Secondary batteries and electronic devices
By adjusting the electrode coating capacity ratio and compaction density, and optimizing the electrode design, the problems of lithium plating and purple spots in stacked lithium-ion batteries were solved, improving the battery's safety and energy density, and enhancing its structural stability and versatility.
Patent Information
- Application Number
- CN202510637101.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
The outermost negative electrode of a stacked lithium-ion battery is prone to lithium plating and purple spots during charging and discharging, leading to safety hazards and energy density loss.
By adjusting the capacity ratio and compaction density of the electrode coating, the outermost negative electrode can fully receive lithium ions, reducing relative slippage. A single-sided positive electrode design is adopted to save space. The capacity ratio of the inner electrode is optimized to adapt to volume changes, increasing the embedding sites of the negative electrode active material and improving the stability between the electrodes.
It effectively reduces the occurrence of lithium plating and purple spots, improves the safety and energy density of secondary batteries, reduces costs and the risk of high-temperature cycling degradation, and enhances the stability and versatility of battery structure.
Smart Images

Figure CN123120827A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a secondary battery and electronic device. Background Technology
[0002] With the rapid development of modern technology, the demand for high-performance energy storage devices is increasing in fields such as portable electronic devices and electric vehicles. Lithium-ion rechargeable batteries, as a highly efficient and environmentally friendly energy storage device, have been widely used in many fields.
[0003] Lithium-ion batteries are generally classified into stacked and wound types. Stacked batteries have better application prospects due to their high energy density and high charge / discharge rate performance. However, for stacked lithium-ion batteries, the outermost negative electrode has a higher risk of lithium plating. Summary of the Invention
[0004] This application aims to provide a secondary battery and electronic device that reduces the technical problems of purple spots or lithium plating in secondary batteries.
[0005] In a first aspect, this application proposes a secondary battery, including an electrode assembly. The electrode assembly includes a first single-sided positive electrode, a first negative electrode, a first inner positive electrode, and a first inner negative electrode, which are sequentially stacked along a first direction. The first single-sided positive electrode is the outermost electrode of the electrode assembly. The first single-sided positive electrode includes a first positive electrode coating facing the first negative electrode, and the capacity of the first positive electrode coating is C. 11 The first negative electrode includes a first negative electrode coating facing the first positive electrode coating, and the capacity of the first negative electrode coating is C. 21 The first inner positive electrode includes a first inner positive electrode coating facing the first inner negative electrode, and the capacity of the first inner positive electrode coating is C. 31 The first inner negative electrode includes a first inner negative electrode coating facing the first inner positive electrode coating, and the capacity of the first inner negative electrode coating is C. 41 Satisfies: 1 < (C 21 / C 11 ) / (C 41 / C 31 )≤1.12.
[0006] In the above technical solution, 1 < (C) 21 / C 11 ) / (C 41 / C 31 A value ≤ 1.12 means that the capacity ratio of the outermost (outermost layer in the opposite direction of the first direction Z) positive and negative electrode plates is increased relative to the capacity ratio of the inner positive and negative electrode plates. This can compensate for the relative slippage between the first negative electrode plate and the first single-sided positive electrode plate caused by the larger expansion rate of the first negative electrode plate during charging and discharging. This can be achieved by increasing C...21 With C 11 Even when the first negative electrode experiences relative slippage, it still allows for better reception of lithium ions extracted from the first single-sided positive electrode, effectively reducing purple spots and lithium plating, thus improving the safety of the secondary battery. Simultaneously, it effectively reduces energy density loss, increased cost, and high-temperature cycling degradation caused by excessive coating on the first negative electrode.
[0007] In some embodiments, 1.05 ≤ (C 21 / C 11 ) / (C 41 / C 31 The ratio ≤1.11 allows the first negative electrode to more fully receive lithium ions extracted from the first single-sided positive electrode, reducing the risk of lithium ion deposition on the surface of the first negative electrode. Simultaneously, it reduces the negative impacts of an excessively high capacity ratio, such as further reducing costs and energy density loss.
[0008] In some embodiments, 1.03 ≤ (C 21 / C 11 A value ≤ 1.2 allows the first negative electrode to better fit with the first single-sided positive electrode during expansion, providing sufficient space and capacity for the first negative electrode to accommodate the volume changes caused by expansion. This reduces the risk of excessive expansion between electrodes damaging the overall electrode assembly structure, thus improving the stability of the secondary battery's internal structure. Furthermore, it enables the secondary battery to store and release more energy per unit volume, increasing its energy density.
[0009] In some embodiments, 1.02 ≤ (C 41 / C 31 The ratio ≤1.18 allows the first inner positive electrode and the first inner negative electrode to better adapt to each other when the volume changes, reducing structural damage caused by mismatch between the electrodes and helping to improve the integrity of the internal structure of the secondary battery.
[0010] In some embodiments, 75mAh≤C 11 ≤500mAh; 78mAh≤C 21 ≤520mAh; 75mAh≤C 31 ≤500mAh; 77mAh≤C 41 ≤510mAh. This helps reduce purple spots and lithium plating, and the capacity of each electrode coating can be adjusted within a range, improving the versatility of secondary batteries.
[0011] In some embodiments, the compaction density of the first negative electrode coating is less than that of the first inner negative electrode coating, which helps to improve the stability of lithium ion transport between the positive and negative electrodes, making the lithium ion distribution on the surface of the first negative electrode more uniform and reducing lithium ion aggregation and lithium plating.
[0012] In some embodiments, the first negative electrode sheet further includes a third negative electrode coating facing the first inner positive electrode sheet, wherein the compaction density of the first negative electrode coating is lower than that of the third negative electrode coating. The first negative electrode coating, being closer to the outer layer, has a lower compaction density, which facilitates the full absorption of lithium ions, thereby reducing purple spots and lithium plating. The third negative electrode coating, with its higher compaction density, is more conducive to a fuller reaction with the first inner positive electrode sheet, thus improving the energy density of the secondary battery.
[0013] In some embodiments, the coating quality of the first negative electrode coating is greater than that of the first inner negative electrode coating. The first negative electrode coating with a larger coating quality has more negative electrode active material. More negative electrode active material can provide more lithium ion insertion sites, allowing lithium ions to be inserted into the negative electrode material more uniformly, thereby reducing lithium plating caused by excessively high local lithium ion concentration and improving the safety of the secondary battery.
[0014] In some embodiments, the first negative electrode coating includes a negative electrode active material, which includes silicon, wherein the mass percentage of silicon in the negative electrode active material is G. 21 2.5% ≤ G 21 ≤50%. The secondary battery in this application can effectively reduce purple spots and lithium plating, therefore, it can be adapted to silicon-based negative electrode sheets with large expansion rates and high capacities, which is beneficial to improving the energy density of the secondary battery. Furthermore, 10% ≤G 21 With a purity of ≤30%, purple spots and lithium plating can be further reduced, and the energy density of secondary batteries can be improved.
[0015] In some embodiments, the secondary battery further includes a casing, with a first single-sided positive electrode plate fixed to the inner wall of the casing. This improves the stability of the internal structure of the secondary battery, making the internal structure more compact and contributing to increased energy density. Furthermore, it facilitates direct heat transfer from the electrode plate to the outer surface of the casing, improving the heat dissipation performance of the secondary battery.
[0016] In some embodiments, the electrode assembly further includes a second inner negative electrode, a second inner positive electrode, a second negative electrode, and a second single-sided positive electrode, which are sequentially stacked along a first direction. Along the first direction, the outermost electrode layers on both sides of the electrode assembly are a first single-sided positive electrode and a second single-sided positive electrode, respectively. The second single-sided positive electrode includes a second positive electrode coating facing the second negative electrode, and the capacity of the second positive electrode coating is C. 12The second negative electrode includes a second negative electrode coating facing the second positive electrode coating, and the capacity of the second negative electrode coating is C. 22 The second inner positive electrode includes a second inner positive electrode coating facing the second inner negative electrode, and the capacity of the second inner positive electrode coating is C. 32 The second inner negative electrode includes a second inner negative electrode coating facing the second inner positive electrode coating, and the capacity of the second inner negative electrode coating is C. 42 Satisfies: 1 < (C 22 / C 12 ) / (C 42 / C 32 )≤1.12.
[0017] In some embodiments, 1.02 ≤ (C 22 / C 12 A value ≤ 1.2 allows the second negative electrode to better fit with the second single-sided positive electrode during expansion, providing sufficient space and capacity for the second negative electrode to accommodate volume changes. This reduces the risk of compression damage to the overall electrode assembly structure caused by excessive expansion between electrodes, thus improving the stability of the internal structure of the secondary battery. Furthermore, it enables the secondary battery to store and release more electrical energy per unit volume, increasing its energy density.
[0018] In some embodiments, one or more third negative electrode sheets are stacked between the first inner negative electrode sheet and the second inner negative electrode sheet along the first direction. When multiple third negative electrode sheets are stacked between the first inner negative electrode sheet and the second inner negative electrode sheet, a third positive electrode sheet is stacked between adjacent third negative electrode sheets along the first direction. The stacking of multiple third negative electrode sheets and multiple third positive electrode sheets increases the total amount of active material, enabling the storage of more electrical energy, thereby improving the energy density of the secondary battery and meeting the demand of electronic devices for high-energy-density power supplies. Furthermore, the multilayer structure allows for more active material to come into contact with the electrolyte, which is beneficial for the rapid insertion and extraction of lithium ions during charging and discharging, thus improving the charge and discharge rate of the secondary battery.
[0019] Secondly, this application also proposes an electronic device including a secondary battery as described in any of the embodiments of the first aspect above.
[0020] Additional aspects and advantages of the embodiments of this application will be described, shown, or illustrated in part by way of implementation of the embodiments of this application in the following description. Attached Figure Description
[0021] One or more embodiments are illustrated by way of example with reference to the accompanying drawings, which are not intended to limit the embodiments, and elements having the same reference numerals in the drawings are designated as similar elements.
[0022] Figure 1 This is a schematic diagram of the structure of a secondary battery according to some embodiments of this application;
[0023] Figure 2 This is a schematic diagram of the stacked structure of the positive electrode, separator, and negative electrode in some embodiments of this application;
[0024] Figure 3 This is a schematic diagram of the stacked structure of electrode assemblies in some embodiments of this application;
[0025] Figure 4 This is a schematic diagram of the stacked structure of electrode assemblies in some embodiments of this application.
[0026] Explanation of reference numerals in the attached figures:
[0027] 1000, secondary battery;
[0028] 100. Electrode assembly;
[0029] 200. Shell;
[0030] 10. Positive electrode sheet; 11. Positive current collector; 111. First surface; 112. Second surface; 12. Positive electrode coating; 10a. First single-sided positive electrode sheet; 1011. First positive electrode coating; 10b. Second single-sided positive electrode sheet; 1012. Second positive electrode coating; 10c. First inner layer positive electrode sheet; 1031. First inner layer positive electrode coating; 10d. Second inner layer positive electrode sheet; 1032. Second inner layer positive electrode coating; 10e. Third positive electrode sheet;
[0031] 20. Negative electrode sheet; 21. Negative current collector; 211. Third surface; 212. Fourth surface; 22. Negative electrode coating; 20a. First negative electrode sheet; 2021. First negative electrode coating; 2023. Third negative electrode coating; 20b. Second negative electrode sheet; 2022. Second negative electrode coating; 20c. First inner layer negative electrode sheet; 2041. First inner layer negative electrode coating; 20d. Second inner layer negative electrode sheet; 2042. Second inner layer negative electrode sheet; 20e. Third negative electrode sheet;
[0032] 30. Separating membrane;
[0033] Z, first direction; X, second direction; Y, third direction. Detailed Implementation
[0034] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are some embodiments of this application, but not all embodiments.
[0035] In this application, the reference to "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment that is mutually exclusive with other embodiments.
[0036] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.
[0037] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0038] The technical features involved in the different embodiments of this application described below can be combined with each other as long as they do not conflict with each other.
[0039] Firstly, this application proposes a secondary battery 1000, please refer to... Figure 1 The secondary battery 1000 includes an electrode assembly 100, a housing 200, and an electrolyte (not shown in the figure). The housing 200 can accommodate the electrode assembly 100 and the electrolyte. The electrolyte wets the electrode assembly 100 inside the housing 200, thereby causing an electrochemical reaction.
[0040] For the electrode assembly 100 mentioned above, please refer to... Figure 1 and Figure 2 The electrode assembly 100 includes a positive electrode 10, a negative electrode 20, and a separator 30. Among them, Figure 2 The diagram shows a stacked structure of a positive electrode 10, a separator 30, and a negative electrode 20. For example, along the thickness direction (first direction Z) of the positive electrode 10 and / or the negative electrode 20, a plurality of positive electrode 10 and a plurality of negative electrode 20 are stacked alternately. A separator 30 is stacked between adjacent positive electrode 10 and negative electrode 20. The separator 30 is used to insulate and separate the positive electrode 10 and the negative electrode 20.
[0041] Please refer to Figure 2The positive electrode 10 includes a positive current collector 11 and a positive electrode coating 12. The positive current collector 11 can be made of a flat aluminum foil, titanium foil, nickel foil, or stainless steel foil. The positive electrode coating 12 can be disposed on at least one surface of the positive current collector 11 in the thickness direction, for example, along the first direction Z. The positive current collector 11 includes a first surface 111 and a second surface 112 disposed opposite to each other. The positive electrode coating 12 can be disposed on the first surface 111 and / or the second surface 112. The positive electrode coating 12 includes a positive electrode active material, a conductive agent, and a binder. The above material components are mixed, stirred evenly, and coated on the first surface 111 and / or the second surface 112 to obtain the positive electrode coating 12. The positive electrode active material includes one or more of lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium manganese oxide, or lithium manganese iron phosphate.
[0042] Please refer to Figure 2 The negative electrode sheet 20 includes a negative electrode current collector 21 and a negative electrode coating 22. The negative electrode current collector 21 can be made of a flat copper foil, titanium foil, nickel foil, stainless steel foil, or silver foil. The negative electrode coating 22 can be disposed on at least one surface of the negative electrode current collector 21 in the thickness direction, for example, along the first direction Z. The negative electrode current collector 21 includes a third surface 211 and a fourth surface 212 disposed opposite to each other, and the negative electrode coating 22 can be disposed on the third surface 211 and / or the fourth surface 212. The negative electrode coating 22 includes a negative electrode active material, a conductive agent, and a binder, etc. These materials are mixed, stirred evenly, and coated on the third surface 211 and / or the fourth surface 212 to obtain the negative electrode coating 22. The negative electrode active material includes one or more of elemental silicon, silicon carbide, silicon oxide, silicon alloy, etc.
[0043] In the embodiments of this application, please further refer to Figure 3 ,in Figure 3 The “…” indicates that parts of the positive electrode 10, separator 30, and negative electrode 20 are omitted. The positive electrode 10 can be divided into a first single-sided positive electrode 10a and a first inner positive electrode 10c, and the negative electrode 20 can be divided into a first negative electrode 20a and a first inner negative electrode 20c. Along the first direction Z, the first single-sided positive electrode 10a, the first negative electrode 20a, the first inner positive electrode 10c, and the first inner negative electrode 20c are stacked sequentially. The first single-sided positive electrode 10a is the outermost electrode of the electrode assembly 100. For example, in the opposite direction of the first direction Z, the outermost electrode of the electrode assembly 100 is the first single-sided positive electrode 10a, the electrode adjacent to the first single-sided positive electrode 10a is the first negative electrode 20a, and the first inner positive electrode 10c is disposed between the first negative electrode 20a and the first inner negative electrode 20c.
[0044] In one example, a three-dimensional coordinate system is defined using three perpendicular directions: Z, X, and Y. Z represents the thickness of the positive electrode 10 and / or the negative electrode 20; X represents the length of the positive electrode 10 and / or the negative electrode 20; and Y represents the width of the positive electrode 10 and / or the negative electrode 20. In other embodiments, X may also be the width of the positive electrode 10 and / or the negative electrode 20, in which case Y may be the length of the positive electrode 10 and / or the negative electrode 20.
[0045] It should be noted that in the embodiments of this application, the first single-sided positive electrode 10a is provided with the positive electrode coating 12 on only one side. For example, the first single-sided positive electrode 10a is provided with the first positive electrode coating 1011 only on the surface facing the first negative electrode 20a. The side of the first single-sided positive electrode 10a facing away from the first negative electrode 20a does not have a corresponding negative electrode coating 22. Therefore, there is no need to provide the positive electrode coating 12. Compared to double-sided coating, the outermost first single-sided positive electrode 10a having the first positive electrode coating 1011 on only one side is advantageous for saving space and can improve the energy density of the secondary battery 1000.
[0046] For the first negative electrode 20a, a negative electrode coating 22 can be provided on both sides. For example, the first negative electrode 20a includes a first negative electrode coating 2021 and a third negative electrode coating 2023. The first negative electrode coating 2021 is disposed facing the first single-sided positive electrode 10a and can undergo a lithium-ion intercalation / deintercalation reaction with the first single-sided positive electrode 10a to provide capacity for the secondary battery 1000. The third negative electrode coating 2023 is disposed facing the first inner layer positive electrode 10c and can undergo a lithium-ion intercalation / deintercalation reaction with the first inner layer positive electrode 10c, which can also provide capacity for the secondary battery 1000. Corresponding positive electrode 10s are provided on both sides of the first negative electrode 20a in the thickness direction. The first negative electrode 20a can have a negative electrode coating 22 on both sides, which is beneficial to make full use of the internal space of the secondary battery 1000 and improve the energy density of the secondary battery 1000.
[0047] However, the inventors of this application have discovered that during the charging and discharging process of the secondary battery 1000, lithium-ion insertion and extraction reactions occur between the positive electrode coating 12 and the negative electrode coating 22. For the negative electrode coating 22, lithium-ion insertion easily causes a large volume change. Taking silicon-containing negative electrode active materials as an example, when lithium-ion insertion occurs, expansion occurs between the silicon-containing negative electrode active materials, resulting in a large extension of the negative electrode sheet 20 in the second direction X and the third direction Y. Especially for the negative electrode sheet 20 near the outer layer, the outer negative electrode sheet 20 is less restricted than the inner negative electrode sheet 20, which further increases the expansion rate of the outer negative electrode sheet 20. On the other hand, the volume change of the positive electrode coating 12 during the charging and discharging process is relatively small, especially for the outermost first single-sided positive electrode sheet 10a, which only has the positive electrode coating 12 on one side, further reducing the expansion rate of the first single-sided positive electrode sheet 10a and thus making its extension smaller.
[0048] In this application, the first single-sided positive electrode 10a serves as the outermost electrode. During the charge-discharge cycle of the secondary battery 1000, the expansion rate of the first negative electrode 20a is greater than that of the first single-sided positive electrode 10a. This difference in expansion rate leads to different elongations between the two. The first negative electrode 20a elongates significantly in the second direction X and the third direction Y, while the first single-sided positive electrode 10a elongates less in these directions. This makes it easier for the first negative electrode 20a to slip relative to the first single-sided positive electrode 10a. Especially when the first single-sided positive electrode 10a is fixed to the casing 100, its expansion-induced elongation is limited by the casing 100, which may further increase the slippage between it and the first negative electrode 20a.
[0049] During the assembly of the secondary battery 1000, the separator 30 separates the first single-sided positive electrode 10a from the first negative electrode 20a and can be fixed between them by means of adhesive bonding. However, due to the relative slippage between the first negative electrode 20a and the first single-sided positive electrode 10a, the four corners of the first negative electrode 20a experience significant tensile stress. Over time, this tensile stress gradually breaks the bond between the separator 30 and the four corners of the first negative electrode 20a, causing the corners to lose adhesion to the separator 30 first. Once the corners of the first negative electrode 20a lose adhesion to the separator 30, they are directly exposed to the electrolyte, creating a large gap between the corners and the first single-sided positive electrode 10a. This results in a reduction in the corresponding portion of the first negative electrode 20a and the first single-sided positive electrode 10a, leading to insufficient capacity of the first negative electrode 20a. During the charging process of the secondary battery 1000, purple spots may appear at the interface of the first negative electrode 20a, and lithium plating may further occur, which may cause the secondary battery 1000 to short circuit or thermal runaway, posing a safety hazard.
[0050] To reduce the above-mentioned problems, please refer to the embodiments of this application. Figure 3 The capacity of the first positive electrode coating 1011 is C. 11 The capacity of the first negative electrode coating 2021 is C. 21 The first inner positive electrode 10c includes a first inner positive electrode coating 1031 facing the first inner negative electrode 20c, and the capacity of the first inner positive electrode coating 1031 is C. 31 The first inner negative electrode 20c includes a first inner negative electrode coating 2041 facing the first inner positive electrode coating 1031, and the capacity of the first inner negative electrode coating 2041 is C. 41 Satisfies: 1 < (C 21 / C 11 ) / (C 41 / C 31 If 1.01 ≤ 1.12, you can choose any value from 1 (excluding 1) to 1.12, such as 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11 or 1.12, etc.
[0051] In the above technical solution, for adjacent first single-sided positive electrode 10a and first negative electrode 20a, the capacity ratio C between them is... 21 / C 11 This reflects the relative amounts of positive and negative electrode active materials. When the capacity C of the first negative electrode coating 2021... 21 The capacity C relative to the first positive electrode coating 1011 11When the size is large, during the charging and discharging process, the first negative electrode 20a can accommodate more lithium ions that have been extracted from the first single-sided positive electrode 10a, thereby reducing the deposition of lithium ions on the surface of the first negative electrode 20a and the occurrence of lithium plating.
[0052] For adjacent first inner layer positive electrode 10c and first inner layer negative electrode 20c, the expansion difference between them is small, the risk of relative slippage is small, and that is, the risk of lithium plating in the inner layer is small. In the embodiments of this application, 1 < (C 21 / C 11 ) / (C 41 / C 31 A value ≤ 1.12 means that the capacity ratio of the outermost (outermost layer in the opposite direction of the first direction Z) positive and negative electrode plates is increased relative to the capacity ratio of the inner positive and negative electrode plates. This can compensate for the relative slippage between the first negative electrode plate 20a and the first single-sided positive electrode plate 10a caused by the large expansion rate of the first negative electrode plate 20a during charging and discharging. By increasing C... 21 With C 11 Even when the first negative electrode 20a experiences relative slippage, it can still effectively receive lithium ions extracted from the first single-sided positive electrode 10a, reducing lithium ion aggregation, effectively reducing purple spots and lithium plating, and improving the safety of the secondary battery 1000.
[0053] Meanwhile, in the embodiments of this application, it is limited to (C) 21 / C 11 ) / (C 41 / C 31 )≤1.12, which can also effectively reduce excessive capacity ratio. For example, a large capacity ratio may make it difficult for some negative electrode active materials to participate in the electrochemical reaction. Excessive negative electrode active material not only leads to increased costs, but also causes the first negative electrode coating 2021 to occupy a large space inside the secondary battery 1000, which will directly cause the energy density loss of the secondary battery 1000. At the same time, excessive capacity ratio also poses risks such as high-temperature cycling deterioration. Limit (C 21 / C 11 ) / (C 41 / C 31 With a value of ≤1.12, it can effectively reduce problems such as energy density loss, cost increase and high-temperature cycle deterioration caused by excessive first negative electrode coating 2021.
[0054] Furthermore, 1.05 ≤ (C 21 / C 11 ) / (C 41 / C 31The ratio ≤ 1.11 allows for a better difference between the capacity ratios of the outermost and innermost positive and negative electrodes. For example, when the ratio is above 1.05, the first negative electrode 20a has sufficient capacity relative to the first single-sided positive electrode 10a. During the charge and discharge process of the secondary battery 1000, even considering changes in the lithium-ion migration path and reaction caused by factors such as relative slippage of the first negative electrode 20a, the first negative electrode 20a can still more fully receive lithium ions extracted from the first single-sided positive electrode 10a, reducing the risk of lithium ions accumulating on the surface of the first negative electrode 20a and causing purple spots or lithium plating. At the same time, limiting the upper limit of the ratio to 1.1 reduces the negative impacts caused by an excessively large capacity ratio, such as further reducing costs, energy density loss, and high-temperature cycling degradation.
[0055] Regarding the capacity ratio of the first inner negative electrode coating 2041 to the first inner positive electrode coating 1031, in the embodiments of this application, it is limited to 1.02 ≤ (C 41 / C 31 The value ≤ 1.18 can be selected from any value between 1.02 and 1.18, such as 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, or 1.18. It should be noted that, generally, the capacity of the negative electrode coating is greater than that of the positive electrode coating. This is beneficial for the negative electrode coating to fully embed the lithium ions extracted from the positive electrode coating, i.e., C. 41 / C 31 >1.
[0056] In the embodiments of this application, 1.02 ≤ (C 41 / C 31 The value ≤ 1.18, within this range, is beneficial for matching the capacity of the first inner negative electrode coating 2041 with that of the first inner positive electrode coating 1031. During charging, lithium ions extracted from the first inner positive electrode coating 1031 can be fully embedded in the first inner negative electrode coating 2041, reducing lithium ion deposition due to insufficient inner negative electrode capacity and lowering the risk of purple spots and lithium plating. During discharging, lithium ions can also smoothly extract from the first inner negative electrode coating 2041 and return to the first inner positive electrode coating 1031, which is beneficial for the efficient and reversible electrochemical reaction inside the secondary battery 1000, improving the overall performance of the secondary battery 1000.
[0057] Furthermore, considering the relatively stable environment of the inner electrode, the limit is 1.02 ≤ (C 41 / C 31The ratio ≤1.18 allows the first inner positive electrode 10c and the first inner negative electrode 20c to better adapt to each other during volume changes, reducing structural damage caused by mismatch between the electrodes. For example, it reduces structural damage caused by compression due to excessive expansion, thus helping to improve the integrity of the internal structure of the secondary battery 1000. At the same time, it can reduce energy density loss caused by excessive coating 2041 on the first inner negative electrode.
[0058] Regarding the capacity ratio of the first negative electrode coating 2021 to the first positive electrode coating 1011, based on the capacity ratio of the first inner negative electrode coating 2041 to the first inner positive electrode coating 1031, the capacity ratio of the first negative electrode coating 2021 to the first positive electrode coating 1011 can be appropriately increased. In the embodiments of this application, 1.03 ≤ (C 21 / C 11 The value ≤ 1.2 can be any value from 1.03 to 1.2, such as 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, or 1.12. Within this range, it means that the capacity C of the first negative electrode coating 2021 is... 21 The capacity C relative to the first positive electrode coating 1011 11 It has a better ratio. However, due to the large expansion rate of the first negative electrode 20a during charging and discharging, there is a risk of relative slippage between it and the first single-sided positive electrode 10a. The limit is 1.03 ≤ (C). 21 / C 11 The value of ≤1.2 allows the first negative electrode 20a to better adapt to the first single-sided positive electrode 10a during the expansion process, giving the first negative electrode 20a sufficient space and capacity to adapt to its volume change, reducing the squeezing damage to the overall structure of the electrode assembly 100 caused by excessive expansion between the electrodes, and helping to improve the stability of the internal structure of the secondary battery 1000.
[0059] Furthermore, the constraint is 1.03 ≤ (C 21 / C 11 A value ≤ 1.2 allows for more efficient use of the internal space of the secondary battery 1000. The first negative electrode 20a will not occupy excessive space due to its large capacity, and it also reduces the difficulty in fully accepting lithium ions due to its smaller capacity. By limiting the value to 1.03 ≤ (C 21 / C 11 The value ≤1.2 allows the secondary battery 1000 to store and release more electrical energy per unit volume, thus increasing the energy density of the secondary battery 1000.
[0060] Among them, the capacity C of the first positive electrode coating 1011 11 75mAh≤C 11The capacity is ≤500mAh, and any value from 75mAh to 500mAh can be selected, such as 75mAh, 80mAh, 90mAh, 100mAh, 120mAh, 140mAh, 160mAh, 180mAh, 200mAh, 220mAh, 240mAh, 260mAh, 280mAh, 300mAh, 320mAh, 340mAh, 360mAh, 380mAh, 400mAh, 420mAh, 440mAh, 460mAh, 480mAh, or 500mAh. The lower limit of 75mAh provides a basic capacity for the 1000 rechargeable battery, sufficient to power small, low-power devices such as smartwatches and Bluetooth headsets, meeting their basic operating needs. The upper limit of 500mAh can meet the requirements of devices with higher power demands, such as wireless mice and portable massagers. By adjusting the capacity of each electrode coating within the range of 75mAh to 500mAh, the versatility of the 1000 rechargeable battery is improved. If the capacity is too small, such as less than 75mAh, it may result in insufficient battery life for the 1000 rechargeable battery. On the other hand, if the capacity is too large, such as greater than 500mAh, the active materials may not be able to react fully, resulting in a loss of energy density in the 1000 rechargeable battery.
[0061] The capacity of the first negative electrode coating 2021 is C. 21 The negative electrode coating can be set to be slightly larger than the positive electrode coating; for example, a coating size of 78mAh≤C can be selected. 21 ≤520mAh. Similarly, the capacity C of the first inner positive electrode coating. 31 Selectable 75mAh≤C 31 ≤500mAh, the capacity C of the first inner negative electrode coating 41 Selectable 77mAh≤C 41 ≤510mAh. This helps reduce purple spots and lithium plating, and the capacity of each electrode coating can be adjusted within a range, improving the versatility of the 1000 secondary battery.
[0062] In some embodiments, please refer to Figure 3 The compaction density of the first negative electrode coating 2021 is less than the compaction density of the first inner negative electrode coating 2041. For example, the compaction density of the first negative electrode coating 2021 is F. 21 The compaction density of the first inner negative electrode coating 2041 is F. 41 F 21 <F 41This means that the gaps between the active materials in the first negative electrode coating 2021 are larger, providing more space for the expansion of the active materials. During the charging and discharging process of the secondary battery 1000, the negative electrode active material will undergo volume changes due to the insertion and extraction of lithium ions. The larger expansion space can reduce the expansion rate of the first negative electrode 20a and reduce the extension of the first negative electrode 20a in the second direction X and the third direction Y.
[0063] Because the expansion and extension of the first negative electrode 20a are relatively small, the relative slippage between it and the adjacent first single-sided positive electrode 10a is reduced. Relative slippage between electrodes leads to structural changes at the electrode interface, affecting lithium-ion transport and reaction. Reducing slippage helps maintain interface stability, improves the stability of lithium-ion transport between the positive and negative electrodes, and promotes a more uniform distribution of lithium-ions on the surface of the first negative electrode 20a, reducing purple spots or lithium plating caused by lithium-ion aggregation.
[0064] The capacity of each coating can be adjusted by changing the compaction density and the coating quality. Appropriately reducing the compaction density helps to fully insert lithium ions, reducing the relative slippage between the first negative electrode 20a and the first single-sided positive electrode 10a caused by expansion. Increasing the coating quality directly increases the loading of active material in the coating, thereby improving the coating capacity and reducing purple spots or lithium plating caused by the relative slippage between the first negative electrode 20a and the first single-sided positive electrode 10a.
[0065] Please refer to Figure 3 The first negative electrode 20a also includes a third negative electrode coating 2023 facing the first inner positive electrode 10c. The compaction density of the first negative electrode coating 2021 is less than the compaction density of the third negative electrode coating 2023. For example, the compaction density of the third negative electrode coating 2023 is F. 23 The compaction density of the first negative electrode coating 2021 is F. 21 F 21 <F 23 The first negative electrode coating 2021 is closer to the outermost layer of the electrode assembly 100 (the outermost layer in the opposite direction of the first direction Z), and its compaction density F 21 The smaller spacing means that the active materials in the first negative electrode coating 2021 have a larger spacing, which provides a larger buffer space, which is conducive to the full reception of lithium ions and thus reduces purple spots and lithium plating. The third negative electrode coating 2023 has a larger compaction density, which is conducive to the full reaction with the first inner positive electrode 10c and improves the energy density of the secondary battery 1000.
[0066] Wherein, provided that the above-mentioned relationships between the compaction densities of each coating are satisfied, in the embodiments of this application, 0.8 g / cm³ can be selected. 3 ≤F21 ≤2g / cm 3 0.8g / cm 3 ≤F 23 ≤2g / cm 3 and 0.8g / cm 3 ≤F 41 ≤2g / cm 3 Both can be selected at 0.8g / cm³. 3 Up to 2g / cm 3 Any value in the range, for example, choosing 0.8 g / cm. 3 0.9g / cm 3 1g / cm 3 1.1g / cm 3 1.2g / cm 3 1.3g / cm 3 1.4g / cm 3 1.5g / cm 3 1.6g / cm 3 1.7g / cm 3 1.8g / cm 3 1.9g / cm 3 or 2g / cm 3 Within this range, each electrode can maintain good structural stability, allowing suitable porous structures to form between the active material particles, which is conducive to the full absorption of lithium ions and reduces purple spots and lithium plating.
[0067] If the compaction density is low, for example less than 0.8 g / cm³ 3 If the pores are too large, it can lead to wasted space and a loss of energy density in the secondary battery. If the compaction density is too high, for example, greater than 2 g / cm³, it will also cause problems. 3 During charging and discharging, the expansion rate may be relatively large, which can easily cause severe relative slippage between the first single-sided positive electrode 10a and the first negative electrode 20a, leading to an increased risk of purple spots and lithium plating. Furthermore, if the compaction density is too high, the electrolyte may not be able to fully wet the coating, resulting in some active materials not being able to fully undergo electrochemical reactions, which may deteriorate the cycle performance of the secondary battery.
[0068] In some embodiments, please refer to Figure 3 The coating quality of the first negative electrode coating 2021 is greater than that of the first inner negative electrode coating 2041. For example, the coating quality of the first negative electrode coating 2021 is Y. 21 The coating quality of the first inner negative electrode coating 2041 is Y. 41 Y 21 >Y 41The first negative electrode coating 2021 is closer to the outer layer. The first negative electrode coating 2021 with a larger coating quality has more negative electrode active material. More negative electrode active material can provide more lithium ion insertion sites, so that lithium ions can be inserted into the negative electrode material more uniformly. This reduces purple spots and lithium plating caused by excessive local lithium ion concentration, and improves the safety of the secondary battery 1000.
[0069] In some embodiments, please refer to Figure 3 The coating quality of the first negative electrode coating 2021 is Y. 21 This application specifies 0.03g / 1540.25mm. 2 ≤Y 21 ≤0.2g / 1540.25mm 2 Available in 0.03g / 1540.25mm. 2 Up to 0.2g / 1540.25mm 2 Any value in the range, for example, choosing 0.03g / 1540.25mm. 2 0.04g / 1540.25mm 2 0.05g / 1540.25mm 2 0.06g / 1540.25mm 2 0.07g / 1540.25mm 2 0.08g / 1540.25mm 2 0.09g / 1540.25mm 2 0.1g / 1540.25mm 2 0.11g / 1540.25mm 2 0.12g / 1540.25mm 2 0.13g / 1540.25mm 2 0.14g / 1540.25mm 2 0.15g / 1540.25mm 2 0.16g / 1540.25mm 2 0.17g / 1540.25mm 2 0.18g / 1540.25mm 2 0.19g / 1540.25mm 2 Or 0.2g / 1540.25mm 2 wait.
[0070] On the one hand, it provides sufficient lithium-ion insertion and extraction sites, enabling the secondary battery 1000 to undergo sufficient electrochemical reactions during charging and discharging, thereby giving the secondary battery 1000 high capacity and energy density. On the other hand, it can reduce the energy density loss caused by some active materials failing to effectively contact the electrolyte due to excess electrolyte.
[0071] Furthermore, this coating quality range helps to form a coating structure with stable structure and suitable porosity. If the coating quality is low, for example less than 0.03 g / 1540.25 mm... 2 If the first negative electrode coating 2021 is too porous, it may be prone to damage during charging and discharging due to structural instability. If the coating quality is high, for example greater than 0.2g / 1540.25mm... 2 If the first negative electrode coating 2021 is too dense, the electrolyte will not be able to fully wet it, and lithium ions will not be able to diffuse in the first negative electrode coating 2021, which may affect the cycle performance of the secondary battery 1000. Furthermore, due to the slowed diffusion rate of lithium ions, lithium ions are prone to accumulation, which leads to purple spots and lithium plating.
[0072] The second inner negative electrode coating 2041 can also be configured similarly to the first negative electrode coating 2021. For example, the coating quality of the second inner negative electrode coating 2041 is Y. 41 0.03g / 1540.25mm 2 ≤Y 41 ≤0.2g / 1540.25mm 2 .
[0073] In some other embodiments, the coating quality of the first positive electrode coating 1011 is Y. 11 This application specifies 0.2g / 1540.25mm. 2 ≤Y 11 ≤0.6g / 1540.25mm 2 The coating quality of the first inner positive electrode coating 1031 is Y. 31 0.2g / 1540.25mm 2 ≤Y 31 ≤0.6g / 1540.25mm 2 This ensures that sufficient lithium ions participate in the reaction during the charging and discharging process of the secondary battery 1000, thereby increasing its capacity and meeting the power requirements of the equipment. If the coating quality is too low, for example, less than 0.2g / 1540.25mm... 2 Insufficient active material will lead to a decrease in battery capacity, making it difficult to provide enough power to the device. Conversely, excessively high coating quality, such as greater than 0.6g / 1540.25mm, will also negatively impact battery capacity. 2If this is not done properly, the electrode may become too thick, making it more difficult for the electrolyte to wet the material and hindering the full reaction of the active material.
[0074] In some embodiments, the first negative electrode coating 2021 includes silicon, for example, the negative electrode active material includes one or more of elemental silicon, silicon carbide, silicon oxide, silicon alloy, etc. Silicon has a theoretical specific capacity of up to 4200 mAh / g, while graphite has a theoretical specific capacity of only 372 mAh / g. When the first negative electrode coating 2021 includes silicon, it is beneficial to increase the capacity of the first negative electrode 20a, increase the energy density of the secondary battery 1000, and facilitate meeting the requirements for long-lasting battery life.
[0075] Among them, the mass percentage of silicon in the negative electrode active material is G 21 2.5% ≤ G 21 ≤50%, any value from 2.5% to 50% can be selected, such as 2.5%, 3%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50%, etc. In the embodiments of this application, 1<(C) is defined as ≤50%. 21 / C 11 ) / (C 41 / C 31 With a value ≤1.12, the purple spots and lithium plating caused by relative slippage between the first single-sided positive electrode 10a and the first negative electrode 20a can be effectively reduced. Therefore, it can be adapted to silicon-based negative electrode 20 with a large expansion rate and high capacity. Furthermore, in this application, 2.5% ≤ G is specified. 21 ≤50% is beneficial to improving the energy density of the secondary battery 1000.
[0076] If G 21 If the expansion is too large, for example, greater than 50%, the volume expansion effect may be too severe, which will cause large stress inside the negative electrode coating 22, which may damage the structure of the negative electrode coating 22 and cause large slippage between the first single-sided positive electrode 10a and the first negative electrode 20a, resulting in a higher risk of purple spots and lithium plating.
[0077] If G 21 If the content is relatively small, for example, less than 2.5%, the effect on improving the overall capacity of the negative electrode 20 will be limited. Compared with using pure graphite negative electrodes or negative electrodes with high silicon content, the energy density improvement of the secondary battery 1000 is not significant, and it is difficult to meet the demand for high energy density of the secondary battery 1000.
[0078] Furthermore, 10% ≤ G 21 With a capacity of ≤30%, the internal chemical reactions of the secondary battery 1000 are more mild and controllable, which can further reduce purple spots and lithium plating, and improve the energy density of the secondary battery 1000.
[0079] It should be noted that in the embodiments of this application, other negative electrode coatings may also include silicon elements, such as one or more of elemental silicon, silicon carbide, silicon oxide, silicon alloy, etc., which can further improve the capacity of each negative electrode coating, thereby increasing the energy density of the secondary battery 1000.
[0080] In some embodiments, the first single-sided positive electrode 10a is fixed to the inner wall of the housing 200, for example, by bonding or other means. Fixing the outermost first single-sided positive electrode 10a improves the stability of the internal structure of the secondary battery 1000. Furthermore, the housing 200 of the secondary battery 1000 typically has good heat dissipation performance; for example, the housing 200 can be made of aluminum-plastic film or copper-plastic film, giving it a certain degree of thermal conductivity. The fixing of the first single-sided positive electrode 10a to the housing 200 facilitates direct heat conduction from the first single-sided positive electrode 10a to the outer surface of the housing 200, thus improving the heat dissipation performance of the secondary battery 1000. Furthermore, it is evident that the electrode assembly 100 moves within the housing 200, which reduces the movement of the electrode assembly 100 within the housing 200 caused by collisions with the secondary battery 1000. This helps to improve the bonding strength of the electrode assembly 100 within the housing 200, making the internal layout of the secondary battery 1000 more compact, effectively utilizing the space within the housing 200, and thereby increasing the energy density of the battery.
[0081] In the embodiments of this application, 1 < (C) 21 / C 11 ) / (C 41 / C 31 With a value of ≤1.12, the slippage between the first single-sided positive electrode 10a and the first negative electrode 20a can be effectively reduced, thereby reducing purple spots and lithium plating. Therefore, it is particularly suitable for secondary batteries 1000 in which the first single-sided positive electrode 10a is fixed to the casing 200.
[0082] In some embodiments, please refer to Figure 4 The positive electrode 10 is further divided into a second inner positive electrode 10d and a second single-sided positive electrode 10b, and the negative electrode 20 is further divided into a second inner negative electrode 20d and a second negative electrode 20b. Along the first direction Z, the second inner negative electrode 20d, the second inner positive electrode 10d, the second negative electrode 20b, and the second single-sided positive electrode 10b are sequentially stacked. For example, along the first direction Z, the outermost electrodes on both sides of the electrode assembly 100 are the second single-sided positive electrode 10b and the first single-sided positive electrode 10a, respectively. The electrode adjacent to the second single-sided positive electrode 10b is the second negative electrode 20b, and the second inner positive electrode 10d is disposed between the second negative electrode 20b and the second inner negative electrode 20d.
[0083] The second single-sided positive electrode 10b has a positive electrode coating 12 on only one side. For example, the first single-sided positive electrode 10a has a second positive electrode coating 1012 on only the surface facing the second negative electrode 20b. The side of the second single-sided positive electrode 10b facing away from the second negative electrode 20b has no corresponding negative electrode 20, therefore, there is no need to provide a positive electrode coating 12, which helps save space and improves the energy density of the secondary battery 1000. For the second negative electrode 20b, a negative electrode coating 22 can be provided on both sides, which helps to fully utilize the internal space of the secondary battery 1000 and improve the energy density of the secondary battery 1000.
[0084] In the embodiments of this application, the second single-sided positive electrode 10b includes a second positive electrode coating 1012 facing the second negative electrode 20b, and the capacity of the second positive electrode coating 1012 is C. 12 The second negative electrode 20b includes a second negative electrode coating 2022 facing the second positive electrode coating 1012, and the capacity of the second negative electrode coating 2022 is C. 22 The second inner positive electrode 10d includes a second inner positive electrode coating 1032 facing the second inner negative electrode 20d, and the capacity of the second inner positive electrode coating 1032 is C. 32 The second inner negative electrode 20d includes a second inner negative electrode coating 2042 facing the second inner positive electrode coating 1032, and the capacity of the second inner negative electrode coating 2042 is C. 42 Satisfies: 1 < (C 22 / C 12 ) / (C 42 / C 32 If 1.01 ≤ 1.12, you can choose any value from 1 (excluding 1) to 1.12, such as 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11 or 1.12, etc.
[0085] Limited 1 < (C 22 / C 12 ) / (C 42 / C 32 A value ≤ 1.12 means that the capacity ratio of the outermost (outermost layer along the first direction Z) positive and negative electrode plates is increased relative to the capacity ratio of the inner positive and negative electrode plates. This can compensate for the relative slippage between the second negative electrode plate 20b and the second single-sided positive electrode plate 10b caused by the large expansion rate and elongation of the second negative electrode plate 20b during charging and discharging. By increasing (C... 22 / C 12Even if the second negative electrode 20b experiences relative slippage, it can still better receive lithium ions extracted from the second single-sided positive electrode 10b, which can effectively reduce the appearance of purple spots, reduce lithium ion deposition on the surface of the second negative electrode 20b caused by slippage, and improve the safety of the secondary battery 1000.
[0086] At the same time, limit (C) 22 / C 12 ) / (C 42 / C 32 A capacity ratio ≤ 1.12 can effectively reduce excessive capacity ratio. For example, a large capacity ratio may prevent some negative electrode active materials from participating in the electrochemical reaction, leading not only to increased costs but also occupying a large amount of internal space in the secondary battery 1000, resulting in energy density loss. It also poses risks such as high-temperature cycling degradation. (C) 22 / C 12 ) / (C 42 / C 32 With a value of ≤1.12, it can effectively reduce problems such as energy density loss, cost increase and high-temperature cycle deterioration caused by excessive second negative electrode coating 2022.
[0087] In some embodiments, 1.02 ≤ (C 22 / C 12 The value can be ≤1.2, and any value from 1.01 to 1.2 can be selected, such as 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, or 1.12. This allows the second negative electrode 20b to better fit with the second single-sided positive electrode 10b during expansion, giving the second negative electrode 20b sufficient space and capacity to accommodate its volume changes. This reduces the squeezing damage to the overall structure of the electrode assembly 100 caused by excessive expansion between the electrodes, which is beneficial to improving the stability of the internal structure of the secondary battery 1000. Furthermore, it allows the secondary battery 1000 to store and release more electrical energy per unit volume, increasing the energy density of the secondary battery 1000.
[0088] The structures of the second single-sided positive electrode 10b and the second negative electrode 20b can be similar to those of the first single-sided positive electrode 10a and the first negative electrode 20a, and will not be described in detail in this application.
[0089] In some embodiments, please refer to Figure 4Along the first direction Z, one or more third negative electrode sheets 20e are stacked between the first inner negative electrode sheet 20c and the second inner negative electrode sheet 20d. When multiple third negative electrode sheets 20e are stacked between the first inner negative electrode sheet 20c and the second inner negative electrode sheet 20d, a third positive electrode sheet 10e is stacked between adjacent third negative electrode sheets 20e along the first direction Z. The stacking of multiple third negative electrode sheets 20e and multiple third positive electrode sheets 10e increases the total amount of active material, enabling the storage of more electrical energy, thereby improving the energy density of the secondary battery 1000 and meeting the demand of electronic devices for high-energy-density power supplies. Furthermore, the multilayer structure allows more active material to come into contact with the electrolyte, which is beneficial for the rapid insertion and extraction of lithium ions during charging and discharging, thus improving the charge and discharge rate of the secondary battery 1000.
[0090] Secondly, this application also proposes an electronic device, including a secondary battery 1000 as described in any embodiment of the first aspect above. The electronic device in this application is not particularly limited and can be any electronic device known in the prior art. For example, electronic devices include, but are not limited to, Bluetooth headsets, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc., while spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.
[0091] Test methods
[0092] Obtaining the film:
[0093] The lithium-ion secondary battery was discharged at a constant current of 0.5C to the discharge cutoff voltage at 25°C. The secondary battery was then disassembled under an argon atmosphere, and the negative electrode was soaked in dimethyl carbonate solvent for 2 hours and dried at 60°C for 1 hour to obtain the desired positive and negative electrode sheets. The discharge cutoff voltage of the secondary battery in the embodiments and comparative examples of this application is 3.0V. It is understood that when the voltage range marked on the battery packaging is 3.0V to 4.5V, the charging cutoff voltage is 4.5V and the discharging cutoff voltage is 3.0V. Unless otherwise specified, the charging cutoff voltage of the example secondary battery is 4.5V and the discharging cutoff voltage is 3.0V.
[0094] Unless otherwise specified, the following test methods shall be performed using the electrode sheets obtained in the above manner.
[0095] Coating capacity testing:
[0096] Remove the corresponding positive and negative electrode sheets, each with an area of S. Cut the sheet into a regular shape with an area of S0 using a die-cutting or cutting machine. Clean the negative electrode sheet with DMC and then dry it in an oven at 60°C. Select a lithium sheet as the negative electrode sheet and the cut negative / positive electrode sheet as the positive electrode. Assemble a button cell using the same separator and electrolyte as described in this manual. Charge the assembled cell at a constant voltage of 0.2C to the secondary battery charging cutoff voltage, cut off at 0.05C, and then discharge at 0.2C to the discharge cutoff voltage. Record the capacity C0. The electrode capacity C = C0 * S / S0.
[0097] Testing of coating compaction density:
[0098] A punching or cutting machine cuts electrodes of regular shape with an area of S. The mass m of the electrode is weighed using a precision balance (accuracy 0.1 mg). After deducting the mass of the current collector, the result is m1 (the mass of a blank current collector of the same area is measured separately and deducted). The thickness is measured at different locations on the electrode using a micrometer (1 μm accuracy) or a laser thickness gauge, and the average value is taken. This average thickness is then subtracted from the average thickness of the empty foil to obtain the active material coating thickness h. Compacted density = m1 / Sh (g / cm³) 3 )
[0099] Inspection of coating quality:
[0100] The total mass m2 of the entire electrode was measured using a high-precision electronic balance. A section of the exposed current collector (uncoated portion) was cut off and its mass m3 was measured. The effective coated area A, the total area A' of the electrode, and the area B of the exposed current collector were measured using vernier calipers. The mass of the current collector per unit area was m3 / B. The mass of a single-layer coating was calculated as (m2 - A'm3 / B) / A / 1540.25g / 1540.25mm. 2 .
[0101] Detection of silicon elemental mass percentage:
[0102] Energy-dispersive X-ray spectroscopy (EDS) testing:
[0103] 1. Sample preparation:
[0104] Disassemble the battery and remove the negative electrode.
[0105] Use DMC to clean the negative electrode to remove electrolyte and other impurities from the surface.
[0106] Dry the cleaned negative electrode sheet in a drying oven.
[0107] 2. Sample loading:
[0108] The dried negative electrode sheet was fixed on the sample tray of the SEM using conductive tape.
[0109] Adjust the sample position to ensure that the electron beam of the SEM can accurately irradiate the surface of the negative electrode.
[0110] Instrument settings:
[0111] The SEM was set with an accelerating voltage of 15kV, a moderate beam current, and a magnification of 1000x.
[0112] In the EDS attachment, select the point analysis mode and set the acquisition time to 30 seconds.
[0113] 3. Sample Analysis:
[0114] Use SEM to observe the surface morphology of the negative electrode sheet, and select a flat area for EDS analysis.
[0115] Point analysis was performed to record the intensity of the characteristic peak signal of silicon.
[0116] 4. Data Processing:
[0117] The characteristic peaks of silicon were identified by analyzing the X-ray signal using EDS software.
[0118] Background signal is removed, and matrix effect correction is performed.
[0119] Output results:
[0120] A test report is generated, showing the mass percentage of silicon in the sample.
[0121] Perform multiple tests on the same sample to ensure the repeatability and accuracy of the results.
[0122] Lithium plating / purple spot test method:
[0123] Place the secondary battery in an environment with a test temperature of 25℃ for 30 minutes, then charge it to 4.5V in stages according to the following charging steps:
[0124] (1) Charge at a constant current of 2.5C to 4.23V;
[0125] (2) Charge at 2C constant current to 4.3V;
[0126] (3) Charge at a constant current of 1.6C to 4.5V;
[0127] (4) Charge at 1C constant current to 4.5V, and charge at constant voltage to cut off current to 0.05C;
[0128] After letting it stand for 10 minutes, proceed with the following steps to discharge:
[0129] Discharge at a constant current of 0.2C to 3V.
[0130] The above charge-discharge process constitutes one cycle. After repeating 100 cycles, when the secondary battery is fully charged (maximum designed voltage 4.5V), the secondary battery is disassembled to obtain the first negative electrode. The non-lithium deposited area on the surface of the first negative electrode is golden yellow, the purple-spotted area is dark purple, and the lithium-deposited area is grayish-white. If the lithium deposition area on the surface of the first negative electrode is found to be greater than or equal to 1 mm², then the battery is considered to be in good condition. 2 If lithium plating is detected, the test fails. Each group tests 20 samples; the number of failed samples is N, and the lithium plating rate is N / 20. If a purple spot area greater than or equal to 1 mm² is found on the surface of the first negative electrode, the test is considered unsuccessful. 2 If any of the above are not present, they are considered purplish spots and the test is failed. Each group has 20 samples tested, and the number of failed samples is M, resulting in a purplish spot rate of M / 20.
[0131] Energy density test method: Charge the secondary battery with a constant current of 1C to the cutoff voltage, then charge the secondary battery with a constant voltage of the cutoff voltage to 0.05C, and then discharge the secondary battery with a constant current of 0.2C to 3V. Record the discharge energy E; measure the external dimensions of the secondary battery and calculate its volume, which is V; then the energy density W = E / V.
[0132] Example 1-1:
[0133] <Preparation of the positive electrode>
[0134] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is acetylene black, and the positive electrode binder is polyvinylidene fluoride (PVDF, with a weight average molecular weight of 5×10⁻⁶). 5 The materials were mixed at a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a positive electrode slurry with a solid content of 75 wt%. The slurry was then stirred uniformly under a vacuum mixer. An aluminum foil with a thickness of 10 μm, a length of 75 mm, and a width of 55 mm was used as the positive electrode current collector. The positive electrode slurry was uniformly coated on one surface of the aluminum foil and dried at 110 °C to obtain a first single-sided positive electrode sheet with a single-sided positive electrode coating. A second single-sided positive electrode sheet was prepared similarly. Subsequently, a positive electrode coating was coated on both surfaces of an aluminum foil to obtain a first inner layer positive electrode sheet with a double-sided positive electrode coating. A second inner layer positive electrode sheet and a third positive electrode sheet with double-sided positive electrode coating were similarly prepared.
[0135] <Preparation of Negative Electrode Sheets>
[0136] The negative electrode active material graphite powder, silicon powder, conductive agent conductive carbon black (Super P), and binder styrene-acrylic rubber (SD-3) were mixed in a mass ratio of 67.5:30:1:1.5, which is the mass percentage of silicon in the negative electrode active material G. 21The content was 30%. Then, deionized water was added as a solvent to prepare a negative electrode slurry with a solid content of 50 wt%, and stirred evenly. A copper foil with a thickness of 8 μm, a length of 75 mm, and a width of 55 mm was selected as the negative electrode current collector. The negative electrode slurry was uniformly coated on one surface of the copper foil and dried at 90°C. Then, the above steps were repeated on the other surface of the negative electrode current collector to obtain the first negative electrode sheet with a double-sided negative electrode coating. The second and third negative electrode sheets with double-sided negative electrode coatings were prepared similarly. The mass percentage of silicon in the negative electrode active material was the same for all negative electrode sheets.
[0137] <Preparation of the separating membrane>
[0138] A porous separator membrane was prepared by using polyethylene as a 7μm substrate layer and polyvinylidene fluoride as an adhesive layer, with an alumina ceramic layer of 2μm thickness placed on the side of the adhesive layer away from the substrate layer.
[0139] <Preparation of Electrolyte>
[0140] In a dry argon atmosphere, ethylene carbonate, methyl ethyl carbonate and diethyl carbonate were mixed in a mass ratio of 30:50:20 to obtain an organic solution. Then, lithium hexafluorophosphate was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.
[0141] <Preparation of Lithium-ion Secondary Batteries>
[0142] The first single-sided positive electrode, the first negative electrode, the first inner positive electrode, the first inner negative electrode, the third positive electrode, the third negative electrode, the third positive electrode, the second inner negative electrode, the second inner positive electrode, the second negative electrode, and the second single-sided positive electrode are stacked to form a structure as described above. Figure 4 The electrode assembly shown has an insulating membrane between adjacent positive and negative electrodes. The first and second single-sided positive electrodes are the outermost electrodes on both sides, and the electrode assembly has a total of 20 layers of positive and negative electrodes.
[0143] The coating on the first single-sided positive electrode facing the first negative electrode is the first positive electrode coating. The first positive electrode coating has a length of 70.2 mm, a width of 50.5 mm, and a thickness of 95 μm. The coating quality Y of the first positive electrode coating is... 11 It is 0.28g / 1540.25mm 2 The capacity C of the first positive electrode coating 11 The capacity is 300mAh. The coating on the first negative electrode facing the first positive electrode coating is the first negative electrode coating. The first negative electrode coating has a length of 72mm, a width of 51.8mm, and a thickness of 82μm. The coating quality Y of the first negative electrode coating is...21 It is 0.11g / 1540.25mm 2 The capacity C of the first negative electrode coating 21 The capacity is 309mAh. The third negative electrode coating on the first negative electrode sheet is identical to the first negative electrode coating, except for its thickness of 102μm. The coating on the first inner positive electrode sheet facing the first inner negative electrode sheet is the first inner positive electrode coating. The first inner positive electrode coating has a length of 70.2mm, a width of 50.5mm, and a thickness of 100μm. The coating quality Y of the first inner positive electrode coating... 31 It weighs 70.2g and has a thickness of 1540.25mm. 2 The capacity C of the first inner positive electrode coating 31 The capacity is 300mAh. The coating on the first inner negative electrode facing the first inner positive electrode coating is the first inner negative electrode coating. The length of the first inner negative electrode coating is 72mm, the width is 51.8mm, and the thickness is 82μm. The coating quality Y of the first inner negative electrode coating is... 41 It is 0.102g / 1540.25mm 2 The capacity C of the first inner negative electrode coating 41 It has a capacity of 306mAh.
[0144] The parameters of the third positive electrode are the same as those of the first inner positive electrode, and the parameters of the third negative electrode are the same as those of the first inner negative electrode coating. The parameters of the second inner negative electrode are the same as those of the first inner negative electrode, the parameters of the second inner positive electrode are the same as those of the first inner positive electrode, the parameters of the second negative electrode are the same as those of the first negative electrode, and the parameters of the second single-sided positive electrode are the same as those of the first single-sided positive electrode.
[0145] The punched aluminum-plastic film is placed in the assembly fixture with the punched surface facing upwards. The electrode assembly is then placed in the punched surface and pressed firmly. Another punched aluminum-plastic film is then placed on the electrode assembly with the punched surface facing downwards. After processes such as encapsulation, electrolyte injection, hot pressing, and shaping, a lithium-ion secondary battery is obtained.
[0146] Unlike Example 1, the relevant parameters in Examples 1-2 to 26 and Comparative Examples 1 to 2 are shown in Table 1 below.
[0147] Table 1
[0148]
[0149]
[0150] According to Table 1 above, and in conjunction with Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-2, in Comparative Example 1-1, (C 21 / C 11 ) / (C 41 / C31 A value smaller than or equal to 1 means that the capacity ratio of the outer positive and negative electrodes of the secondary battery is equal to that of the inner positive and negative electrodes. This means that the outer first negative electrode may slip and have difficulty accepting lithium ions released from the first single-sided positive electrode, easily leading to purple spots, and lithium ions are prone to deposit on the surface of the first negative electrode, resulting in lithium plating. In Comparative Examples 1-2, (C) 21 / C 11 ) / (C 41 / C 31 A smaller capacity may result in an excessive capacity ratio, making it difficult for some negative electrode active materials to participate in the electrochemical reaction, causing a loss of energy density in the secondary battery. There is also a risk of deterioration during high-temperature cycling, resulting in a smaller number of cycle capacity cutoff cycles. Furthermore, deterioration during high-temperature cycling may also lead to purple spots and lithium plating.
[0151] In Examples 1-1 to 1-7, it is defined that 1 < (C 21 / C 11 ) / (C 41 / C 31 A ratio ≤ 1.12 means that by increasing the capacity ratio of the outer positive and negative electrodes, based on the capacity ratio of the inner positive and negative electrodes, even if the first negative electrode experiences relative slippage, it can still better receive lithium ions extracted from the first single-sided positive electrode. This effectively reduces the appearance of purple spots and the deposition of lithium ions on the surface of the first negative electrode caused by slippage, thus improving the safety of the secondary battery. It also effectively reduces problems such as energy density loss, increased cost, and high-temperature cycling degradation caused by excessive coating on the first negative electrode.
[0152] In Examples 1-3 to 1-6, the lithium plating rate and purple spot rate are both low, and the impact on the energy density of the secondary battery is small. Furthermore, the high-temperature cycling degradation of the secondary battery is minimal, and its cycle capacity cutoff number is relatively large. Considering reducing lithium plating and purple spot occurrence while improving the high-temperature cycle capacity retention of the secondary battery, in the embodiments of this application, a value of 1.05 ≤ (C) is preferred. 21 / C 11 ) / (C 41 / C 31 )≤1.11.
[0153] In conjunction with Examples 1-1 to 1-17, in Example 1-17, C 21 And C 41A larger value may result in an excessive amount of the first negative electrode coating and the first inner negative electrode coating, leading to a significant energy density loss and a lower cycle capacity cutoff number. Furthermore, in Examples 1-17, the lithium plating rate and purple spot rate are similar to those in Examples 1-16. However, the impact on energy density in Examples 1-16 is less than that in Examples 1-17. Therefore, in the embodiments of this application, 1.03 ≤ (C) can be selected. 21 / C 11 )≤1.2, and 1.02≤(C 41 / C 31 )≤1.18.
[0154] In conjunction with Examples 1-18 to 1-26 and Comparative Examples 1-1 to 1-2, the lithium plating rate and purple spot rate in Examples 1-18 to 1-26 are lower than those in Comparative Examples 1 to 2. Within different capacity ranges, the limit is 1 < (C 21 / C 11 ) / (C 41 / C 31 A value ≤1.12 is beneficial for reducing lithium plating rate and purple spot rate. In Examples 1-26, C 11 C 21 C 31 And C 41 The values are all relatively large, which easily leads to the deterioration of the secondary battery during high-temperature cycling, and the lithium plating rate and purple spot rate are also relatively high. In Examples 1-18, C 11 C 21 C 31 And C 41 The average size is relatively small, making it difficult to meet the long-lasting requirements of secondary batteries. Furthermore, the single-layer coating is thin, easily leading to uneven processing, lithium plating, and potentially worsening high-temperature cycling. In the embodiments of this application, in conjunction with embodiments 1-19 to 1-25, a capacity of 75mAh ≤ C can be selected. 11 ≤500mAh, 78mAh≤C 21 ≤520mAh, 75mAh≤C 31 ≤500mAh and 77mAh≤C 41 With a capacity of ≤510mAh, it can reduce purple spots and lithium plating, and improve the versatility of the 1000 rechargeable battery.
[0155] Unlike Examples 1-4, the relevant parameters in Examples 2-1 to 2-8 are shown in Table 2 below.
[0156] Table 2
[0157]
[0158] According to Table 2 above, and in conjunction with Examples 2-1 to 2-8, in Example 2-1, the mass percentage G of silicon in the first negative electrode coating...21 The energy density is relatively small, making it difficult to improve the energy density of the secondary battery. Furthermore, the purple spot rate and lithium plating rate are similar in Examples 2-1 and 2-2, while Example 2-2, compared to Example 2-1, has a lower G... 21 A larger mass percentage of silicon in the first negative electrode coating is beneficial for improving the energy density of the secondary battery. In Examples 2-8, the mass percentage G of silicon in the first negative electrode coating... 21 A larger value might cause an excessively severe volume expansion effect, leading to greater stress within the negative electrode coating and consequently higher purple spot rate and lithium plating rate. Therefore, in the embodiments of this application, 2.5% ≤ G 21 ≤50%, corresponding to its capacity C 21 Alternatively, a capacity of 164mAh≤C can be preferred. 21 ≤446mAh.
[0159] Combining Examples 2-4 to 2-5 and Examples 1-4 in Table 1, the lithium plating rate and purple spot rate are both relatively low, and G 21 Given the relatively large size, and considering both reducing lithium plating and increasing energy density, a value of 10% ≤ G is preferred. 21 ≤30%, corresponding to its capacity C 21 Alternatively, a capacity of 208mAh≤C can be further preferred. 21 ≤330mAh.
[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them; under the concept of this application, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of different aspects of this application as described above, which are not provided in detail for the sake of brevity; although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the foregoing embodiments, or make equivalent substitutions for some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A secondary battery, comprising an electrode assembly, the electrode assembly comprising a first single-sided positive electrode, a first negative electrode, a first inner positive electrode, and a first inner negative electrode, sequentially stacked along a first direction; the first single-sided positive electrode is the outermost electrode of the electrode assembly, characterized in that: The first single-sided positive electrode includes a first positive electrode coating facing the first negative electrode, and the capacity of the first positive electrode coating is C. 11 The first negative electrode includes a first negative electrode coating facing the first positive electrode coating, and the capacity of the first negative electrode coating is C. 21 ; The first inner positive electrode includes a first inner positive electrode coating facing the first inner negative electrode, and the capacity of the first inner positive electrode coating is C. 31 The first inner negative electrode sheet includes a first inner negative electrode coating facing the first inner positive electrode coating, and the capacity of the first inner negative electrode coating is C. 41 ; Satisfy: 1 < (C 21 / C 11 ) / (C 41 / C 31 )≤1.
12.
2. The secondary battery according to claim 1, characterized in that, 1.05≤(C 21 / C 11 ) / (C 41 / C 31 )≤1.11。 3. The secondary battery according to claim 1, characterized in that, 1.03≤(C 21 / C 11 )≤1.2。 4. The secondary battery according to claim 1, characterized in that, 1.02≤(C 41 / C 31 )≤1.18。 5. The secondary battery according to claim 1, characterized in that, 75mAh≤C 11 ≤500mAh; 78mAh≤C 21 ≤520mAh; 75mAh≤C 31 ≤500mAh; 77mAh≤C 41 ≤510mAh。 6. The secondary battery according to claim 1, characterized in that, The compaction density of the first negative electrode coating is less than that of the first inner negative electrode coating.
7. The secondary battery according to claim 6, characterized in that, The first negative electrode sheet further includes a third negative electrode coating facing the first inner positive electrode sheet, wherein the compaction density of the first negative electrode coating is less than that of the third negative electrode coating.
8. The secondary battery according to claim 1, characterized in that, The coating quality of the first negative electrode coating is greater than that of the first inner negative electrode coating.
9. The secondary battery according to claim 1, characterized in that, The first negative electrode coating includes a negative electrode active material, the negative electrode active material includes silicon, and the mass percentage G of the silicon in the negative electrode active material is... 21 2.5% ≤ G 21 ≤50%.
10. The secondary battery according to claim 9, characterized in that, 10%≤G 21 ≤30%。 11. The secondary battery according to claim 1, characterized in that, The secondary battery also includes a casing, and the first single-sided positive electrode is fixed to the inner wall of the casing.
12. The secondary battery according to any one of claims 1 to 11, characterized in that, The electrode assembly further includes a second inner negative electrode sheet, a second inner positive electrode sheet, a second negative electrode sheet, and a second single-sided positive electrode sheet, which are sequentially stacked along the first direction. Along the first direction, the outermost electrode plates on both sides of the electrode assembly are the second single-sided positive electrode plate and the first single-sided positive electrode plate, respectively; The second single-sided positive electrode includes a second positive electrode coating facing the second negative electrode, and the capacity of the second positive electrode coating is C. 12 The second negative electrode includes a second negative electrode coating facing the second positive electrode coating, and the capacity of the second negative electrode coating is C. 22 ; The second inner positive electrode includes a second inner positive electrode coating facing the second inner negative electrode, and the capacity of the second inner positive electrode coating is C. 32 The second inner negative electrode sheet includes a second inner negative electrode coating facing the second inner positive electrode coating, and the capacity of the second inner negative electrode coating is C. 42 ;1<(C 22 / C 12 ) / (C 42 / C 32 )≤1.
12.
13. The secondary battery according to claim 12, characterized in that, 1.02≤(C 22 / C 12 )≤1.2。 14. The secondary battery according to claim 12, characterized in that, Along the first direction, one or more third negative electrode sheets are stacked between the first inner negative electrode sheet and the second inner negative electrode sheet; When multiple third negative electrode sheets are stacked between the first inner negative electrode sheet and the second inner negative electrode sheet, a third positive electrode sheet is stacked between two adjacent third negative electrode sheets along the first direction.
15. An electronic device, characterized in that, Includes the secondary battery as described in any one of claims 1 to 14.