A method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials and its application.

By characterizing and classifying the polarity of active materials and combining them with external field effects, the problems of long stirring time and poor uniformity of lithium-ion battery slurry were solved, achieving efficient and low-cost battery slurry preparation and improving battery performance and production efficiency.

CN123120903APending Publication Date: 2026-11-17XINGTAI HAI YU LITHIUM BATTERY EQUIP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618437.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery slurry mixing technologies suffer from problems such as long mixing time, high energy consumption, easy agglomeration of active materials, poor uniformity of slurry solid content, and lack of effective control over interfacial polarity interactions, resulting in poor battery performance.

Method used

By characterizing the surface polarity of the active material and classifying its polarity levels, matching solvents and dispersants of corresponding polarities, and applying external fields such as DC electric fields, low-frequency alternating electric fields, or constant magnetic fields during stirring, the active material particles are dispersed and oriented to form a conductive network by utilizing the principles of repulsion between like polarities and attraction between opposite polarities.

Benefits of technology

It significantly shortens the stirring time, improves the uniformity and stability of the slurry's solid content, enhances the conductivity and cycle stability of the electrodes, reduces energy consumption and equipment modification costs, and is suitable for the industrial production of lithium-ion and sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120903A_ABST
    Figure CN123120903A_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the stirring efficiency of lithium-ion battery slurry by utilizing the polarity of active materials, and its application, belonging to the field of battery manufacturing technology. This invention measures the surface polarity of the active material and classifies it into polarity grades. Based on these polarity grades, solvents and dispersants of corresponding polarities are matched. Simultaneously, an external field is applied during stirring. Like-polarity repulsion disperses the active material particles, while opposite-polarity attraction causes the active material particles to directionally bind with conductive agents and binders. Field-induced orientation ensures the active material particles are orderly arranged to form continuous conductive channels. This invention requires no large-scale modification to existing stirring equipment and can be directly integrated into existing slurry mixing processes. The resulting slurry exhibits small deviations in solid content uniformity, shorter stirring time, and smaller fluctuations in electrode resistivity. It is applicable to the preparation of positive and negative electrode slurries for lithium-ion and sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery manufacturing technology, specifically a method and its application for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials. Background Technology

[0002] Lithium-ion batteries possess outstanding advantages such as light weight, large energy storage, high power, no pollution, long lifespan, low self-discharge coefficient, and wide temperature adaptability, making them widely used in mobile devices and electric vehicles. In the manufacturing process of lithium-ion batteries, slurry preparation is the first and one of the most critical steps. Slurry preparation involves thoroughly mixing active materials, conductive agents, binders, and solvents in a mixing tank to create a battery slurry. This slurry is then coated onto the surface of a current collector and dried to form the electrode sheets. The uniformity and stability of the battery slurry directly determine the quality of the electrode sheets and ultimately affect the battery's energy density, cycle life, and safety.

[0003] However, existing battery slurry mixing technologies still have many shortcomings. First, battery slurry is a complex multiphase mixture of non-Newtonian fluids, with significant differences in the physical and chemical properties of its components. Active material powders, especially nanoscale active materials, have high surface energy and are prone to agglomeration during storage and transportation, requiring high shear forces for dispersion. Second, under conventional feeding methods, whether all the powder is added to the tank first and then the solvent, or the solvent is added to the tank first and then the powder, the small contact area between the solvent and powder, and the large differences in the properties of the components, easily lead to the formation of large particle agglomerates or even clumps. These agglomerates are difficult to eliminate before thorough mixing, increasing not only the operating resistance of the mixing components but also the energy consumption during the mixing and dispersion process, severely limiting the slurry mixing efficiency. Third, existing mixing processes mainly rely on mechanical shear force for dispersion, resulting in long mixing times and high energy consumption, typically requiring several hours or even longer to achieve the desired dispersion effect. Fourth, in traditional processes, there is a lack of effective means to control the interfacial polar interactions between active materials and solvents, dispersants, conductive agents and binders. The compatibility between the components is poor, resulting in poor uniformity of solid content in the slurry and difficulty in ensuring coating consistency, which in turn affects the electrochemical performance of the battery.

[0004] To address the aforementioned issues, existing research has attempted to improve mixing efficiency by optimizing the feeding sequence, adding grinding and dispersion processes, or improving mixing equipment. For example, adding a high-speed grinding and dispersion process during the batching process can improve the dispersion efficiency of conductive agents, or the main and auxiliary materials can be mixed and then dispersed and extruded multiple times to improve the dispersion effect. However, such improvements are still limited to the effect of pure mechanical force and cannot fundamentally solve the problems of active material agglomeration and the difficulty in precisely controlling the interfacial interactions between the components of the slurry. Summary of the Invention

[0005] The purpose of this invention is to provide a method and its application for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials, in order to solve the prominent problems in the prior art, such as long stirring time, high energy consumption, easy agglomeration of active materials, poor uniformity of slurry solid content, difficulty in ensuring coating consistency, and lack of effective means to control the interfacial polarity interaction between active materials and solvents, dispersants, conductive agents, and binders, which are caused by relying solely on mechanical shear force.

[0006] During the research process of this invention, it was discovered that by characterizing the surface polarity of the active material and classifying it into polarity grades, and matching solvents and dispersants of corresponding polarities according to the polarity grades, the interfacial compatibility of each component in the slurry at the molecular level can be optimized. Simultaneously, an external field is applied during stirring, utilizing the repulsion of like polarities to disperse the active material particles and ensure uniform dispersion of the dispersant, binder, and conductive agent, preventing agglomeration. Without the need for multiple grinding and dispersion processes or complex equipment modifications, the agglomeration tendency of the active material can be reduced at its source, stirring time shortened, and the uniformity and stability of the slurry's solid content improved. The resulting slurry, after coating, produces electrode sheets with uniform surface resistivity and minimal fluctuations.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows:

[0008] In a first aspect, a method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials is provided, comprising the following steps:

[0009] S1. Measure the surface polarity of the active material, and classify the active material into polarity grades based on the measurement results, wherein the polarity grades include high polarity grades and low polarity grades;

[0010] S2. For highly polar active materials, use polar solvents and polar dispersants; for low-polar active materials, use weakly polar solvents and weakly polar dispersants.

[0011] S3. Mix the graded active material with the selected solvent, dispersant, conductive agent and binder, and apply an external field while stirring;

[0012] S4. Under the action of the external field, the active material particles are dispersed by the repulsion of like polarities, and the active material particles are oriented to combine with the conductive agent and binder by the attraction of opposite polarities. The active material particles are arranged in an orderly manner by the field-induced orientation effect generated by the external field to form a conductive network, and the stirring ends.

[0013] By characterizing and classifying the surface polarity of active materials and matching solvents and dispersants of corresponding polarities according to polarity differences, the interfacial compatibility of each component in the slurry was optimized at the molecular level, reducing the tendency of active materials to agglomerate from the source. On this basis, by utilizing the synergistic effect of like-polarity repulsion, dissimilar-polarity attraction and field-induced orientation generated by external fields, the rapid and uniform dispersion and orderly arrangement of active materials were achieved, thereby significantly reducing the shear resistance during the stirring process and greatly shortening the stirring time.

[0014] As a limitation of the present invention, the active material includes lithium transition metal oxide positive electrode active material, sodium transition metal oxide positive electrode active material, carbon-based negative electrode active material, silicon-based negative electrode active material or alloy-based negative electrode active material.

[0015] The external field is at least one of a DC electric field, a low-frequency alternating electric field with a frequency ≤ 1 kHz, and a constant magnetic field.

[0016] Since different types of active materials have different electrical conductivity and magnetic susceptibility characteristics, by selecting appropriate external field types, such as electric field acting on charged particles, magnetic field acting on magnetic or conductive particles, and electromagnetic field combining the advantages of both, the directional migration and arrangement efficiency of each component in the slurry system after polarity matching can be specifically enhanced, ensuring that different material systems can obtain the best dispersion effect and conductive network construction capability.

[0017] As another limitation of the present invention, when the external field includes an electric field, the electric field strength is 1~100 kV / m; when the external field includes a magnetic field, the magnetic field strength is 0.1~2T.

[0018] The specific values ​​of the electric field strength and magnetic field strength are set according to the dielectric constant and magnetic susceptibility of the active material in the slurry, so as to generate dipole polarization or magnetic dipole orientation on the surface of the active material particles, thereby enhancing the dispersion uniformity between particles.

[0019] By controlling the external field parameters within the above range, sufficient field force can be generated to overcome the van der Waals forces and electrostatic forces between active material particles, effectively breaking up agglomerates and inducing particle orientation. At the same time, it avoids adverse effects such as local overheating of the slurry, solvent evaporation, or damage to the active material structure caused by excessive field strength, while ensuring the safety and feasibility of industrial applications.

[0020] As a further limitation of the present invention, step S1 includes the following steps:

[0021] The polarity index of the active material is measured to obtain a polarity measurement value. The polarity index is at least one of surface functional group polarity, dipole moment and surface energy polarity component.

[0022] The polarity measurement values ​​are compared with the corresponding polarity index thresholds, and the active materials are classified into high polarity grades or low polarity grades based on the comparison results.

[0023] The surface functional group polarity is characterized by the presence or absence of oxygen-containing and / or nitrogen-containing functional groups. The presence of oxygen-containing and / or nitrogen-containing functional groups qualifies as a high polarity level, while the absence of these groups qualifies as a low polarity level. A dipole moment measurement > 1.5D qualifies as a high polarity level, otherwise a low polarity level. A surface energy polarity component measurement > 10 mJ / m 2 If the polarity is high, it is classified as a high polarity level; otherwise, it is classified as a low polarity level.

[0024] When the same active material is measured using at least two indicators simultaneously and the results of the determination of the indicators are contradictory, the final grade shall be determined according to the following rules:

[0025] Weighting rules: Surface functional group polarity weight 40%, dipole moment weight 35%, surface energy polarity component weight 25%; high polarity level is scored 2 points, low polarity level is scored 0 points; unmeasured indicators do not participate in the weighting, and their weights are normalized according to the other participating indicators; when the total weighted score is ≥1.5, it is a high polarity level, otherwise it is a low polarity level;

[0026] Special determination rule: When the surface functional group polarity is determined to be of a high polarity level and the dipole moment is determined to be of a low polarity level, the surface functional group polarity determination result shall be used as the final level. This special determination rule takes precedence over the weighted rule.

[0027] By employing various characterization methods such as surface energy, dipole moment, and functional group polarity, the surface polarity characteristics of active materials can be comprehensively evaluated from multiple dimensions, including charge state, surface tension, molecular dipole, and chemical bond properties. This avoids the judgment bias that may be caused by a single indicator, thereby achieving accurate classification of the polarity of active materials and providing a reliable basis for the subsequent scientific matching of solvents and dispersants.

[0028] As a further limitation of the present invention, in step S2:

[0029] For the aforementioned high-polarity grade active material, a polar solvent and a polar dispersant are mixed, wherein the polar solvent is N-methylpyrrolidone and the polar dispersant is polyvinylpyrrolidone;

[0030] For the aforementioned low-polarity grade active material, a weakly polar solvent and a weakly polar dispersant are used for mixing. The weakly polar solvent is an aqueous ethanol solution, and the weakly polar dispersant is sodium carboxymethyl cellulose; and / or

[0031] The high-polarity active material is a ternary material, lithium iron phosphate, lithium manganese oxide, or a material with SiO2 on its surface. XThe material is selected from at least one of silicon-based anode materials containing hydroxyl groups on the surface; the low polarity grade active material is selected from at least one of graphite and lithium cobalt oxide; wherein X is 0 or 2.

[0032] As a further limitation of the present invention, the stirring in step S3 includes a pre-stirring stage, a high-speed dispersion stage and a vacuum degassing stage performed sequentially, and the external field is applied at least in the high-speed dispersion stage; the conductive agent includes at least one of carbon nanotubes and conductive carbon black, and when the conductive agent is a combination of carbon nanotubes and conductive carbon black, the mass ratio of the carbon nanotubes to the conductive carbon black is (0.3~0.8):(1~2).

[0033] The adhesive includes polyvinylidene fluoride, or at least one of styrene-butadiene rubber and sodium carboxymethyl cellulose; when the adhesive is a combination of styrene-butadiene rubber and sodium carboxymethyl cellulose, the mass ratio of styrene-butadiene rubber to sodium carboxymethyl cellulose is (1-3):(1-2).

[0034] The pre-mixing stage achieves initial mixing of the components, avoiding dust generation and localized agglomeration caused by direct high-speed mixing of powders. The high-speed dispersion stage, combined with the application of an external field, utilizes the synergistic effect of mechanical shear force and field-induced force to achieve full dispersion and directional alignment of the active materials. The vacuum degassing stage removes air bubbles introduced during high-speed dispersion, ensuring the density of the slurry and the quality of coating. Applying an external field at least throughout the high-speed dispersion stage maximizes its control over particle dispersion and alignment. Furthermore, by optimizing the synergistic combination of conductive agents and binders, the electronic conduction path and mechanical properties of the slurry are further improved.

[0035] As another limitation of the present invention, the pre-stirring stage involves dissolving the binder in a solvent, then adding the dispersant, conductive agent and active material and stirring to mix the components.

[0036] The stirring rate during the high-speed dispersion stage is 1800~4000 rpm, and the dispersion time is 30~60 min;

[0037] The vacuum degassing stage involves stirring the slurry that has undergone the high-speed dispersion stage under vacuum conditions to remove air bubbles.

[0038] As a further limitation of the present invention, in step S4, the active material particles are oriented and distributed from the electrode current collector side to the slurry surface layer along the direction of the external field, thereby forming a continuous conductive channel in the electrode thickness direction.

[0039] The orientation distribution is observed under a scanning electron microscope, and the proportion of particles with an angle ≤30° between the long axis of the active material particles and the direction of the external field is ≥60% of the total number of particles.

[0040] By utilizing field-induced orientation, the active material particles are arranged in an orderly manner from the current collector side to the slurry surface along the direction of the external field, forming a continuous conductive channel that runs through the entire electrode thickness. This significantly shortens the electron transport path from the active material to the current collector and reduces the electrode resistivity. At the same time, this orderly arrangement avoids the random stacking of active material particles, reduces the contact resistance between particles, and improves the rate performance and cycle stability of the electrode.

[0041] As a further limitation of the present invention, the uniformity deviation of the solid content of the battery slurry is controlled within ±1%, the sedimentation rate after standing for 24 hours is ≤5%, and the resistivity fluctuation range of the electrode obtained after coating the battery slurry is ≤10%.

[0042] Secondly, the present invention also provides the application of the above-mentioned method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials in the preparation of sodium-ion or lithium-ion battery slurry.

[0043] By adopting the above technical solution, the technical progress achieved by this invention compared with the prior art is as follows:

[0044] (1) This invention characterizes the active material by measuring its surface energy, dipole moment, or surface functional group polarity, and classifies the measured values ​​into high-polarity and low-polarity levels by comparing them with preset thresholds. Based on this classification, solvents and dispersants of corresponding polarities are matched according to the classification results, thereby optimizing the interfacial compatibility between the active material and the solvent and dispersant at the molecular level, reducing the driving force for the aggregation of active material particles from the source. The comparison of the dispersion state of the slurry before and after polarity matching shows that the aggregation of active materials is obvious without polarity matching, while the dispersion uniformity of the slurry is significantly improved after polarity matching, proving the key role of classification based on surface polarity measurement results and matching solvents and dispersants of corresponding polarities in inhibiting the aggregation of active materials.

[0045] (2) This invention applies at least one external field, including a DC electric field, an alternating electric field, and a constant magnetic field, during the stirring process. This utilizes the principle of repulsion between like polarities to disperse the active material particles, and the principle of attraction between opposite polarities to form a directional bond between the active material, the conductive agent, and the binder. Simultaneously, the field-induced orientation causes the active material to align orderly along the direction of the external field, forming continuous conductive channels. This achieves the synergistic dispersion of mechanical shear force and field-induced force. The comparison of stirring time results shows that the method of this invention can shorten the slurry stirring time to less than 50% of the conventional stirring time, proving that the synergistic effect of polarity matching and the external field can significantly reduce the shear resistance during stirring and greatly shorten the stirring time.

[0046] (3) This invention improves the compatibility of active materials with solvents and dispersants from the source by polarity matching, reducing the driving force of particle agglomeration; it fully disperses active material particles through the repulsion of like polarities in the external field, avoiding slurry stratification caused by gravity sedimentation; and it forms a strong interfacial bond and orderly spatial arrangement between active materials, conductive agents, and binders through the attraction of opposite polarities and field-induced orientation. The synergistic effect of the three ensures the long-term stability and consistency of the slurry during storage and coating. The uniformity deviation of the slurry solid content can be controlled within ±1%, the sedimentation rate after standing for 24 hours is ≤5%, and the resistivity fluctuation range of the electrode after coating is ≤10%. This shows that the method of this invention significantly improves the storage stability, coating consistency, and electrode conductivity uniformity of the slurry, thereby improving the first discharge specific capacity and cycle stability of the battery.

[0047] (4) The method of the present invention is simple to operate and does not require large-scale modification of existing stirring equipment. It only requires the addition of at least one of an electric field generating device, a magnetic field generating device, or an electromagnetic wave irradiation device to the existing stirring equipment. The equipment modification cost is low, the footprint is small, and the operation interface is user-friendly. It is suitable for the large-scale industrial production of positive and negative electrode slurries for lithium-ion batteries and sodium-ion batteries. At the same time, due to the significant reduction in stirring time, the equipment's capacity per unit time is significantly increased, and energy consumption and labor costs are correspondingly reduced, resulting in significant cost and production efficiency advantages. Attached Figure Description

[0048] Figure 1 This is a schematic flowchart of the method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to the present invention.

[0049] Figure 2 This is a schematic diagram of the dispersion state of the active material in the slurry treated by the method of the present invention in Example 1 of the present invention;

[0050] Figure 3 This is a SEM image of the battery slurry after polarity matching and external field synergistic treatment applied to the substrate and dried in Example 1 of the present invention.

[0051] Figure 4 This is a SEM image of the battery slurry in Comparative Example 1 after it was coated onto the substrate and dried, without polarity matching and external field treatment.

[0052] Figure 5 This is a comparison chart of the resistivity variation coefficient (COV) and long-term stability of battery electrodes made from the slurries obtained in Example 1 and Comparative Example 1 of the present invention. Detailed Implementation

[0053] The technical solution of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. Figure 1This is a flowchart illustrating the method for improving the stirring efficiency of ion battery slurry using the polarity of active materials according to the present invention. The method mainly includes four core steps: surface polarity measurement and classification, polarity matching of solvent and dispersant, application of an external field, and uniform mixing and dispersion of slurry components by repulsion of like polarities. The following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention.

[0054] This invention provides a method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials. The following description, in conjunction with specific embodiments, illustrates this method.

[0055] Example 1

[0056] This embodiment uses the preparation of lithium-ion battery negative electrode slurry as an example to illustrate the method of the present invention.

[0057] S1. Measure the surface polarity of the active material and classify the active material into polarity grades based on the measurement results.

[0058] Spherical graphite samples, used as negative electrode active materials, were analyzed using XPS and infrared spectroscopy. The graphite basal surface showed virtually no polarity, with the surface functional group polarity entirely contributed by oxygen-containing functional groups at the edge defects. Overall, the graphite exhibited weak polarity and was therefore classified as low polarity. The surface energy polarity component, measured using a contact angle meter, was found to be 2.4 ± 0.8 mJ / m. 2 Because its surface energy measurement value is <10mJ / m 2 Therefore, it is classified as a low polarity level.

[0059] Based on the above determination of the surface functional group polarity and surface energy of spheroidal graphite, the conclusion is consistent: all are classified as low polarity. In other embodiments, surface polarity measurement is not limited to the above method; other characterization methods known in the art, such as dipole moment measurement, can also be used.

[0060] S2. For low-polarity active materials, use weakly polar solvents and weakly polar dispersants.

[0061] Based on the S1 classification results, this type of spherical graphite active material belongs to the low polarity category. Therefore, a mixed solvent of deionized water and ethanol, with a volume ratio of 95:5, was selected as the solvent. Sodium carboxymethyl cellulose, a weakly polar dispersant, was chosen as the dispersant. A combination of equal masses of styrene-butadiene rubber latex and sodium carboxymethyl cellulose was selected as the binder, and conductive carbon black was selected as the conductive agent.

[0062] S3. Mix the graded active material with the selected solvent, dispersant, conductive agent and binder, and apply an external field while stirring.

[0063] The stirring in this step includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage.

[0064] Pre-stirring stage: Sodium carboxymethyl cellulose dispersant is added to a mixed solvent of water and ethanol and fully dissolved under low-speed stirring to form a uniform colloid; then conductive carbon black conductive agent is added and stirring is continued to disperse it initially; then spherical graphite negative electrode active material after S1 polarity classification is slowly added and pre-stirred to allow the components to mix initially.

[0065] High-speed dispersion stage: The pre-mixed slurry is transferred to a high-speed dispersion mixer equipped with an electric field generator. The mixing speed is set to 1800 rpm and the dispersion time is 30 min. The mixer is started to carry out high-speed dispersion and mixing. At the same time, a DC electric field is applied as an external field with an electric field strength of 10 kV / m.

[0066] Finally, add the binder styrene-butadiene rubber latex and stir at low speed to obtain the non-defoamed negative electrode slurry.

[0067] Vacuum degassing stage: After adding styrene-butadiene rubber latex binder and stirring at low speed, the slurry is transferred to a vacuum mixer and stirred at low speed under vacuum conditions to remove the air bubbles introduced during high-speed dispersion, thereby obtaining a uniform and stable negative electrode slurry.

[0068] S4. Under the action of an external field, the active material particles are dispersed from the dispersant, binder and conductive agent by the repulsion of like polarities, and the active material particles are oriented to bind with the conductive agent and binder by the attraction of opposite polarities. The field-induced orientation effect generated by the external field causes the active material particles to be arranged in an orderly manner to form a conductive network, and the stirring ends.

[0069] Specifically, under the action of a 10kV / m DC electric field, the spherical graphite active material with the same polarity repels the binder and conductive agent due to the repulsion of the same polarity, effectively preventing the agglomeration of the binder and conductive agent. Figure 2 This is a schematic diagram of the dispersion state of each component in the slurry after polarity matching and external field synergistic treatment in Embodiment 1 of the present invention. As shown in the figure, the binder and conductive agent are uniformly distributed in the gaps between the active material particles, overlapping to form a through-hole three-dimensional conductive network. Each active material particle is in contact with the conductive agent, resulting in low electron transport resistance and low internal resistance; at the same time, lithium ions can contact the surface of all active material particles, ensuring sufficient charging and discharging.

[0070] Figure 3 The image shows SEM images of the components in the slurry after polarity matching and external field synergistic treatment in Example 1 of the present invention. No agglomerated binder or conductive agent is shown in the image, indicating that the components in the slurry are evenly distributed.

[0071] Testing revealed that the stirring time for the negative electrode slurry prepared in this embodiment was 2.5 hours, while the same slurry prepared using conventional methods required 6 hours, reducing the stirring time to approximately 42% of the conventional stirring time. The uniformity deviation of the slurry solid content was controlled within ±0.8%, which is better than the ±3% of conventional methods. The coated electrode surface was uniform, free of agglomeration spots, and the electrode resistivity was significantly reduced.

[0072] Example 2

[0073] This embodiment uses the preparation of lithium-ion battery cathode slurry as an example to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a ternary 811 sample of the cathode active material is used. XPS and infrared spectroscopy are used to detect the surface functional group polarity of the ternary 811 sample, and the detection shows that it belongs to a high-polarity oxide, thus classifying it as a high-polarity grade. The surface energy polarity component measured using a contact angle meter is 18 ± 0.8 mJ / m. 2 Because its surface energy measurement value is >10mJ / m 2 Therefore, it is classified as a high polarity level.

[0074] Based on the above determination of the polarity of the surface functional groups and surface energy of the ternary 811, the conclusion is consistent: all are classified as high polarity.

[0075] Based on the classification results of the high polarity level in S2, polar solvents and polar dispersants are selected. Specifically, N-methylpyrrolidone is selected as the polar solvent, polyvinylpyrrolidone as the polar dispersant, non-polar polyvinylidene fluoride is selected as the binder, and a composite conductive agent of non-polar carbon nanotubes and conductive carbon black Super-P is selected as the conductive agent.

[0076] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. In the pre-stirring stage, polyvinylidene fluoride and polyvinylpyrrolidone are dissolved and dispersed in N-methylpyrrolidone solvent, followed by the addition of a composite conductive agent consisting of carbon nanotubes and conductive carbon black, and a ternary 811 active material, followed by stirring. During the high-speed dispersion stage, a constant magnetic field with a strength of 0.5T is applied as the external field. The vacuum degassing stage is the same as S3 in Example 1.

[0077] In S4, under the influence of a 0.5T magnetic field, the ternary 811 active material particles are uniformly dispersed due to the repulsion between particles of the same polarity and between the active particles and the dispersant. Utilizing the principle of attraction between opposite polarities, the active material forms a directional bond with the conductive agent and binder. Simultaneously, through field-induced orientation, the active material is ordered along the direction of the external field to form a continuous conductive channel. Testing showed that the stirring time of the negative electrode slurry prepared in this embodiment was shortened from 5 hours in the conventional method to 2 hours, reducing the stirring time to 40% of the conventional stirring time. The uniformity deviation of the slurry solid content was controlled within ±0.9%. The surface of the coated positive electrode sheet was uniform.

[0078] Example 3

[0079] This embodiment uses the preparation of sodium-ion battery cathode slurry as an example to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a sample of layered oxide NaNi1 / 3Fe1 / 3Mn1 / 3O2, a sodium-ion battery cathode active material, was taken. After testing, all polarity measurement values ​​were higher than the preset threshold, so this batch of sodium-ion battery cathode active material was classified as high polarity grade.

[0080] Based on the classification results of high polarity levels in S2, N-methylpyrrolidone, a polar solvent, was selected as the solvent, and polyvinylpyrrolidone, a polar dispersant, was selected as the dispersant. Non-polar polyvinylidene fluoride was selected as the binder, and a composite conductive agent of non-polar carbon nanotubes and conductive carbon black Super-P was selected as the conductive agent.

[0081] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. The pre-stirring stage is the same as the S3 pre-stirring stage in Example 1. During the high-speed dispersion stage, a DC electric field and a constant magnetic field are applied simultaneously as external fields, i.e., an electromagnetic field, where the DC electric field strength is 5 kV / m and the constant magnetic field strength is 0.1 T. The vacuum degassing stage is the same as S3 in Example 1.

[0082] In S4, under the combined effect of a DC electric field and a constant magnetic field, the layered oxide active material particles repel and disperse each other due to the repulsion of like polarities, and form directional bonds with the conductive agent and binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect makes the active material particles arrange themselves in an orderly manner along the direction of the external field.

[0083] Testing revealed that the stirring time of the positive electrode slurry prepared in this embodiment was significantly shortened, and the slurry solid content uniformity was good, proving that the method of the present invention is also applicable to sodium-ion battery systems.

[0084] Example 4

[0085] This embodiment uses the preparation of lithium-ion battery anode slurry as an example, and selects silicon suboxide (SiO) as a silicon-based anode active material to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a silicon suboxide sample is taken, its surface Zeta potential is measured using a Zeta potential analyzer, its molecular dipole moment is determined using a dipole moment measurement method, and the polarity of its surface functional groups is analyzed using infrared spectroscopy. The test results show that the absolute value of the surface Zeta potential and the measured dipole moment of the silicon suboxide sample are both higher than the preset threshold, indicating strong polarity of the surface oxygen-containing functional groups. Since all measured values ​​are higher than the preset threshold, this batch of silicon-based anode active material is classified as high polarity material.

[0086] Based on the classification results of high polarity levels in S2, N-methylpyrrolidone, a polar solvent, was selected as the solvent, and polyvinylpyrrolidone, a polar dispersant, was selected as the dispersant. Non-polar polyvinylidene fluoride was selected as the binder, and non-polar carbon nanotubes were selected as the conductive agent.

[0087] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. In the pre-stirring stage, the polyvinylidene fluoride binder is dissolved in N-methylpyrrolidone solvent, followed by the addition of carbon nanotubes and silica-containing active materials and stirring. During the high-speed dispersion stage, a low-frequency alternating electric field with a frequency of 1 kHz and a field strength of 50 kV / m is applied as the external field. The vacuum degassing stage is the same as S3 in Example 1.

[0088] In S4, under the action of a low-frequency alternating electric field of 50kV / m and 1kHz, the silicon suboxide active material particles repel and disperse each other due to the repulsion of like polarities, and form directional bonds with the carbon nanotube conductive agent and polyvinylidene fluoride binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect makes the silicon suboxide active material particles arrange themselves in an orderly manner along the direction of the alternating electric field.

[0089] Testing revealed that the stirring time for silicon-based anode slurry dispersed using an alternating electric field was reduced to less than 45% of the conventional stirring time, and the uniformity deviation of the slurry solid content was controlled within ±1%. The coated electrode surface was uniform and free of agglomeration.

[0090] Example 5

[0091] This embodiment uses the preparation of lithium-ion battery negative electrode slurry as an example, and selects tin-cobalt alloy as an alloy-type negative electrode active material to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a tin-cobalt alloy sample is taken, and its surface zeta potential is measured using a zeta potential analyzer, and its surface energy is measured using a contact angle meter. Upon testing, the absolute value of the surface zeta potential and the measured surface energy of the tin-cobalt alloy sample are both lower than the preset threshold; therefore, this batch of alloy-type negative electrode active material is classified as low polarity.

[0092] Based on the classification results of the low polarity grades in S2, a weakly polar solvent, ethanol aqueous solution, was selected as the solvent, and a weakly polar dispersant, sodium carboxymethyl cellulose, was selected as the dispersant. A combination of styrene-butadiene rubber and sodium carboxymethyl cellulose was selected as the binder, and conductive carbon black was selected as the conductive agent.

[0093] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. In the pre-stirring stage, styrene-butadiene rubber and sodium carboxymethyl cellulose are added to an ethanol-water solution and dispersed evenly, followed by the addition of conductive carbon black and tin-cobalt alloy active material and stirring. During the high-speed dispersion stage, a constant magnetic field with a strength of 2T is applied as the external field. The vacuum degassing stage is the same as S3 in Example 1.

[0094] In S4, under the action of a constant magnetic field of 2T, the active material particles of tin-cobalt alloy repel each other due to the repulsion of like polarities and disperse, while forming a directional bond with conductive carbon black and styrene-butadiene rubber / sodium carboxymethyl cellulose binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect causes the active material particles of tin-cobalt alloy to be arranged in an orderly manner along the direction of the magnetic field.

[0095] Testing showed that the stirring time of the alloy anode slurry dispersed by magnetic field was reduced to less than 48% of the conventional stirring time, and the uniformity deviation of the solid content of the slurry was controlled within ±0.9%, proving the applicability of the method of the present invention to alloy anode materials.

[0096] Example 6

[0097] This embodiment uses the preparation of lithium-ion battery cathode slurry as an example, selecting lithium cobalt oxide (LiCoO2) as the cathode active material to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a lithium cobalt oxide sample is taken, its surface Zeta potential is measured using a Zeta potential analyzer, its surface energy is measured using a contact angle meter, its dipole moment is determined using a dipole moment measurement method, and the polarity of its surface functional groups is analyzed using infrared spectroscopy. The test results show that the absolute value of the surface Zeta potential, surface energy, and dipole moment of this lithium cobalt oxide sample are all higher than preset thresholds, indicating strong surface functional group polarity. Since all measured values ​​are higher than the preset thresholds, this batch of cathode active material is classified as high polarity material.

[0098] Based on the classification results of high polarity levels in S2, N-methylpyrrolidone, a polar solvent, was selected as the solvent, and polyvinylpyrrolidone, a polar dispersant, was selected as the dispersant. Non-polar polyvinylidene fluoride was selected as the binder, and a composite conductive agent of non-polar carbon nanotubes and conductive carbon black Super-P was selected as the conductive agent.

[0099] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. The pre-stirring stage is the same as the S3 pre-stirring stage in Example 1. During the high-speed dispersion stage, a low-frequency electric field with a frequency ≤1kHz is applied as the external field, with an electric field strength of 100kV / m. The vacuum degassing stage is the same as S3 in Example 1.

[0100] In S4, under the action of a 100kV / m electric field, the lithium cobalt oxide active material particles repel and disperse from each other due to the repulsion of like polarities, and form directional bonds with the conductive agent and polyvinylidene fluoride binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect makes the lithium cobalt oxide active material particles arrange themselves in an orderly manner along the direction of the pulsed electric field.

[0101] Testing revealed that the stirring time for the positive electrode slurry dispersed using a pulsed electric field was reduced to less than 42% of the conventional stirring time, and the uniformity deviation of the slurry solid content was controlled within ±0.7%. The resistivity fluctuation range of the coated electrode was ≤10%, demonstrating the effectiveness of the pulsed electric field implementation method in this invention.

[0102] Example 7

[0103] This embodiment uses the preparation of sodium-ion battery negative electrode slurry as an example, and selects hard carbon as the negative electrode active material to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a hard carbon sample is taken, and its surface Zeta potential is measured using a Zeta potential analyzer, and its surface energy is measured using a contact angle meter. Upon testing, the absolute value of the surface Zeta potential and the measured surface energy of the hard carbon sample are both lower than the preset threshold; therefore, this batch of carbon-based negative electrode active material is classified as low polarity.

[0104] Based on the classification results of the low polarity grades in S2, a weakly polar solvent, ethanol aqueous solution, was selected as the solvent, and a weakly polar dispersant, sodium carboxymethyl cellulose, was selected as the dispersant. A combination of styrene-butadiene rubber and sodium carboxymethyl cellulose was selected as the binder, and conductive carbon black Super-P was selected as the conductive agent.

[0105] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. In the pre-stirring stage, styrene-butadiene rubber and sodium carboxymethyl cellulose are dispersed in an aqueous ethanol solution, followed by the addition of conductive carbon black Super-P and hard carbon active material, and then stirred. During the high-speed dispersion stage, a constant magnetic field with a strength of 1T is applied as the external field. The vacuum degassing stage is the same as S3 in Example 1.

[0106] In S4, under the action of a constant magnetic field of 1T, the hard carbon active material particles repel and disperse each other due to the repulsion of like polarities, and form a directional bond with conductive carbon black Super-P and styrene-butadiene rubber / sodium carboxymethyl cellulose binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect makes the hard carbon active material particles arrange themselves in an orderly manner along the direction of the constant magnetic field.

[0107] Testing revealed that the stirring time of the hard carbon negative electrode slurry dispersed with constant magnetic field assistance was reduced to less than 48% of the conventional stirring time, the uniformity deviation of the slurry solid content was controlled within ±0.8%, and the sedimentation rate after standing for 24 hours was ≤5%, proving the effectiveness of the constant magnetic field implementation method in this invention.

[0108] Example 8

[0109] This embodiment uses the preparation of lithium-ion battery cathode slurry as an example, selecting lithium iron phosphate (LiFePO4) as the cathode active material to illustrate the method of the present invention. The difference between S1 and S1 in Example 1 is that in this embodiment, a lithium iron phosphate sample is taken, its surface zeta potential is measured using a zeta potential analyzer, its surface energy is measured using a contact angle meter, and the polarity of its surface functional groups is analyzed using infrared spectroscopy. The test results show that the absolute value of the surface zeta potential and the measured surface energy of the lithium iron phosphate sample are both higher than the preset thresholds, indicating strong surface functional group polarity. Since all measured values ​​are higher than the preset thresholds, this batch of cathode active material is classified as high polarity material.

[0110] Based on the classification results of high polarity levels in S2, N-methylpyrrolidone, a polar solvent, was selected as the solvent, and polyvinylpyrrolidone, a polar dispersant, was selected as the dispersant. Non-polar polyvinylidene fluoride was selected as the binder, and non-polar carbon nanotubes were selected as the conductive agent.

[0111] The stirring in S3 also includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, with an external field applied during the high-speed dispersion stage. In the pre-stirring stage, the polyvinylidene fluoride binder is dissolved in N-methylpyrrolidone solvent, followed by the addition of carbon nanotubes and lithium iron phosphate active material, and then stirred. Electromagnetic wave irradiation is applied as the external field during the high-speed dispersion stage. The vacuum degassing stage is the same as S3 in Example 1.

[0112] In S4, under the irradiation of electromagnetic waves, the lithium iron phosphate active material particles repel and disperse from each other due to the repulsion of like polarities, and form directional bonds with the carbon nanotube conductive agent and polyvinylidene fluoride binder due to the attraction of opposite polarities. At the same time, the field-induced orientation effect makes the lithium iron phosphate active material particles arrange themselves in an orderly manner along the direction of electromagnetic waves.

[0113] Testing revealed that the stirring time of the lithium iron phosphate cathode slurry dispersed by electromagnetic wave irradiation was significantly shortened, the uniformity deviation of the slurry solid content was controlled within ±1%, and the resistivity fluctuation range of the coated electrode was ≤10%, proving the effectiveness of the electromagnetic wave irradiation implementation method in this invention.

[0114] Comparative Example 1

[0115] This comparative example uses the same negative electrode active material as in Example 1: spherical graphite, a mixed solvent consisting of deionized water and ethanol, dispersant sodium polymethyl cellulose, conductive agent conductive carbon black, and binder styrene-butadiene rubber latex, prepared according to conventional processes. The specific operation is as follows: the mixed solvents deionized water and ethanol, dispersant sodium polymethyl polycellulose, conductive carbon black, spherical graphite negative electrode active material, and styrene-butadiene rubber latex are added to a planetary mixer in the same proportions as in Example 1, and the mixture undergoes a pre-stirring stage, a high-speed dispersion stage, and a low-speed stirring and vacuum degassing stage with the binder. The polarity measurement and polarity classification of the active material in step S1 are not performed, nor is the selection of polarity-matching solvent and dispersant in step S2. No external field is applied during the high-speed dispersion stage.

[0116] The results showed that the stirring time of Comparative Example 1 was 6 hours, which was much longer than the 2.5 hours of Example 1. Significant agglomeration of the components in the slurry was observed, and the uniformity of the solid content deviated by more than ±3%. Uneven spots were present on the surface of the coated electrode, and the electrode resistivity was high. Figure 4 The image shows a SEM image of the slurry from Comparative Example 1 that was not subjected to polarity matching and external field treatment. As shown in the figure, the agglomeration of the binder and conductive agent is obvious, and the agglomerates are attached to the surface of the active graphite particles. Figure 5 This is a comparison chart of the resistivity fluctuations of the battery electrode sheet prepared in Example 1 of this invention and the battery electrode sheet prepared in Comparative Example 1. COV1-10 represents the coefficient of variation of the resistance values ​​at 10 locations on 10 sample electrode sheets, used to characterize the resistivity fluctuations of the electrode sheets. The electrode resistance was measured using an electrode internal resistance meter, with resistance values ​​in mΩ. The test data are shown in Tables 1 and 2.

[0117] Table 1. Resistivity fluctuation of the battery electrode prepared in Example 1

[0118] Table 2. Resistivity fluctuation of the battery electrode prepared in Comparative Example 1

[0119] As shown in Table 1, the resistivity variation coefficient COV of the electrode prepared in Example 1 of the present invention has been stable in the range of 0.2% to 0.45% for a long time, with a smooth curve and minimal fluctuation.

[0120] As shown in Table 2 and Figure 5As shown, the resistivity variation coefficient (COV) of the electrode prepared in Comparative Example 1 was as high as 1.1% to 1.65%, with significant batch-to-batch fluctuations. Compared with traditional processes, this technical solution can significantly reduce the resistivity dispersion of the electrode, significantly improve the conductivity consistency and batch-to-batch production stability of the electrode, and effectively optimize the uniformity of cell internal resistance, cycle durability, and rate electrochemical performance, demonstrating significant and superior technical benefits. The electrochemical performance of the battery is inferior to that of Example 1.

[0121] Comparative Example 2

[0122] This comparative example uses the same negative electrode active material as in Example 1: spherical graphite, deionized water, and ethanol as the mixed solvent. The dispersant is sodium polymethyl cellulose, the conductive carbon black is used as the conductive agent, and the binder is styrene-butadiene rubber latex. Only step S1 (active material polarity measurement and polarity classification) and step S2 (polarity matching solvent and dispersant selection) are performed. However, no external field is applied during the high-speed dispersion stage in step S3. The specific operation is as follows: First, the spherical graphite is measured for surface polarity in step S1 and classified into a low polarity level, using the same method as in Example 1. Then, the components are added to a planetary mixer and sequentially subjected to a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage. No electric, magnetic, or electromagnetic fields are applied during the high-speed dispersion stage.

[0123] The results showed that the stirring time of Comparative Example 2 was 4 hours, which was better than that of Comparative Example 1, but still longer than that of Example 1. The uniformity of slurry dispersion was improved, but the directional alignment of the active material particles in step S4 was not good, and the continuity of the conductive network was not as good as that of Example 1. This indicates that although simple polarity matching has a certain improvement effect, the best stirring efficiency improvement effect can only be achieved by the synergistic effect of polarity matching and external field.

[0124] Comparative Example 3

[0125] This comparative example uses the same negative electrode active material as Example 2: artificial graphite; solvent: a mixture of deionized water and ethanol; binders: styrene-butadiene rubber and sodium carboxymethyl cellulose; and conductive agent: conductive carbon black. An alternating magnetic field is applied as an external field during the high-speed dispersion stage in step S3. However, the polarity measurement and polarity classification of the active material in step S1 are not performed, nor is the selection of the polarity-matching solvent and dispersant in step S2. The specific operation is as follows: Artificial graphite, styrene-butadiene rubber, sodium carboxymethyl cellulose, and conductive carbon black are added to a planetary mixer in the same proportions as in Example 2. Conventional deionized water is used as the solvent instead of the ethanol-water solution matched in S2. Sodium carboxymethyl cellulose is not added as the dispersant matched in S2. The mixture undergoes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage sequentially. An alternating magnetic field of 0.5T is applied during the high-speed dispersion stage.

[0126] The results showed that the stirring time of Comparative Example 3 was 4.5 h, longer than the 2 h of Example 2. The uniformity deviation of the slurry solid content exceeded ±2.5%, and there were uneven areas on the surface of the coated electrode. This indicates that without S1 polarity grading and S2 polarity matching, even with the application of an external field, the dispersion effect of the external field is significantly limited due to the poor interfacial compatibility between the active material and the solvent and dispersant, resulting in strong particle agglomeration driving force.

[0127] Comparative Example 4

[0128] This comparative example uses the same layered oxide NaNi1 / 3Fe1 / 3Mn1 / 3O2 as the sodium-ion battery positive electrode active material in Example 3. The polarity of the active material is measured and the polarity grade is classified in step S1, and the polarity matching solvent and dispersant are selected in step S2. However, no external field is applied in the high-speed dispersion stage of step S3, so as to verify the necessity of the external field in the sodium-ion battery system in step S4.

[0129] The specific operation is as follows: First, the surface polarity of the layered oxide is measured and assigned to the corresponding polarity level according to the same method as in Example 3. Then, the solvent and dispersant of the corresponding polarity are matched according to S2. Then, each component is added to the planetary mixer and carried out the pre-stirring stage, high-speed dispersion stage and vacuum degassing stage in sequence. No electric field, magnetic field or electromagnetic field is applied during the high-speed dispersion stage.

[0130] The results showed that the stirring time in Comparative Example 4 was significantly longer than that in Example 3, and the slurry dispersion uniformity was significantly worse than that in Example 3. The directional alignment of the active material particles in step S4 was lacking, and the continuity of the conductive network was insufficient. This indicates that in sodium-ion battery systems, the polarity matching in S1 and S2, along with the synergistic effect of the external field in step S3, are also necessary conditions for achieving the optimal stirring efficiency improvement, thus verifying the applicability of the method of this invention in sodium-ion battery systems.

[0131] In other embodiments, the external field is at least one of a DC electric field, a low-frequency alternating electric field with a frequency ≤ 1 kHz, and a constant magnetic field. When the external field includes an electric field, the electric field strength is 1 kV / m, 5 kV / m, or 100 kV / m; when the external field includes a magnetic field, the magnetic field strength is 0.1 T, 1.3 T, or 2 T. The polarity index is one, two, or three of the following: surface functional group polarity, dipole moment, and surface energy.

[0132] The polarity measurement values ​​are compared with the corresponding polarity index thresholds, and the active materials are classified into high polarity grades or low polarity grades based on the comparison results.

[0133] The surface functional group polarity is characterized by the presence or absence of oxygen-containing functional groups and / or the density of nitrogen-containing functional groups. When oxygen-containing functional groups and / or nitrogen-containing functional groups are present, it is classified as high polarity; otherwise, it is classified as low polarity. When the measured dipole moment is >1.5D, it is classified as high polarity; otherwise, it is classified as low polarity. When the measured surface energy polarity component is >10 mJ / m², it is classified as high polarity. 2 If the polarity is high, it is classified as a high polarity level; otherwise, it is classified as a low polarity level.

[0134] When the same active material is measured using at least two indicators simultaneously and the results of the determination of the indicators are contradictory, the final grade shall be determined according to the following rules:

[0135] Weighting rules: Surface functional group polarity weight 40%, dipole moment weight 35%, surface energy polarity component weight 25%; high polarity level is scored 2 points, low polarity level is scored 0 points; unmeasured indicators do not participate in the weighting, and their weights are normalized according to the other participating indicators; when the total weighted score is ≥1.5, it is a high polarity level, otherwise it is a low polarity level;

[0136] Special determination rule: When the surface functional group polarity is determined to be of a high polarity level and the dipole moment is determined to be of a low polarity level, the surface functional group polarity determination result shall be used as the final level. This special determination rule takes precedence over the weighted rule.

[0137] In step S2: For the high-polarity active material, a polar solvent and a polar dispersant are mixed, wherein the polar solvent is N-methylpyrrolidone and the polar dispersant is polyvinylpyrrolidone; for the low-polarity active material, a weakly polar solvent and a weakly polar dispersant are mixed, wherein the weakly polar solvent is an aqueous ethanol solution and the weakly polar dispersant is sodium carboxymethyl cellulose; and / or the high-polarity active material is a ternary material, lithium iron phosphate, lithium manganese oxide, or a material with a surface containing SiO2. X The active material is one, two or more of the following: silicon-based anode materials containing hydroxyl groups on their surface; the low polarity grade active material is a single graphite, a single lithium cobalt oxide, or a combination of graphite and lithium cobalt oxide in any proportion; wherein X is 0 or 2.

[0138] In step S3: the conductive agent includes at least one of carbon nanotubes and conductive carbon black. When the conductive agent is a combination of carbon nanotubes and conductive carbon black, the mass ratio of carbon nanotubes to conductive carbon black is any ratio within the range of (0.3 to 0.8): (1 to 2), such as 0.3:1, 0.3:2, 0.5:1, 0.5:1.5, 0.4:1.7, 0.8:2, 0.8:1, 0.8:1.3, or 0.3:1.2.

[0139] The adhesive includes polyvinylidene fluoride, or at least one of styrene-butadiene rubber and sodium carboxymethyl cellulose; when the adhesive is a combination of styrene-butadiene rubber and sodium carboxymethyl cellulose, the mass ratio of styrene-butadiene rubber to sodium carboxymethyl cellulose is any ratio within the range of (1 to 3): (1 to 2), such as 1:1, 2:1.3, 1:2, 2:1, 3:1, 1:1.5, 2:1.5 or 3:2;

[0140] The stirring rate during the high-speed dispersion stage is 1800 rpm, 2000 rpm, or 4000 rpm, and the dispersion time is 30 min, 40 min, or 60 min.

[0141] In step S4, the active material particles are oriented and distributed from the electrode current collector side to the slurry surface along the direction of the external field, thereby forming a continuous conductive channel in the electrode thickness direction.

[0142] The orientation distribution is observed under a scanning electron microscope, and the proportion of particles with an angle ≤30° between the long axis of the active material particles and the direction of the external field is ≥60% of the total number of particles.

[0143] The uniformity deviation of the solid content of the battery slurry is controlled within ±1%, the sedimentation rate after standing for 24 hours is ≤5%, and the resistivity fluctuation range of the electrode obtained after coating the battery slurry is ≤10%.

[0144] In summary, this invention measures the surface polarity of active materials and classifies them into polarity grades. Based on these polarity grades, solvents and dispersants of corresponding polarities are matched. Simultaneously, an external field is applied during stirring. This utilizes the repulsion of like polarities to disperse active material particles and the attraction of opposite polarities to orient the active material particles with conductive agents and binders. Through field-induced orientation, the active material particles are arranged in an orderly manner to form conductive channels. This achieves a synergistic effect of polarity matching and the external field, effectively reducing slurry agglomeration and shear resistance during stirring, significantly shortening stirring time, and improving the uniformity and stability of the slurry's solid content. This, in turn, enhances coating consistency and the electrochemical performance of the battery. The method of this invention is simple to operate, suitable for large-scale industrial production, and has significant efficiency and cost advantages.

Claims

1. A method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials, characterized in that, Includes the following steps: S1. Measure the surface polarity of the active material, and classify the active material into polarity grades based on the measurement results. The polarity grades include high polarity grades and low polarity grades. S2. For highly polar active materials, use polar solvents and polar dispersants; for low-polar active materials, use weakly polar solvents and weakly polar dispersants. S3. Mix the graded active material with the selected solvent, dispersant, conductive agent and binder, and apply an external field while stirring; S4. Under the action of the external field, the active material particles are dispersed by the repulsion of like polarities, and the active material particles are oriented to combine with the conductive agent and binder by the attraction of opposite polarities. The active material particles are arranged in an orderly manner by the field-induced orientation effect generated by the external field to form a conductive network, and the stirring ends.

2. The method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 1, characterized in that, The active materials include lithium transition metal oxide positive electrode active materials, sodium transition metal oxide positive electrode active materials, carbon-based negative electrode active materials, silicon-based negative electrode active materials, or alloy-based negative electrode active materials; The external field is at least one of a DC electric field, a low-frequency alternating electric field with a frequency ≤ 1 kHz, and a constant magnetic field.

3. The method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 2, characterized in that, When the external field includes an electric field, the electric field strength is 1~100 kV / m; when the external field includes a magnetic field, the magnetic field strength is 0.1~2T.

4. A method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 1, 2, or 3, characterized in that, Step S1 includes the following steps: The polarity index of the active material is measured to obtain a polarity measurement value. The polarity index is at least one of surface functional group polarity, dipole moment and surface energy polarity component. The polarity measurement values ​​are compared with the corresponding polarity index thresholds, and the active materials are classified into high polarity grades or low polarity grades based on the comparison results. The surface functional group polarity is characterized by the presence or absence of oxygen-containing and / or nitrogen-containing functional groups. When the test result shows the presence of oxygen-containing and / or nitrogen-containing functional groups, it is classified as a high polarity level; otherwise, it is classified as a low polarity level. Similarly, a dipole moment measurement value > 1.5D is classified as a high polarity level; otherwise, it is classified as a low polarity level. A surface energy polarity component measurement value > 10 mJ / m 2 If the polarity is high, it is classified as a high polarity level; otherwise, it is classified as a low polarity level.

5. The method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 4, characterized in that, In step S2: For the aforementioned high-polarity grade active material, a polar solvent and a polar dispersant are mixed, wherein the polar solvent is N-methylpyrrolidone and the polar dispersant is polyvinylpyrrolidone; For the aforementioned low-polarity grade active material, a weakly polar solvent and a weakly polar dispersant are used for mixing. The weakly polar solvent is an aqueous ethanol solution, and the weakly polar dispersant is sodium carboxymethyl cellulose; and / or The high-polarity active material is a ternary material, lithium iron phosphate, lithium manganese oxide, or a material with SiO2 on its surface. X The material is selected from at least one of silicon-based anode materials containing hydroxyl groups on the surface; the low polarity grade active material is selected from at least one of graphite and lithium cobalt oxide; wherein X is 0 or 2.

6. The method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 5, characterized in that, The stirring in step S3 includes a pre-stirring stage, a high-speed dispersion stage, and a vacuum degassing stage performed sequentially, and the external field is applied at least during the high-speed dispersion stage; The conductive agent includes at least one of carbon nanotubes and conductive carbon black. When the conductive agent is a combination of carbon nanotubes and conductive carbon black, the mass ratio of carbon nanotubes to conductive carbon black is (0.3-0.8):(1-2). The adhesive includes polyvinylidene fluoride, or at least one of styrene-butadiene rubber and sodium carboxymethyl cellulose; when the adhesive is a combination of styrene-butadiene rubber and sodium carboxymethyl cellulose, the mass ratio of styrene-butadiene rubber to sodium carboxymethyl cellulose is (1-3):(1-2).

7. The method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 6, characterized in that, The pre-mixing stage involves dissolving the binder in a solvent, then adding the dispersant, conductive agent, and active material and stirring to mix the components. The stirring rate during the high-speed dispersion stage is 1800~4000 rpm, and the dispersion time is 30~60 min; The vacuum degassing stage involves stirring the slurry that has undergone the high-speed dispersion stage under vacuum conditions to remove air bubbles.

8. A method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to claim 7, characterized in that, In step S4, the active material particles are oriented and distributed from the electrode current collector side to the slurry surface along the direction of the external field, thereby forming a continuous conductive channel in the electrode thickness direction. The orientation distribution is observed under a scanning electron microscope, and the proportion of particles with an angle ≤30° between the long axis of the active material particles and the direction of the external field is ≥60% of the total number of particles.

9. A method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials according to any one of claims 5 to 8, characterized in that, The uniformity deviation of the solid content of the battery slurry is controlled within ±1%, the sedimentation rate after standing for 24 hours is ≤5%, and the resistivity fluctuation range of the electrode obtained after coating the battery slurry is ≤10%.

10. The application of the method for improving the stirring efficiency of ion battery slurry by utilizing the polarity of active materials as described in claim 9 in the preparation of sodium-ion or lithium-ion battery slurries.