A flame-retardant polymer composite electrolyte and lithium-ion battery
By covalently anchoring DOPO-VTMS on the surface of LLZTO, the problems of flame retardant migration and insufficient electrochemical performance in composite gel polymer electrolytes are solved, achieving efficient improvement in flame retardancy and electrochemical performance, thereby enhancing battery safety and lifespan.
Patent Information
- Application Number
- CN202611238510.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing composite gel polymer electrolytes often sacrifice electrochemical performance to improve flame retardant properties, and traditional flame retardants are prone to migration at the filler-polymer interface, interfering with ion transport and affecting battery cycle life.
DOPO-VTMS is covalently anchored to the surface of LLZTO. By grafting DOPO-VTMS onto the surface of the lithium-ion conductive ceramic filler LLZTO, phosphorus-containing flame-retardant groups are arranged at specific points with a low grafting amount, which improves dispersibility and promotes interfacial ion transport, forming a covalently anchored structure.
It achieves a synergistic improvement in flame retardant and electrochemical performance, increases room temperature ionic conductivity, enhances battery flame retardancy and cycle stability, and reduces the migration risk of free flame retardants.
Smart Images

Figure CN123120853A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, and particularly relates to a flame-retardant polymer composite electrolyte and a lithium-ion battery. Background Technology
[0002] Gel polymer electrolytes are gel-state systems formed by a polymer matrix, plasticizer, and lithium salt, combining the high ionic conductivity of liquid electrolytes with the good mechanical properties of solid electrolytes. Among them, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) based gel polymer electrolytes have attracted widespread attention due to their high ionic conductivity and good electrochemical stability.
[0003] To further improve ionic conductivity and mechanical properties, ceramic fillers are typically added to the polymer matrix. The addition of ceramic fillers reduces the crystallinity of the polymer and provides additional ion transport pathways, thereby improving ionic conductivity. However, composite gel polymer electrolytes still pose safety hazards: the PVDF-HFP matrix decomposes at high temperatures, releasing flammable gases, and the large amount of carbonate plasticizers it contains has a low flash point and is highly volatile, making it a major fuel source for battery thermal runaway and fire.
[0004] Currently, the flame retardant modification of polymer electrolytes mainly employs the following strategies: Strategy 1: Physical blending with added flame retardants. The drawback is that the large amount of flame retardant added leads to a significant decrease in ionic conductivity, and it is prone to aggregation, migration, and precipitation.
[0005] Strategy 2: Covalently bond phosphorus-containing monomers to the polymer backbone. The drawback is that phosphorus-containing monomers can affect the degree of polymerization and the flexibility of the polymer chain, interfering with ion transport.
[0006] Strategy 3: Microencapsulated flame retardants. The drawback is that the microcapsules are large, affecting the uniformity of the electrolyte membrane, and the process is complex.
[0007] Strategy 4: Surface functionalization of ceramic fillers. Surface modification of ceramic fillers can improve their compatibility with polymer matrices. However, existing surface modification methods only focus on dispersibility and interfacial compatibility, and have not yet integrated surface modification with flame retardant functions.
[0008] A core contradiction exists in existing technologies: improvements in flame retardant performance often come at the expense of electrochemical performance. Furthermore, in composite gel polymer electrolytes, the interface region between the filler and the polymer is prone to becoming an unstable region under the coupling of thermal, mechanical, and electrochemical forces. Traditional free flame retardants are difficult to achieve long-term stable enrichment in this region, resulting in insufficient interfacial flame retardant protection. More critically, free phosphorus-containing flame retardants introduced by conventional physical blending are prone to undergoing harmful side reactions with the electrodes during battery cycling, damaging the integrity of the solid electrolyte interfacial membrane (SEI membrane) and deteriorating the battery's cycle life.
[0009] It is worth noting that existing technologies have reported the use of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and its derivatives in combination with silane coupling agents for surface modification of inorganic fillers. However, the targets of these modifications are all inert flame-retardant fillers (such as aluminum hydroxide, magnesium hydroxide, etc.), and the purpose of the modifications is only to improve powder dispersibility or to impart flame-retardant properties to the filler itself. There are also reports of using silane coupling agents to modify the surface of lithium-ion conductive ceramic fillers to improve dispersibility, but without imparting flame-retardant properties. In gel polymer electrolyte systems, the interface between lithium-ion conductive ceramic fillers and polymers is an essential channel for ion transport. Existing technologies have not yet provided a technical solution for anchoring DOPO-VTMS at a low grafting amount of 1.0% to 4.0% on the surface of PVDF-HFP liquid-absorbing gel-based membranes for LLZTO lithium-ion conductive ceramic fillers, and simultaneously improving ionic conductivity, flame retardancy, and cycle stability compared to systems modified with equal amounts of free DOPO and ordinary silane. Summary of the Invention
[0010] This invention provides a flame-retardant polymer composite electrolyte and a lithium-ion battery, aiming to solve the problem that in composite gel polymer electrolytes, the filler-polymer interface lacks effective flame-retardant protection, while traditional physical blending flame-retardant strategies have defects such as large addition of flame retardants, easy migration, interference with ion transport, and deterioration of electrode interface stability, making it difficult to simultaneously achieve both flame-retardant performance and electrochemical performance.
[0011] This invention is achieved as follows: a flame-retardant polymer composite electrolyte, the core concept of which is: The addition product DOPO-VTMS, derived from vinyltrimethoxysilane (VTMS), was covalently anchored to the garnet-type lithium-ion conductive ceramic filler Li6.4La3Zr1.4Ta0.6O with a controlled low grafting amount via a silicon-oxygen structure. 12 (LLZTO) surface; This grafted structure positions phosphorus-containing flame-retardant groups at the filler-polymer interface, while the organic segments of DOPO-VTMS improve the dispersibility of the filler and the polar P=O groups of DOPO assist the dissociation of lithium salt to promote interfacial ion transport, thereby achieving a synergistic improvement in flame retardant performance and electrochemical performance with extremely low phosphorus addition.
[0012] (a) Core material: DOPO-VTMS phosphorus-containing silane coupling agent DOPO-VTMS is prepared by the pH addition reaction of DOPO and vinyltrimethoxysilane. Its molecule contains: DOPO group, which provides the flame retardant function of phosphorus element; trimethoxysilane group, which can be hydrolyzed and condensed with hydroxyl groups on the filler surface; silicon element, which can be converted into silicon-containing ceramic components at high temperature.
[0013] (ii) Surface grafting modification of ceramic fillers The filler is LLZTO, preferably with a particle size of 100-200 nm. In an ethanol / water mixed solvent, the methoxysilyl group of DOPO-VTMS hydrolyzes to generate silanol group, which condenses with the hydroxyl group on the surface of LLZTO to form a silicon-oxygen structure containing Si-OM bonds. The silicon-oxygen structure may also contain Si-O-Si bonds (M=La, Zr, Ta), realizing the covalent anchoring of DOPO-VTMS on the surface of the filler. After the reaction, it is thoroughly washed with anhydrous ethanol and vacuum dried at 100-150℃ for 2-12 hours to remove adsorbed water and residual acidic substances on the surface.
[0014] (III) Composition of Flame-Retardant Polymer Composite Electrolyte The composite electrolyte is composed of the following components: Polymer base film: PVDF-HFP, wherein the molar content of hexafluoropropylene (HFP) is 8% to 12% and the weight average molecular weight is 400,000 to 600,000; The LLZTO filler grafted with DOPO-VTMS (DOPO-Si-LLZTO) has a mass fraction of 8% to 18% in the base film; The grafting amount of DOPO-VTMS onto the LLZTO surface is 1.0% to 4.0% of the LLZTO mass; Lithium salts: lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium bis(fluorosulfonyl)imide (LiFSI); Plasticizer: A mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).
[0015] (iv) Preparation method Step 1: Under nitrogen protection, DOPO and VTMS are dissolved in an organic solvent at a molar ratio of 1:1 to 1:1.2. Azobisisobutyronitrile (AIBN) of 1% to 3% by mass of DOPO is added as an initiator. The reaction is carried out at 70 to 90°C for 6 to 12 hours. DOPO-VTMS is obtained by vacuum distillation.
[0016] Step 2: Disperse the dried LLZTO in an ethanol / water mixed solvent (volume ratio 95:5), add DOPO-VTMS at 1%–6% of the LLZTO mass, adjust the acidity of the reaction solution to pH 5.5–6.5 with glacial acetic acid, and react at 60–80℃ for 4–8 hours; after the reaction is completed, separate by centrifugation, wash thoroughly with anhydrous ethanol, and vacuum dry at 100–150℃ for 2–12 hours to obtain DOPO-Si-LLZTO modified filler.
[0017] Step 3: Add PVDF-HFP and DOPO-Si-LLZTO to N-methylpyrrolidone (NMP) and mix evenly to obtain a casting solution. Cast the solution into a film and dry it at 60-80℃ to obtain an electrolyte base film. The liquid absorption rate of the base film is calculated as (m1-m0) / m0×100%, where m0 is the mass of the base film before immersion and m1 is the mass after immersion in the electrolyte solution and drying the surface liquid with filter paper. The liquid absorption rate is 150-250wt%.
[0018] Step 4: In an argon glove box with H2O and O2 contents both below 1 ppm, the base film is immersed in a 1 mol / L lithium salt EC / EMC / DMC (volume ratio 1:1:1) solution for 0.5 to 2 hours for activation. The film is then removed and the surface liquid is dried to obtain the polymer composite electrolyte.
[0019] (v) Lithium-ion batteries The present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, and the aforementioned flame-retardant polymer composite electrolyte. The positive electrode active material is lithium iron phosphate (LiFePO4); the negative electrode is graphite.
[0020] Compared with the prior art, the embodiments of this application have the following main advantages: The low grafting amount anchoring of DOPO-VTMS achieves a synergistic improvement in flame retardancy and electrochemical performance: In this invention, DOPO-VTMS is covalently anchored to the surface of LLZTO with a low grafting amount of 1.0% to 4.0%, so that the phosphorus-containing flame retardant groups are arranged in a fixed position at the filler-polymer interface; This interface modification layer plays the following roles: (1) improving the dispersion uniformity of the filler in the PVDF-HFP matrix; (2) promoting interfacial ion transport by using the polar P=O group of DOPO to assist the dissociation of lithium salt; (3) providing the flame retardant function of phosphorus element; (4) significantly reducing the risk of migration of free flame retardant molecules and the initiation of electrode side reactions through covalent anchoring; In the examples, the room temperature ionic conductivity of the DOPO-Si-LLZTO system reaches 1.19 mS / cm, which is about 13% higher than that of the unmodified LLZTO system; the limiting oxygen index (LOI) reaches 30.5%, and the vertical combustion reaches V-0 level; The simultaneous improvement of flame retardant performance and electrochemical performance proves the technical effect of this low grafting amount interface anchoring strategy.
[0021] Phosphorus-Silicon Synergistic Flame Retardancy: In the electrolyte system of this invention, phosphorus (derived from DOPO) and silicon (derived from silane coupling agents) work synergistically in both the gas and condensed phases. Specifically, phosphorus releases phosphorus-containing free radicals at high temperatures to capture active combustion free radicals and promote char formation in the condensed phase, while silicon transforms into silicon-containing ceramic components at high temperatures to enhance the density of the char layer. Fluorine in the PVDF-HFP matrix contributes to the formation of fluorine-containing interfacial components and the char structure in the condensed phase. The synergistic effect of multiple elements significantly improves the flame retardant efficiency with limited flame retardant dosage.
[0022] Covalent anchoring reduces the risk of harmful side reactions from free flame retardants: DOPO-VTMS is fixed to the LLZTO surface through a silicon-oxygen structure containing Si-OM bonds, significantly reducing the tendency for migration, precipitation, or leakage. Compared with a physically blended equivalent amount of free DOPO, the covalently anchored system exhibits a significantly reduced interfacial impedance growth rate and cycle capacity decay rate, demonstrating that the covalent anchoring strategy significantly reduces the risk of electrode interfacial side reactions initiated by free small-molecule flame retardants.
[0023] The process is mature and easy to implement: the synthesis of DOPO-VTMS and the surface grafting of LLZTO are both mature chemical reactions with mild process conditions and controllable costs, without the need for large-scale modification of existing battery manufacturing processes. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the preparation process of DOPO-Si-LLZTO modified filler.
[0025] Figure 2 The bar chart shows the comparison of ionic conductivity for each embodiment and comparative example.
[0026] Figure 3 A bar chart comparing the limiting oxygen index (LOI) of each embodiment and comparative example.
[0027] Figure 4 A comparison chart of the cycling performance of LiFePO4 / GPE / graphite full cells. Detailed Implementation
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs; the terminology used herein in the specification of the application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application; the terms "comprising" and "having," and any variations thereof, in the specification, claims, and foregoing drawings of this application are intended to cover non-exclusive inclusion. The terms "first," "second," etc., in the specification, claims, or foregoing drawings of this application are used to distinguish different objects, not to describe a particular order.
[0029] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0030] I. Preparation of DOPO-VTMS phosphorus-containing silane coupling agent Example 1-1 In a 250 mL three-necked flask equipped with a stirrer, condenser, and nitrogen inlet, 21.6 g (0.1 mol) of DOPO and 14.8 g (0.1 mol) of vinyltrimethoxysilane (VTMS) were added, followed by 100 mL of anhydrous toluene. The mixture was stirred to dissolve the DOPO. 0.5 g of azobisisobutyronitrile (AIBN, approximately 2.3% of the DOPO mass) was added as an initiator. Nitrogen gas was purged for 30 minutes to remove oxygen, and the mixture was heated to 80 °C and reacted for 8 hours. After the reaction was completed, the solvent and unreacted monomers were removed by vacuum distillation to obtain a pale yellow viscous liquid, DOPO-VTMS, with a yield of approximately 92%.
[0031] 31 p nuclear magnetic resonance spectrum ( 31 P NMR: δ approximately 33 ppm (the chemical shift of P in DOPO changes from approximately 15 ppm to 33 ppm, indicating an addition reaction of the PH bond).
[0032] Fourier transform infrared (FTIR) spectrum: 2380 cm⁻¹ -1 The characteristic absorption peak of the pH bond disappears at 1240 cm⁻¹. -1 The absorption peak at the P=O bond is enhanced, at 1080 cm⁻¹. -1 The Si-O-CH3 absorption peak is present.
[0033] II. Preparation of DOPO-Si-LLZTO Modified Filler Example 2-1 10g of LLZTO nanoparticles (approximately 200nm in diameter) were vacuum dried at 120℃ for 12 hours, then ultrasonically dispersed in 200mL of an ethanol / water mixed solvent (95:5 by volume) for 30 minutes. 0.4g of DOPO-VTMS (4% of the LLZTO mass) was added, and the acidity of the reaction solution was adjusted to pH 5.5–6.5 with glacial acetic acid. The mixture was stirred at 70℃ for 6 hours. After centrifugation, the mixture was washed three times with anhydrous ethanol and vacuum dried at 120℃ for 6 hours to obtain the DOPO-Si-LLZTO modified filler.
[0034] Thermogravimetric analysis (TGA): Tested under a nitrogen atmosphere at a heating rate of 10℃ / min; the mass loss of pure LLZTO in the 250–650℃ range is Δw0, and the mass loss of DOPO-Si-LLZTO modified filler in the same temperature range is Δw1; the grafting rate is calculated by the following formula: grafting rate = Δw1 - Δw0, where Δw0 and Δw1 are calculated based on the initial mass of the corresponding sample; the test results show that the grafting rate is approximately 2.5wt% (i.e., approximately 0.025g of DOPO-VTMS is grafted onto the surface of each gram of LLZTO); the weight loss of adsorbed water below 200℃ and the possible decomposition of carbonates above 650℃ have been deducted in the calculation.
[0035] X-ray photoelectron spectroscopy (XPS): The P 2p peak appears at 133.5 eV, and the intensity of the Si 2p peak increases; Contact angle: The water contact angle increases from approximately 25° for pure LLZTO to approximately 55°.
[0036] X-ray diffraction (XRD): The characteristic diffraction peaks did not change significantly before and after modification, indicating that the main crystalline phase of LLZTO was not significantly affected under the treatment conditions.
[0037] Examples 2-2 to 2-4 Following the method in Example 2-1, the amount of DOPO-VTMS added was controlled to be 2%, 4%, and 6% of the mass of LLZTO, respectively. The resulting modified fillers were measured by TGA, and the grafting rates were approximately 1.2%, 2.5%, and 3.8%, respectively, and were denoted as DOPO-Si-LLZTO-1.2%, DOPO-Si-LLZTO-2.5%, and DOPO-Si-LLZTO-3.8%. When the amount of DOPO-VTMS added was increased to 6%, the grafting rate tended to saturate (approximately 3.8%), indicating that the reactive hydroxyl sites on the surface of LLZTO had been basically occupied.
[0038] III. Preparation of Flame-Retardant Polymer Composite Electrolyte Membranes Example 3-1 0.85 g of PVDF-HFP (HFP molar content 10%, weight average molecular weight approximately 500,000) and 0.15 g of DOPO-Si-LLZTO-2.5% were added to 8 mL of N-methylpyrrolidone (NMP), and stirred at 60 °C for 12 hours to obtain a casting solution. The film was then coated onto a glass plate with a 300 μm doctor blade, the solvent was evaporated at 60 °C for 2 hours, and the film was vacuum dried at 80 °C for 12 hours to obtain a base film with a thickness of approximately 60 μm. The liquid absorption rate was calculated as (m1-m0) / m0×100%, where m0 is the mass of the base film before immersion, and m1 is the mass of the film after immersion in the electrolyte for 1 hour and drying the surface liquid with filter paper. The liquid absorption rate was tested to be approximately 200 wt%. The base film was immersed in an argon glove box (H2O < 1 ppm, O2 < 1 ppm) in an EC / EMC / DMC electrolyte of 1 mol / L LiTFSI (volume ratio 1:1:1) for 1 hour. The film was then removed and the surface liquid was dried to obtain a gel polymer composite electrolyte (denoted as DOPO-Si-LLZTO-2.5% GPE).
[0039] Example 3-2 According to the method of Example 3-1, DOPO-Si-LLZTO-1.2% modified filler was used with a filler addition amount of 15wt% to obtain DOPO-Si-LLZTO-1.2% GPE.
[0040] Example 3-3 According to the method in Example 3-1, DOPO-Si-LLZTO-3.8% modified filler was used with a filler addition amount of 15wt% to obtain DOPO-Si-LLZTO-3.8% GPE.
[0041] IV. Comparative Examples Comparative Example 1 According to Example 3-1, without adding any ceramic filler, pure PVDF-HFP GPE is obtained.
[0042] Comparative Example 2 According to Example 3-1, PVDF-HFP / LLZTO GPE was obtained by using unmodified LLZTO (15wt%).
[0043] Comparative Example 3 According to Example 3-1, 15wt% pure LLZTO and 0.6wt% free DOPO were added simultaneously (calculation basis: 15wt% filler addition amount × 4% feed amount ≈ 0.6wt%, which is equivalent to the grafted DOPO content in Example 3-1), and PVDF-HFP / LLZTO / DOPO GPE was obtained by physical blending.
[0044] Comparative Example 4 LLZTO was surface modified using γ-glycidoxypropyltrimethoxysilane (KH560) according to the method in Example 2-1. The amount of KH560 added was controlled so that the amount of organic modification was about 2.5 wt% and the amount of filler added was 15 wt%, to obtain PVDF-HFP / KH560-LLZTO GPE.
[0045] Comparative Example 5 Based on Comparative Example 4, an additional 0.6 wt% free DOPO was added through physical blending (calculated according to the same method as above) to obtain PVDF-HFP / KH560-LLZTO / DOPO GPE.
[0046] V. Performance Testing and Results (a) Ionic conductivity test A symmetrical cell was assembled by sandwiching an electrolyte membrane between stainless steel blocking electrodes using the electrochemical impedance spectroscopy (EIS) method. The cell was tested at 25°C in a frequency range of 1 Hz to 1 MHz. Each sample was tested in triplicate, and the results are expressed as mean ± standard deviation.
[0047] Results analysis: The DOPO-Si-LLZTO system exhibited superior conductivity compared to the unmodified LLZTO system (1.05 mS / cm) at all grafting ratios. The highest conductivity (1.19 mS / cm) was observed at a grafting ratio of 2.5%, representing an improvement of approximately 13%. The conductivity at a grafting ratio of 3.8% was slightly lower than that at 2.5%, possibly due to the slight obstruction of interfacial ion transport by the increased organic layer thickness, but it was still significantly better than the unmodified system. The conductivity difference between Example 3-1 and Comparative Example 2 was statistically significant (p<0.05). The comparison between Comparative Example 5 and Example 3-1 (1.06 vs 1.19 mS / cm) indicates that covalently anchoring DOPO to the filler surface can prevent interference from free small molecules on ion transport.
[0048] (ii) Flame retardant performance test Limiting oxygen index (LOI) and vertical burning tests were conducted in accordance with GB / T 2406-2009 and GB / T 2408-2008 standards. The thickness of a single electrolyte membrane was approximately 60 μm. Fourteen membranes were stacked to a total thickness of approximately 0.84 mm (meeting the standard requirement of a sample thickness ≥ 0.8 mm). The samples were then uniformly cut into 50 mm long × 10 mm wide specimens for reference testing.
[0049] Results analysis: Comparative Example 5 showed a 1.5 percentage point increase in LOI compared to Comparative Example 3, indicating a synergistic flame-retardant effect between phosphorus and silicon. Example 3-1 showed a 2.2 percentage point increase in LOI compared to Comparative Example 5. This gain is mainly attributed to the targeted anchoring of DOPO-VTMS on the LLZTO surface, which concentrates the flame-retardant elements in the filler-polymer interface region. All grafted samples showed significantly better LOIs than the unmodified system.
[0050] (iii) Thermal stability test (TGA) Thermogravimetric analysis was performed under a nitrogen atmosphere at a heating rate of 10 °C / min.
[0051] Results analysis: The initial decomposition temperature (T5%) of the DOPO-Si-LLZTO system was 20℃ higher than that of Comparative Example 2, and the maximum decomposition rate temperature (T5%) was also higher. max The temperature was increased by 23°C. The improved thermal stability is due to the DOPO groups at the filler interface promoting char formation of the condensed phase, while the fluorine element in the PVDF-HFP matrix helps to form stable fluorine-containing interface components and residual char structure.
[0052] (iv) Interface stability test An electrolyte membrane was sandwiched between two stainless steel electrodes to assemble a blocking battery. The initial interfacial impedance and the interfacial impedance after 7 days were tested at 25°C.
[0053] Results analysis: Example 3-1 had the lowest initial interfacial impedance, with a 7-day impedance growth rate of only 18%, which was much lower than that of Comparative Example 3 (42%) and Comparative Example 5 (39%) containing free DOPO; this demonstrates that fixing DOPO to the filler surface via covalent anchoring can significantly reduce the risk of side reactions at the electrode interface caused by free small molecule flame retardants.
[0054] (v) Half-cell cycle performance test Assemble a LiFePO4 / GPE / Li half-cell, cycle at 0.5C rate and 25°C, with a voltage range of 2.5-3.8V. The specific capacity is expressed as the mass of the positive electrode active material, LiFePO4.
[0055] Results analysis: Example 3-1 showed the highest initial capacity (148 mAh / g) and the best capacity retention rate after 100 cycles (92.1%). The comparative example of physically blended free DOPO exhibited the worst cycling performance, with a capacity retention rate approximately 14 percentage points lower than that of Example 3-1. This is because free DOPO molecules migrate to the electrode surface during cycling and undergo side reactions, disrupting the integrity of the SEI film. In contrast, the DOPO groups covalently anchored to the filler surface are fixed at a position far from the electrode interface, significantly reducing the risk of the aforementioned side reactions.
[0056] (vi) Electrochemical stability window test Linear scanning voltammetry (LSV) was used, with a stainless steel electrode as the working electrode and a lithium sheet as the reference / counter electrode, at a scan rate of 1 mV / s.
[0057] Results analysis: The oxidation decomposition potential of Example 3-1 reached 4.82V, which was 0.17V higher than that of Comparative Example 2, indicating that the DOPO-Si-LLZTO interface modification layer helps to suppress the oxidation decomposition of carbonate solvent under high pressure.
[0058] (vii) Cycle stability test of lithium symmetric battery Assemble a Li / GPE / Li symmetric cell at 0.2 mA / cm 2 Constant current charge-discharge cycles were performed at the current density, with each cycle consisting of 0.5 hours of charge and discharge.
[0059] Results analysis: Example 3-1 had a lower initial overpotential, and after 200 hours of cycling, the overpotential only increased to 34mV, which was much lower than the 62mV of Comparative Example 2. This indicates that the DOPO-Si-LLZTO interface modification layer promoted the uniform deposition of lithium ions and effectively suppressed interface degradation.
[0060] (viii) Cyclic performance testing of graphite full cells Using the gel polymer composite electrolytes of Examples 3-1 and Comparative Example 2 as examples, LiFePO4 / GPE / graphite full cells were assembled for cycle performance comparison. The positive electrode was lithium iron phosphate (LiFePO4), and the negative electrode was artificial graphite. Charge-discharge cycles were performed at 0.5C rate and 25°C, with a voltage range of 2.5-3.65V. The specific capacity is based on the mass of the positive electrode active material, LiFePO4.
[0061] Results Analysis: The initial discharge specific capacity of the full cell in Example 3-1 was 142 mAh / g, and the capacity retention rate after 100 cycles was 90.1%, both significantly better than that of Comparative Example 2 (138 mAh / g, 84.8%). The comparison results of the full cell cycle performance were consistent with the trend of the half cell test, proving that the DOPO-Si-LLZTO interface modification layer can also effectively stabilize the electrode / electrolyte interface, suppress side reactions, and improve cycle stability in the graphite anode system.
[0062] It should be noted that, for the sake of simplicity, the foregoing embodiments are all described as a series of actions. However, those skilled in the art should understand that the present invention is not limited to the described order of actions, as some steps may be performed in other orders or simultaneously according to the present invention. Furthermore, those skilled in the art should also understand that the embodiments described in the specification are preferred embodiments, and the actions and modules involved are not necessarily essential to the present invention.
[0063] It should be understood that the disclosed technical solutions in the embodiments provided in this application can be implemented in other ways. For example, the embodiments described above are merely illustrative, and the division of the units described above is only a logical functional division. In actual implementation, there may be other division methods. For example, multiple units or components may be combined or integrated into another system, or some features may be ignored or not executed. Furthermore, the coupling or communication connections shown or discussed may be indirect coupling or communication connections between devices or units through some interfaces, and may be in telecommunications or other forms.
[0064] The units described above as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the units can be selected to achieve the purpose of this embodiment according to actual needs.
[0065] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on these embodiments, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still combine, add, delete, or otherwise adjust the features of the various embodiments of the present invention according to the circumstances without conflict or creative effort, thereby obtaining different technical solutions that do not fundamentally depart from the concept of the present invention. These technical solutions also fall within the scope of protection of the present invention.
Claims
1. A flame-retardant polymer composite electrolyte, comprising a PVDF-HFP polymer base film, a lithium-ion conductive ceramic filler, a lithium salt, and a carbonate plasticizer, characterized in that: The lithium ion conductive ceramic filler is LLZTO particle grafted with DOPO-VTMS on the surface, the chemical composition of the LLZTO is Li6.4La3Zr1.4Ta0.6O12, and the particle size is 100-200 nm. 12 , particle size is 100-200 nm. The DOPO-VTMS is an addition product of DOPO and vinyltrimethoxysilane. The DOPO-VTMS is bonded to the LLZTO surface through a silicon-oxygen structure containing Si-OM bonds. The silicon-oxygen structure may also contain Si-O-Si bonds, where M is La, Zr or Ta. The grafting amount of DOPO-VTMS is 1.0% to 4.0% of the mass of LLZTO; The mass fraction of the LLZTO particles with DOPO-VTMS grafted on the surface in the polymer base film is 8% to 18%.
2. The flame-retardant polymer composite electrolyte as described in claim 1, characterized in that, The PVDF-HFP contains 8% to 12% hexafluoropropylene in molar amounts and has a weight-average molecular weight of 400,000 to 600,000.
3. The flame-retardant polymer composite electrolyte as described in claim 1, characterized in that, The lithium salt is selected from at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI); the plasticizer is a mixed solvent of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate.
4. The flame-retardant polymer composite electrolyte as described in claim 1, characterized in that, The liquid absorption rate of the polymer base film is 150-250 wt%, and the liquid absorption rate is calculated as (m1-m0) / m0×100%, where m0 is the mass of the base film before immersion, and m1 is the mass of the base film after immersion in the electrolyte and removal and blotting of the surface liquid with filter paper.
5. A method for preparing a flame-retardant polymer composite electrolyte as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Under nitrogen protection, DOPO and vinyltrimethoxysilane were dissolved in an organic solvent at a molar ratio of 1:1 to 1:1.2, and 1% to 3% of azobisisobutyronitrile (AIBN) was added as an initiator. The mixture was reacted at 70 to 90 °C for 6 to 12 hours and then distilled under reduced pressure to obtain DOPO-VTMS. (2) Disperse the dried LLZTO in an ethanol / water mixed solvent (volume ratio 95:5), add DOPO-VTMS accounting for 1% to 6% of the LLZTO mass, adjust the acidity of the reaction solution to pH 5.5 to 6.5 with glacial acetic acid, react at 60 to 80°C for 4 to 8 hours, separate by centrifugation, wash thoroughly with anhydrous ethanol, and vacuum dry at 100 to 150°C for 2 to 12 hours to obtain LLZTO filler with DOPO-VTMS grafted on the surface; (3) Add PVDF-HFP and the filler obtained in step (2) to N-methylpyrrolidone and mix evenly. Cast into a film and dry at 60-80℃ to obtain a polymer base film. (4) In an inert atmosphere where the H2O and O2 contents are both less than 1 ppm, the base film obtained in step (3) is immersed in a mixed solution of ethylene carbonate / ethyl methyl carbonate / dimethyl carbonate with 1 mol / L lithium salt for 0.5 to 2 hours for activation. The film is then removed and the surface liquid is dried to obtain the polymer composite electrolyte.
6. A lithium-ion battery, comprising a positive electrode, a graphite negative electrode, and an electrolyte, characterized in that, The electrolyte is the flame-retardant polymer composite electrolyte as described in any one of claims 1 to 4.
7. The lithium-ion battery according to claim 6, characterized in that, The positive electrode is lithium iron phosphate; the lithium salt in the polymer composite electrolyte is LiTFSI.