Battery cells and their preparation methods, secondary batteries and electrical devices

By injecting carbon dioxide gas into the battery components at low temperature and allowing it to adsorb, the hydrogen bonds of water molecules in the battery electrodes are broken, solving the problem of difficult removal of moisture from the battery electrodes and improving the electrochemical performance of the battery.

CN123120809APending Publication Date: 2026-11-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510634464.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing battery manufacturing processes, it is difficult to effectively remove moisture from battery electrodes, which affects the battery's electrochemical performance, especially its initial charge-discharge efficiency, cycle life, and high-temperature storage performance.

Method used

Carbon dioxide gas is injected into the battery components at a low temperature of 0℃~10℃. After static adsorption, the components are baked. The carbon dioxide forms a strong bond with water molecules in the micro-nano pores, which breaks the hydrogen bonds of the water molecules and promotes ionization. The moisture is then removed by baking.

Benefits of technology

It effectively reduces the water content of battery components, improving the battery's initial charge/discharge efficiency, cycle performance, and high-temperature storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120809A_ABST
    Figure CN123120809A_ABST
Patent Text Reader

Abstract

This application provides a battery cell, its preparation method, a secondary battery, and an electrical device, belonging to the field of battery manufacturing technology. The preparation method of the battery cell includes the following steps: placing the battery component in a sealed device, injecting a gas including carbon dioxide into the sealed device at 0℃~10℃, allowing it to stand for a period of time, and then baking it to obtain the battery cell. By injecting a gas including carbon dioxide at a low temperature and completing the static adsorption, followed by baking, moisture in the micro-nano pores of the battery component can be effectively removed, reducing the water content, thereby improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery manufacturing technology, and more specifically, to a battery cell and its manufacturing method, a secondary battery, and an electrical device. Background Technology

[0002] Residual moisture in battery electrodes can severely affect the battery's electrochemical performance, such as reducing cycle life. Therefore, current battery manufacturing processes involve baking the battery before electrolyte injection to reduce its water content. However, this method of water removal is not very effective. Summary of the Invention

[0003] This application is made in view of the above-mentioned issues, and its purpose is to provide a battery cell and its preparation method, a secondary battery and an electrical device, so as to effectively remove moisture in the micro-nano pores of the battery components, reduce the water content, and thereby improve the battery's first charge-discharge efficiency (hereinafter referred to as first efficiency), cycle performance and high-temperature storage performance.

[0004] The first aspect of this application provides a method for preparing a battery cell, comprising the following steps:

[0005] The battery components are placed in a sealed device, and gas including carbon dioxide is injected into the sealed device at 0℃~10℃. After standing for a period of time, the device is baked to obtain a single battery cell.

[0006] In the above technical solution, this application involves injecting a gas including carbon dioxide into a sealed device at a low temperature of 0℃ to 10℃ and allowing it to stand for adsorption, followed by baking. The carbon dioxide gas can form strong bonds with water molecules within the micro- and nano-pores of the battery components, breaking the hydrogen bonds between water molecules and promoting the ionization of water molecules. This disrupts the tight adsorption between water molecules and the material interface, effectively removing moisture after baking. This preparation method is simple to operate and can effectively reduce the water content of battery components, thereby improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.

[0007] In some embodiments, the battery component is an electrode assembly, and the sealed device is a battery casing; the method for preparing a battery cell includes the following steps: placing the electrode assembly inside the battery casing, injecting a gas including carbon dioxide into the battery casing at 0°C to 10°C, allowing it to stand for a period of time, and then baking it; injecting liquid and forming the baked electrode assembly to obtain a battery cell.

[0008] In the above technical solution, the electrode assembly typically includes a positive electrode, a negative electrode, and a separator, all of which have a large number of micro- and nano-porous structures. By injecting a gas including carbon dioxide at a low temperature of 0℃ to 10℃ and allowing it to stand for adsorption before baking, the moisture on the surface of the electrode assembly and in the micro- and nano-porous structures can be effectively removed, reducing the water content of the electrode assembly and thus improving the battery's first efficiency, cycle performance, and high-temperature storage performance.

[0009] In some embodiments, the electrode assembly includes a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film layer attached to at least one side surface of the negative current collector, the negative electrode film layer including a porous carbon material.

[0010] In the above technical solution, when the negative electrode film layer includes porous carbon material, carbon dioxide molecules not only form strong bonds with water molecules on the surface of the porous carbon material, but also, because the average radius of motion of water molecules (0.27nm~0.32nm) is comparable to that of carbon dioxide molecules (0.33nm), carbon dioxide molecules can enter the micro-nano pores (pore size ≤10nm) that adsorb water molecules. The pores of the porous carbon material can generate strong intermolecular forces with carbon dioxide molecules, disrupting the interfacial interaction between water molecules and the carbon material, resulting in competitive adsorption. At low temperatures, water molecules within the micro-nano pores can combine with adsorbed carbon dioxide molecules to form carbonic acid, making water molecules more prone to transition from a liquid to a gaseous state, which is easily removed during subsequent baking. Therefore, by allowing the electrode assembly to adsorb carbon dioxide molecules at low temperatures and then combining this with baking, the moisture within the micro-nano pores of the porous carbon material can be effectively removed, reducing the water content of the negative electrode sheet, thereby further improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.

[0011] In some embodiments, the electrode assembly includes a positive electrode sheet, which includes a positive current collector and a positive electrode film layer attached to at least one side of the positive current collector. The positive electrode film layer includes a positive electrode active material with a carbon layer coated on its surface.

[0012] In the above technical solution, when the surface of the positive electrode active material is coated with a carbon layer, carbon dioxide molecules not only form strong bonds with water molecules on the carbon layer surface, but also can enter the micro-nano pores (pore size ≤10nm) that adsorb water molecules. The carbon layer pores can then generate strong intermolecular forces with the carbon dioxide molecules, disrupting the interfacial interaction between water molecules and the carbon material, resulting in competitive adsorption. At low temperatures, water molecules within the micro-nano pores can combine with the adsorbed carbon dioxide molecules to form carbonic acid, making the water molecules more prone to changing from a liquid to a gaseous state, which is easily removed during subsequent baking. Therefore, by allowing the electrode assembly to adsorb carbon dioxide molecules at low temperatures and then combining this with baking, the moisture within the micro-nano pores of the carbon layer can be effectively removed, reducing the water content of the positive electrode sheet, thereby further improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.

[0013] In some embodiments, the battery component is an electrode, which includes a positive electrode and / or a negative electrode; the method for preparing a battery cell includes the following steps: placing the electrode in a sealed device, injecting a gas including carbon dioxide into the sealed device at 0°C to 10°C, allowing it to stand for a period of time, and then baking it; assembling the positive electrode, separator, and negative electrode into an electrode assembly, placing the electrode assembly in a battery casing, and then drying, liquid injection, and formation to obtain a battery cell.

[0014] In the above technical solution, by subjecting the electrode to static carbon dioxide adsorption at low temperature and combining it with baking, the moisture in the micro-nano pores of the electrode can be effectively removed; and some of the moisture that may be adsorbed during subsequent assembly can be removed by further drying, thereby effectively reducing the water content of the electrode and improving the battery's first efficiency, cycle performance and high-temperature storage performance.

[0015] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer attached to at least one side surface of the negative current collector, the negative electrode film layer comprising a porous carbon material.

[0016] In the above technical solution, by first subjecting the negative electrode sheet to carbon dioxide adsorption at low temperature and then baking it, the moisture in the micro-nano pores of the porous carbon material can be effectively removed. Even if there is moisture during the subsequent assembly of the electrode assembly, it is not easy to enter these micro-nano pores again and can be effectively removed by further drying. This can effectively reduce the water content of the negative electrode sheet, thereby further improving the battery's initial efficiency, cycle performance and high-temperature storage performance.

[0017] In some embodiments, the positive electrode sheet includes a positive current collector and a positive electrode film layer attached to at least one side of the surface of the positive current collector, wherein the positive electrode film layer includes a positive electrode active material with a carbon layer coated on its surface.

[0018] In the above technical solution, by first subjecting the positive electrode sheet to carbon dioxide adsorption at low temperature and then baking it, the moisture in the micro-nano pores of the carbon layer can be effectively removed. Even if there is moisture during the subsequent assembly of the electrode components, it is not easy for it to enter these micro-nano pores again. It can be effectively removed by further drying, thereby effectively reducing the water content of the positive electrode sheet and improving the battery's first efficiency, cycle performance and high-temperature storage performance.

[0019] In some embodiments, in the porous carbon material, at least a portion of the pores have a diameter of less than 10 nm.

[0020] In the aforementioned technical solutions, compared to pore structures with larger pore sizes, porous carbon materials contain micro- and nano-pores with pore sizes less than 10 nm. This makes the intermolecular forces of water molecules within the pores more significant, and the interaction forces between water molecules and pores are also significantly enhanced. Water molecules are firmly adsorbed onto the pore walls, further increasing the difficulty of moisture removal. This makes conventional vacuum baking ineffective in removing moisture from these micro- and nano-pores. In this application, even though porous carbon contains pores with smaller pore sizes, carbon dioxide adsorption at low temperatures allows it to combine with water molecules to form easily removable carbonic acid. This enables subsequent baking to effectively remove moisture from the micro- and nano-pores, resulting in a better water removal effect.

[0021] In some embodiments, the volume percentage of pores with a pore size of less than 10 nm in the porous carbon material is 50% to 90%.

[0022] In the aforementioned technical solutions, porous carbon materials have a high volume ratio of pores with a diameter less than 10 nm. The smaller pores form more complex and tortuous diffusion paths, making water molecule diffusion more difficult and further increasing the difficulty of water removal. In this application, by injecting a gas including carbon dioxide and then allowing it to stand for adsorption, the carbon dioxide combines with the water in the micro- and nano-pores, enabling effective removal of moisture from the micro- and nano-pores during subsequent baking, resulting in a better water removal effect.

[0023] In some embodiments, the porous carbon material includes at least one of hard carbon or soft carbon.

[0024] In the aforementioned technical solutions, both hard carbon and soft carbon are commonly used battery anode materials. Both have complex micro- and nano-porous structures, making it difficult to effectively remove moisture using only conventional vacuum baking. In this application, a gas including carbon dioxide is injected, followed by static adsorption, allowing carbon dioxide molecules to combine with water molecules within the complex pores. This enables effective removal of moisture from the complex pores during subsequent baking, resulting in a better water removal effect.

[0025] In some embodiments, when a gas including carbon dioxide is injected into the sealed device, the pressure inside the sealed device is controlled to be between one atmosphere and five atmospheres.

[0026] In the above technical solution, by controlling the injection of gas including carbon dioxide, the sealed equipment has a high pressure. Under low temperature and high pressure, the battery components can adsorb more carbon dioxide, which is beneficial to further improve the dehydration effect.

[0027] In some embodiments, the settling time is 2h to 5h.

[0028] In the above technical solution, by allowing the battery components to stand for an appropriate time after injecting gas including carbon dioxide, it is beneficial to adsorb more carbon dioxide, which is beneficial to further improve the water removal effect.

[0029] In some embodiments, the step of injecting a gas including carbon dioxide into a sealed device and allowing it to stand for a period of time is repeated 6 to 12 times.

[0030] In the above technical solution, by repeatedly injecting gas including carbon dioxide into the sealed equipment and letting it stand, the battery components can adsorb more carbon dioxide, which is beneficial to further improve the water removal effect.

[0031] In some embodiments, the concentration of carbon dioxide in the gas injected into the sealed device is ≥80%.

[0032] In the above technical solution, by controlling the injected gas to have a high carbon dioxide concentration, it is beneficial for the battery components to adsorb more carbon dioxide, which is beneficial to further improve the water removal effect.

[0033] In some embodiments, baking is vacuum baking.

[0034] In the above technical solution, the air pressure is reduced in a vacuum environment, and the boiling point of water is also reduced, which is more conducive to removing moisture from battery components.

[0035] In some embodiments, the baking temperature is 100°C to 110°C and the baking time is 8 hours to 48 hours.

[0036] In the above technical solution, since the boiling point of water under standard atmospheric pressure is 100℃, controlling the baking temperature to be close to the boiling point range of water facilitates the rapid vaporization and removal of moisture and carbonic acid formed by moisture and carbon dioxide. Further controlling the baking time within a suitable range further improves the dehydration effect.

[0037] The second aspect of this application also provides a battery cell, which is prepared using the preparation method provided in the first aspect of this application.

[0038] A third aspect of this application also provides a secondary battery, which includes the battery cell provided in the second aspect of this application.

[0039] A fourth aspect of the present application also provides an electrical device, which includes the secondary battery provided in the third aspect of the present application. Attached Figure Description

[0040] Figure 1 This is a process flow diagram of the first method for preparing a battery cell provided in the embodiments of this application.

[0041] Figure 2 This is a process flow diagram of the second method for preparing a battery cell provided in the embodiments of this application.

[0042] Figure 3 This is a process flow diagram of the third method for preparing battery cells provided in the embodiments of this application.

[0043] Figure 4 This is a schematic diagram of a single battery cell provided in an embodiment of this application.

[0044] Figure 5 yes Figure 4 The diagram shown is an exploded view of a single battery cell.

[0045] Figure 6 This is a schematic diagram of a battery module provided in an embodiment of this application.

[0046] Figure 7 This is a schematic diagram of a secondary battery provided in an embodiment of this application.

[0047] Figure 8 yes Figure 7 The diagram shown is an exploded view of a secondary battery.

[0048] Figure 9 This is a schematic diagram of an electrical device provided in an embodiment of this application.

[0049] Explanation of reference numerals in the attached figures:

[0050] 1-Secondary battery; 2-Upper casing; 3-Lower casing; 4-Battery module; 5-Battery cell; 51-Body; 52-Electrode assembly; 53-Cover plate. Detailed Implementation

[0051] The following detailed description, with appropriate reference to the accompanying drawings, discloses the method for preparing the battery cell, the battery cell itself, the secondary battery, and embodiments of the power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0052] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0053] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0054] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0055] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0056] In existing technologies, after the electrode assembly is fabricated, it is placed in the battery casing and then baked to remove water, in order to reduce the generation of side reactions within the battery and improve the battery's electrical performance. However, this baking method is not very effective at removing water.

[0057] Currently, conventional solutions to improve water removal include: (1) increasing the temperature and time of vacuum baking. However, due to the heat resistance of the separator, it is not possible to significantly improve the water removal effect by increasing the temperature; and when the moisture content reaches the equilibrium point, long-term baking cannot further reduce the moisture content. (2) adding water removal additives (e.g., dicyclohexylcarbodiimide, hexamethyldisilazane, N,N'-diisopropylcarbodiimide, heptamethyldisilazane, etc.). However, water removal additives are difficult to produce water removal effect by adding them to the slurry, and it is difficult to ensure that the water removal additives can adsorb water better than porous carbon materials. Water removal additives are also difficult to effectively remove water from micro and nano pores, and may also reduce battery load and deteriorate battery performance.

[0058] Based on this, the first aspect of this application provides a method for preparing a battery cell, comprising the following steps: placing a battery component in a sealed device, injecting a gas including carbon dioxide into the sealed device at 0°C to 10°C, allowing it to stand for a period of time, and then baking it to obtain a battery cell.

[0059] By injecting a gas including carbon dioxide into a sealed device at a low temperature of 0℃ to 10℃ and allowing it to adsorb, followed by baking, the carbon dioxide gas can form strong bonds with water molecules on the surface of battery components and in the micro- and nano-pores, breaking the hydrogen bonds between water molecules and promoting the ionization of water molecules. This disrupts the tight adsorption of water molecules at the material interface, effectively removing moisture from the micro- and nano-pores of the battery components after baking. This preparation method is simple to operate and can effectively reduce the water content of battery components, thereby improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.

[0060] The present application is further illustrated below with reference to embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.

[0061] [The first method for preparing battery cells]

[0062] In some embodiments, the battery component is an electrode assembly, and the sealing device is a battery casing. Figure 1 This is a process flow diagram of the first method for preparing a battery cell provided in this application embodiment. Please refer to [link / reference]. Figure 1 The preparation method of a single battery cell includes the following steps:

[0063] S11: Place the electrode assembly inside the battery casing, inject gas including carbon dioxide into the battery casing at 0℃~10℃, let it stand for a period of time, and then bake it.

[0064] In this application, "electrode assembly" refers to an electrode assembly that has not yet been immersed in electrolyte (i.e., the structure before electrolyte is injected), which may include a negative electrode, a positive electrode, and a separator disposed between the negative electrode and the positive electrode. The negative electrode, the positive electrode, and the separator can be obtained by winding or alternatingly stacking the electrode assembly.

[0065] In some embodiments, the electrode assembly includes a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative electrode film layer attached to at least one side surface of the negative current collector, the negative electrode film layer including a porous carbon material.

[0066] In this application, "porous carbon material" refers to a carbon material with a three-dimensional interconnected nanopore structure and a high specific surface area. Porous carbon can be biomass porous carbon or resin porous carbon. The numerous pores can be categorized by diameter into micropores (less than 2 nm), mesopores (2 nm to 50 nm), and macropores (greater than 50 nm), providing attachment space for water and carbon dioxide molecules. Understandably, porous carbon can be used directly as a negative electrode active material, or as a matrix material, providing a substrate for the deposition and attachment of other negative electrode active materials. The porous carbon matrix and other negative electrode active materials together serve as the negative electrode material. In this case, the other negative electrode active materials can be one or more of silicon-based materials, aluminum-containing materials, tin-containing materials, and antimony-containing materials. Further, silicon-based materials may include nano-silicon particles.

[0067] When the negative electrode comprises porous carbon material, the porous carbon material contains a large number of micro- and nano-pores (e.g., pores with a diameter of 10 nm or less). These micro- and nano-pores contain numerous active sites (e.g., oxygen-containing functional groups), which undergo physical and chemical adsorption with water molecules. On one hand, oxygen-containing functional groups, such as hydroxyl, carboxyl, and carbonyl groups, can form stable hydrogen bonds with water molecules. Furthermore, due to the presence of numerous defects (e.g., N and S heteroatoms and dangling bonds) and oxygen-containing functional groups within the pores, strong physical and chemical adsorption of water molecules occurs, forming layered water structures. This increases the local water concentration and reduces the distance between water molecules, strengthening the hydrogen bonding and intermolecular forces between adsorbed water molecules. On the other hand, the numerous irregular pore structures form tortuous channels, lengthening the diffusion path of water and increasing collisions between water molecules, making it difficult for water molecules to escape from the pores. Moreover, water molecules tend to form oriented arrangements within the micro- and nano-pores, further enhancing intermolecular forces and making water molecules even more difficult to remove. Therefore, relying solely on vacuum baking is insufficient for effectively removing moisture.

[0068] In this application, by adsorbing carbon dioxide molecules onto the electrode assembly at low temperature and then baking, moisture in the micro- and nano-pores of porous carbon materials can be effectively removed, reducing the water content of the negative electrode. Firstly, due to the numerous defects (e.g., nitrogen heteroatoms) and oxygen-containing functional groups (e.g., hydroxyl groups) present in the pores of porous carbon materials, the electron-rich graphite structure and the high charge density of the nitrogen sites readily form local dipole-quadrupole interactions with polarizable acidic carbon dioxide molecules. The nitrogen atom of the pyridine group contributes its lone pair electrons to the carbon atom of the carbon dioxide, thus generating a Lewis acid-base interaction. The hydrogen atom in the hydroxyl group can form hydrogen bonds with the oxygen atom of the carbon dioxide molecule, and the oxygen in the hydroxyl group has a partial charge of -0.444e, thus possessing a high electrostatic potential, which can provide electrons to the carbon dioxide molecule, thereby forming an electrostatic interaction. In other words, the pores of the porous carbon material can generate strong intermolecular forces with carbon dioxide, disrupting the interface between water molecules and the carbon layer, resulting in competitive adsorption. Secondly, since the average radius of motion of water molecules (0.27 nm to 0.32 nm) is comparable to that of carbon dioxide molecules (0.33 nm), carbon dioxide molecules can enter the micro- and nano-pores where water molecules are adsorbed and come into contact with them. The oxygen in the water molecule forms σ bonds with two hydrogen atoms, leaving two unbonded electron pairs. Again, because oxygen is more electronegative, the oxygen in the water molecule exhibits a negative charge, while the hydrogen atoms exhibit a positive charge. The oxygen in the water molecule and the carbon in the carbon dioxide molecule are attracted to each other by their opposite charges, and the unbonded electron pairs of the oxygen in the water molecule invade the carbon atom's bond site, breaking one of the π bonds and pushing the lone electrons originally belonging to the carbon atom to the oxygen atom, making that oxygen atom negatively charged. This allows the oxygen in the carbon dioxide to gain two electrons, and the oxygen in the water and the carbon in the carbon dioxide share the electron pairs originally held by the oxygen in the water, forming σ bonds. The hydrogen atoms in the water undergo atomic rearrangement, moving to the negatively charged oxygen atom. In other words, water molecules within the micro- and nano-pores can combine with adsorbed carbon dioxide molecules at low temperatures to form carbonic acid, making the water molecules more likely to change from a liquid to a gaseous state and thus easier to remove during the subsequent baking process.

[0069] In some embodiments, in porous carbon materials, at least some pores have a pore size of less than 10 nm. Understandably, porous carbon materials can contain pore structures with pore sizes of 10 nm, 5 nm, 2 nm, 1 nm, or even less than 1 nm.

[0070] Furthermore, in porous carbon materials, the volume percentage of pores with a pore size of less than 10 nm is 50% to 90%. As examples, the volume percentage of pores with a pore size of less than 10 nm in porous carbon materials is 50%, 60%, 65%, 70%, 75%, 80%, 90%, etc.

[0071] The pore size distribution of porous carbon materials can be determined using any conventional testing method, such as nitrogen adsorption. By measuring the nitrogen adsorption-desorption isotherm of the porous carbon material, the specific surface area can be calculated using the BET model (Brunauer-Emmett-Teller theory). Combined with the BJH model (Barrett-Joyner-Halenda method), the pore size distribution can be obtained, thus revealing the presence of pores smaller than 10 nm. The volume percentage of pores smaller than 10 nm can also be calculated. In some embodiments, the porous carbon material includes at least one of hard carbon or soft carbon.

[0072] In some embodiments, the electrode assembly includes a positive electrode sheet, which includes a positive current collector and a positive electrode film layer attached to at least one side of the positive current collector. The positive electrode film layer includes a positive electrode active material with a carbon layer coated on its surface.

[0073] In this application, the material and preparation method of the carbon layer are not specifically limited. As an example, a method for coating a carbon layer on the surface of a positive electrode active material may include: mixing a precursor and a carbon source in a solvent and ball milling the mixture, wherein the precursor includes a precursor material for forming the positive electrode active material; and then sintering at high temperature to form a carbon layer on the surface of the positive electrode active material.

[0074] The ball milling process may include: ball milling at a speed of 100 r / min to 1500 r / min for 5 h to 20 h. The sintering process may include: sintering at a temperature of 300℃ to 800℃ in an inert gas atmosphere for 10 h to 24 h.

[0075] In some embodiments, the carbon source includes one or more of organic carbon sources, carbon black, carbon nanotubes, and graphene.

[0076] Furthermore, the organic carbon source includes one or more of sucrose, glucose, starch, citric acid, polyaniline, polyacrylic acid, and polyvinyl alcohol.

[0077] When a carbon layer is coated on the surface of the positive electrode active material, this carbon layer is typically an amorphous carbon material obtained by carbonizing carbon-containing precursors (such as sucrose and glucose). The material's surface and interior contain numerous defects and dangling bonds, resulting in strong hydrophilicity. Furthermore, amorphous carbon materials contain a large number of oxygen-containing groups (such as hydroxyl and carboxyl groups) and possess complex micro / nanopore structures. This leads to strong physical and chemical adsorption of water molecules, making water molecules difficult to remove. Additionally, positive electrode active materials (such as lithium iron phosphate) are typically micro / nanomaterials with a large specific surface area and high hydrophilicity, readily adsorbing water molecules.

[0078] In this application, the electrode assembly is first statically placed at a low temperature to adsorb carbon dioxide, and then baked. In addition to forming a strong bond with water molecules on the carbon layer surface, carbon dioxide molecules can also enter the micro-nano pores (pore size ≤10nm) where water molecules are adsorbed. The carbon layer pores can generate strong intermolecular forces with carbon dioxide molecules, which disrupts the interfacial interaction between water molecules and carbon materials, resulting in competitive adsorption. At low temperature, water molecules in the micro-nano pores can combine with adsorbed carbon dioxide molecules to form carbonic acid, making water molecules more likely to change from liquid to gaseous state. This makes them easier to remove during the subsequent baking process. Therefore, the water in the micro-nano pores of the carbon layer can be effectively removed, reducing the water content of the positive electrode sheet, thereby further improving the battery's initial efficiency, cycle performance, and high-temperature storage performance.

[0079] In this application, the "0℃~10℃ condition" refers to placing the battery casing containing the electrode assembly in a low-temperature chamber or refrigeration equipment, so that the temperature inside the battery casing reaches 0℃~10℃. Further, the temperature at which carbon dioxide gas is injected into the battery casing can be 0℃~5℃. As an example, the temperature at which carbon dioxide gas is injected into the battery casing can be 0℃, 2℃, 5℃, 6℃, 8℃, or 10℃.

[0080] In some embodiments, when a gas including carbon dioxide is injected into the battery casing, the pressure inside the battery casing is controlled to be between one atmosphere and five atmospheres. As an example, when a gas including carbon dioxide is injected into the battery casing, the pressure inside the battery casing is controlled to be one atmosphere, two atmospheres, three atmospheres, four atmospheres, or five atmospheres.

[0081] In practical applications, the battery casing containing the electrode assembly can be placed in a low-temperature chamber to control the temperature inside the battery casing from 0°C to 10°C. A pressure sensor is installed inside the battery casing, and then a gas injector is used to inject gas including carbon dioxide until the pressure inside the battery casing is between one atmosphere and five atmospheres.

[0082] In some embodiments, the settling time is 2 to 5 hours. As an example, after injecting a gas including carbon dioxide into the battery casing, the battery is left to stand for 2, 3, 4, or 5 hours.

[0083] In some embodiments, the step of injecting a gas including carbon dioxide into the battery casing and allowing it to stand for a period of time is repeated 6 to 12 times. As an example, the step of injecting a gas including carbon dioxide into the battery casing and allowing it to stand for a period of time is repeated 6, 8, 10, or 12 times.

[0084] In some embodiments, the concentration of carbon dioxide in the gas injected into the battery casing is ≥80%. As an example, the concentration of carbon dioxide in the gas injected into the battery casing can be 80%, 90%, or 100%. Understandably, when the gas including carbon dioxide is first injected, if air is present in the battery casing, the gas will replace the air, filling the battery casing with the gas including carbon dioxide, thereby ensuring that the concentration of carbon dioxide gas in the battery casing is ≥80%, or even reaches 100%.

[0085] In some embodiments, baking is vacuum baking.

[0086] Furthermore, the baking temperature is 100℃~110℃, and the baking time is 8h~48h. As an example, the baking temperature can be 100℃, 105℃ or 110℃, and the baking time can be 8h, 12h, 24h, 36h or 48h.

[0087] In some embodiments, the vacuum baking step may include: placing the part to be baked in a vacuum baking oven, evacuating it, heating it to 100°C to 110°C, and baking it for 8 to 48 hours.

[0088] In some embodiments, the vacuum degree during vacuum baking is 0.1 Pa to 100 Pa.

[0089] In other embodiments, vacuum baking may not be required.

[0090] S12: The baked parts are injected with liquid and formed to obtain battery cells.

[0091] In this application, "electrolyte injection" refers to injecting electrolyte into the battery casing, and "formation" refers to the first charging of the battery after electrolyte injection, which aims to form a passivation layer, i.e., an SEI film, on the surface of the electrode. In some embodiments, a settling step is also included between the electrolyte injection and formation steps, which is beneficial for the electrode to be fully wetted by the electrolyte.

[0092] [Second method for preparing battery cells]

[0093] In some embodiments, the battery component is an electrode, which may include a positive electrode and / or a negative electrode. Figure 2 This is a process flow diagram of the second preparation method of the battery cell provided in the embodiments of this application. Please refer to [link / reference]. Figure 2 The preparation method of a single battery cell includes the following steps:

[0094] S21: Place the electrode in a sealed device, inject gas including carbon dioxide into the sealed device at 0℃~10℃, let it stand for a period of time, and then bake it.

[0095] Understandably, the negative electrode can be processed in the manner described in step S21; the positive electrode can be processed in the manner described in step S21; or both the positive and negative electrodes can be processed in the manner described in step S21.

[0096] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer attached to at least one surface of the negative current collector, wherein the negative electrode film layer comprises a porous carbon material. For information on water removal using porous carbon materials, please refer to the foregoing description, which will not be repeated here.

[0097] In some embodiments, the positive electrode includes a positive current collector and a positive electrode film layer attached to at least one surface of the positive current collector, wherein the positive electrode film layer includes a positive electrode active material with a carbon layer coated on its surface. Regarding the carbon layer's water removal properties, please refer to the foregoing description, which will not be repeated here.

[0098] In some embodiments, the enclosed device may be a baking oven or the like.

[0099] In some embodiments, when a gas including carbon dioxide is injected into a sealed device, the pressure inside the sealed device can be controlled to be between one atmosphere and five atmospheres. As an example, when a gas including carbon dioxide is injected into a sealed device, the pressure inside the sealed device can be controlled to be one atmosphere, two atmospheres, three atmospheres, four atmospheres, or five atmospheres.

[0100] In some embodiments, the settling time can be 2 hours to 5 hours. As an example, after injecting a gas including carbon dioxide into a sealed device, it is left to stand for 2 hours, 3 hours, 4 hours, or 5 hours.

[0101] In some embodiments, the step of injecting a gas including carbon dioxide into a sealed device and allowing it to stand for a period of time is repeated 6 to 12 times. As an example, the step of injecting a gas including carbon dioxide into a sealed device and allowing it to stand for a period of time is repeated 6, 8, 10, or 12 times.

[0102] In some embodiments, the concentration of carbon dioxide in the gas injected into the sealed device is ≥80%. As an example, the concentration of carbon dioxide in the gas injected into the sealed device may be 80%, 90%, or 100%.

[0103] In some embodiments, the baking in step S21 is vacuum baking.

[0104] Further, in step S21, the baking temperature is 100℃~110℃, and the baking time is 24h~72h. As an example, the baking temperature can be 100℃, 105℃ or 110℃, and the baking time can be 24h, 36h, 48h or 72h.

[0105] S22: Assemble the negative electrode, separator and positive electrode into an electrode assembly, place the electrode assembly in the battery casing, and then perform drying, liquid injection and formation to obtain a battery cell.

[0106] Understandably, in step S22, only the negative electrode may undergo the water removal process in step S21, only the positive electrode may undergo the water removal process in step S21, or both the negative and positive electrode may undergo the water removal process in step S21.

[0107] In some embodiments, the drying in step S22 can be vacuum baking.

[0108] Further, in step S22, the vacuum baking temperature is 100℃~110℃, and the time is 24h~72h. As an example, the vacuum baking temperature can be 100℃, 105℃ or 110℃, and the baking time can be 24h, 36h, 48h or 72h.

[0109] [A third method for preparing battery cells]

[0110] In some embodiments, the battery component is an active material, which may be a positive electrode active material and / or a negative electrode active material. Figure 3 This is a process flow diagram of the third method for preparing battery cells provided in the embodiments of this application. Please refer to [link / reference]. Figure 3 The preparation method of a single battery cell includes the following steps:

[0111] S31: Place the active material in a sealed device, inject gas including carbon dioxide into the sealed device at 0℃~10℃, let it stand for a period of time, and then bake it.

[0112] Understandably, the negative electrode active material can be treated in the manner described in step S21; the positive electrode active material can also be treated in the manner described in step S21; or both the positive electrode active material and the negative electrode active material can be treated in the manner described in step S21.

[0113] In some embodiments, the negative electrode active material includes porous carbon material. For information on water removal using porous carbon materials, please refer to the foregoing description, which will not be repeated here.

[0114] In some embodiments, the surface of the positive electrode active material is coated with a carbon layer. For information on water removal using the carbon layer, please refer to the foregoing description, which will not be repeated here.

[0115] S32: The baked active material, conductive agent, and binder are mixed to obtain a mixed slurry. The mixed slurry is applied to the surface of the current collector to form an electrode film layer, thereby obtaining an electrode sheet.

[0116] Understandably, when the active material is a positive electrode active material, the corresponding current collector is a positive electrode current collector, and the corresponding electrode sheet is a positive electrode sheet; while when the active material is a negative electrode active material, the corresponding current collector is a negative electrode current collector, and the corresponding electrode sheet is a negative electrode sheet.

[0117] S33: Assemble the negative electrode, separator and positive electrode into an electrode assembly, place the electrode assembly in the battery casing, and then perform drying, liquid injection and formation to obtain a battery cell.

[0118] Understandably, in step S33, the negative electrode may include only the negative electrode active material after baking and dehydration, or the positive electrode may include only the positive electrode active material after baking and dehydration, or the negative electrode may include the negative electrode active material after baking and dehydration, while the positive electrode may include the positive electrode active material after baking and dehydration.

[0119] [Battery cell]

[0120] A second aspect of this application also provides a battery cell prepared using the method described in the first aspect of this application. The battery cell includes an electrode assembly, a battery casing, and an electrolyte, with the electrode assembly and electrolyte disposed within the battery casing. The electrode assembly includes a negative electrode, a positive electrode, and a separator disposed between the negative and positive electrode.

[0121] For more detailed technical features of the components in a single battery cell, please refer to the following:

[0122] [Negative electrode plate]

[0123] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0124] In other embodiments, the negative electrode current collector may also include a current collector body and a base coating. The base coating may be disposed on at least one side of the current collector body. The base coating does not contain negative electrode active material, but may contain a small amount of carbon material. However, the carbon material forms a thin coating and cannot function as a negative electrode active material.

[0125] In some embodiments, the negative electrode film layer may optionally include an adhesive. The adhesive may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0126] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0127] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0128] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as porous carbon materials, conductive agents, binders, and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry. The negative electrode slurry is then coated onto a negative electrode current collector, and after drying, cold pressing, and other processes, the negative electrode sheet is obtained.

[0129] [Positive electrode plate]

[0130] The positive electrode active material may be any positive electrode active material known in the art for use in battery cells.

[0131] In some embodiments, when the battery cell is a lithium-ion battery cell, the positive electrode active material may be a known positive electrode active material for lithium-ion batteries to prepare a lithium-ion secondary battery. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more.

[0132] Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, and lithium nickel manganese oxides. Examples of lithium phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4, also known as LFP), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.

[0133] In some embodiments, to further increase the energy density of the secondary battery, the positive electrode active material for lithium-ion batteries may include a general formula of Li a Ni b Co c M d O e A f one or more of lithium transition metal oxides and modified compounds thereof, wherein 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes at least one of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A is selected from at least one of N, F, S and Cl.

[0134] By way of example, the positive electrode active material for a lithium-ion battery cell may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), LiNi 0.85 Co 0.15 Al 0.05 O2, at least one of LiNi 0.8 Co 0.15 Al 0.05 O2.

[0135] In the present application, the modified compound of each of the above positive electrode active materials may be a doping modification and / or surface coating modification performed on the positive electrode active material.

[0136] As an optional technical solution of the present application, the polyanionic compound may be Li 1+x Mn 1-y A y P 1-z R zO4. Wherein, x is any value in the range of -0.100 to 0.100, y is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, A includes at least one element selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and R includes at least one element selected from B, S, Si and N.

[0137] As an optional technical approach in this application, the polyanionic compound can be Li a A e Mn 1-f B f P 1-g C g O 4-n D n Wherein, A includes at least one element selected from Zn, Al, Na, K, Mg, Nb, Mo, and W. B includes at least one element selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge. C includes at least one element selected from B, S, Si, and N. D includes at least one element selected from S, F, Cl, and Br. a is selected from the range of 0.9 to 1.1, e is selected from the range of 0.001 to 0.1, f is selected from the range of 0.001 to 0.5, g is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the second positive electrode active material is electrically neutral.

[0138] During the charging and discharging process of a battery, Li undergoes insertion / extraction and consumption, resulting in varying molar Li content at different discharge states. In the examples of cathode materials in this application, the molar Li content refers to the initial state of the material, i.e., the state before feeding. When the cathode material is applied to the battery system, the molar Li content changes after charge-discharge cycles.

[0139] In the examples of positive electrode active materials in this application, the molar content of O is only a theoretical value. Oxygen release from the crystal lattice will cause changes in the molar content of oxygen, and the actual molar content of O will fluctuate.

[0140] In some embodiments, when the battery cell is a sodium-ion battery cell, the positive electrode active material may be a known positive electrode active material for sodium-ion batteries to prepare a sodium-ion secondary battery. As an example, the positive electrode active material may include at least one of the following materials: polyanionic compounds, sodium transition metal oxides, Prussian blue compounds, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more.

[0141] In some embodiments, the positive electrode active material of the sodium-ion battery may be a sodium transition metal compound, and the general formula of the positive electrode active material is Na x XO2, X includes at least one of transition metals which may be Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, 0<x≤1. By way of example, the positive electrode active material of the sodium-ion battery includes Na x MnO2, Na x CoO2, Na x FeO2, NaNi 0.2 Fe 0.6 Mn 0.2 at least one of O2.

[0142] In some embodiments, the polyanionic compound may be Na a A e Mn 1-f B f P 1-g C g O 4-n D n , where A includes at least one element selected from Zn, Al, Na, K, Mg, Nb, Mo and W. B includes at least one element selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge. C includes at least one element selected from B, S, Si and N. D includes at least one element selected from S, F, Cl and Br. a is selected from the range of 0.9 to 1.1, e is selected from the range of 0.001 to 0.1, f is selected from the range of 0.001 to 0.5, g is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the second positive electrode active material is electrically neutral.

[0143] As an optional technical solution of the present application, the polyanionic compound may be Na 4+x R 3-y P 4-m O 15 / C. Wherein 0<x<0.5, 0<y≤0.5, 0<m≤0.2, R includes at least one of Mg, Al, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Cr, Nb, Mo, In, Ga, Sn, Hf, Ta, W and Pb.

[0144] As an optional technical solution of the present application, the polyanionic compound may be Na x-a A a V y-b M b (PO4) 2-2c (DO4)2c F z-d Q d Wherein, element A represents an alkali metal element that substitutes for element Na, element M represents a metal element that substitutes for element V, element D represents a dopant element that substitutes for element Phosphorus, and element Q represents a dopant element that substitutes for element F. Element D includes at least one of Si and S, and element Q includes at least one of Cl and O. 3.5≤x≤4.5, 0≤a≤0.15x, 0.8≤y≤1.1, 0≤b≤0.3y, 0≤c≤0.15, 0.8≤z≤1.1, 0≤d≤0.2z. Optionally, element A includes at least one of K and Li. Element M includes at least one of Fe, Cr, Al, Sc, Ga, In, Ti, Zr, Mn, Zn, Ni, Cu, and Co.

[0145] Prussian blue compounds can be compounds containing sodium ions, transition metal ions, and cyanide ions (CN). - A class of compounds. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Prussian blue compounds include, for example, Na. a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Mn, Fe, Ni, Co, Cu and Zn, 0 < a ≤ 2, 0 < b < 1, 0 < c < 1.

[0146] In some embodiments, the positive electrode may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0147] In some embodiments, the positive electrode may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0148] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0149] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as a positive active material with a carbon coating layer, a conductive agent, a binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto a positive current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.

[0150] Electrolyte

[0151] In some embodiments, the electrolyte includes an electrolyte salt and a solvent.

[0152] In some embodiments, when it is necessary to prepare a lithium-ion battery cell, the electrolyte salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0153] In some embodiments, when it is necessary to prepare sodium-ion battery cells, the electrolyte salt includes at least one of sodium hexafluorophosphate (NaPF6) and sodium perchlorate.

[0154] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0155] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0156] [Septum]

[0157] This application does not impose any particular restrictions on the type of diaphragm; any well-known porous diaphragm with good chemical and mechanical stability can be selected.

[0158] In some embodiments, the diaphragm material may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The diaphragm may be a single-layer film or a multi-layer composite film, without particular limitation. When the diaphragm is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0159] [Battery casing]

[0160] In some embodiments, the battery casing can be a hard casing, such as a hard plastic casing, an aluminum casing, a steel casing, etc. It can also be a soft-pack, such as a pouch-type soft-pack. The material of the soft-pack can be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0161] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 4 This is a schematic diagram of a single battery cell provided in an embodiment of this application.

[0162] In some implementations... Figure 5 yes Figure 4 The exploded view of the battery cell shown is for reference. Figure 5 The battery casing may include a body 51 and a cover plate 53. The body 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The body 51 has an opening communicating with the receiving cavity, and the body 51 can cover the opening to close the receiving cavity. Positive electrode sheets, negative electrode sheets, and a separator may be formed into electrode assemblies 52 through a winding process or a stacking process. The electrode assemblies 52 are encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assemblies 52. The number of electrode assemblies 52 contained in a single battery cell 5 may be one or more, which can be selected by those skilled in the art according to specific practical needs.

[0163] In some embodiments, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.

[0164] Figure 6 This is a schematic diagram of a battery module provided in an embodiment of this application. (Refer to...) Figure 6 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0165] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0166] In some embodiments, the battery modules described above can also be assembled into a secondary battery. The secondary battery may contain one or more battery modules, and the specific number can be selected by those skilled in the art based on the application and capacity of the secondary battery.

[0167] Figure 7 This is a schematic diagram of a secondary battery provided in an embodiment of this application. Figure 8 yes Figure 7 The diagram shown is an exploded view of a secondary battery. Please refer to it. Figure 7 and Figure 8 The secondary battery 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0168] In addition, this application also provides an electrical device, which includes at least one of the battery cell, battery module, or secondary battery provided in this application. The battery cell, battery module, or secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0169] As an electrical device, you can choose individual battery cells, battery modules, or secondary batteries according to your usage requirements.

[0170] Figure 9 This is a schematic diagram of an electrical device provided in an embodiment of this application. Please refer to it. Figure 9 The electrical device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this electrical device, secondary batteries or battery modules can be used.

[0171] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.

[0172] Example

[0173] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0174] Example 1

[0175] This embodiment provides a sodium-ion battery, the preparation method of which includes the following steps:

[0176] (1) Preparation of positive electrode sheet

[0177] Sodium iron pyrophosphate (Na4Fe3(PO4)2(P2O7), abbreviated as NFPP, with a carbon layer coated on the surface, the carbon layer accounting for 5% by mass) was mixed with conductive carbon black (Super P), PVDF, and positive electrode dispersant (BYK Chemicals, BYK-23676) in a mass ratio of 96:1:2.5:0.5. An appropriate amount of solvent N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated onto aluminum foil, and then dried to obtain a positive electrode sheet.

[0178] (2) Preparation of negative electrode sheet

[0179] Porous hard carbon (with 70% of its pores smaller than 10 nm in volume), conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly mixed in a deionized water solvent system at a mass ratio of 90:4:4:2 to obtain a negative electrode slurry. The negative electrode slurry is then coated onto a copper foil of the negative electrode current collector with a thickness equal to that of the negative electrode current collector, and the negative electrode sheet is obtained by cold pressing and slitting.

[0180] (3) Diaphragm

[0181] The diaphragm is a polyethylene film.

[0182] (4) Electrolyte

[0183] Ethylene carbonate, diethyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 1:1:1. NaPF6 was then dissolved in the mixed solvent to obtain the electrolyte. The concentration of NaPF6 in the electrolyte was 1 mol / L.

[0184] (5) Battery assembly

[0185] The positive electrode, separator, and negative electrode are alternately stacked to obtain the electrode assembly (i.e., battery component), and the electrode assembly is placed inside the battery casing (i.e., sealed device).

[0186] At 0°C, carbon dioxide gas (100% concentration) is injected into the battery casing, and the pressure inside the battery casing is controlled at 2 atmospheres. The casing is left to stand for 4 hours. The above operation is repeated 6 times to obtain the part to be baked.

[0187] Transfer the parts to be baked to a vacuum baking oven, vacuum process them, and bake them at 105°C for 24 hours.

[0188] Electrolyte is injected into the battery casing and formation is carried out to obtain a sodium-ion battery.

[0189] Example 2

[0190] Example 2 provides a sodium-ion battery, which differs from Example 1 in that:

[0191] In step (5), the temperature when injecting carbon dioxide gas into the battery casing is 5°C.

[0192] Example 3

[0193] Example 3 provides a sodium-ion battery, which differs from Example 1 in that:

[0194] In step (5), the temperature when injecting carbon dioxide gas into the battery casing is 10°C.

[0195] Example 4

[0196] Example 4 provides a sodium-ion battery, which differs from Example 1 in that:

[0197] In step (5), when injecting carbon dioxide gas into the battery casing, the pressure inside the battery casing is controlled to be 5 atmospheres.

[0198] Example 5

[0199] Example 5 provides a sodium-ion battery, which differs from Example 1 in that:

[0200] In step (2), the injected gas is a mixture of carbon dioxide and nitrogen, with a carbon dioxide volume concentration of 80%.

[0201] Example 6

[0202] Example 6 provides a sodium-ion battery, the preparation method of which includes the following steps:

[0203] (1) Preparation of positive electrode sheet

[0204] Sodium iron pyrophosphate (Na4Fe3(PO4)2(P2O7), abbreviated as NFPP, with a carbon layer coating on the surface, the carbon layer accounting for 5% by mass) was mixed with conductive carbon black (Super P), PVDF, and sodium carboxymethyl cellulose in a mass ratio of 96:1:2.5:0.5. An appropriate amount of solvent N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated onto aluminum foil, and after coating, it was dried to obtain a positive electrode sheet.

[0205] (2) Preparation of negative electrode sheet

[0206] Porous hard carbon (with 70% of its pores smaller than 10 nm in volume), conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly mixed in a deionized water solvent system at a mass ratio of 90:4:4:2 to obtain a negative electrode slurry. The negative electrode slurry is then coated onto a copper foil of the negative electrode current collector with a thickness equal to that of the negative electrode current collector, and the negative electrode sheet is obtained by cold pressing and slitting.

[0207] The negative electrode (i.e., battery component) is placed in a low-temperature chamber (i.e., a sealed device). Carbon dioxide gas (100% concentration) is injected into the low-temperature chamber at 0°C, and the pressure inside the chamber is controlled at 2 atmospheres. The chamber is left to stand for 4 hours. The above operation is repeated 6 times to obtain the part to be baked.

[0208] The parts to be baked are transferred to a vacuum baking oven, vacuumed, and then baked at 105°C for 24 hours.

[0209] (3) Diaphragm

[0210] The diaphragm is a polyethylene film.

[0211] (4) Electrolyte

[0212] Ethylene carbonate, diethyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 1:1:1. NaPF6 was then dissolved in the mixed solvent to obtain the electrolyte. The concentration of NaPF6 in the electrolyte was 1 mol / L.

[0213] (5) Battery assembly

[0214] The positive electrode, separator, and negative electrode are alternately stacked to obtain an electrode assembly. The electrode assembly is placed inside the battery casing and then placed in a vacuum baking oven. After vacuum treatment, it is baked at 105°C for 24 hours. Electrolyte is injected into the battery casing and formation is carried out to obtain a sodium-ion battery.

[0215] Example 7

[0216] Example 7 provides a sodium-ion battery, the preparation method of which includes the following steps:

[0217] (1) Preparation of positive electrode sheet

[0218] Sodium iron pyrophosphate (Na4Fe3(PO4)2(P2O7), abbreviated as NFPP, with a carbon layer coating on the surface, the carbon layer accounting for 5% by mass) was mixed with conductive carbon black (Super P), PVDF, and sodium carboxymethyl cellulose in a mass ratio of 96:1:2.5:0.5. An appropriate amount of solvent N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated onto aluminum foil, and after coating, it was dried to obtain a positive electrode sheet.

[0219] The positive electrode (i.e., battery component) is placed in a low-temperature chamber (i.e., a sealed device). Carbon dioxide gas (100% concentration) is injected into the low-temperature chamber at 0°C, and the pressure inside the chamber is controlled at 2 atmospheres. The chamber is left to stand for 4 hours. The above operation is repeated 6 times to obtain the part to be baked.

[0220] The parts to be baked are transferred to a vacuum baking oven, vacuumed, and then baked at 105°C for 24 hours.

[0221] (2) Preparation of negative electrode sheet

[0222] Porous hard carbon (with 70% of its pores smaller than 10 nm in volume), conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are thoroughly mixed in a deionized water solvent system at a mass ratio of 90:4:4:2 to obtain a negative electrode slurry. The negative electrode slurry is then coated onto a copper foil of the negative electrode current collector with a thickness equal to that of the negative electrode current collector, and the negative electrode sheet is obtained by cold pressing and slitting.

[0223] (3) Diaphragm

[0224] The diaphragm is a polyethylene film.

[0225] (4) Electrolyte

[0226] Ethylene carbonate, diethyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 1:1:1. NaPF6 was then dissolved in the mixed solvent to obtain the electrolyte. The concentration of NaPF6 in the electrolyte was 1 mol / L.

[0227] (5) Battery assembly

[0228] The positive electrode, separator, and negative electrode are alternately stacked to obtain an electrode assembly. The electrode assembly is placed inside the battery casing and then placed in a vacuum baking oven. After vacuum treatment, it is baked at 105°C for 24 hours. Electrolyte is injected into the battery casing and formation is carried out to obtain a sodium-ion battery.

[0229] Comparative Example 1

[0230] Comparative Example 1 provides a sodium-ion battery, which differs from Example 1 in that:

[0231] Step (5) includes: alternatingly stacking the positive electrode sheet, separator and negative electrode sheet to obtain the electrode assembly, placing the electrode assembly in the battery casing and transferring it to a vacuum baking oven, vacuuming it and baking it at 105°C for 24 hours;

[0232] Electrolyte is injected into the battery casing and formation is carried out to obtain a sodium-ion battery.

[0233] Comparative Example 2

[0234] Comparative Example 2 provides a sodium-ion battery, which differs from Example 1 in that:

[0235] Step (5) includes:

[0236] The positive electrode, separator, and negative electrode are alternately stacked to obtain the electrode assembly, which is then placed inside the battery casing.

[0237] At room temperature (25°C), carbon dioxide gas (100% concentration) is injected into the battery casing, and the pressure inside the battery casing is controlled at 2 atmospheres. After standing for 4 hours, the above operation is repeated 6 times to obtain the part to be baked.

[0238] Transfer the parts to be baked to a vacuum baking oven, vacuum process them, and bake them at 105°C for 24 hours.

[0239] Electrolyte is injected into the battery casing and formation is carried out to obtain a sodium-ion battery.

[0240] The process parameters for some of the batteries used in Examples 1 to 7, Comparative Examples 1 and 2 are shown in Table 1.

[0241] Table 1. Some process parameters for battery fabrication in the examples and comparative examples.

[0242]

[0243] Experimental Example

[0244] The water content of the electrodes obtained in Examples 1 to 7 and Comparative Examples 1 and 2, as well as the initial efficiency, cycle life, and high-temperature storage performance of the batteries, were tested. The test methods and results are analyzed below:

[0245] 1. Electrode

[0246] (1) Porous hard carbon pores: Using the nitrogen adsorption method, porous hard carbon powder was placed in a sample tube, and nitrogen gas was introduced into the sample tube. The nitrogen adsorption-desorption isotherm of the carbon dioxide material was measured. The pore size distribution of hard carbon can be obtained by analyzing the BET model (Brunauer-Emmett-Teller theory) combined with the BJH model (Barrett-Joyner-Halenda method). The volume percentage of pores with a pore size of less than 10 nm can be calculated.

[0247] (2) Electrode moisture content: The sodium-ion batteries baked in Examples 1 to 7 and Comparative Examples 1 and 2 were disassembled in a glove box, and the negative electrode and positive electrode were taken. 0.1g-0.2g of powder was scraped off the electrode and tested in a Karl Fischer moisture analyzer. At least three parallel samples were tested each time, and the average value was taken as the final moisture content.

[0248] 2. Sodium-ion battery

[0249] (1) First effect

[0250] At 25°C, the sodium-ion batteries prepared in Examples 1 to 7 and Comparative Examples 1 and 2 were charged at a constant current rate of 0.2C for 1 hour, denoted as IGC0; then discharged at a rate of 0.1C to 2.0V, denoted as AGD0, and left to stand for 5 minutes; then the batteries were charged at a rate of 0.5C to 3.65V, denoted as AGC0, and left to stand for 5 minutes; then discharged at a rate of 0.1C to 2.5V, denoted as AGD1; where C0 is IGC0-AGD0+AGC0; D0 is AGD1, and the first-efficiency calculation method is D0 / C0.

[0251] (2) Cyclic performance (cycle life)

[0252] At 25°C, the sodium-ion batteries prepared in Examples 1 to 7, Comparative Examples 1 and 2 were charged at a rate of 0.5C to 3.65V, then charged at a constant voltage until the current was below 0.05C, and then discharged at a rate of 1C to 2.5V. The discharge capacity was recorded. Cyclic tests were performed in this full charge-discharge manner until the discharge capacity of the sodium-ion battery decayed to 80% of the initial discharge capacity, and the number of cycles at this point was recorded.

[0253] (3) High-temperature storage performance

[0254] In a 60°C oven, the sodium-ion batteries prepared in Examples 1-7 and Comparative Examples 1 and 2 were stored for t (days), and the battery discharge capacity (Ct) was tested. The ratio of Ct to the initial discharge capacity (C0), Ct / C0, is the capacity retention rate after high-temperature storage. The battery capacity testing method includes: at 25°C, the sodium-ion batteries prepared in Examples 1-7 and Comparative Examples 1 and 2 were charged at a rate of 0.5C to 3.65V, then charged at a constant voltage until the current is below 0.05C, and then discharged at a rate of 1C to 2.5V. The discharge capacity was recorded, and the number of days when the capacity retention rate decreased to 80% was also recorded.

[0255] The performance test results are shown in Table 2.

[0256] Table 2 shows the performance test results of the electrode and battery in the examples and comparative examples.

[0257]

[0258] As can be seen from Tables 1 and 2, compared with Comparative Examples 1 and 2, the sodium-ion batteries provided in Examples 1 to 7 of this application have lower water content in the negative electrode and positive electrode, and the batteries have higher initial efficiency and cycle life, as well as better high-temperature storage performance.

[0259] Compared to Example 1, in Comparative Example 1, the direct baking without carbon dioxide adsorption resulted in a significant increase in the water content of both the negative and positive electrode sheets, leading to a significant decrease in the battery's initial efficiency, cycle life, and high-temperature storage performance. In Comparative Example 2, the injection of carbon dioxide at room temperature prevented the porous carbon material and the micro-nano pores in the carbon layer from effectively adsorbing carbon dioxide gas. Consequently, the moisture in both the negative and positive electrode sheets could not be effectively removed after baking, resulting in a significant increase in water content and a corresponding significant decrease in the battery's initial efficiency, cycle life, and high-temperature storage performance.

[0260] The above indicates that when the negative electrode contains porous carbon material, or when the surface of the positive electrode active material in the positive electrode is coated with a carbon layer, this application can effectively remove moisture from the micro-nano pores of the porous carbon material by adsorbing carbon dioxide into the electrode assembly or negative electrode at low temperature and then baking it. This reduces the water content of the negative electrode, thereby improving the battery's initial efficiency, cycle life, and high-temperature storage performance. This application can also effectively remove moisture from the micro-nano pores of the carbon layer coating the surface of the positive electrode active material by adsorbing carbon dioxide into the electrode assembly or positive electrode at low temperature and then baking it. This reduces the water content of the positive electrode, thereby improving the battery's initial efficiency, cycle life, and high-temperature storage performance.

[0261] The following describes a method for removing water from pores of 10 nm and below in porous carbon materials, as described in this application:

[0262] (1) Take two portions of porous carbon material and bake them under vacuum. Then place one portion of porous carbon material in a sealed container, introduce carbon dioxide gas (100% concentration), and control the pressure inside the sealed container to 2 atmospheres. Let it stand for 4 hours. Repeat the above operation 6 times as the experimental group. The other portion does not adsorb carbon dioxide as the control group.

[0263] (2) The mercury intrusion porosimetry method is used, and the test pressure is adjusted (less than 80 MPa) to test only pores with a pore size of 10 nm or larger. Mercury is then filled into the pores of the porous carbon material. At this time, in the pores with a pore size of 10 nm or larger, the mercury will completely replace the water and carbon dioxide gas adsorbed in the pores. Only in the pores with a pore size of less than 10 nm, there is still carbon dioxide gas and water that has not been removed by vacuum baking.

[0264] (3) The obtained porous carbon material samples were sealed and tested using gas chromatography-mass spectrometry (GC-MS). A heating chamber could be installed during the test to measure the water content in the gas phase at 105℃. Comparing the test results of the two groups of porous carbon material samples, it was found that the water content of the control group was 150 ppm, while the water content of the experimental group was 320 ppm. This indicates that adsorbing carbon dioxide is beneficial for removing water from pores below 10 nm.

[0265] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for producing a battery cell, characterized by, Includes the following steps: The battery components are placed in a sealed device, and gas including carbon dioxide is injected into the sealed device at 0℃~10℃. After standing for a period of time, the device is baked to obtain a single battery cell.

2. The production method according to claim 1, characterized by, The battery component is an electrode assembly, the sealed device is a battery casing, and the preparation method includes the following steps: The electrode assembly is placed inside the battery casing. Under conditions of 0℃ to 10℃, a gas including carbon dioxide is injected into the battery casing. After standing for a period of time, it is baked. The baked electrode assembly is then injected with liquid and formed to obtain a battery cell.

3. The production method according to claim 2, characterized by, The electrode assembly includes a negative electrode sheet, the negative electrode sheet includes a negative current collector and a negative electrode film layer attached to at least one side surface of the negative current collector, the negative electrode film layer includes a porous carbon material; And / or, the electrode assembly includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive electrode film layer attached to at least one side surface of the positive current collector, the positive electrode film layer including a positive electrode active material with a carbon layer coated on its surface.

4. The method of claim 1, wherein, The battery component is an electrode, which includes a positive electrode and / or a negative electrode, and the preparation method includes: The electrode is placed in a sealed device, and gas including carbon dioxide is injected into the sealed device at 0℃~10℃. After standing for a period of time, it is baked. The positive electrode, separator, and negative electrode are assembled into an electrode assembly, which is then placed inside the battery casing. The assembly is then dried, injected with electrolyte, and formed to obtain a single battery cell.

5. The production method according to claim 4, characterized by, The negative electrode sheet includes a negative current collector and a negative electrode film layer attached to at least one side surface of the negative current collector, wherein the negative electrode film layer includes a porous carbon material. And / or, the positive electrode includes a positive current collector and a positive electrode film layer attached to at least one side of the positive current collector, the positive electrode film layer including a positive electrode active material with a carbon layer coated on its surface.

6. The production method according to claim 3 or 5, characterized by, In the porous carbon material, at least some of the pores have a diameter of less than 10 nm; And / or, in the porous carbon material, the volume percentage of pores with a pore size of less than 10 nm is 50% to 90%; And / or, the porous carbon material includes at least one of hard carbon or soft carbon.

7. The preparation method according to any one of claims 1 to 6, characterized in that, When a gas including carbon dioxide is injected into the sealed device, the pressure inside the sealed device is controlled to be between one atmosphere and five atmospheres. And / or, the settling time is 2h to 5h; And / or, repeat the step of injecting gas including carbon dioxide into the sealed device and letting it stand for a period of time, repeating 6 to 12 times. And / or, the concentration of carbon dioxide in the gas injected into the sealed device is ≥80%.

8. The preparation method according to any one of claims 1 to 7, characterized in that, The baking is vacuum baking; And / or, the baking temperature is 100℃~110℃, and the time is 8h~48h.

9. A single battery cell, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 8.

10. A secondary battery, characterized in that, Includes the battery cell as described in claim 9.

11. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 10.