and TEA permeability coefficient is also shown in Table 2. Figure 6 .
[0072] Table 2. Comparison of performance of modified films with different degrees of sulfonation Table 2 shows that when DS=0.65, the membrane structure is dense, and although the TEA permeability coefficient is relatively low (0.6×10⁻⁶), the membrane structure is dense. -7 cm 2 ( / min), but the surface resistivity increased significantly to 0.85 Ω·cm. 2 The energy efficiency dropped to 81.5%, indicating that the low sulfonation level resulted in insufficient bulk ionic conductivity of the membrane; the sheet resistivity was moderate (0.50-0.65 Ω·cm) within the DS = 0.70-0.80 range. 2 Triethanolamine (TEA) has good barrier properties (0.7-1.0×10⁻⁶). -7 cm 2 ( / min), with optimal overall performance; at DS=0.85, the swelling rate reached 78%, and the TEA permeability coefficient increased to 1.5×10. -7 cm 2 / min; at DS=0.90, the swelling ratio increased sharply to 95%, the mechanical strength of the membrane decreased significantly (tensile strength <20 MPa), and the TEA permeability coefficient further increased to 3.2×10 -7 cm 2 / min, the coulombic efficiency drops to 99.2%. Considering ion conduction, barrier properties and mechanical strength, DS=0.70-0.85 is a reasonable window, and the deterioration direction at the boundary of the range can be explained by the correlation mechanism of sulfonation degree-swelling-conductivity.
[0073] Comparative Examples 9-13 This group comparatively investigated the effect of hydrophobic silane coupling agent concentration on the modification effect to verify the rationality of its concentration range (1%-5%, preferably 2%-3%). On the base film of Example 1, hydrophobic modification of the first surface was performed using FAS toluene solutions with volume concentrations of 0.5%, 1%, 2%, 3%, and 6%, respectively. The second surface was grafted with SPMA according to the method of Example 1. The test results are shown in Table 3 (where data for samples with FAS volume concentrations of 1% and 2% are from Example 6 and Example 1, respectively). The comparison of contact angle and sheet resistance is shown in Table 3. Figure 7 .
[0074] Table 3. Performance comparison of membranes modified with different FAS concentrations From Table 3 and Figure 7 It is evident that when the FAS concentration does not exceed 1%, the hydrophobic layer is discontinuous or too thin, the first surface contact angle does not exceed 108°, and the TEA permeability coefficient is not less than 3.2 × 10⁻⁶. -7 cm 2 / min, insufficient seepage barrier effect; when FAS concentration is 2%-3%, the hydrophobic layer is intact (thickness 0.8-1.2 μm), the contact angle is greater than 120°, and the TEA permeability coefficient does not exceed 0.8×10 -7 cm 2 / min, with moderate surface resistivity (0.55-0.58 Ω·cm) 2 It exhibits the best overall performance; at a FAS concentration of 6%, the hydrophobic layer thickness reaches 2.8 μm, and the surface resistivity significantly increases to 0.72 Ω·cm. 2 The energy efficiency dropped to 82.5%, which was caused by excessive silane self-polymerization to form macrophase polysiloxane. Therefore, the volume concentration of hydrophobic silane coupling agents is reasonably within the range of 1%-5%, with 2%-3% being preferred.
[0075] Comparative Example 14 This comparative example is a thick-layer modified SPEEK film, used to demonstrate the necessity of limiting the thickness of the functional layers. The preparation process of Example 1 was repeated, except that the volume concentration of FAS in step two was increased to 8%, and the reaction time was extended to 8 hours, resulting in a SPEEK film with a hydrophobic functional layer thickness of approximately 3.5 μm (the single-layer thickness exceeded the 1.5 μm upper limit, and the total thickness of the two functional layers also exceeded 2 μm). The second surface modification was the same as in Example 1. Test results showed that the sheet resistivity of this film was 0.88 Ω·cm.2 It is significantly higher than 0.55 Ω·cm in Example 1. 2 At 60 mA / cm 2 At the specified current density, the voltage efficiency is only 78.5%, the energy efficiency is 78.2%, and the coulombic efficiency is 99.7%. Although its TEA penetration coefficient further decreases to 0.5 × 10⁻⁶. -7 cm 2 However, the excessively thick hydrophobic layer significantly increases the ohmic resistance, leading to increased battery polarization and a significant decrease in efficiency. This comparative example demonstrates that the thickness of a single functional layer should not exceed 1.5 μm, and the total thickness of two functional layers should not exceed 2 μm; otherwise, interface functionalization will come at the cost of sacrificing ohmic properties.
[0076] The performance data of the main embodiments and comparative examples are summarized in Table 4.
[0077] Table 4 Summary of performance data for main embodiments and comparative examples Note: Performance data for Comparative Examples 3-8 are detailed in Table 2, and performance data for Comparative Examples 9-13 are detailed in Table 3.
[0078] As can be seen from the above embodiments and comparative examples, and the data in Table 4: First, Janus' asymmetric interface functionalization design achieves decoupling of triethanolamine (TEA) blocking and ion conduction: the SPEEK films in Examples 1-5 maintain a low sheet resistance (0.50-0.65 Ω·cm). 2 Meanwhile, the TEA permeation coefficient was significantly higher than that of the unmodified membrane in Comparative Example 2 (8.2 × 10⁻⁶). -7 cm 2 / min) and the bilateral hydrophilic membrane of Comparative Example 1 (7.5×10 -7 cm 2 The efficiency was reduced by nearly an order of magnitude ( / min), the coulombic efficiency was increased to over 99.7%, and the energy efficiency reached over 83.7% (with Examples 1 and 3 reaching over 85%). Figure 3 , Figure 4 As shown, its polarization behavior and charge / discharge efficiency are both superior to the two comparative examples. This indicates that the contradictory properties of barrier and conduction can only be achieved when both sides of the film possess interfacial properties that match the corresponding electrode environment.
[0079] Secondly, the covalently grafted interfacial functional layer endows the membrane with excellent long-term cycling stability: such as Figure 5As shown, the membrane of Example 1 maintained a capacity retention of 94.2% after 8000 cycles, with a sheet resistance increase of only 3.5% per 500 cycles; while the capacity retention of Comparative Examples 1 and 2 under the same conditions was only 88.1% and 86.5%, respectively. The functional layers on both sides are firmly bonded to the SPEEK base membrane through Si-OC bonds and CC bonds, respectively, and do not detach or fail during long-term immersion in alkaline electrolyte and electrochemical cycling. The negative electrode side continuously inhibits triethanolamine (TEA) permeation, while the positive electrode side maintains a stable ion transport channel. The two work together to ensure capacity stability during long-term cycling.
[0080] Third, the sulfonation degree window of the base film has clear boundary experimental evidence: the series of experiments of Comparative Examples 3-8 show that the samples in the range of DS=0.70-0.85 have both moderate sheet resistivity and good permeability barrier properties; when the sheet resistivity is below 0.70, it increases significantly due to insufficient bulk conductivity; when it is above 0.85, excessive swelling leads to deterioration of permeability barrier properties and mechanical strength. The deterioration direction of the samples outside the range can be explained by mechanism, which constitutes a complete chain of evidence that "it is feasible within the range and not feasible outside the range".
[0081] Fourth, the concentration window of hydrophobic silane and the limitation on the thickness of the functional layer are also supported by boundary experimental evidence: Comparative Examples 9-13 show that a continuous and complete hydrophobic layer can be obtained when the FAS concentration is 1%-5%, with 2%-3% being the performance peak. Beyond the upper limit, silane self-polymerization leads to a significant increase in sheet resistivity. Comparative Example 14 further shows that when the thickness of a single functional layer exceeds 1.5 μm and the total thickness exceeds 2 μm, ohmic polarization increases significantly, and energy efficiency decreases sharply. The above negative data corroborate the parameter change results of Examples 6-8, fully demonstrating the scientific validity and necessity of the parameter ranges defined in this invention.
[0082] Fifth, the SPEEK membrane exhibits wide operating condition adaptability: Example 9 shows that the membrane of the present invention operates at 40-100 mA / cm². 2 It maintains a coulombic efficiency of >99.5% and an energy efficiency of >80% across the current density range, and can adapt to the variable load operation requirements of actual energy storage scenarios.
[0083] It should be noted that in existing publicly reported tests, the homogeneous SPEEK membranes used in flow batteries are mostly in the hundreds of cycles range, while the SPEEK membrane of this invention still retains more than 93% of its capacity and has an intact membrane structure after 8,000 cycles. The difference between the two is more than an order of magnitude, which fully demonstrates the contribution of bilateral covalent grafting interface functionalization to long-term cycle stability.
[0084] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings and specific examples. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
Claims
1. A Janus asymmetric interfacially functionalized SPEEK membrane comprising a SPEEK base membrane, characterized in that: The SPEEK base film has a first surface facing the negative electrode of the alkaline all-iron flow battery and a second surface facing the positive electrode when in use; the first surface is covalently grafted with a hydrophobic functional layer, and the water contact angle of the first surface is greater than or equal to 115°; the hydrophobic functional layer is formed by hydrolysis and condensation reaction of a fluorinated silane coupling agent and / or a long-chain alkyl silane coupling agent on the surface of the SPEEK base film; the second surface is covalently grafted with a hydrophilic ion-conducting functional layer, and the water contact angle of the second surface is less than or equal to 22°; the hydrophilic ion-conducting functional layer is formed by graft polymerization of a polymerizable hydrophilic monomer containing sulfonic acid groups on the surface of the SPEEK base film; the thickness of the hydrophobic functional layer and the hydrophilic ion-conducting functional layer are each independently 0.3-1.5 μm, and the sum of the two does not exceed 2 μm.
2. The Janus asymmetric interfacially functionalized SPEEK membrane of claim 1, wherein: The fluorinated silane coupling agent is selected from any one of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and perfluorooctylethyltrichlorosilane, and the long-chain alkylsilane coupling agent is octadecyltrimethoxysilane.
3. The Janus asymmetric interfacially functionalized SPEEK membrane of claim 1, wherein: The polymerizable hydrophilic monomer containing sulfonic acid groups is selected from any one of sodium vinyl sulfonate, potassium 3-sulfonopropyl methacrylate, and sulfonate betaine monomer, wherein the chemical name of the sulfonate betaine monomer is [2-(methacryloyloxy)ethyl]dimethyl(3-sulfonopropyl)ammonium hydroxide inner salt; the surface sulfonic acid group density of the hydrophilic ion-conducting functional layer is 1.8-2.7 mmol / g.
4. The Janus asymmetric interfacially functionalized SPEEK membrane of claim 1, wherein: The SPEEK base film is a dense film with a sulfonation degree of 0.70-0.85 and a thickness of 25-40 μm.
5. The Janus asymmetric interfacially functionalized SPEEK membrane of claim 4, wherein: The SPEEK base film is prepared by sulfonation of polyether ether ketone with a number average molecular weight of 80,000-200,000 with concentrated sulfuric acid. The concentrated sulfuric acid has a mass fraction of 95%-98%, the sulfonation temperature is 40-60 ℃, and the sulfonation time is 1-8 hours.
6. A method of preparing a Janus asymmetric interfacially functionalized SPEEK membrane according to any one of claims 1 to 5, characterized in that, Includes the following steps: Step 1: Tightly protect the second surface of the SPEEK base film with solvent-resistant tape to isolate the second surface from the subsequent processing environment; Step 2: Expose the unprotected first surface to low-temperature plasma for activation treatment. The plasma power is 50-80 W and the treatment time is 3-6 minutes to generate active sites on the first surface. Step 3: Immerse the activated membrane in an organic solution containing a hydrophobic silane coupling agent, heat it under normal pressure to 70%-95% of the boiling point of the selected solvent, and react for 2-6 hours to form a hydrophobic functional layer on the first surface; the volume concentration of the hydrophobic silane coupling agent in the organic solution is 1%-5%. Step 4: Remove the solvent-resistant tape, wash and dry the membrane, and then tightly protect the first surface where the hydrophobic functional layer has been formed with new solvent-resistant tape. Step 5: Expose the unprotected second surface to low-temperature plasma for activation treatment. The plasma power is 50-80 W and the treatment time is 3-6 minutes to generate active sites on the second surface. Step 6: The membrane is then immersed in an aqueous solution containing hydrophilic monomers and persulfate initiators, and reacted at 60-80 °C for 1-4 hours under nitrogen protection to form a hydrophilic ion-conducting functional layer on the second surface; the mass concentration of the hydrophilic monomers in the aqueous solution is 5%-15%, and the mass concentration of the persulfate initiator is 0.05%-0.2%. Step 7: Remove the membrane, wash and dry it to obtain the Janus asymmetric interface functionalized SPEEK membrane.
7. The preparation method according to claim 6, characterized in that: In steps 2 and 5, the low-temperature plasma is selected from oxygen plasma, argon plasma, and nitrogen plasma; in steps 1 and 3, the solvent-resistant tape is selected from polyimide tape or polytetrafluoroethylene tape.
8. The method of claim 6, wherein: In step 3, the volume concentration of the hydrophobic silane coupling agent in the organic solution is 2%-3%, the organic solvent used in the organic solution is toluene or n-hexane, and the reaction time is 3-5 hours; the reaction temperature matches the boiling point of the selected organic solvent: when the organic solvent is toluene, the reaction temperature is 80-100 ℃; when the organic solvent is n-hexane, the reaction temperature is 60-65 ℃.
9. The method of claim 6, wherein: In step 6, the mass concentration of the hydrophilic monomer in the aqueous solution is 8%-12%, the mass concentration of the persulfate initiator is 0.08%-0.15%, the reaction temperature is 65-75 ℃, and the reaction time is 1.5-2.5 hours; the persulfate initiator is selected from any one of potassium persulfate, ammonium persulfate, and sodium persulfate.
10. An alkaline full iron liquid flow battery characterized by, include: Positive electrode electrolyte: Contains ferrocyanide and / or ferricyanide as the positive electrode active material, dissolved in an alkaline aqueous solution; Negative electrode electrolyte: Contains triethanolamine iron complex as the negative electrode active material, dissolved in an alkaline aqueous solution; Separator: The Janus asymmetric interface functionalized SPEEK membrane according to any one of claims 1 to 5 is assembled in the alkaline all-iron flow battery with its first surface facing the negative electrode and its second surface facing the positive electrode.
Citation Information
Patent Citations
Alkaline zinc-iron flow battery diaphragm as well as preparation and application thereof
CN121905887A