Battery
By optimizing the compaction density and porosity matching of the negative electrode sheet, the risk of lithium plating caused by the thickness difference of the negative electrode sheet in lithium-ion batteries was solved, thereby improving the cycle life and energy density of the battery.
Patent Information
- Application Number
- CN202611518745.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
In lithium-ion batteries, the reduced thickness of the negative electrode leads to a significant difference in expansion between the single-sided and double-sided regions during cycling, increasing the risk of internal resistance polarization and lithium plating.
The negative electrode structure is designed so that the compaction density of the negative electrode active layer in both the bifacial and single-sided regions meets the requirement of 0.85≤ρ1/ρ2≤1.2. The negative electrode tabs are led out in the bifacial region to avoid excessively high local current density. By optimizing the matching of compaction density and porosity, the risk of lithium plating is reduced.
It improves battery cycle life and energy density, reduces the risk of lithium plating, ensures uniform electrolyte wetting and uniform lithium ion insertion, and enhances the overall performance of the battery.
Smart Images

Figure CN123120833A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and more particularly to a battery. Background Technology
[0002] In related technologies, lithium-ion batteries include a casing, a core disposed within the casing, and an electrolyte. The core is formed by winding a positive electrode sheet, a separator, and a negative electrode sheet. Since the negative electrode sheet increases its specific capacity by doping with silicon-based materials, its overall thickness tends to decrease. Furthermore, because the negative electrode sheet has a single-sided region coated with silicon-based material on one side and a double-sided region coated with silicon-based material on both sides, the reduced thickness of the negative electrode sheet leads to a more significant difference in expansion between the single-sided and double-sided regions during cycling, thereby exacerbating internal resistance polarization within the battery. Further, for the negative electrode sheet, since its double-sided region is wound outside the single-sided region, and the single-sided region is located at the innermost two folds of the core, it experiences greater stress. This causes problems such as pore compression, ion channel blockage, and electrolyte extrusion in the single-sided region, resulting in localized electrolyte shortage and worsened concentration polarization, thus increasing the risk of lithium plating inside the lithium-ion battery. Summary of the Invention
[0003] This application provides a battery to solve the above-mentioned technical problems.
[0004] The battery in this embodiment of the application includes:
[0005] A battery cell includes a positive electrode, a separator, and a negative electrode. The positive electrode, separator, and negative electrode are wound around a winding center. The negative electrode includes a negative single-sided region and a negative double-sided region adjacent to each other along its own length direction. The end of the negative double-sided region away from the negative single-sided region constitutes the winding termination end of the negative electrode.
[0006] The negative electrode sheet includes a negative current collector and a negative active layer arranged along its own thickness direction, and a negative tab led out from one side of the negative current collector in the width direction. Multiple negative tabs are arranged at intervals along the length direction of the negative current collector. Multiple negative tabs are stacked in the thickness direction of the cell and connected to each other. The negative active layer includes silicon-based material. Based on the total mass of the negative active layer on any side of the negative current collector, the mass fraction of silicon element in the negative active layer is greater than or equal to 5%.
[0007] In the single-sided region of the negative electrode, the negative electrode active layer is formed on the side of the negative electrode current collector away from the winding center. In the double-sided region of the negative electrode, the negative electrode active layer is formed on opposite sides in the thickness direction of the negative electrode current collector. All negative electrode tabs correspond to the negative electrode current collector in the double-sided region of the negative electrode.
[0008] The compaction density ρ1 of the negative electrode active layer located in the double-sided region of the negative electrode and the compaction density ρ2 of the negative electrode active layer located in the single-sided region of the negative electrode satisfy the following condition: 0.85≤ρ1 / ρ2≤1.2.
[0009] In one possible embodiment, the compaction density ρ1 of the negative electrode active layer located in the negative electrode double-sided region satisfies: 1 g / cm³ 3 ≤ρ1≤1.55g / cm 3 ;
[0010] And / or, the compaction density ρ2 of the negative electrode active layer located in the negative electrode single-sided region satisfies: 0.9 g / cm³ 3 ≤ρ2≤1.45g / cm 3 .
[0011] In one possible embodiment, the compaction density of the negative electrode active layer on both sides of the negative electrode current collector is the same in the negative electrode double-sided region.
[0012] In one possible embodiment, the negative electrode active layer includes a first active layer and a second active layer, which are respectively disposed on opposite sides of the negative electrode current collector in the thickness direction. A portion of the projection of the first active layer overlaps with the projection of the second active layer and is formed on the double-sided region of the negative electrode, while another portion of the projection of the first active layer is offset from the projection of the second active layer and is formed on the single-sided region of the negative electrode. The compaction density of the first active layer is different from that of the second active layer. The compaction density of the negative electrode active layer located in the double-sided region of the negative electrode is the average of the compaction densities of the first and second active layers, while the compaction density of the negative electrode active layer located in the single-sided region of the negative electrode is the compaction density of the first active layer.
[0013] In one possible embodiment, the average porosity P1 of the negative electrode active layer located in the single-sided region of the negative electrode and the average porosity P2 of the negative electrode active layer located in the double-sided region of the negative electrode satisfy |P1-P2|≤5%;
[0014] And / or, the average porosity P1 of the negative electrode active layer located in the negative electrode single-sided region satisfies: 30%≤P1≤45%;
[0015] And / or, the average porosity P2 of the negative electrode active layer located in the negative electrode double-sided region satisfies: 28%≤P2≤40%.
[0016] In one possible embodiment, the cell includes a flat region and arcuate regions located on opposite sides of the flat region, with the boundary between the negative double-sided region and the negative single-sided region located in the flat region.
[0017] In one possible embodiment, the negative electrode single-sided region includes a first embossed region, the first embossed region having a first concave-convex portion, and the negative electrode double-sided region includes a second embossed region, the second embossed region having a second concave-convex portion, the first concave-convex portion including a first concave portion and a first convex portion, the second concave-convex portion including a second concave portion and a second convex portion, the first concave portion and the second concave portion both being recessed from the side of the negative electrode sheet away from the winding center to the side closer to the winding center.
[0018] The depth of the first recess, H1, is greater than the depth of the second recess, H2.
[0019] And / or, the negative electrode single-sided area also includes a first clearance area, and the two first clearance areas are located on both sides of the first embossed area along the width direction of the negative electrode sheet;
[0020] And / or, the negative electrode double-sided region also includes a second clearance region, with the two second clearance regions located on both sides of the second embossed region along the width direction of the negative electrode sheet;
[0021] And / or, the negative electrode double-sided region also includes a third clearance region, which is located on the side of the second embossed region away from the negative electrode single-sided region.
[0022] In one possible embodiment, the recess depth H1 of the first recess and the recess depth H2 of the second recess satisfy: 1 / 3≤H2 / H1≤1 / 2;
[0023] And / or, the recess depth H1 of the first recess satisfies: 20μm≤H1≤80μm;
[0024] And / or, the recess depth H2 of the second recess satisfies: 20μm≤H2≤60μm;
[0025] And / or, along the length of the negative electrode sheet, the length L1 of the negative electrode single-sided area and the length L2 of the third evacuation area satisfy: L2≥1.25*L1.
[0026] In one possible embodiment, the positive electrode sheet includes a positive electrode double-sided region and a positive electrode single-sided region adjacent to each other along its own length direction, with at least a portion of the positive electrode single-sided region wound around the outermost ring of the positive electrode sheet;
[0027] The positive electrode double-sided region includes a third embossed region, a fourth clearance region, a fifth clearance region, and a sixth clearance region. The two fourth clearance regions are located on both sides of the third embossed region along the width direction of the positive electrode sheet, and the fifth and sixth clearance regions are located on both sides of the third embossed region along the length direction of the positive electrode sheet. The fifth clearance region is located close to the positive electrode single-sided region.
[0028] The third embossing area is provided with a third concave and convex part, which includes a third concave part and a third convex part. The third concave part is recessed from the side of the positive electrode sheet away from the winding center to the side closer to the winding center.
[0029] The depth H3 of the third recess satisfies: 10μm≤H3≤60μm; and / or, in the length direction of the positive electrode sheet, the length L3 of the fifth clearance zone and the length L4 of the positive electrode single-sided zone satisfy: L3≥0.75*L4; and / or, in the length direction of the positive electrode sheet, the length L5 of the sixth clearance zone and the length L4 of the positive electrode single-sided zone satisfy: L5≥0.5*L4.
[0030] In one possible embodiment, the diameter D1 of the first protrusion satisfies: 0.5mm ≤ D1 ≤ 10mm;
[0031] And / or, the diameter D2 of the second protrusion satisfies: 0.5mm≤D2≤10mm;
[0032] And / or, the diameter D3 of the third protrusion satisfies: 1mm≤D3≤15mm;
[0033] And / or, the diameter D1 of the first protrusion and the distance T1 between two adjacent first protrusions satisfy: D1 < T1;
[0034] And / or, the diameter D2 of the second protrusion and the distance T2 between two adjacent second protrusions satisfy: D2 < T2;
[0035] And / or, the diameter D3 of the third protrusion and the distance T3 between two adjacent third protrusions satisfy: D3 < T3;
[0036] And / or, the depth of the second recess H2 and the depth of the third recess H3 satisfy: H2 > H3.
[0037] In addition to the technical problems solved by the embodiments of this application, the technical features constituting the technical solutions, and the beneficial effects brought about by the technical features of these technical solutions described above, other technical problems that the battery provided by this application can solve, other technical features included in the technical solutions, and the beneficial effects brought about by these technical features will be further described in detail in the specific embodiments. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0039] Figure 1 This is a schematic diagram of the battery structure provided in an embodiment of this application;
[0040] Figure 2 This is a schematic diagram of the structure of the negative electrode in the battery provided in the embodiments of this application. Figure 1 ;
[0041] Figure 3 This is a schematic diagram of the structure of the negative electrode in the battery provided in the embodiments of this application. Figure 2 ;
[0042] Figure 4 This is a schematic diagram of the structure of the negative electrode in the battery provided in the embodiments of this application. Figure 3;
[0043] Figure 5 This is a schematic diagram of the structure of the negative electrode in the battery provided in the embodiments of this application. Figure 4 ;
[0044] Figure 6 This is a schematic diagram of the structure of the positive electrode in the battery provided in the embodiments of this application;
[0045] Figure 7 This is another structural schematic diagram of the positive electrode sheet in the battery provided in the embodiments of this application.
[0046] Explanation of reference numerals in the attached figures:
[0047] 100 - Positive electrode sheet; 110 - Positive electrode single-sided area; 120 - Positive electrode double-sided area; 121 - Third embossed area; 122 - Fourth void area; 123 - Fifth void area; 124 - Sixth void area; 130 - Positive electrode empty foil area;
[0048] 200-diaphragm;
[0049] 300 - Negative electrode sheet; 310 - Negative electrode single-sided region; 311 - First embossed region; 312 - First void-avoiding region; 320 - Negative electrode double-sided region; 321 - Second embossed region; 322 - Second void-avoiding region; 323 - Third void-avoiding region; 330 - Negative electrode empty foil region; 300a - Negative electrode current collector; 300b - Negative electrode active layer; 300c - Negative electrode tab. Detailed Implementation
[0050] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be described in more detail below with reference to the accompanying drawings. In the drawings, the same or similar reference numerals denote the same or similar components or components having the same or similar functions throughout. The described embodiments are some, but not all, embodiments of this application. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application. The embodiments of this application will be described in detail below with reference to the accompanying drawings.
[0051] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, an indirect connection through an intermediate medium, or the internal communication between two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0052] In the description of this application, it should be understood that the terms "upper", "lower", "front", "back", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0053] The terms "first," "second," and "third" (if any) in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a particular order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein.
[0054] Furthermore, the terms “comprising” and “having”, and any variations thereof, are intended to cover non-exclusive inclusion, such that a process, method, system, product, or display that includes a series of steps or units is not necessarily limited to those steps or units that are explicitly listed, but may include other steps or units that are not explicitly listed or that are inherent to such process, method, product, or display.
[0055] Reference Figures 1 to 4As shown, this application provides a battery, which includes a casing and a cell housed within the casing. The cell is formed by winding a positive electrode 100, a separator 200, and a negative electrode 300 around a winding center. The negative electrode 300 has a negative electrode single-sided region 310 and a negative electrode double-sided region 320 disposed adjacent to each other along its own length direction, and the end of the negative electrode double-sided region 320 away from the negative electrode single-sided region 310 constitutes the winding termination end of the negative electrode 300. The negative electrode 300 includes a negative electrode current collector 300a disposed along its thickness direction, a negative electrode active layer 300b formed on the negative electrode current collector 300a, and negative electrode tabs 300c extended from one side of the width direction of the negative electrode current collector 300a. Multiple negative electrode tabs 300c are spaced apart along the length direction of the negative electrode current collector 300a and are stacked and connected in the cell thickness direction. The negative electrode active layer 300b comprises a silicon-based material, and the mass fraction of silicon in the negative electrode active layer is greater than or equal to 5% based on the total mass of the negative electrode active layer 300b on any side of the negative electrode current collector 300a. In the single-sided negative electrode region 310, the negative electrode active layer 300b is formed on the side of the negative electrode current collector 300a away from the winding center. In the double-sided negative electrode region 320, the negative electrode active layer 300b is formed on opposite sides in the thickness direction of the negative electrode current collector 300a. All negative electrode tabs 300c correspond to the negative electrode current collector 300a in the double-sided negative electrode region 320. The compaction density ρ1 of the negative electrode active layer 300b located in the negative electrode double-sided region 320 and the compaction density ρ2 of the negative electrode active layer 300b located in the negative electrode single-sided region 310 satisfy 0.85≤ρ1 / ρ2≤1.2.
[0056] In this embodiment, the battery cell is an electrochemical energy storage unit formed by winding a positive electrode 100, a separator 200, and a negative electrode 300. The battery cell is used to complete the insertion and extraction of lithium ions and the directional transport of electrons during charging and discharging, and serves as the main body for energy conversion in the battery. The winding center can be used as the geometric reference during the winding of the battery cell. The positive electrode 100, the separator 200, and the negative electrode 300 are sequentially attached and form a stable stacked winding body around the winding center. The length, width, and thickness of the battery cell can be matched and set according to the battery specifications, and this embodiment does not impose specific limitations on them.
[0057] The positive electrode 100 is a positive electrode sheet used to provide reversible lithium ion insertion and extraction. During the winding process, the positive electrode 100 is arranged adjacent to the separator 200 and together with the negative electrode 300 forms an electrochemical reaction interface. The positive electrode 100 extends continuously along the winding path, maintaining surface contact with the separator 200 to ensure continuous ion migration channels.
[0058] The separator 200 is a porous insulating film layer disposed between the positive electrode 100 and the negative electrode 300. The separator 200 is used to prevent direct physical contact between the positive and negative electrodes while allowing lithium ions to pass through. During winding, the separator 200 is wound synchronously with the positive electrode 100 and the negative electrode 300, and covers the space between the positive electrode 100 and the negative electrode 300. Its width may be slightly larger than that of the negative electrode 300 to form the necessary insulation margin at the edge in the height direction of the cell, ensuring electrical isolation between the layers of the cell and electrolyte wetting channels.
[0059] The negative electrode 300 is a negative electrode sheet including a negative current collector 300a, a negative active layer 300b, and a negative tab 300c. The positive electrode 100 and the negative electrode 300 together form an electrochemical reaction interface. The negative electrode 300 forms a negative single-sided region 310 and a negative double-sided region 320 in sequence along its length.
[0060] Among them, the negative electrode single-sided region 310 refers to the region where the negative electrode active layer 300b is formed only on the side of the negative electrode current collector 300a away from the winding center. The negative electrode single-sided region 310 is located at the beginning section of the negative electrode sheet 300 along the winding direction. After winding, the negative electrode single-sided region 310 is closer to the innermost layer of the cell. During winding, after the negative electrode single-sided region 310 is attached to the adjacent separator 200, only one side participates in the electrochemical reaction, while the other side is adjacent to the separator 200 by the negative electrode current collector 300a.
[0061] The negative electrode double-sided region 320 is the region on both sides of the negative electrode active layer 300b formed in the thickness direction of the negative electrode current collector 300a. The negative electrode double-sided region 320 is located in the middle and end sections of the negative electrode sheet 300 along the winding direction. After winding, the negative electrode double-sided region 320 is closer to the middle and outermost layers of the cell. The negative electrode active layer 300b is simultaneously provided on both sides of the negative electrode current collector 300a to form a symmetrical reaction interface, so that the two sides of the negative electrode double-sided region 320 can form effective electrochemical contact with the adjacent positive electrode sheet 100 after winding.
[0062] The negative electrode tab 300c is a conductive connection structure led out from one side of the width direction of the negative electrode current collector 300a. The negative electrode tab 300c is used to collect the current on the negative electrode sheet 300 and transmit it to the circuit outside the battery. Multiple negative electrode tabs 300c are spaced apart along the length direction of the negative electrode current collector 300a and are stacked and connected in the thickness direction of the cell.
[0063] It should be understood that the negative electrode tab 300c is the current convergence point of the negative electrode sheet 300. If the negative electrode tab 300c is led out from the negative electrode current collector 300a of the negative electrode single-sided region 310, due to the difference in thickness between the negative electrode single-sided region 310 and the negative electrode double-sided region 320, and the relatively poor interfacial adhesion between the negative electrode active layer 300b and the negative electrode current collector 300a in the negative electrode single-sided region 310, these factors can easily lead to excessively high local current density in the negative electrode single-sided region 310, which in turn can easily lead to lithium plating in the negative electrode single-sided region 310.
[0064] In this embodiment, each of the multiple negative electrode tabs 300c corresponds to the negative double-sided region 320, meaning that each of the multiple negative electrode tabs 300c can be led out from the negative current collector 300a of the negative double-sided region 320. This avoids the negative electrode tabs 300c corresponding to the negative single-sided region 310, thereby preventing excessively high local current density in the negative single-sided region 310 and reducing the risk of lithium plating in the negative single-sided region 310.
[0065] Among them, the negative electrode tab 300c and the negative electrode current collector 300a can be integrally formed. Multiple negative electrode tabs 300c form a stacked current-collecting structure along the thickness direction after winding. The width and spacing of the negative electrode tabs 300c can be matched according to the cell thickness, capacity and allowable current density, so that it can maintain good mechanical continuity and conductive continuity in the winding and bending state.
[0066] Since the negative electrode active layer 300b in this embodiment includes a silicon-based material, the silicon-based material can be used to improve the specific capacity of the negative electrode active layer 300b and synergistically form a composite lithium storage structure with graphite or carbon-based materials. Based on the total mass of the negative electrode active layer 300b on any side surface of the negative electrode current collector 300a, the mass fraction of silicon in the negative electrode active layer is greater than or equal to 5%. The silicon-based material can be coated onto the surface of the negative electrode current collector 300a after forming a slurry with a conductive agent, binder, and solvent. The particle size and content of the silicon-based material can be matched and set according to requirements; this embodiment does not impose specific limitations on this.
[0067] In this embodiment, the compaction density of the negative electrode active layer 300b of the negative electrode sheet 300 refers to the mass of the negative electrode active layer 300b per unit volume after the negative electrode sheet 300 has been rolled, also called the rolling density. The compaction density of the negative electrode active layer 300b is equal to the areal density of the negative electrode active layer 300b per unit area and the thickness of the negative electrode active layer 300b per unit area.
[0068] When measuring the areal density of the negative electrode active layer 300b per unit area, a weighing method can be used. Specifically: use a punching machine to punch out a circular or square sample of a unit area from the negative electrode sheet 300. Weigh the sample retaining only one side of the negative electrode active layer 300b using an analytical balance. Wipe, scrape, or dissolve the negative electrode active layer 300b with a solvent to completely expose the negative electrode current collector 300a. Alternatively, it can be scraped off directly with a blade. After cleaning and drying the negative electrode current collector 300a, weigh its mass using an analytical balance. The areal density of the negative electrode active layer 300b per unit area = (mass of the sample with the negative electrode active layer 300b - mass of the sample without the negative electrode active layer 300b) / sample area. Alternatively, a β-ray areal density meter can be used to measure the areal density of the negative electrode active layer 300b per unit area.
[0069] In this embodiment, ρ1 and ρ2 correspond to the unit volume mass state of the negative electrode active layer 300b in the negative electrode double-sided region 320 and the negative electrode single-sided region 310 after roll forming, respectively. They are used to characterize the compactness and pore distribution difference of the negative electrode active layer 300b in the two regions of negative electrode double-sided region 320 and negative electrode single-sided region 310, respectively.
[0070] It should be noted that when the mass fraction of silicon in the negative electrode active layer is greater than or equal to 5%, the specific capacity of the negative electrode 300 increases with the increase of the mass fraction of silicon-based material. Consequently, the amount of negative electrode slurry coated during coating is reduced, and the negative electrode 300 becomes thinner overall. Due to the limited precision of the rolling equipment, the risk of uneven thickness of the negative electrode 300 increases, which in turn leads to a significant increase in the risk of lithium plating of the negative electrode 300.
[0071] In this embodiment, the relationship between the compaction density ρ1 of the negative electrode active layer 300b in the negative electrode double-sided region 320 and the compaction density ρ2 of the negative electrode active layer 300b in the negative electrode single-sided region 310 is optimized, and the two satisfy 0.85≤ρ1 / ρ2≤1.2.
[0072] On the one hand, if ρ1 / ρ2 < 0.85, it will result in ρ1 being too small and ρ2 being too large, which will lead to a smaller thickness of the single-sided negative electrode region 310 and a larger thickness of the double-sided negative electrode region 320. This will increase the thickness difference between the single-sided negative electrode region 310 and the double-sided negative electrode region 320, thereby increasing the uneven lithium-ion intercalation caused by the uneven thickness. This will result in an excessively high local current density of the negative electrode sheet 300, which will increase the risk of lithium plating in the battery and thus affect the cycle life of the battery. When ρ2 is too large, a large rolling pressure needs to be applied to the negative electrode single-sided region 310 during rolling. Since the negative electrode single-sided region 310 only has a negative electrode active layer 300b on one side, during rolling, the elongation of the negative electrode current collector 300a is greater than that of the negative electrode active layer 300b, causing asynchronous elongation deformation on both sides of the negative electrode single-sided region 310. This deformation difference will cause a difference in internal stress on the two sides of the negative electrode single-sided region 310, which in turn will lead to the negative electrode single-sided region 310... The negative electrode single-sided region 310 is prone to curling. Under excessive roller pressure, the curling phenomenon becomes more severe. Since the negative electrode single-sided region 310 is wound in the inner layer of the cell, it is already subjected to significant compressive stress. Curling causes wrinkles and stress concentration, which further compresses the porosity of the negative electrode single-sided region 310, leading to a decrease in its porosity. This makes it difficult for the electrolyte to wet the electrode, increases the difficulty of lithium-ion intercalation, and affects the uniform intercalation of lithium ions, thus causing lithium deposition in the negative electrode single-sided region 310. In addition, since the energy density of the negative electrode sheet 300 is mainly contributed by the negative electrode double-sided region 320, an excessively small ρ1 will reduce the energy density of the negative electrode double-sided region 320, thereby significantly reducing the energy density of the negative electrode sheet 300.
[0073] Therefore, in this embodiment, ρ1 / ρ2≥0.85, so that the compaction density of the negative electrode single-sided region 310 and the negative electrode double-sided region 320 is close, thereby improving the overall thickness uniformity of the negative electrode sheet 300 and avoiding excessively high compaction density of the negative electrode double-sided region 320, so as to ensure the porosity of the negative electrode single-sided region 310, thereby improving the electrolyte wettability of the inner layer of the cell and ensuring the uniform embedding of lithium ions into the negative electrode single-sided region 310, thereby reducing the risk of lithium plating in the inner layer of the cell and helping to maintain the energy density of the negative electrode double-sided region 320, which in turn helps to improve the energy density of the cell.
[0074] On the other hand, if ρ1 / ρ2 > 1.2, it will result in ρ1 being too large and ρ2 being too small, leading to over-compaction of the negative electrode double-sided region 320. This will result in insufficient porosity in the negative electrode double-sided region 320, poor electrolyte wetting, and hindered lithium-ion transport, making it more prone to lithium plating. Conversely, if the compaction density of the negative electrode single-sided region 310 is too low, it will result in insufficient mechanical support for the negative electrode active layer 300b. The negative electrode active layer 300b is prone to local collapse and interface debonding, leading to powder shedding in the negative electrode single-sided region 310, and also easily causing lithium plating.
[0075] Therefore, in this embodiment, ρ1 / ρ2≤1.2, so as to reduce the risk of lithium plating in the negative electrode double-sided region 320, thereby reducing the risk of lithium plating in the battery, thus improving the cycle life of the battery, and improving the mechanical properties of the negative electrode active layer 300b in the negative electrode single-sided region 310, preventing lithium plating in the negative electrode single-sided region 310 due to powder shedding.
[0076] For example, ρ1 / ρ2 can be any one of 0.85, 0.9, 0.95, 1, 1.1, 1.2 or fall within any two value ranges. In specific implementations, the compaction density can be adjusted in conjunction with the roller pressure, roller gap, and thickness of the negative electrode active layer 300b.
[0077] In one possible implementation, the compaction density ρ1 of the negative electrode active layer 300b located in the negative electrode double-sided region 320 satisfies: 1 g / cm³ 3 ≤ρ1≤1.55g / cm 3 The compaction density ρ2 of the negative electrode active layer 300b located in the negative electrode single-sided region 310 satisfies: 0.9 g / cm³. 3 ≤ρ2≤1.45g / cm 3 .
[0078] For example, ρ1 can be 1 g / cm³. 3 1.1g / cm 3 1.25g / cm 3 1.3g / cm 3 1.4g / cm 3 1.55g / cm 3 It can be any one of the values or fall within the range of any two values. ρ2 can be 0.9 g / cm³. 3 1g / cm 3 1.15g / cm 3 1.2g / cm 3 1.3g / cm 3 1.45g / cm 3 It can be any one of the values or fall within the range of any two values.
[0079] Compacted density is used to characterize the balance between densification, porosity, and electrolyte wettability of the negative electrode active layer 300b. The compacted density ρ1 is limited to 1 g / cm³. 3 Up to 1.55 g / cm 3 Between these elements, the negative electrode double-sided region 320 can maintain relatively stable skeleton strength when bearing the negative electrode tab 300c busbar, winding, and cyclic expansion loads, and provides suitable transport channels for electron conduction and ion diffusion. The compaction density ρ2 is limited to 0.9 g / cm³.3 Up to 1.45 g / cm 3 Between them, the negative electrode single-sided region 310 can have a moderate buffer space and wetting ability when it is wound together with the negative electrode double-sided region 320, thereby reducing the mismatch between the negative electrode single-sided region 310 and the negative electrode double-sided region 320 in the compaction state.
[0080] During the process, the compaction density can be adjusted by means of roller pressure, roller gap, slurry solid content, coating thickness, and segmented compaction. For example, the thick coating area can be pre-compacted first, and then the final coating layer can be finely compacted so that ρ1, ρ2, and ρ1 / ρ2 fall within the above range respectively.
[0081] For the double-sided region 320 and the single-sided region 310 of the negative electrode, excessively low compaction density will result in insufficient mechanical support for the negative electrode active layer 300b, making it prone to local collapse and interface debonding during cycling. Conversely, excessively high compaction density will reduce pore connectivity and increase lithium-ion migration resistance. Furthermore, for the single-sided region 310 of the negative electrode, excessively high compaction density will also increase the risk of curling.
[0082] In this embodiment, by controlling ρ1 and / or ρ2 within the above range, the negative electrode double-sided region 320 and the negative electrode single-sided region 310 can form a synergistic match in terms of the stress state, ion transport path and electrolyte distribution state after winding, thereby suppressing polarization differences caused by insufficient or excessive local densification and reducing the probability of lithium plating and capacity decay during battery cycling.
[0083] In some embodiments, on the negative electrode double-sided region 320, the compaction density of the negative electrode active layer 300b located on both sides of the negative electrode current collector 300a is the same.
[0084] In this embodiment, the negative electrode active layer 300b located on the negative electrode double-sided region 320 and on both sides of the negative electrode current collector 300a can be understood as a two-layer coating structure formed in the negative electrode double-sided region 320 and located on opposite sides of the thickness direction of the negative electrode current collector 300a. The same compaction density means that the compaction density measured on both sides of the negative electrode active layer 300b after roll forming is consistent or approximately consistent.
[0085] Because the porosity, conductive network continuity, and material densification on both sides of the negative electrode double-sided region 320 are matched, the insertion and extraction impedances of lithium ions on both sides of the negative electrode current collector 300a tend to be consistent, and the negative electrode double-sided region 320 forms a relatively balanced mechanical support state during the winding and expansion process. Since the negative electrode double-sided region 320 corresponds to multiple negative electrode tabs 300c and undertakes the main current collection function, the consistent compaction density of the two negative electrode active layers 300b can also reduce uneven local current distribution and uneven stress in the thickness direction.
[0086] Among them, the negative electrode current collector 300a can be copper foil, and the negative electrode active layer 300b is coated on opposite sides of the copper foil in the thickness direction, and forms a symmetrical coating through the same formulation system or the same solid content slurry.
[0087] To achieve the same compaction density on both sides, a synchronous rolling process with the same roll gap, pressure, and linear speed can be used on the negative electrode double-sided area 320 after coating. Alternatively, consistency can be achieved through a double-sided synchronous rolling press, a roller compensation mechanism, and an online closed-loop feedback control system, so that the thickness and areal density of the negative electrode active layer 300b on both sides remain consistent after rolling.
[0088] In specific implementation, silicon-based materials may include silicon-carbon composite materials, silicon-oxygen composite materials, or elemental silicon materials, and the two negative electrode active layers 300b can use conductive agents, binders, and thickeners with the same particle size distribution to reduce the difference in compaction density caused by differences in material composition.
[0089] It should be understood that since the compaction density is the same on both sides of the negative electrode double-sided region 320, when measuring the compaction density of the negative electrode double-sided region 320, the negative electrode active layer 300b on either side of the negative electrode double-sided region 320 can be selected for measurement, and multiple measurements can be performed, and their arithmetic mean can be taken as the compaction density ρ1.
[0090] In some embodiments, the negative electrode active layer 300b includes a first active layer and a second active layer, which are respectively disposed on opposite sides of the negative electrode current collector 300a in the thickness direction. A portion of the projection of the first active layer overlaps with the projection of the second active layer and is formed on the negative electrode double-sided region 320, while another portion of the projection of the first active layer is offset from the projection of the second active layer and is formed on the negative electrode single-sided region 310. The compaction density of the first active layer is different from that of the second active layer. The compaction density of the negative electrode active layer 300b located in the negative electrode double-sided region 320 is the average of the compaction density of the first active layer and the compaction density of the second active layer, while the compaction density of the negative electrode active layer 300b located in the negative electrode single-sided region 310 is the compaction density of the first active layer.
[0091] In this embodiment, the first active layer and the second active layer refer to two negative electrode active layers 300b formed on opposite sides of the negative electrode current collector 300a, and the two negative electrode active layers 300b can be prepared by different formulations or different compaction processes to make them have different compaction densities.
[0092] The first and second active layers are respectively disposed on opposite sides of the negative electrode current collector 300a in the thickness direction. They can be formed by double-sided coating, segmented coating, or sequential coating. In the wound and unfolded state, a portion of the area where the first and second active layers overlap on the plane projection corresponds to the negative electrode double-sided area 320, and another portion of the area where the first and second active layers are offset on the plane projection corresponds to the negative electrode single-sided area 310. The compaction densities of the first and second active layers are different, which can be adjusted by roller pressure, roller gap, drying conditions, or differences in slurry solid content.
[0093] For example, the first active layer can use a formulation with a high silicon-carbon content and high porosity, while the second active layer can use a formulation with a lower porosity or a higher binder ratio, in order to create a difference in compaction density while meeting the areal volume requirements. Alternatively, the first and second active layers can use the same active material system, but different compaction densities can be obtained by using different roller compaction parameters.
[0094] It should be noted that, since the compaction densities on both sides of the negative electrode double-sided region 320 are different, when measuring the compaction density of the negative electrode double-sided region 320, it is necessary to measure the first negative electrode active layer 300b and the second active layer separately. During the measurement process, multiple measurements can be taken at the first negative electrode active layer 300b, and their arithmetic mean can be taken as the compaction density of the first negative electrode active layer 300b. Multiple measurements can be taken at the second negative electrode active layer 300b, and their arithmetic mean can be taken as the compaction density of the second negative electrode active layer 300b. Then, the average of the compaction densities of the first negative electrode active layer 300b and the second negative electrode active layer 300b is taken as the compaction density ρ1.
[0095] In one possible implementation, the average porosity P1 of the negative electrode active layer 300b located in the single-sided negative electrode region 310 and the average porosity P2 of the negative electrode active layer 300b located in the double-sided negative electrode region 320 satisfy |P1-P2|≤5%. The average porosity P1 of the negative electrode active layer 300b located in the single-sided negative electrode region 310 satisfies: 30%≤P1≤45%. The average porosity P2 of the negative electrode active layer 300b located in the double-sided negative electrode region 320 satisfies: 28%≤P2≤40%.
[0096] For example, P1-P2 can be any one of -5%, -2%, 0, 1%, 2.5%, 4%, 5% or any two of the above values; P1 can be any one of 30%, 32%, 35%, 41%, 45% or any two of the above values; and P2 can be any one of 28%, 30%, 33%, 38%, 40% or any two of the above values.
[0097] In this embodiment, the average porosity is used to characterize the statistical result of the pore volume fraction inside the negative electrode active layer 300b. The average porosity can be defined as the ratio of the pore volume in the sample to the total volume of the negative electrode active layer 300b. The average porosity can reflect the comprehensive state of the liquid storage space, ion transport channels and compressible buffer space inside the negative electrode active layer 300b.
[0098] When the battery is in fast charging mode, if the average porosity difference between the negative electrode single-sided region 310 and the negative electrode double-sided region 320 is greater than 5%, if the porosity is too low, lithium-ion diffusion will be hindered, which will increase the local current density and increase the risk of lithium plating. If the porosity is too high, there will be too much electrolyte, which will aggravate side reactions. In this embodiment, the average porosity of the negative electrode single-sided region 310 and the negative electrode double-sided region 320 is less than or equal to 5%, which can control the average porosity of the two to be in a similar range. When the cell undergoes the first electrolyte injection, static wetting and subsequent cycling, the negative electrode single-sided region 310 and the negative electrode double-sided region 320 with similar porosity can absorb electrolyte at a closer rate and establish a stable interface, so that the two can achieve a more consistent electrolyte wetting degree, thereby avoiding the formation of local concentration polarization due to the large difference in the wetting degree of the negative electrode single-sided region 310 and the negative electrode double-sided region 320.
[0099] When the average porosity P1 of the negative electrode single-sided region 310 is less than 30%, a larger rolling force is required during rolling. Since one side of the negative electrode single-sided region 310 does not have a negative electrode active layer 300b for buffer support, the large rolling stress acts directly on the negative electrode current collector 300a, which can easily lead to problems such as curling deformation and microcracks in the negative electrode current collector 300a. This can result in severe gas production in the cell, cycle degradation, and lithium plating during fast charging. When the average porosity P1 of the negative electrode single-sided region 310 is greater than 45%, the negative electrode active layer 300b of the negative electrode single-sided region 310 will be too loose, and the negative electrode active layer 300b will easily fall off from the negative electrode current collector 300a. The poor continuity of the conductive network in the negative electrode single-sided region 310 will significantly increase the impedance of the negative electrode single-sided region 310, which will lead to uneven local current distribution in the negative electrode single-sided region 310, resulting in lithium plating in the inner layer of the cell.
[0100] Therefore, limiting P1 to 30% to 45% can avoid applying excessive roller pressure to the negative electrode single-sided region 310 due to over-compaction, thereby preventing curling deformation and microcracks in the negative electrode single-sided region 310, thus reducing the risk of lithium plating inside the cell. It can also avoid insufficient compaction of the negative electrode single-sided region 310, thereby reducing the interface impedance of the negative electrode single-sided region 310, thereby improving the current density distribution of the negative electrode single-sided region 310, and thus reducing the probability of lithium plating inside the cell.
[0101] In this embodiment, P2 is limited to 28% to 40%. When P2 is less than or equal to 40%, it can avoid insufficient compaction of the negative electrode active layer 300b in the negative electrode double-sided region 320 due to excessively high P2, thereby improving the energy density of the negative electrode sheet 300 and reducing the interface impedance and specific surface area of the negative electrode double-sided region 320, thereby improving the rate performance of the battery and reducing the risk of lithium plating in the battery.
[0102] When P2 is greater than or equal to 28%, the negative electrode active layer 300b of the negative electrode double-sided region 320 can be prevented from being over-compacted, so that the negative electrode active layer 300b retains a certain porosity structure. This provides space for the volume expansion of silicon-based materials during charging and discharging, provides sufficient channels for lithium-ion transport, and provides wetting space for electrolyte. In this way, the wetting effect and ion transport efficiency of electrolyte in the negative electrode double-sided region 320 can be improved, thereby reducing the risk of lithium plating in the battery and effectively alleviating the volume expansion problem of the battery during cycling.
[0103] It should be understood that porosity can be achieved by adjusting the particle size distribution of active materials, the ratio of conductive agent to binder, solvent evaporation conditions, coating thickness, and rolling process parameters, and these parameters can be adapted according to different negative electrode systems and winding specifications.
[0104] In practical implementation, the average porosity can be set through the formulation design of the negative electrode active layer 300b. The negative electrode active layer 300b can be composed of silicon-carbon composite particles, graphite particles, conductive agents, binders, and solvents. Among them, silicon-carbon composite particles provide high specific capacity, graphite particles provide skeletal support, conductive agents are used to establish an electron conduction network, and binders are used to maintain the adhesion between particles and form stable channels after rolling. By changing the solid content, binder content, or slurry rheological properties, the single-sided negative electrode region 310 can form a more suitable loose density and channel connectivity, while the double-sided negative electrode region 320 can obtain a porosity level close to that of the single-sided negative electrode region 310 while maintaining symmetrical pressure on both sides of the negative electrode active layer 300b.
[0105] The average porosity can be obtained by mercury intrusion method, image method, gas adsorption method or statistical analysis method based on cross-sectional micrograph. Samples can be taken from the single-sided region 310 and the double-sided region 320 of the negative electrode and measured at multiple points. The average value of the measurement results can then be calculated to obtain P1 and P2.
[0106] In some embodiments, the battery cell includes a flat region and arcuate regions located on opposite sides of the flat region, with the boundary line between the negative electrode double-sided region 320 and the negative electrode single-sided region 310 located in the flat region.
[0107] The flat area and the arc area together constitute the geometric division of the battery cell. The flat area refers to the relatively parallel area with small curvature changes after winding, while the arc area refers to the curved area formed at the end of the battery cell.
[0108] The boundary line between the negative electrode double-sided region 320 and the negative electrode single-sided region 310 refers to the dividing position where the negative electrode sheet 300 transitions from a single-sided coating to a double-sided coating along its length. The boundary line between the negative electrode double-sided region 320 and the negative electrode single-sided region 310 is arranged in a straight region, which allows the boundary line to be located in a position with less bending stress. Furthermore, its spatial offset from the arc region ensures that the boundary position between the negative electrode double-sided region 320 and the negative electrode single-sided region 310 avoids the arc region. This prevents structural abrupt changes between the negative electrode single-sided region 310 and the negative electrode double-sided region 320 due to variations in thickness, compaction state, or pore distribution from being superimposed on bending stress. This, in turn, helps to reduce stress concentration and local fatigue risk at the boundary between the negative electrode double-sided region 320 and the negative electrode single-sided region 310.
[0109] In practical implementation, in order to achieve a layout where the boundary line is located in the straight area, the negative electrode sheet 300 can pre-set the end position of the negative electrode single-sided area 310 during the cutting, coating or winding arrangement stage, so that the starting position of the negative electrode double-sided area 320 corresponds to the straight area after winding. Equivalent arrangement can also be achieved through winding tension control, length compensation or local coating boundary correction.
[0110] Reference Figure 5 As shown, in one possible implementation, the negative electrode single-sided region 310 includes a first embossed region 311, which has a first concave-convex portion. The negative electrode double-sided region 320 includes a second embossed region 321 and a second clearance region 322. The second embossed region 321 has a second concave-convex portion. The first concave-convex portion includes a first concave portion and a first convex portion. The second concave-convex portion includes a second concave portion and a second convex portion. Both the first concave portion and the second concave portion are recessed from the side of the negative electrode sheet 300 away from the winding center to the side closer to the winding center. The recess depth H1 of the first concave portion is greater than the recess depth H2 of the second concave portion. And / or, the negative electrode single-sided region 310 further includes a first clearance region 312, with the two first clearance regions 312 located on both sides of the first embossed region 311 along the width direction of the negative electrode sheet 300. And / or, the negative electrode double-sided region 320 further includes a second clearance region 322, the two second clearance regions 322 being located on both sides of the second embossed region 321 along the width direction of the negative electrode sheet 300. And / or, the negative electrode double-sided region 320 further includes a third clearance region 323, the third clearance region 323 being located on the side of the second embossed region 321 opposite to the negative electrode single-sided region 310.
[0111] In this embodiment, the first embossed area 311 is a partial embossed area disposed within the negative electrode single-sided area 310. The first uneven portion is used to construct local undulations on the negative electrode single-sided area 310 and to create micro gaps between adjacent layers after the negative electrode single-sided area 310 is wound. The second embossed area 321 is a partial embossed area disposed within the negative electrode double-sided area 320. The second uneven portion formed thereon is used to construct local undulations on the negative electrode double-sided area 320 and to create interlayer gaps between adjacent separators 200 after the negative electrode double-sided area 320 is wound.
[0112] The first recess is a recessed structure that recedes towards the winding center relative to its plane. A first protrusion is arranged alternately with the first recess to form a periodic or aperiodic protrusion structure. The protrusion height of the first protrusion can be coordinated with the recess depth of the first recess. The second recess is also a recessed structure that recedes towards the winding center relative to its plane. A second protrusion is arranged alternately with the second recess to form a periodic or aperiodic protrusion structure. The protrusion height of the second protrusion can be coordinated with the recess depth of the second recess.
[0113] Compared to the second recess, the first recess has a larger indentation relative to the reference plane, which gives the negative electrode single-sided region 310 stronger mechanical buffering and deformation absorption capabilities. The first recess and the first protrusion allow the negative electrode single-sided region 310 to undergo pre-deformation, appropriately increasing the elongation of the negative electrode current collector 300a in the negative electrode single-sided region 310, and forming internal stress opposite to the direction of the curling internal stress, thereby resisting the bending deformation of the negative electrode single-sided region 310 and effectively improving the curling problem of the negative electrode single-sided region 310. The structure of the negative electrode double-sided region 320 is relatively stable, and this region usually corresponds to the effective reaction area of the cell, which has high requirements for ion transport and interface contact stability. There is no need to relieve stress through a deep second recess; an excessively deep second recess may become the starting point for crack initiation.
[0114] It should be understood that the first embossed area 311 and the second embossed area 321 are still composed of the negative electrode current collector 300a and the negative electrode active layer 300b thereon. The material composition of the local area after embossing remains unchanged, only its surface morphology and local compaction state change.
[0115] The first clearance zone 312, the second clearance zone 322, and the third clearance zone 323 are all areas that have not been embossed. The first clearance zone 312 is located on both sides of the width direction of the first embossed zone 311, the second clearance zone 322 is located on both sides of the width direction of the second embossed zone 321, and the third clearance zone 323 is located on the side of the second embossed zone 321 that is away from the negative electrode single-sided area 310. Their function is to provide a transition buffer for the edge of the embossed zone and release the end stress, so as to avoid cracking of the negative electrode active layer 300b, warping of the negative electrode current collector 300a, or cracking and warping of the negative electrode tab 300c caused by geometrical abrupt changes at the embossed boundary.
[0116] In summary, when the negative electrode sheet 300 is wound, the first embossed area 311 and the second embossed area 321 sequentially move into their corresponding positions along with the negative electrode sheet 300. Since the depth H1 of the first concave portion is greater than the depth H2 of the second concave portion, the single-sided negative electrode area 310 will form a larger local deformation space and buffer space in the inner layer of the cell after winding, thereby more effectively alleviating the bending stress of the single-sided negative electrode area 310 and absorbing the expansion stress generated by the single-sided negative electrode area 310. When the first concave portion and the first convex portion, as well as the second concave portion and the second convex portion are alternately distributed, the interlayer gap of the cell can be increased, thereby improving the electrolyte wetting effect of the single-sided negative electrode area 310 and the double-sided negative electrode area 320. Furthermore, the first clearance zone 312 can prevent powder shedding from the negative electrode single-sided region 310 due to pressure acting on both sides of the negative electrode double-sided region 320 in the width direction during the formation of the first concave-convex part. The second clearance zone 322 can prevent pressure acting on both sides of the negative electrode double-sided region 320 in the width direction during the formation of the second concave-convex part, thereby preventing powder shedding from the negative electrode double-sided region 320. Since the third clearance zone 323 corresponds to the outer layer of the cell after winding, the third clearance zone 323 is not embossed to avoid increasing the interlayer gap of the outer layer of the cell, thereby avoiding lithium plating on the outer layer of the cell in the later stages of cycling.
[0117] Reference Figure 5 As shown, in one possible implementation, the recess depth H1 of the first recess and the recess depth H2 of the second recess satisfy: 1 / 3≤H2 / H1≤1 / 2; and / or, the recess depth H1 of the first recess satisfies: 20μm≤H1≤80μm; and / or, the recess depth H2 of the second recess satisfies: 20μm≤H2≤60μm; and / or, in the length direction of the negative electrode sheet 300, the length L1 of the negative electrode single-sided region 310 and the length L2 of the third clearance region 323 satisfy: L2≥1.25*L1.
[0118] For example, the depth H1 of the first recess can be any one of 20μm, 30μm, 40μm, 50μm, 60μm, and 80μm, or fall within any two of these values. The depth H2 of the second recess can be any one of 20μm, 25μm, 40μm, 45μm, 55μm, and 60μm, or fall within any two of these values. The depth of the first recess is measured using a high-precision microscope or a three-dimensional profilometer. The morphology of the first embossed area 311 is measured, and the point height is tested. Any area of the first embossed area 311 is randomly selected, and the depths of multiple first recesses within that area are quantitatively measured and their arithmetic mean is calculated.
[0119] In this embodiment, the first recess corresponds to the first embossed area 311 in the single-sided negative electrode area 310, and the second recess corresponds to the second embossed area 321 in the double-sided negative electrode area 320. Both are recessed from the side of the negative electrode sheet 300 away from the winding center to the side closer to the winding center. The fit and pressure buffering capacity of the negative electrode sheet 300 after winding are adjusted by different recess depths.
[0120] When the depth ratio of the first recess to the second recess is limited to between 1 / 3 and 1 / 2, the recess depth of the first recess can be greater than that of the second recess, effectively alleviating the curling stress, bending stress, and expansion stress of the negative electrode single-sided region 310, and improving the interfacial contact performance of the negative electrode double-sided region 320. The third clearance region 323 is located on the side of the second embossed region 321 away from the negative electrode single-sided region 310, and its length L2 is not less than 1.25 times the length L1 of the negative electrode single-sided region 310, so as to reserve a more sufficient un-embossed area at the winding tail end of the negative electrode sheet 300, thereby reducing the stacking and boundary abruptness at the winding tail end, and improving the ion supply uniformity and structural stability near the winding tail end of the negative electrode sheet 300.
[0121] Thus, during the liquid injection, formation, and cycling processes, the differentiated depressions of the first and second recesses allow the single-sided region 310 and the double-sided region 320 of the negative electrode to undertake different degrees of expansion buffering and support. The third clearance region 323 forms a longer transition buffer section at the winding end of the negative electrode sheet 300 to stabilize the stress state of the negative electrode sheet 300, thereby suppressing the increase of local polarization, reducing uneven distribution of electrolyte, and reducing the stress concentration and lithium plating risk caused by the expansion of silicon-based materials.
[0122] In some embodiments, when H1 is in the range of 20 μm to 80 μm and H2 is in the range of 20 μm to 60 μm, and H2 / H1 is between 1 / 3 and 1 / 2, the negative electrode single-sided region 310 and the negative electrode double-sided region 320 can form a relatively stable thickness gradient and compaction density gradient after winding.
[0123] Reference Figure 6 and Figure 7As shown, in one possible implementation, the positive electrode 100 includes a double-sided positive electrode region 120 and a single-sided positive electrode region 110 adjacent to each other along its length direction, with at least a portion of the single-sided positive electrode region 110 wound around the outermost ring of the positive electrode 100; the double-sided positive electrode region 120 includes a third embossed region 121, a fourth clearance region 122, a fifth clearance region 123, and a sixth clearance region 124, with the two fourth clearance regions 122 located on both sides of the third embossed region 121 along the width direction of the positive electrode 100, and the fifth clearance region 123 and the sixth clearance region 124 located on both sides of the third embossed region 121 along the length direction of the positive electrode 100, with the fifth clearance region 123 close to the single-sided positive electrode region. 110 is configured; the third embossing area 121 is provided with a third concave-convex portion, which includes a third concave portion and a third convex portion. The third concave portion is recessed from the side of the positive electrode sheet 100 away from the winding center to the side closer to the winding center. The concavity depth H3 of the third concave portion satisfies: 10μm≤H3≤60μm; and / or, in the length direction of the positive electrode sheet 100, the length L3 of the fifth clearance area 123 and the length L4 of the positive electrode single-sided area 110 satisfy: L3≥0.75*L4; and / or, in the length direction of the positive electrode sheet 100, the length L5 of the sixth clearance area 124 and the length L4 of the positive electrode single-sided area 110 satisfy: L5≥0.5*L4.
[0124] In this embodiment, the positive electrode 100 is the positive electrode structure in the battery cell used to react with the negative electrode 300. The positive electrode 100 is composed of a positive current collector and a positive active layer coated on the surface of the positive current collector. The positive double-sided region 120 refers to the region where the positive current collector has a positive active layer on both sides in the thickness direction. The positive single-sided region 110 refers to the region where the positive current collector forms a positive active layer only on the side near the winding center. At least part of the positive single-sided region 110 is wound around the outermost ring of the positive electrode 100 to give the outer layer of the battery cell a more stable coating and support relationship.
[0125] The positive electrode double-sided region 120 is configured with a third embossed region 121, a fourth void region 122, a fifth void region 123, and a sixth void region 124. The two fourth void regions 122 are located on either side of the third embossed region 121 along the width direction of the positive electrode sheet 100, while the fifth void regions 123 and 124 are located on either side of the third embossed region 121 along the length direction of the positive electrode sheet 100. The fifth void region 123 is located close to the positive electrode single-sided region 110. The third concave-convex portion on the third embossed region 121 includes a third concave portion and a third convex portion. The third concave portion is recessed from the side of the positive electrode sheet 100 away from the winding center towards the side closer to the winding center, forming a space for electrolyte retention and stress relief during winding and cyclic expansion. The concavity depth H3 of the third concave portion is controlled within the range of 10 μm to 60 μm, balancing local support strength and pore channel continuity.
[0126] Along the length of the positive electrode 100, the length L3 of the fifth clearance region 123 and the length L4 of the single-sided positive electrode region 110 satisfy L3≥0.75*L4, so that a sufficient buffer distance and transition length are formed between the single-sided positive electrode region 110 and the double-sided positive electrode region 120, reducing the thickness abruptness and stress concentration between the single-sided positive electrode region 110 and the double-sided positive electrode region 120. Moreover, after winding, the fifth clearance region 123 is located on the outermost layer of the positive electrode 100 and close to the winding tail of the positive electrode 100. The presence of the fifth clearance region 123 can reduce the unevenness of the outermost positive electrode 100, thereby improving the interfacial contact performance of the outermost positive electrode 100 and reducing the risk of lithium plating at the winding tail of the negative electrode 300.
[0127] Along the length of the positive electrode 100, the length L5 of the sixth clearance region 124 and the length L4 of the positive electrode single-sided region 110 satisfy L5≥0.5*L4. In this way, the sixth clearance region 124 can be located in the innermost layer of the positive electrode 100 after winding. The presence of the sixth clearance region 124 can reduce the stress of the innermost positive electrode 100, so as to avoid the superposition of bending stress, curling stress and stress generated by embossing, which would affect the structural strength and electrochemical performance of the innermost positive electrode 100.
[0128] When the depth H3 of the third recess is between 10 μm and 60 μm, if the depth is too small, the third embossing region 121 will not be able to effectively provide buffer and liquid storage space; if the depth is too large, it will easily weaken the local mechanical strength of the positive electrode 100 and increase the risk of molding defects.
[0129] When the positive electrode sheet 100 is wound, it is wound layer by layer around the winding center, with at least a portion of the single-sided positive electrode area 110 located on the outermost ring. This ensures that the outermost positive electrode sheet 100 of the cell is adjacent to the external space in a single-sided coating form, while the double-sided positive electrode area 120 is wound inside the single-sided positive electrode area 110. The third embossing area 121 in the double-sided positive electrode area 120 provides local support and stress relief space, and generates compressible deformation in the thickness direction of the positive electrode sheet 100, reducing the contact pressure between the outer and inner rings and preventing local wear or warping caused by high-voltage contact between adjacent rings. Since the fifth clearance area 123 is close to the single-sided positive electrode area 110 and its length forms a preset proportional relationship with the single-sided positive electrode area 110, a smooth transition can be achieved between the double-sided positive electrode area 120 and the single-sided positive electrode area 110, thereby improving the interlayer stress, thickness variation, and electrolyte wetting effect near the winding tail of the positive electrode sheet 100. At the same time, the sixth evacuation zone 124 can provide a transition margin on the other side of the third embossing zone 121. In this way, the cell can maintain a more stable outer ring coating state and a more continuous ion channel, reduce local concentration polarization, and thus reduce the risk of lithium plating in the battery.
[0130] It should be noted that when determining the range of the second embossed area 321, the area enclosed by the outermost edge of the second concave and convex portion is defined as the second embossed area 321, and a similar method can be used for the first embossed area 311.
[0131] In one possible implementation, the diameter D1 of the first protrusion satisfies: 0.5mm ≤ D1 ≤ 10mm; and / or, the diameter D2 of the second protrusion satisfies: 0.5mm ≤ D2 ≤ 10mm; and / or, the diameter D3 of the third protrusion satisfies: 1mm ≤ D3 ≤ 15mm; and / or, the diameter D1 of the first protrusion and the distance T1 between two adjacent first protrusions satisfy: D1 < T1; and / or, the diameter D2 of the second protrusion and the distance T2 between two adjacent second protrusions satisfy: D2 < T2; and / or, the diameter D3 of the third protrusion and the distance T3 between two adjacent third protrusions satisfy: D3 < T3; and / or, the depth H2 of the second concave portion and the depth H3 of the third concave portion satisfy: H2 > H3.
[0132] For example, the diameter D1 of the first protrusion can be any one of 0.5mm, 1mm, 0.5mm, 2mm, 3.5mm, 5mm, 8mm, and 10mm, or somewhere in between. The diameter D2 of the second protrusion can be any one of 0.5mm, 1.5mm, 2.5mm, 4mm, 5mm, 6mm, 9mm, and 10mm, or somewhere in between. The diameter D3 of the third protrusion can be any one of 1mm, 1.5mm, 5mm, 8mm, 9mm, 10mm, 12mm, and 15mm, or somewhere in between.
[0133] The first convex portion corresponds to the protruding structure within the single-sided negative electrode region 310, the second convex portion corresponds to the protruding structure within the double-sided negative electrode region 320, and the third convex portion corresponds to the protruding structure within the double-sided positive electrode region 120. The function of the first, second, and third convex portions is to form local support points and electrolyte storage spaces distributed on the surfaces of the negative electrode sheet 300 and the positive electrode sheet 100 after winding, so that the negative electrode sheet 300 and the positive electrode sheet 100 can still maintain appropriate electrolyte channels after being compressed, and to avoid abrupt changes in thickness due to excessively large protruding structures, or squeezing interference between adjacent protruding structures due to excessively dense protruding structures.
[0134] The first, second, and third protrusions can be circular, elliptical, spherical, strip-shaped, or protrusions composed of multiple geometric units.
[0135] Since the diameter D1 of the first protrusion is limited to 0.5 mm to 10 mm, the diameter D2 of the second protrusion is limited to 0.5 mm to 10 mm, so that it can form effective local support without significantly weakening the rollability of the negative electrode 300, and the diameter D3 of the third protrusion is limited to 1 mm to 15 mm, so that it can form effective local support without significantly weakening the rollability of the positive electrode 100.
[0136] The distance T1 between two adjacent first protrusions is greater than D1, the distance T2 between two adjacent second protrusions is greater than D2, and the distance T3 between two adjacent third protrusions is greater than D3. This ensures that the adjacent protruding structures do not contact or overlap each other, thereby avoiding a reduction in the structural strength of the negative electrode 300 and the positive electrode 100. The depth H2 of the second concave part is greater than the depth H3 of the third concave part, indicating that the embossing of the negative electrode double-sided region 320 is deeper than that of the positive electrode double-sided region 120. This is beneficial for providing stronger liquid storage and buffering capacity on the negative electrode side to adapt to the more significant volume expansion of silicon-based materials during cycling.
[0137] Because the second recess is deeper than the third recess, the second embossed region 321 can form a more significant buffer space to absorb the local stress caused by the expansion of the silicon-based material. Meanwhile, the positive electrode double-sided region 120 maintains a relatively shallow third concave-convex portion to balance the areal density difference and winding stress distribution between the positive electrode 100 and the negative electrode 300. Therefore, the positive electrode 100 can maintain a more stable geometric state and ion transport channels during winding, wetting, and cycling, reducing the probability of local contact imbalance, increased polarization, and interface drying, and avoiding capacity decay and cycle fatigue caused by excessively dense first recesses or mismatched recess depths.
[0138] In some embodiments, the positive electrode active layer may include a ternary polycrystalline material Li(Nix1Coy1Mnz1)O2, wherein the contents of Ni, Co, and Mn satisfy the following relationship: x1 + y1 + z1 = 1, 3 <x1<0.98,0<y1<0.3,0<z1<0.3。
[0139] In some embodiments, the average particle size of the polycrystalline ternary material can be controlled between 8 μm and 25 μm. It can be modified by doping with any one of the cations Mg, Al, Ti, Zr, Cr, Y, and Zn, or by doping with the anion F, or by mixed doping with cations and anions, or by coating with any one of the oxides MgO, ZrO2, TiO2, and Al2O3, or by coating with any one of the non-oxides AlPO4, LiAlO2, LiTiO2, and AlF3.
[0140] Reference Figures 2 to 5As shown, in some embodiments, the negative electrode sheet 300 further includes a negative electrode empty foil region 330. The negative electrode empty foil region 330, the negative electrode single-sided region 310, and the negative electrode double-sided region 320 are arranged sequentially along the length direction of the negative electrode sheet 300, and the end of the negative electrode empty foil region 330 facing away from the negative electrode single-sided region 310 constitutes the winding start end of the negative electrode sheet 300. (Refer to...) Figure 6 , Figure 7 As shown, the positive electrode 100 also includes a positive electrode empty foil region 130. The positive electrode empty foil region 130, the positive electrode single-sided region 110 and the positive electrode double-sided region 120 are arranged sequentially along the length direction of the positive electrode 100, and the end of the positive electrode empty foil region 130 away from the positive electrode single-sided region 110 constitutes the winding tail end of the positive electrode 100.
[0141] The following describes the preparation process and related tests of the battery in Example 1.
[0142] I. Preparation of Positive Electrode 100
[0143] Ternary materials, polyvinylidene fluoride (PVDF), and conductive agent (Super P) are dissolved in N-methylpyrrolidone (NMP) in a ratio of 97.6:1.05:1.35 and stirred evenly to form a slurry. The slurry is then uniformly coated onto aluminum foil, with some aluminum foil being coated on both sides and others on one side. After drying, rolling, and die-cutting, a positive electrode sheet 100 is formed.
[0144] II. Preparation of negative electrode 300
[0145] Silicon-carbon composite material, graphite, conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber were mixed in a ratio of 15:80.8:1.2:1.0:2.0. The mixture was then stirred in deionized water to form a slurry, which was then uniformly coated onto both surfaces of a copper foil. Part of the copper foil was coated on both sides to form a negative electrode double-sided region 320, and part was coated on one side to form a negative electrode single-sided region 310. After drying, rolling, die-cutting, and slitting, an integral structure of negative electrode tabs 300c and negative electrode current collectors 300a was obtained. Multiple negative electrode tabs 300c are led out from the negative electrode double-sided region 320. The mass fraction of silicon in the negative electrode active layer 300b, based on the total mass of the negative electrode active layer 300b on either side of the negative electrode current collector 300a, is 8%.
[0146] III. Battery Assembly
[0147] A battery is obtained by stacking and winding the positive electrode 100, separator 200, and negative electrode 300 together, and then performing processes such as encapsulation, electrolyte injection, secondary sealing, formation, and sorting.
[0148] Among them, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.1 g / cm³. 3 The compaction density ρ2 of the negative electrode single-sided region 310 is 1 g / cm³.3 ρ1 / ρ2 is 1.1.
[0149] Example 2
[0150] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 0.85 g / cm³. 3 .
[0151] Example 3
[0152] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.2 g / cm³. 3 .
[0153] Example 4
[0154] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.55 g / cm³. 3 The compaction density ρ2 of the negative electrode single-sided region 310 is 1.45 g / cm³. 3 .
[0155] Example 5
[0156] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1 g / cm³. 3 The compaction density ρ2 of the negative electrode single-sided region 310 is 0.9 g / cm³. 3 .
[0157] Comparative Example 1
[0158] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.55 g / cm³. 3 .
[0159] Comparative Example 2
[0160] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.1 g / cm³. 3 The compaction density ρ2 of the negative electrode single-sided region 310 is 0.9 g / cm³. 3 .
[0161] Comparative Example 3
[0162] Unlike Example 1, the compaction density ρ1 of the negative electrode double-sided region 320 is 1.1 g / cm³. 3 The compaction density ρ2 of the negative electrode single-sided region 310 is 1.45 g / cm³. 3 .
[0163] Comparative Example 4
[0164] Unlike Embodiment 1, a negative electrode tab 300c is provided on the negative electrode single-sided region 310.
[0165] Lithium plating test
[0166] Test method: The batteries obtained in the above examples and comparative examples were placed at 25±2℃ and left to stand for 10 min; discharged at 0.2C to the lower limit voltage of 3V and left to stand for 5 min; fully charged at 0.8C with a cutoff current of 0.05C and left to stand for 10 min; discharged at 0.2C to the lower limit voltage.
[0167] Cyclic conditions: Charge at a constant current of 2C to 4.3V, then charge at a constant current of 1.5C to 4.45V, and finally charge at a constant current of 0.5C to the upper limit voltage of 4.55V (cutoff current 0.05C), and then discharge at a constant current of 0.5C to the lower limit voltage of 3C. Rest for 5 minutes between each charge and discharge step.
[0168] The above cyclic conditions were repeated 600 times to conclude the test, and the cells were then dissected to observe whether lithium plating occurred on the single-sided region 310 and the double-sided region 320 of the negative electrode. Ten cells were tested in each group. The lithium plating test rate X = number of cells without lithium plating in the single-sided region 310 of the negative electrode / total number of cells tested. The lithium plating test rate Y = number of cells without lithium plating in the double-sided region 320 of the negative electrode / total number of cells tested.
[0169] Table 1 Battery parameters and test results
[0170]
[0171] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A battery, characterized in that, include: A battery cell, comprising: a positive electrode, a separator, and a negative electrode, wherein the positive electrode, the separator, and the negative electrode are wound around a winding center, and the negative electrode comprises a negative electrode single-sided region and a negative electrode double-sided region adjacent to each other along its own length direction, wherein the end of the negative electrode double-sided region away from the negative electrode single-sided region constitutes the winding termination end of the negative electrode. The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed along its own thickness direction, and a negative electrode tab extending from one side of the negative electrode current collector in the width direction. Multiple negative electrode tabs are spaced apart along the length direction of the negative electrode current collector, and are stacked and interconnected in the cell thickness direction. The negative electrode active layer comprises a silicon-based material, and the mass fraction of silicon in the negative electrode active layer, based on the total mass of the negative electrode active layer on any side of the negative electrode current collector, is greater than or equal to 5%. In the single-sided negative electrode region, the negative electrode active layer is formed on the side of the negative electrode current collector away from the winding center. In the double-sided negative electrode region, the negative electrode active layer is formed on opposite sides in the thickness direction of the negative electrode current collector. All the negative electrode tabs correspond to the negative electrode current collector in the double-sided negative electrode region. The compaction density ρ1 of the negative electrode active layer located in the double-sided region of the negative electrode and the compaction density ρ2 of the negative electrode active layer located in the single-sided region of the negative electrode satisfy the following condition: 0.85≤ρ1 / ρ2≤1.
2.
2. The battery according to claim 1, characterized in that, The compaction density p1 of the negative electrode active layer in the negative electrode double-faced region satisfies: 1 g / cm 3 ≤ p1 ≤ 1.55 g / cm 3 ; And / or, the compaction density ρ2 of the negative electrode active layer located in the negative electrode single-sided region satisfies: 0.9 g / cm³ 3 ≤ρ2≤1.45g / cm 3 .
3. The battery according to claim 1, characterized in that, On the negative electrode double-sided region, the compaction density of the negative electrode active layer located on both sides of the negative electrode current collector is the same.
4. The battery according to claim 1, characterized in that, The negative electrode active layer includes a first active layer and a second active layer, which are respectively disposed on opposite sides of the negative electrode current collector in the thickness direction. A portion of the projection of the first active layer overlaps with the projection of the second active layer and is formed on the negative electrode double-sided region. Another portion of the projection of the first active layer is offset from the projection of the second active layer and is formed on the negative electrode single-sided region. The compaction density of the first active layer is different from that of the second active layer. The compaction density of the negative electrode active layer located in the negative electrode double-sided region is the average of the compaction densities of the first and second active layers. The compaction density of the negative electrode active layer located in the negative electrode single-sided region is the compaction density of the first active layer.
5. The battery according to claim 1, characterized in that, The average porosity P1 of the negative electrode active layer located in the single-sided region of the negative electrode and the average porosity P2 of the negative electrode active layer located in the double-sided region of the negative electrode satisfy |P1-P2|≤5%; And / or, the average porosity P1 of the negative electrode active layer located in the negative electrode single-sided region satisfies: 30% ≤ P1 ≤ 45%; And / or, the average porosity P2 of the negative electrode active layer located in the negative electrode double-sided region satisfies: 28% ≤ P2 ≤ 40%.
6. The battery according to claim 1, characterized in that, The battery cell includes a flat region and arc regions located on opposite sides of the flat region, and the boundary line between the negative electrode double-sided region and the negative electrode single-sided region is located in the flat region.
7. The battery according to claim 1, characterized in that, The negative electrode single-sided area includes a first embossed area, which has a first concave-convex portion. The negative electrode double-sided area includes a second embossed area, which has a second concave-convex portion. The first concave-convex portion includes a first concave portion and a first convex portion. The second concave-convex portion includes a second concave portion and a second convex portion. Both the first concave portion and the second concave portion are recessed from the side of the negative electrode sheet away from the winding center to the side closer to the winding center. The recess depth H1 of the first recess is greater than the recess depth H2 of the second recess; And / or, the negative electrode single-sided area further includes a first clearance area, and the two first clearance areas are respectively located on both sides of the first embossed area along the width direction of the negative electrode sheet; And / or, the negative electrode double-sided region further includes a second clearance region, and the two second clearance regions are respectively located on both sides of the second embossed region along the width direction of the negative electrode sheet; And / or, the negative electrode double-sided region further includes a third clearance region, which is located on the side of the second embossed region away from the negative electrode single-sided region.
8. The battery according to claim 7, characterized in that, The recess depth H1 of the first recess and the recess depth H2 of the second recess satisfy: 1 / 3≤H2 / H1≤1 / 2; And / or, the recess depth H1 of the first recess satisfies: 20μm≤H1≤80μm; And / or, the recess depth H2 of the second recess satisfies: 20μm≤H2≤60μm; And / or, in the length direction of the negative electrode sheet, the length L1 of the negative electrode single-sided area and the length L2 of the third clearance area satisfy: L2≥1.25*L1.
9. The battery according to claim 7, characterized in that, The positive electrode sheet includes a positive electrode double-sided region and a positive electrode single-sided region adjacent to each other along its own length direction, and at least a portion of the positive electrode single-sided region is wound around the outermost ring of the positive electrode sheet; The positive electrode double-sided region includes a third embossed region, a fourth clearance region, a fifth clearance region, and a sixth clearance region. The two fourth clearance regions are respectively located on both sides of the third embossed region along the width direction of the positive electrode sheet. The fifth clearance region and the sixth clearance region are located on both sides of the third embossed region along the length direction of the positive electrode sheet. The fifth clearance region is located close to the positive electrode single-sided region. The third embossing area is provided with a third concave-convex portion, which includes a third concave portion and a third convex portion. The third concave portion is recessed from the side of the positive electrode sheet away from the winding center to the side closer to the winding center. The recess depth H3 of the third recess satisfies: 10μm≤H3≤60μm; and / or, in the length direction of the positive electrode sheet, the length L3 of the fifth clearance area and the length L4 of the positive electrode single-sided area satisfy: L3≥0.75*L4; and / or, in the length direction of the positive electrode sheet, the length L5 of the sixth clearance area and the length L4 of the positive electrode single-sided area satisfy: L5≥0.5*L4.
10. The battery according to claim 9, characterized in that, The diameter D1 of the first protrusion satisfies: 0.5mm ≤ D1 ≤ 10mm; And / or, the diameter D2 of the second protrusion satisfies: 0.5mm≤D2≤10mm; And / or, the diameter D3 of the third protrusion satisfies: 1mm≤D3≤15mm; And / or, the diameter D1 of the first protrusion and the distance T1 between two adjacent first protrusions satisfy: D1 < T1; And / or, the diameter D2 of the second protrusion and the distance T2 between two adjacent second protrusions satisfy: D2 < T2; And / or, the diameter D3 of the third protrusion and the distance T3 between two adjacent third protrusions satisfy: D3 < T3; And / or, the recess depth H2 of the second recess and the recess depth H3 of the third recess satisfy: H2 > H3.