A bismuth iodide-based core-shell structured sulfide solid electrolyte, its preparation and application
By generating a composite interface protective layer of LiBiS2 and LiI through high-temperature vapor phase coating, the problem of poor interface compatibility between sulfide solid electrolyte and lithium metal anode is solved, and the air stability of electrolyte and battery cycle performance are improved.
Patent Information
- Application Number
- CN202611576302.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing sulfide solid electrolytes have poor interfacial compatibility with lithium metal anodes, which easily leads to electrochemical side reactions, resulting in high-impedance interfacial byproducts and lithium dendrite growth, affecting the cycle life and safety of all-solid-state lithium batteries.
A high-temperature vapor-phase coating method is used to react bismuth iodide with a sulfide solid electrolyte under inert gas protection to generate a composite interface protective layer of LiBiS2 and LiI. The interface damage is repaired by the dynamic migration of LiI, and the lithium deposition is stabilized by LiBiS2, thus achieving interface protection and lithium dendrite suppression.
It improves the air stability and cycle stability of sulfide electrolytes, enhances the voltage window of the battery, suppresses lithium dendrite growth, and improves the performance of all-solid-state lithium batteries.
Smart Images

Figure CN123120849A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy battery materials technology, and in particular to a bismuth iodide-based core-shell structured sulfide solid electrolyte and its preparation and application. Background Technology
[0002] Sulfide solid electrolytes are core materials for high-safety, high-energy-density all-solid-state lithium batteries due to their excellent room-temperature lithium-ion conductivity and flexible adaptability. However, sulfide solid electrolytes have inherent technical defects. They have poor interface compatibility with lithium metal anodes and are prone to electrochemical side reactions, producing high-impedance interface byproducts that significantly increase the battery interface impedance. At the same time, uniform lithium deposition cannot be achieved on the electrolyte surface, which easily induces lithium dendrite growth, leading to problems such as battery cycle life degradation and short-circuit failure, which seriously restricts the industrial application of all-solid-state lithium batteries.
[0003] Currently, the industry mainly optimizes the interfacial properties of sulfide electrolytes through surface coating modification. Existing modification processes are mainly of two types: liquid phase coating and solid-phase powder reaction coating. Among them, liquid phase coating process relies on organic solvents, which are prone to corroding the sulfide electrolyte matrix. It also has the problems of solvent residue and introduction of impurities, which reduce the purity and conductivity of the electrolyte. Traditional solid-phase powder blending reaction coating can only achieve local reaction at the contact sites of powder particles. It has the defects of uneven coating, incomplete coating, and excessively thick local coating layers. Moreover, the reaction is prone to continuously eroding the electrolyte bulk phase structure, destroying the intrinsic crystal structure of the electrolyte, and significantly reducing its ion conduction performance.
[0004] In addition, most existing coating technologies can only achieve single passivation protection or single lithium deposition regulation functions, and cannot simultaneously solve the two core problems of interface side reactions and lithium dendrite growth, resulting in limited modification effects and improvements.
[0005] In summary, existing sulfide electrolyte modification technologies generally suffer from drawbacks such as poor coating uniformity, severe matrix damage, limited modification function, complex processes, and high costs. There is an urgent need to develop an in-situ modification technology that is simple to process, has uniform coating, causes no matrix damage, and can simultaneously achieve interface protection and lithium dendrite suppression. Summary of the Invention
[0006] The present invention aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, the object of the present invention is to provide a bismuth iodide-synthesized core-shell structured sulfide solid electrolyte, its preparation, and its application.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect of the present invention, there is provided a method for preparing a bismuth iodide-synthesized core-shell structured sulfide solid electrolyte, specifically comprising: placing bismuth iodide and a sulfide solid electrolyte into a tube furnace under the protection of an inert gas, then evacuating, heating up and holding the temperature, followed by furnace cooling to obtain the core-shell structured sulfide solid electrolyte.
[0008] In some embodiments of the present invention, the mass ratio of the sulfide solid electrolyte to bismuth iodide is 2-5:1.
[0009] In some embodiments of the present invention, the heating rate is 2-4°C / min.
[0010] In some embodiments of the present invention, the vacuum degree after evacuation is 1-3 Pa.
[0011] In some embodiments of the present invention, the holding temperature is 400~600°C, and the holding time is 1-3 h.
[0012] In some embodiments of the present invention, the sulfide electrolyte is Li (7-a) PS (6-a) X a ; wherein 0<a≤1, and X is selected from one or more of Cl, Br and I.
[0013] In a second aspect of the present invention, there is provided the core-shell structured sulfide solid electrolyte prepared by the preparation method described in the above aspect, which comprises a sulfide electrolyte and a composite layer of lithium bismuthide and lithium iodide coating the sulfide electrolyte.
[0014] In a third aspect of the present invention, there is provided an application of the sulfide solid electrolyte described in the above aspects in an all-solid-state lithium battery.
[0015] Beneficial effects of the present invention: The present invention provides a bismuth iodide-synthesized core-shell structured sulfide solid electrolyte as well as its preparation method and application. The preparation method of the present invention achieves the following effects: 1. The air stability of the sulfide electrolyte is effectively improved, and the retention rate of ionic conductivity after 24 h is increased from 33.75% to 53.25%; 2. Under different forming pressures, the sulfide electrolyte prepared by the present invention can effectively improve the cycle stability of the solid-state battery and inhibit capacity attenuation; under the low-pressure forming working condition, the cycle performance gain brought by the modification is more significant; 3. The process of the present invention can retain the sulfide electrolyte matrix, and the obtained coating layer has uniform element distribution; 4. Compared with pure LPSC, the voltage window of the sulfide electrolyte prepared by the present invention is increased by about 0.25 V. Brief Description of the Drawings
[0016] Figure 1 The image shows the XRD pattern of the sample prepared in Example 1.
[0017] Figure 2 The image shows the EDS scan result of the sulfur element in the sample prepared in Example 1.
[0018] Figure 3 The image shows the EDS scan result of element I in the sample prepared in Example 1.
[0019] Figure 4 The image shows the EDS scan results of the Bi element in the sample prepared in Example 1.
[0020] Figure 5 This is a SEM image of the sample prepared in Example 1.
[0021] Figure 6 This is a SEM image of pure LPSC.
[0022] Figure 7 The image shows the CV detection pattern of the sample prepared in Example 1 and LPSC. Detailed Implementation
[0023] The present invention will be further described in detail below through specific embodiments. Unless otherwise specified, the raw materials, reagents, or apparatus used in the embodiments and comparative examples are all available from conventional commercial sources or can be obtained by existing technical methods. Unless otherwise specified, the test or experimental methods are conventional methods in the art.
[0024] To address the shortcomings of the existing technologies, this invention proposes a bismuth iodide-based core-shell structured sulfide solid electrolyte, its preparation, and its application.
[0025] Specifically, the core technology of this invention is the "high-temperature vapor phase coating" process system: The core of this invention is to use high temperature to evaporate bismuth iodide solid to form bismuth iodide vapor, which reacts uniformly with the surface of sulfide solid electrolyte to generate an adaptive interface system containing both LiI and LiBiS2 in situ; the bismuth iodide vapor reacts in LPSC to generate an interface protective layer containing LiBiS2 and LiI, in which LiBiS2 acts as a stable interface phase anchored on the electrolyte surface to regulate lithium deposition while protecting the internal sulfide solid electrolyte and improving air stability, and LiI, as a dynamic component, migrates under the electric field and repairs interface damage, reducing the fundamental problem of "interface contact failure" and improving the voltage window of the sulfide solid electrolyte.
[0026] The core of this invention is to utilize high temperature to evaporate bismuth iodide solid to form bismuth iodide vapor, which reacts uniformly with the surface of sulfide solid electrolyte to generate an adaptive interface system containing both LiI and LiBiS2 in situ. Lithium iodide vapor reacts in LPSC to generate an interface protective layer containing LiBiS2 and LiI. LiBiS2 acts as a stable interface phase anchored on the electrolyte surface to regulate lithium deposition while protecting the internal sulfide solid electrolyte and improving air stability. LiI, as a dynamic component, migrates under an electric field and repairs interface damage, reducing the fundamental problem of "interface contact failure" and increasing the voltage window of the sulfide solid electrolyte.
[0027] This invention utilizes the high-temperature vaporization of bismuth iodide to react with a sulfide electrolyte to generate a composite coating of lithium bismuthide and lithium iodide. In the composite shell, the lithium iodide phase acts as a chemical passivation barrier, suppressing interfacial side reactions between the sulfide electrolyte and the lithium metal anode and improving the material's air stability. The lithium bismuthide alloy phase provides an ion-electron conduction pathway, preventing the coating from causing interfacial impedance degradation. The dual-phase synergistic modification simultaneously improves the interfacial stability of the sulfide electrolyte and optimizes interfacial charge transport.
[0028] This invention uses only bismuth iodide as a precursor to generate a biphase composite coating layer. BiI3 sublimates into gaseous molecules under sealed high temperature, which then diffuse freely within a sealed cavity and uniformly adsorb onto the entire outer surface of each sulfide electrolyte particle. A gas-solid reaction occurs on the particle surface, with gaseous molecules adsorbed onto the sulfide surface, directly generating the LiBiS2-LiI composite layer at the interface. The reaction is confined to the particle surface, significantly reducing damage to the electrolyte matrix's crystal structure and intrinsic ionic conductivity. The coating layer thickness on a single particle surface is highly consistent, requiring no multi-step post-processing. The process is simple, solvent-free, and does not require high-energy ball milling, making it suitable for industrial scale-up.
[0029] The present invention will be further described in detail below through specific embodiments.
[0030] Example 1 A method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte, specifically comprising: Bismuth iodide and LPSC sulfide solid electrolyte were placed in a tube furnace under an argon atmosphere with a mass ratio of 4:1 between the sulfide solid electrolyte and bismuth iodide. The furnace was then evacuated to 2 Pa, heated at a rate of 3 °C / min, and held at 500 °C for 2 hours before being cooled with the furnace to obtain a core-shell structured sulfide solid electrolyte.
[0031] Example 2 A method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte, specifically comprising: Bismuth iodide and LPSC sulfide solid electrolyte were placed in a tube furnace under an argon atmosphere. The mass ratio of sulfide solid electrolyte to bismuth iodide in the container was 2:1. The furnace was then evacuated to 1 Pa, heated at a rate of 2 °C / min, and held at 400 °C for 1 h. After holding at 400 °C, the core-shell structured sulfide solid electrolyte was cooled with the furnace.
[0032] Example 3 A method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte, specifically comprising: Bismuth iodide and LPSC sulfide solid electrolyte were placed in a tube furnace under an argon atmosphere. The mass ratio of sulfide solid electrolyte to bismuth iodide in the container was 5:1. The furnace was then evacuated to 3 Pa, heated at a rate of 4 °C / min, and held at 600 °C for 3 hours. After holding at 600 °C, the furnace was cooled to obtain a core-shell structured sulfide solid electrolyte.
[0033] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, equal amounts of sulfide electrolyte and bismuth iodide were placed in a planetary high-energy ball mill, and 10 mm zirconia grinding balls were added. Under Ar atmosphere, the ball-to-material ratio was 20:1, the rotation speed was 300 rpm, the ball milling time was 10 h, with milling for 30 min and stopping for 10 min. Then, the temperature was raised to 500 °C at a heating rate of 3 °C / min and held for 4 h. The furnace was cooled with the furnace, and the whole process was protected by an inert atmosphere to obtain the finished product.
[0034] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the mass ratio of sulfide electrolyte to bismuth iodide in Comparative Example 2 is 1:1, while other aspects remain unchanged.
[0035] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the mass ratio of sulfide electrolyte to bismuth iodide in Comparative Example 3 is 6:1, while other aspects remain unchanged.
[0036] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the heating rate of Comparative Example 4 is 1℃ / min, while other aspects remain unchanged.
[0037] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the heating rate of Comparative Example 5 is 6°C / min, while other aspects remain unchanged.
[0038] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that the heat preservation temperature of Comparative Example 6 is 200°C, while other conditions remain unchanged.
[0039] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that the heat preservation temperature of Comparative Example 7 is 700°C, while other conditions remain unchanged.
[0040] Comparative Example 8 The difference between Comparative Example 8 and Example 1 is that the vacuum degree of Comparative Example 8 is 5 Pa, while other aspects remain unchanged.
[0041] Comparative Example 9 The difference between Comparative Example 9 and Example 1 is that the vacuum degree of Comparative Example 9 is 0.5 Pa, while other aspects remain unchanged.
[0042] Test case This test example uses samples from Examples 1-3 and Comparative Examples 1-9 for performance testing. The specific steps are as follows.
[0043] (1) Battery performance testing methods: The electrochemical performance of the assembled mold battery was tested using the Xinwei Battery Testing System in a constant temperature environment of 25±2℃.
[0044] Charge and discharge cycle: Charge to 4.3V with a constant current of 0.1C, then charge to 4.3V with a constant voltage of 4.3V until the current drops to 0.05C, and let stand for 10 minutes; then discharge to 2.8V with a constant current of 0.5C, record the discharge capacity, and repeat the above charge and discharge cycle.
[0045] Capacity retention rate calculation: Capacity retention rate = (Discharge capacity in the nth cycle / Initial discharge capacity) × 100%.
[0046] (2) Electrochemical impedance spectroscopy (EIS) test and air stability test. The standard for electrochemical impedance spectroscopy (EIS) test is mainly based on T / CSAE 475-2025, as follows.
[0047] Sample preparation: Electrolyte powder was cold-pressed at 10 MPa to obtain a dense sheet sample with a diameter of 10 mm and a thickness of approximately 0.5 mm. The thickness (L) of the sample was accurately measured using a micrometer, and the effective contact area (A) was calculated based on the electrode diameter. Thickness measurement using a micrometer is required.
[0048] The sample is held in place using a blocking electrode (such as stainless steel or sputtered metal film), and an AC voltage (amplitude 10mV, frequency range 1MHz to 0.1Hz) is applied.
[0049] The bulk resistance R is obtained by fitting the semicircular intercept in the high-frequency region using EIS. bulk The low-frequency region reflects the interfacial resistance and the double-layer effect.
[0050] Geometric parameter measurement: Thickness (L): The thickness of the compressed tablet is measured directly using a micrometer; Area (A): The effective contact area is calculated based on the electrode diameter; according to the formula... Calculate the ionic conductivity of the corresponding material.
[0051] The samples were placed in a glove box for air stability testing. The glove box atmosphere test was conducted at a temperature of 28°C, a dew point of -35°C, with oxygen <0.01ppm and moisture <0.01ppm.
[0052] (3) X-ray diffraction (XRD) test Sample preparation: The sample powder prepared in the examples was ground until the particle size was uniform, passed through a 200-mesh sieve (particle size ≤75μm), and felt smooth to the touch, similar to the texture of flour, to reduce preferred orientation and enhance the intensity of diffraction peaks. Since sulfide electrolytes are hygroscopic and easily decompose, all grinding, tableting, and sample loading operations must be performed in an argon-filled glove box to avoid oxidation or structural damage.
[0053] Compressing method: The positive pressure method is used to fill the groove of the glass sample holder with the ground powder, and then press it with a glass plate until the surface is flat and flush with the groove, so as to ensure that the sample surface is flat, uniform and dense.
[0054] Instrument setup and testing procedures: Instrument initialization: Turn on the circulating water system and ensure the water temperature is controlled at 17~20℃ and the water pressure is controlled at 0.3~0.4MPa to prevent the equipment from overheating or being damaged. Open the PC-based XRD control software, select the Rigaku Ultimate IV measurement system, initialize the goniometer, and confirm that the sample chamber door is closed.
[0055] Parameter settings: X-ray source: copper target Kα rays (Cu Kα, λ=1.5418 Å), working voltage 40 kV, working current 30 mA to ensure clear diffraction peaks.
[0056] Scanning parameters: The standard wide-angle test range is 5°~90°, the step size is set to 0.02°, and the scanning speed is set to 5° / min.
[0057] Slit settings: The entrance slit width is 0.2~0.6 mm, and the detector slit width is 3~8 mm, in order to optimize resolution and signal-to-noise ratio.
[0058] Sample loading and testing: Gently open the sample chamber door, insert the prepared sample holder into the goniometer slot, ensuring the sample surface is facing upwards and centered. Gently close the door and confirm that the closure indicator light is on. Click the Start button in the software to begin scanning. After the software indicates that the scan is complete, save the data file.
[0059] (4) SEM detection The sample prepared in Example 1 and the sulfide solid electrolyte LPSC were examined by scanning electron microscopy. The specific detection procedure is as follows: the sample to be tested was dispersed on the surface of the conductive adhesive, excess powder was gently blown away to ensure that the particles were dispersed and did not agglomerate, gold sputtering was performed, the sample was loaded, observation and adjustment were performed, and finally the image was acquired; and the sample prepared in Example 1 was analyzed by the accompanying energy dispersive spectrometer (EDS).
[0060] (5) CV test parameter settings and wiring The sample prepared in Example 1 and pure LPSC powder were used for testing; Keep the assembled solid-state test mold in a glove box or quickly move it to room temperature and let it stand for 20 minutes to allow the interface contact to stabilize. The working electrode of the electrochemical workstation is clamped to the lower punch of the mold, while the counter electrode and reference electrode are connected to the upper punch of the mold. Cyclic voltammetry is selected as the testing mode, with the potential window set to 0.01–5.0 V (vs. Li⁺ / Li) to avoid low-potential lithium deposition and high-potential electrolyte oxidation decomposition. The scan rate is set to 0.1 mV / s to ensure testing accuracy. The number of cycles is set to 3–5, with a 300-second rest period before testing. The sampling interval is set to 0.001 V, and the current sensitivity is adjusted to 1 × 10⁻⁻⁻⁶. 5 A, matching the low current response characteristics of LPSC solid electrolyte.
[0061] Test Startup and Real-time Monitoring After confirming that the wiring and parameters are correct, start the CV test and observe the changes in the current-potential curve in real time.
[0062] If the current suddenly and drastically increases to more than 10⁻³A, stop the test immediately. This indicates that the electrolyte sheet is cracked or has an internal short circuit. The test must be returned to the glove box to disassemble the mold and reassemble it. If there are no abnormalities, wait for the test to complete all cycles automatically.
[0063] The results shown in Tables 1 and 2 demonstrate that the sulfide electrolyte prepared in this invention exhibits good long-cycle performance and good air stability.
[0064] The experimental results from the examples and comparative examples show that the ball milling process cannot promote the reaction between bismuth iodide and the surface of the sulfide electrolyte matrix to form a complete and continuous lithium bismuthide and lithium iodide composite coating layer. Most of it is bismuth iodide coating doping, which cannot effectively isolate moisture. At the same time, ball milling damages the matrix crystal, resulting in an increase in interfacial impedance. It is known that the large amount of BiI3 in the system leads to excessively high partial pressure of gaseous BiI3 after high-temperature sublimation, resulting in violent gas-solid reactions that erode the electrolyte phase, damage the crystal structure, and cause a significant decrease in bulk ionic conductivity. The excessive thickness of the coating layer increases the resistance to lithium-ion transport and raises the battery interface impedance.
[0065] It is known that if the amount of bismuth iodide added is too low, the partial pressure of BiI3 in the gas phase will be too low, and a complete Li3Bi-LiI composite protective layer cannot be formed; the exposed sulfide will still undergo serious side reactions with the lithium metal anode, making it difficult to suppress lithium dendrites and greatly weakening the modification effect.
[0066] It is known that heating rates exceeding the scope of this invention will affect the modification performance of sulfide electrolytes. If the heating rate is too fast, BiI3 will sublimate rapidly and in large quantities, and the partial pressure of the gas phase will increase sharply in a short time. The sulfide electrolyte particles are prone to cracking, and the coating uniformity will deteriorate. If the heating rate is too slow, the residence time in the low temperature range will be too long, and BiI3 will sublimate slowly. Some precursors will preferentially condense and be consumed on the container wall, and the layer structure will be difficult to be continuous.
[0067] It can be seen that if the insulation temperature is too high, the vapor pressure of BiI3 will increase sharply, which will easily etch the sulfide matrix. In addition, the grains of the Li3Bi-LiI composite layer generated at high temperature will coarsen, the interfacial bonding will become worse, and non-target impurity phases will be easily generated, which will deteriorate the interfacial performance.
[0068] It can be seen that if the insulation temperature is too low, the amount of BiI3 sublimation is insufficient, the partial pressure of BiI3 in the gas phase is low, the gas-solid reaction kinetics are insufficient, and it is difficult to fully carry out the interfacial reaction; a continuous and complete Li3Bi-LiI dual-phase composite coating layer cannot be formed, and the side reaction between sulfides and lithium anode cannot be effectively blocked, resulting in a weak dendrite suppression effect.
[0069] It is known that the vacuum conditions within the scope of this invention can prevent the hydrolysis and oxidation of sulfide solid electrolytes, promote the sublimation of bismuth iodide upon heating to form a gaseous precursor, and reduce gaseous diffusion resistance. If the vacuum pressure is too high, gas molecules will hinder the diffusion of BiI3 vapor, resulting in uneven coating. If the vacuum pressure is too low, BiI3 vapor will be easily extracted from the cavity, resulting in a thinner and discontinuous coating layer, both of which will affect the performance of the sulfide electrolyte.
[0070] X-ray diffraction (XRD) test results are as follows Figure 1 As shown, the arrow points to the peak corresponding to LiBiS2, indicating that the preparation method of the present invention achieves the reaction coating of bismuth iodide with sulfide electrolyte.
[0071] Energy dispersive spectrometer (EDS) scan results as follows Figures 2-4 As shown, the presence of lithium iodide and lithium bismuthide is demonstrated, and the elements are evenly distributed.
[0072] SEM detection results as follows Figure 5-6 As shown, the preparation method of the present invention does not change the morphology of the sulfide electrolyte.
[0073] CV detection results as follows Figure 7 As shown, the voltage window of the experimental group was increased by about 0.25V compared with the control group. The preparation method of the present invention can improve the voltage window of the sulfide solid electrolyte.
[0074] Table 1. Battery cycle performance test results of sulfide electrolytes
[0075] Table 2. Results of air stability tests for sulfide electrolytes
[0076] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte, characterized in that, Specifically, under the protection of an inert gas, bismuth iodide and a sulfide solid electrolyte are placed in a tube furnace, then a vacuum is drawn, the temperature is raised and held, and then the furnace is cooled to obtain a core-shell structured sulfide solid electrolyte.
2. The method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte according to claim 1, characterized in that, The mass ratio of the sulfide solid electrolyte to bismuth iodide is 2-5:
1.
3. The method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte according to claim 1, characterized in that, The heating rate is 2-4℃ / min.
4. The method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte according to claim 1, characterized in that, The vacuum level of the vacuum pump is 1-3 Pa.
5. The method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte according to claim 1, characterized in that, The insulation temperature is 400~600℃, and the insulation time is 1-3h.
6. The method for preparing a bismuth iodide-based core-shell structured sulfide solid electrolyte according to claim 1, characterized in that, The sulfide electrolyte is Li (7-a) P S (6-a) X a ; where 0 < a ≤ 1, X is selected from one or more of Cl, Br and I.
7. The core-shell structured sulfide solid electrolyte prepared by the preparation method according to any one of claims 1-6.
8. The core-shell structured sulfide solid electrolyte according to claim 7, characterized in that, It contains a sulfide electrolyte and a lithium bismuthide and lithium iodide composite layer coated with the sulfide electrolyte.
9. The application of the sulfide solid electrolyte of claim 7 in an all-solid-state lithium battery.