A carbon and Nb2O5 composite-coated Li5FeO4 lithium supplement additive, its preparation method and application

By constructing a carbon-Nb2O5 composite coating layer on the surface of Li5FeO4, a Li-Nb-O fast ion conductor interface phase is generated, which solves the problems of high delithiation potential and poor air stability of Li5FeO4, and achieves improved energy density and enhanced stability of lithium-ion batteries.

CN123120935APending Publication Date: 2026-11-17湖南防灾科技有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611429207.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing lithium-ion battery cathode lithium replenishment additive Li5FeO4 has a high delithiation potential and poor air stability during the first charge, which limits the improvement of lithium-ion battery energy density. Furthermore, the existing carbon coating method cannot significantly improve lithium-ion conductivity and physical protection.

Method used

The lithium supplement additive Li5FeO4, which is coated with carbon and Nb2O5, constructs a double-shell structure with an inner in-situ carbon layer and an outer Nb2O5 layer. It utilizes the reaction of Nb2O5 with lithium ions to generate a high-conductivity Li-Nb-O fast ion conductor interface phase, thereby reducing the delithiation potential. The inner carbon layer provides an electronic conductive network and physical protection.

Benefits of technology

It significantly reduces the delithiation potential of Li5FeO4, improves lithium-ion conductivity and air stability, enhances lithium replenishment efficiency, and extends the operability of the additive in industrial environments, demonstrating promising prospects for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120935A_ABST
    Figure CN123120935A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery technology, specifically to a carbon and Nb2O5 composite-coated Li5FeO4 lithium replenishing additive, its preparation method, and its application. The method includes: S100, mixing a lithium source, an iron source, and an organic carbon source to obtain a mixture; S200, subjecting the mixture to a first calcination under a protective atmosphere to obtain an in-situ carbon-coated Li5FeO4 precursor. This invention achieves a synergistic improvement in electronic conductivity, ion transport rate, and physical protection by constructing an ordered double-shell structure of an "inner in-situ carbon layer + outer Nb2O5 layer." During the first charging process, the outer Nb2O5 layer can undergo an in-situ interfacial reaction with residual lithium or extracted lithium ions on the core surface, generating a high-conductivity Li-Nb-O fast ion conductor interfacial phase. This effectively controls the delithiation potential of Li5FeO4 to 3.2~3.4V and suppresses interfacial side reactions and gas generation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, specifically to a carbon and Nb2O5 composite-coated Li5FeO4 lithium supplement additive, its preparation method, and its application. Background Technology

[0002] During the first charge of a lithium-ion battery, a solid electrolyte interphase (SEI) film forms on the surface of the negative electrode. This process irreversibly consumes the active lithium in the positive electrode, resulting in a decrease in the initial coulombic efficiency (ICE) and irreversible capacity loss. For graphite negative electrodes, this loss is approximately 7% to 10%; while for high-capacity silicon-based negative electrodes, the initial irreversible capacity loss can reach 50% to 70%, severely limiting further improvements in the energy density of lithium-ion batteries.

[0003] Cathode lithium replenishment technology, by introducing sacrificial lithium replenishment additives with high lithium content into the cathode, releases additional active lithium during the first charge to compensate for the lithium consumed in the formation of the SEI at the anode, thus effectively improving battery energy density. Li5FeO4 (LFO), with its theoretical specific capacity of up to 867 mAh / g, is a promising cathode lithium replenishment additive. In recent years, significant progress has been made in the modification and coating research of LFO lithium replenishers. For example, surface phosphorylation treatment converts residual alkali on the LFO surface into a Li3PO4 fast ion conductor layer, improving both air stability and ionic conductivity. However, LFO still faces two core technical challenges in practical applications: poor air stability and high delithiation potential.

[0004] To address the aforementioned issues, existing technologies primarily employ surface coating strategies to modify LFO. Among these, monolayer carbon coating is a common approach. Existing technology CN119742350A discloses a technique for forming a carbon shell on the surface of the LFO core layer. By controlling the ID / IG ratio (1.0~1.2) and average thickness (60~200 nm) of the carbon layer, the air stability of lithium ferrite supplements is improved to some extent. However, simple carbon coating itself has limited lithium-ion conductivity and cannot significantly improve the delithiation kinetics of LFO; furthermore, the physical protective effect of the carbon layer gradually diminishes under long-term cycling or high-voltage conditions. In addition, studies have also disclosed composite coating schemes using carbon and oxides. Summary of the Invention

[0005] The technical problems to be solved by this invention include: (1) Reduce the delithiation potential of LFO so that it can fully release active lithium at a lower voltage and improve the lithium replenishment efficiency; (2) Significantly improves the air stability of LFO and extends its operability in industrial production environments; (3) A simple and cost-controllable method for preparing LFO composite coating is provided.

[0006] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a carbon and Nb2O5 composite-coated Li5FeO4 lithium supplement additive with a core-shell structure, comprising: Li5FeO4 core; A composite coating layer covering the surface of the Li5FeO4 core; The composite coating layer includes an inner carbon layer and an outer Nb2O5 layer.

[0007] On the other hand, a method for preparing a carbon and Nb2O5 composite coated Li5FeO4 lithium supplement additive includes the following steps: S100, mixing a lithium source, an iron source and an organic carbon source to obtain a mixture; S200, the mixture is calcined for the first time under a protective atmosphere to obtain an in-situ carbon-coated Li5FeO4 precursor; S300, the in-situ carbon-coated Li5FeO4 precursor and Nb2O5 powder are dispersed in an organic solvent, mixed evenly and dried to obtain composite precursor powder; S400, the composite precursor powder is calcined a second time under a protective atmosphere to obtain the carbon and Nb2O5 composite coated Li5FeO4 lithium supplementary additive.

[0008] Furthermore, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide, and lithium oxide; the iron source is selected from at least one of ferric oxide, ferric oxide, and ferric oxalate; and the organic carbon source is selected from at least one of glucose, sucrose, citric acid, starch, and polyvinylpyrrolidone. The organic carbon source is glucose.

[0009] Further, in step S100, the amount of lithium source and iron source added satisfies the following: the molar ratio of Li element to Fe element is 5.5:1; The amount of the organic carbon source is controlled to be 1% to 20% of the total mass of the lithium source and the iron source; The specific operation of step S100 is as follows: the lithium source, iron source and organic carbon source are placed in a ball mill and ball-milled at a speed of 300 r / min for 4 hours to obtain a uniform mixed powder.

[0010] Furthermore, in step S200, the protective atmosphere is an inert atmosphere or a reducing atmosphere; The protective atmosphere is an argon atmosphere or a nitrogen atmosphere; The operating conditions for the first calcination include: the calcination temperature is controlled at 650~850℃, and the holding time is 8~16h; The heating rate of the first calcination is controlled at 2~10℃ / min; preferably, after the holding time is completed, the calcined product is naturally cooled to room temperature; After in-situ carbonization in step S200, an in-situ carbon layer is formed on the surface of the Li5FeO4 core, and the mass ratio of the in-situ carbon layer to the Li5FeO4 core is (0.5~20):100.

[0011] Further, in step S300: The Nb2O5 powder is an amorphous Nb2O5 or orthorhombic T-Nb2O5 nanopowder with an average particle size of 10~200nm, and its addition amount is controlled to be 0.5%~8% of the mass of the in-situ carbon-coated Li5FeO4 precursor, preferably 1%~5%.

[0012] Furthermore, the organic solvent is selected from at least one of ethanol, isopropanol and acetone, and the in-situ carbon-coated Li5FeO4 precursor and Nb2O5 powder are dispersed in the organic solvent by ultrasound and / or stirring to form a uniform suspension.

[0013] Furthermore, the specific action of the drying process is as follows: the uniform suspension is subjected to water bath stirring and evaporation at a temperature of 80°C to obtain the composite precursor powder.

[0014] Furthermore, in step S400, the process conditions for the second calcination are: the heating rate is controlled at 2~5℃ / min, the target calcination temperature is 350~550℃, and the holding time at the target calcination temperature is 2~6h.

[0015] Furthermore, the target calcination temperature is preferably controlled at 400~500℃.

[0016] The beneficial effects of this invention are: This invention achieves a synergistic improvement in electronic conductivity, ion transport rate, and physical protection by constructing an ordered bilayer shell structure consisting of an inner in-situ carbon layer and an outer Nb₂O₅ layer. During the initial charging process, the outer Nb₂O₅ layer undergoes an in-situ interfacial reaction with residual lithium or extracted lithium ions on the core surface, generating a high-conductivity Li-Nb-O fast ion conductor interfacial phase. This effectively regulates the delithiation potential of Li₅FeO₄ to 3.2–3.4 V and suppresses interfacial side reactions and gas generation. Simultaneously, the inner in-situ carbon layer provides an electronic conductivity network and primary protection, synergistically forming a dense physical barrier with the outer Nb₂O₅ layer, significantly enhancing the air stability of Li₅FeO₄. Furthermore, the preparation method of this invention has a clear process route, employing a stepwise calcination process, which is simple to operate and has controllable production costs. The resulting lithium replenishment additive possesses high lithium replenishment efficiency, excellent air stability, and interfacial stability, showing promising prospects for industrial application. Attached Figure Description

[0017] Figure 1 This is a flowchart of the method of the present invention; Figure 2 The XRD pattern of the material obtained in Example 1; Figure 3 The image shows the SEM image of the material obtained in Example 1. Figure 4 The material C element mapping diagram obtained in Example 1; Figure 5 The material O element mapping diagram obtained in Example 1; Figure 6 The Fe element mapping diagram of the material prepared in Example 1; Figure 7 The Nb element mapping diagram of the material prepared in Example 1; Figure 8 The charge-discharge curve of the material prepared in Example 1 is shown below. Figure 9 The charge-discharge curve of the material prepared in Comparative Example 2 is shown. Figure 10 The charge-discharge curves of the material prepared in Comparative Example 3 are shown. Detailed Implementation

[0018] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0019] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0020] The present invention will now be described in further detail with reference to the accompanying drawings: like Figure 1 As shown, a method for preparing a carbon and Nb2O5 composite-coated Li5FeO4 lithium supplement additive includes the following steps: S100, a mixture of lithium source, iron source and organic carbon source is obtained; S200, the mixture is calcined for the first time under a protective atmosphere to obtain an in-situ carbon-coated Li5FeO4 precursor; S300, the in-situ carbon-coated Li5FeO4 precursor and Nb2O5 powder are dispersed in an organic solvent, mixed evenly and dried to obtain composite precursor powder; S400, the composite precursor powder is calcined a second time under a protective atmosphere to obtain the carbon and Nb2O5 composite coated Li5FeO4 lithium supplementary additive.

[0021] The specific implementation process of the further step S100 is as follows: Example 1: like Figure 1 As shown: The specific implementation process of step S100 is as follows: Accurately weigh battery-grade lithium carbonate (Li₂CO₃) as the lithium source and accurately weigh ferric oxide (Fe₂O₃) as the iron source. When weighing the ingredients, calculate based on the stoichiometric ratio of the chemical reaction to control the molar ratio of lithium (Li) to iron (Fe) at 5.5:1. An excess of 10% lithium is used to compensate for the high-temperature volatilization of lithium components during the subsequent heat treatment stage. Next, weigh anhydrous glucose as the organic carbon source, with the added mass being 10% of the total mass of the lithium carbonate and ferric oxide.

[0022] The precisely weighed lithium carbonate powder, ferric oxide powder, and anhydrous glucose powder were fed into the zircon grinding jar of a planetary ball mill. Zirconia-graded grinding balls with diameters of 5 mm and 10 mm were introduced into the jar as grinding media, with a ball-to-material ratio of 15:1 (total grinding ball mass to total material mass). After sealing and locking the jar, it was securely installed on the main disc of the planetary ball mill. The main disc speed of the planetary ball mill was set to 300 r / min, and the mill was started and allowed to run continuously for 4 hours. During operation, the material underwent microscopic dispersion under the combined mechanical shearing and impact forces of planetary revolution and rotation. After the ball milling program was completed, the jar was removed, and the material inside was poured out. Mechanical sieving was performed using a standard vibrating screen to achieve mechanical separation of the zirconium oxide grinding balls and the material powder, ultimately collecting a solid mixture powder with a uniform particle size distribution.

[0023] like Figure 1 As shown: The specific implementation process of step S200 is as follows: The solid mixture powder collected in step S100 is transferred and spread evenly into a high-temperature sintering magnetic boat made of alumina. The magnetic boat containing the material is then pushed into the constant-temperature heating zone of a tubular furnace. The furnace tube is sealed, and high-purity argon gas is continuously introduced into the furnace tube as a protective atmosphere. The argon gas flow rate is controlled to fully replace the air in the furnace cavity, ensuring that the sintering system is in a strictly inert and oxygen-free environment.

[0024] Subsequently, the thermal program of the tubular furnace was initiated for the first calcination: the instrument's heating rate was set to a strictly controlled 5℃ / min, steadily increasing the furnace temperature from room temperature to the target calcination temperature of 750℃. After reaching the target temperature of 750℃, the system automatically switched to a constant temperature operation mode and maintained the temperature for 12 hours. During this high-temperature constant temperature stage, the lithium source and iron source underwent a deep solid-state reaction to generate the bulk crystalline phase of Li5FeO4. Simultaneously, the organic carbon source in the system underwent pyrolysis and in-situ carbonization reactions, forming a tightly bonded amorphous carbon layer on the surface of the generated Li5FeO4 particles.

[0025] After the heat preservation process is completed, heating is stopped, and the furnace body is allowed to cool naturally to room temperature under the protection of high-purity argon gas circulation. The product block after the first calcination is removed and placed in an agate mortar or mechanical grinding equipment for mechanical grinding. Subsequently, the ground powder is physically sieved using a standard test sieve with a 300-mesh aperture. Coarse particles are retained and repeatedly ground and sieved. Finally, the sieve-passing material is collected, which yields the in-situ carbon-coated Li5FeO4 precursor with uniform particle size distribution (denoted as C@LFO). Rigorous determination using a simultaneous thermogravimetric analysis (TGA) instrument shows that the in-situ carbon content in this batch of precursor is approximately 4.2 wt%.

[0026] like Figure 1As shown: The specific implementation process of step S300 is as follows: Accurately weigh 10g of the in-situ carbon-coated Li5FeO4 precursor (C@LFO) powder obtained in step S200, transfer it to a clean glass container, and then add 50mL of anhydrous ethanol as the liquid dispersion medium. Place the glass container in an ultrasonic cleaner and perform stable ultrasonic dispersion treatment at room temperature for 30min. Utilize the ultrasonic cavitation effect to break up the soft agglomerates of the precursor powder, allowing it to form a preliminary uniform suspension in the ethanol medium.

[0027] Subsequently, 0.3 g of amorphous Nb₂O₅ nanoparticles were accurately weighed and added to the suspension. The average particle size of the amorphous Nb₂O₅ powder was approximately 50 nm, and its added mass accounted for 3% of the total mass of the C@LFO precursor powder. To ensure that the nano-sized Nb₂O₅ could be uniformly adsorbed and anchored on the surface of the C@LFO particles, the mixture was ultrasonically treated again for 30 min. Then, the container was transferred to a magnetic stirrer, a magnetic stir bar was added, and an appropriate speed was set. The mixture was continuously magnetically stirred at room temperature for 2 h.

[0028] After the solid and liquid phases have fully mixed and reached dynamic equilibrium through interfacial adsorption, the resulting homogeneous suspension, along with the container, is transferred into a constant-temperature water bath at 80°C. Stirring is continuously maintained while heating in the water bath, utilizing the volatility of ethanol for slow evaporation and desolvation. This continues until the anhydrous ethanol in the suspension is completely evaporated, the solid phase precipitates, and finally, a microscopically homogeneous, dried precursor powder is collected.

[0029] The specific implementation process of step S400 is as follows: The composite precursor powder obtained after drying in step S300 is transferred and spread evenly in a clean alumina sintering boat. The sintering boat is then pushed into the isothermal zone of a tubular high-temperature furnace, and the furnace tubes are sealed. High-purity argon gas is continuously introduced into the furnace cavity as a protective atmosphere to fully replace the air inside the furnace and create a strictly inert heat treatment environment. The second calcination thermal program of the tubular furnace is started: the instrument heating rate is strictly set to 3℃ / min, and the furnace system temperature is steadily increased from room temperature to the target calcination temperature of 450℃. After reaching 450℃, the system enters the isothermal operation mode and is held at that temperature for 3 hours. Under this low-temperature calcination field, nano-sized Nb2O5 particles achieve a firm solid-phase anchorage on the carbon-coated Li5FeO4 precursor surface through interfacial thermodynamic diffusion, forming a dense outer coating layer; simultaneously, this specific low-temperature heat treatment process effectively avoids damage to the Li5FeO4 bulk crystal structure and the integrity of the inner in-situ carbon layer. After the constant temperature holding process is completed, the heating power is cut off, and the furnace body is allowed to cool naturally to room temperature under the protection of continuous argon gas. The product after the second calcination is taken out, ground in an agate mortar, and physically sieved using a standard test sieve. Finally, the carbon and Nb2O5 composite coated Li5FeO4 lithium supplement additive (denoted as Nb2O5-C-LFO) is collected.

[0030] Example 2 differs from Example 1 in that the mass of anhydrous glucose in S100 is adjusted to 2% of the total mass of lithium carbonate and ferric oxide; like Figure 1 As shown: The specific implementation process of step S100 is as follows: Accurately weigh battery-grade lithium carbonate (Li₂CO₃) as the lithium source and accurately weigh ferric oxide (Fe₂O₃) as the iron source, strictly controlling the molar ratio of lithium to iron to be 5.5:1 during the weighing process. Subsequently, weigh anhydrous glucose as the organic carbon source, adjusting the mass of anhydrous glucose to 2% of the total mass of the lithium carbonate and ferric oxide.

[0031] The weighed lithium carbonate powder, ferric oxide powder, and anhydrous glucose powder were placed together in the grinding jar of a planetary ball mill. Zirconia-graded grinding balls were introduced as the grinding media, and the ball-to-powder ratio was controlled at 15:1. After sealing and fixing the grinding jar, the main disc of the ball mill was set to a speed of 300 r / min, and the ball milling operation was performed continuously for 4 hours. After the ball milling was completed, the material was unloaded, and the zirconia grinding balls were removed using a sieve to collect the dry mixture powder.

[0032] The specific implementation process of step S200 is as follows: Using the same thermal loading and atmosphere protection method as in Example 1, the mixed powder was placed in a tube furnace and calcined for the first time under the protection of a continuously purging argon atmosphere. The system temperature was steadily increased to 750°C at a rate of 5°C / min and held at this target temperature for 12 hours, followed by natural cooling to room temperature. The obtained sintered block was thoroughly ground, and all material was ensured to pass through a 300-mesh standard sieve to collect the in-situ carbon-coated Li5FeO4 precursor (C@LFO). Due to the low initial carbon source concentration in this example, a thinner in-situ amorphous carbon coating layer was formed on the LFO surface after thermal calcination.

[0033] The specific implementation process of step S300 is as follows: C@LFO precursor powder with an extremely thin carbon layer was used as the substrate. 10 g of this precursor powder was weighed and dispersed in 50 mL of anhydrous ethanol and sonicated for 30 min. Then, 0.3 g of amorphous Nb₂O₅ nanoparticles with an average particle size of approximately 50 nm were added, and the mixture was followed by ultrasonic dispersion for 30 min and magnetic stirring for 2 h to form a homogeneous suspension. Finally, the system was continuously stirred and evaporated to dryness in an 80 °C water bath to remove the organic solvent, and the composite precursor powder was collected.

[0034] The specific implementation process of step S400 is as follows: Using the same thermodynamic equipment and atmosphere control method as in Example 1 (high-purity argon protection), the composite precursor powder prepared in step S300 of Example 2 was placed in a tube furnace. The same preferred thermal parameters were set: heating to 450°C at a heating rate of 3°C / min and holding at that temperature for 3 hours. After holding, the powder was naturally cooled to room temperature, and then subjected to standard grinding and sieving processes to obtain a Li5FeO4 lithium supplementary additive with an extremely thin inner layer of in-situ carbon and a uniform Nb2O5 outer layer.

[0035] Example 3: The specific implementation process of step S100 is basically the same as that of Example 1, except that the amount of Nb2O5 powder added in the subsequent step S300 is adjusted to 8% of the mass of C@LFO.

[0036] Specifically, in step S100, battery-grade lithium carbonate (Li2CO3) and ferric oxide (Fe2O3) are accurately weighed, maintaining a lithium to iron molar ratio of 5.5:1; and anhydrous glucose, accounting for 10% of the total mass of the lithium carbonate and ferric oxide, is added as an organic carbon source. The raw materials are loaded into a planetary ball mill and ball-milled for 4 hours at a main disc speed of 300 r / min. After separating the grinding media, the mixed powder obtained for subsequent steps is collected.

[0037] The operating procedures, heat treatment parameters, atmosphere conditions (argon, increasing to 750℃ at 5℃ / min and holding for 12h) for step S200, as well as the subsequent grinding and sieving process, are strictly consistent with those in Example 1, and will not be repeated here. Each batch consistently yielded C@LFO precursor powder with a carbon content of approximately 4.2wt%, which will be used in subsequent steps.

[0038] The specific implementation process of step S300 is basically the same as that of Example 1, the main difference being the amount of Nb2O5 coating material added.

[0039] Specifically: 10g of the C@LFO precursor obtained in step S200 of Example 3 was weighed and dispersed in 50mL of anhydrous ethanol. Subsequently, 0.8g of amorphous Nb2O5 nanoparticles (average particle size of approximately 50nm) were weighed and added to the system, at which point the added mass of Nb2O5 accounted for 8% of the mass of C@LFO. After ultrasonic and magnetic stirring, the mixture was also placed in a constant temperature water bath at 80℃ and stirred until dry, finally obtaining a precursor powder mixture with a relatively thick coating layer.

[0040] Using composite precursor powders with different Nb2O5 contents prepared in each step S300, the calcination process and thermal parameters (argon protection, heating to 450℃ at 3℃ / min and holding for 3h) in step S400 are strictly consistent with those in Example 1. After natural cooling, grinding, and sieving, each batch of products is stably prepared to obtain carbon and Nb2O5 composite-coated Li5FeO4 lithium supplementary additives with different Nb2O5 outer layer coating thicknesses.

[0041] Example 4: The specific implementation process of step S100 is basically the same as that of Example 1, except that the amount of Nb2O5 powder added in the subsequent step S300 is adjusted to 0.5% of the mass of C@LFO.

[0042] Specifically, in step S100, battery-grade lithium carbonate (Li2CO3) and ferric oxide (Fe2O3) are accurately weighed, maintaining a lithium to iron molar ratio of 5.5:1; and anhydrous glucose, accounting for 10% of the total mass of the lithium carbonate and ferric oxide, is added as an organic carbon source. The raw materials are loaded into a planetary ball mill and ball-milled for 4 hours at a main disc speed of 300 r / min. After separating the grinding media, the mixed powder obtained for subsequent steps is collected.

[0043] The operating procedures, heat treatment parameters, atmosphere conditions (argon, increasing to 750℃ at 5℃ / min and holding for 12h) for step S200, as well as the subsequent grinding and sieving process, are strictly consistent with those in Example 1, and will not be repeated here. Each batch consistently yielded C@LFO precursor powder with a carbon content of approximately 4.2wt%, which will be used in subsequent steps.

[0044] The specific implementation process of step S300 is basically the same as that of Example 1, and the main difference lies in the amount of Nb2O5 coating material added.

[0045] Specifically: 10g of the C@LFO precursor obtained in step S200 of Example 4 was weighed and dispersed in anhydrous ethanol. Subsequently, only 0.05g of amorphous Nb2O5 nanoparticles (average particle size of approximately 50nm) were weighed and added to the system, at which point the added mass of Nb2O5 accounted for 0.5% of the mass of C@LFO. The composite precursor powder with an extremely low concentration of surface-anchored niobium source was obtained by using the same liquid-phase dispersion and 80°C water bath stirring and evaporation process.

[0046] Using composite precursor powders with different Nb2O5 contents prepared in each step S300, the calcination process and thermal parameters (argon protection, heating to 450℃ at 3℃ / min and holding for 3h) in step S400 are strictly consistent with those in Example 1. After natural cooling, grinding, and sieving, each batch of products is stably prepared to obtain carbon and Nb2O5 composite-coated Li5FeO4 lithium supplementary additives with different Nb2O5 outer layer coating thicknesses.

[0047] Example 5 (Example of changing raw material combination and mixing process) differs from Example 1 in that different raw materials are selected for combination in step S100 to expand the scope of application, and the lower limit of temperature and the upper limit of time are expanded in step S200. The specific implementation process is as follows: Accurately weigh lithium hydroxide monohydrate (LiOH·H2O) as the lithium source and iron oxide (Fe3O4) as the iron source. Through stoichiometric conversion, control the molar ratio of lithium to iron in the raw materials to be 5.5:1. Next, weigh citric acid powder as the organic carbon source, and control the amount of citric acid added to be 5% of the total mass of the lithium hydroxide monohydrate and iron oxide.

[0048] The weighed lithium hydroxide monohydrate, iron(III) oxide, and citric acid were added to a horizontal rolling ball mill, using high-chromium stainless steel balls as the milling medium, with a ball-to-material ratio controlled at 20:1. The ball mill was sealed, and the rolling shaft speed was set to 250 r / min for continuous ball milling and mixing for 6 hours. After the ball milling response was completed, the mixture was mechanically unloaded and then dried in a vacuum drying oven at 60°C under low-pressure dehumidification for 2 hours. Finally, the stainless steel balls were retained through a sieve, and a uniformly dispersed powder of the mixture was collected.

[0049] The specific implementation process of step S200 is as follows: The mixture was loaded into a tube furnace, sealed, and evacuated. High-purity nitrogen was continuously introduced into the furnace chamber as a protective atmosphere. The thermodynamic parameters for the first calcination were set as follows: a relatively low heating rate of 2℃ / min was used to slowly heat the system to the lower limit of the target calcination temperature, 650℃. To compensate for the insufficient reaction kinetic energy at the lower temperature, the isothermal holding time was extended to the upper limit of 16 hours to ensure that both the solid-state phase formation reaction of the lithium iron precursor and the in-situ carbonization reaction of the carbon source were completely converted. After the process was completed, the mixture was allowed to cool naturally to room temperature and then subjected to the same standard grinding and physical sieving treatment to prepare a precursor powder with an in-situ carbon-coated structure.

[0050] In Example 5, step S300 is reasonably adjusted as follows: Accurately weigh 10g of the C@LFO precursor powder obtained in step S200, and add 50mL of isopropanol (or acetone) as the liquid dispersion medium. After ultrasonic dispersion for 30min, weigh 0.5g (5% of the substrate mass) of orthorhombic T-Nb2O5 nanoparticles and add them to the suspension. The average particle size of the orthorhombic T-Nb2O5 powder is controlled to be around 200nm, which is the upper limit of the range. Perform the same standard ultrasonic (30min) and magnetic stirring (2h) process on the mixture, and then evaporate the isopropanol (or acetone) solvent while stirring under the condition of constant temperature water bath at 80℃ to finally obtain the composite precursor powder.

[0051] To fully verify and support the lower limit of the parameter range for this calcination process, the specific implementation process of step S400 in Example 5 is as follows: The composite precursor powder obtained in step S300 was loaded into a tube furnace, sealed, and evacuated. High-purity nitrogen was continuously introduced into the furnace chamber as an inert protective atmosphere. The thermodynamic parameters for the second calcination were set as follows: the system was slowly heated to the lower limit of the target calcination temperature, 350°C, at a heating rate of 2°C / min (the lower limit of the range). To compensate for the insufficient interfacial diffusion solid-phase anchoring kinetic energy at lower temperatures, the isothermal holding time was extended to the upper limit of 6 hours. After the process was completed, the mixture was allowed to cool naturally to room temperature. After grinding and physical sieving, a composite-coated lithium-replenishing additive with strong interfacial bonding was prepared.

[0052] Example 6 (Example of changing raw material combination and mixing process); The implementation process of step S100 is as follows: Industrial-grade lithium oxide (Li₂O) was accurately weighed as the lithium source, and anhydrous ferric oxalate (Fe₂(C₂O₄)₃) was weighed as the iron source, and the materials were precisely proportioned according to a lithium to iron molar ratio of 5.5:1. Subsequently, polyvinylpyrrolidone (PVP, type K30) was introduced as an organic carbon source, with the added mass of PVP accounting for 15% of the total mass of the lithium oxide and ferric oxalate.

[0053] The three solid powder raw materials were placed together in the mixing tank of a high-energy three-dimensional oscillating mixer. This mixing process did not add any hard ball milling media. After locking the tank, the three-dimensional mixer was started, and the spatial oscillation frequency of the mixer was set to 50Hz. The tank was driven to perform compound irregular oscillation and inverting motion in three-dimensional space for 5 hours. Macroscopic uniform mixing of multiple components was achieved by utilizing the material's own gravity diffusion, convection, and shearing action. After the operation was completed, the tank was opened and the material was unloaded, and a free-flowing solid mixture was collected.

[0054] The specific implementation process of step S200 is as follows: A container filled with the material is placed in a high-temperature sintering furnace, and a mixed gas containing 95% argon and 5% hydrogen is introduced into the furnace to create a weakly reducing atmosphere. The first calcination program is initiated: a heating rate of 10℃ / min with high thermal driving force is set to rapidly heat the system to the upper limit of the target calcination temperature, 850℃. Under this high thermal energy temperature field, the isothermal holding time is shortened to the lower limit of 8 hours to complete the deep reaction. After the holding time is completed, the mixture is allowed to cool naturally, and the agglomerated calcined product is ground and sieved to finally obtain a precursor powder with high crystallinity and an in-situ carbon layer on the surface.

[0055] To further expand the upper limit of the process range, in Example 6, the specific implementation process of step S400 is as follows: A sintering boat containing the composite precursor powder was placed in a tubular furnace, and the second calcination process was initiated under a protective atmosphere of continuously purged high-purity argon. A heating rate of 5°C / min, with a relatively high thermal driving force, was set to rapidly heat the system to the upper limit of the target calcination temperature, 550°C. To prevent thermal stress damage to the inner carbon layer network under this high thermodynamic temperature field, the isothermal holding time was shortened to the lower limit of 2 hours. After the holding time, the system was allowed to cool naturally, and the calcined product was subjected to conventional grinding and sieving processes to finally obtain a carbon-Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive with good crystallinity.

[0056] Comparative Example 1 The preparation method is the same as in Example 1, but the Nb2O5 coating in steps S300 and S400 is not performed.

[0057] Comparative Example 2 Without performing step S200 of Example 1, the bare LFO was directly coated with Nb2O5 (without a carbon layer). The coating process was the same as steps S300 and S400 of Example 1, and the other preparation methods were the same as in Example 1.

[0058] Comparative Example 3 The preparation method is the same as in Example 1, except that in step S300, Nb2O5 is replaced with the same mass of Al2O3 nanopowder.

[0059] Comparative Example 4 C@LFO (the product of step S200 in Example 1) was mixed with Nb2O5 and glucose in an aqueous phase and then calcined once at 450°C to obtain LFO coated with carbon and Nb2O5.

[0060] Lithium delithiation potential and air stability test: The delithiation potential of the lithium-replenishing additives prepared in each case and the capacity retention test results after being stored in an air atmosphere at 25°C and 25% humidity for 6 hours are shown in Table 1: Table 1

[0061] Lithium replenishment effect test: The lithium supplementation additives prepared by adding 3 wt% of each case were added to the lithium iron phosphate cathode and assembled with the graphite anode to form a full battery. The energy density and first coulombic efficiency of the battery were tested, as shown in Table 2.

[0062] Table 2

[0063] The data fully demonstrates that the proposed "inner carbon + outer Nb2O5" composite coating structure is significantly superior to single coating and mixed coating. The reduction in delithiation potential brought about by Nb2O5 coating is not achieved by traditional inert oxides such as Al2O3, which is attributed to the in-situ formation of the Li-Nb-O fast ion conductor interface phase. Amorphous Nb2O5, due to its higher reactivity, exhibits a more significant performance improvement. When applied to lithium iron phosphate full batteries, the "inner carbon + outer Nb2O5" composite coating material in Example 1 significantly improves the battery's energy density and initial coulombic efficiency, and demonstrates a significant lithium replenishment effect.

[0064] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A Li5FeO4 lithium supplement additive coated with carbon and Nb2Os, characterized in that, The lithium supplement additive has a core-shell structure and includes: Li5FeO4 core; A composite coating layer covering the surface of the Li5FeO4 core; The composite coating layer includes an inner carbon layer and an outer Nb2O5 layer; The inner carbon layer and L i5 The mass ratio of FeO4 core is 0.5-20:100, and the mass ratio of the outer Nb2O5 layer to the precursor is 0.5%-8%.

2. The preparation method of the carbon and Nb2O5 composite coated Li5FeO4 lithium supplement additive according to claim 1, characterized in that, Includes the following steps: S100, a mixture of lithium source, iron source and organic carbon source is obtained; S200, the mixture is calcined for the first time under a protective atmosphere to obtain an in-situ carbon-coated Li5FeO4 precursor; S300, the in-situ carbon-coated Li5FeO4 precursor and Nb2O5 powder are dispersed in an organic solvent, mixed evenly and dried to obtain composite precursor powder; S400, the composite precursor powder is calcined a second time under a protective atmosphere to obtain the carbon and Nb2O5 composite coated Li5FeO4 lithium supplementary additive.

3. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplement additive according to claim 2, characterized in that, The lithium source is selected from at least one of lithium carbonate, lithium hydroxide, and lithium oxide; the iron source is selected from at least one of ferric oxide, ferric oxide, and ferric oxalate; and the organic carbon source is selected from at least one of glucose, sucrose, citric acid, starch, and polyvinylpyrrolidone.

4. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive according to claim 2, characterized in that, In step S100, the amount of lithium source and iron source added satisfies the following condition: the molar ratio of Li to Fe is 5.5:1; The amount of the organic carbon source used is 1% to 20% of the sum of the mass of the lithium source and the iron source; The specific operation of step S100 is as follows: the lithium source, iron source and organic carbon source are placed in a ball mill and ball-milled at a speed of 300 r / min for 4 hours to obtain a uniform mixed powder.

5. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive according to claim 2, characterized in that, In step S200, the protective atmosphere is an inert atmosphere or a reducing atmosphere; The operating conditions for the first calcination include: the calcination temperature is controlled at 650~850℃, and the holding time is 8~16h; The heating rate for the first calcination is controlled at 2~10℃ / min; After the heat preservation time is completed, the calcined product is allowed to cool naturally to room temperature; After in-situ carbonization in step S200, an in-situ carbon layer is formed on the surface of the Li5FeO4 core, and the mass ratio of the in-situ carbon layer to the Li5FeO4 core is (0.5~20):

100.

6. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive according to claim 2, characterized in that, In step S300: The Nb2O5 powder is amorphous Nb2O5 nanopowder or orthorhombic T-Nb2O5 nanopowder, with an average particle size of 10~200nm, and the amount of niobium oxide powder added is 0.5%~8% of the mass of the in-situ carbon-coated Li5FeO4 precursor.

7. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive according to claim 2, characterized in that, The organic solvent is selected from at least one of ethanol, isopropanol and acetone. The in-situ carbon-coated Li5FeO4 precursor and Nb2O5 powder are dispersed in the organic solvent by ultrasound and / or stirring to form a uniform suspension.

8. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplementary additive according to claim 7, characterized in that, The specific action of the drying process is as follows: the uniform suspension is stirred and evaporated in a water bath at a temperature of 80°C to obtain the composite precursor powder.

9. The method for preparing a carbon and Nb₂O₅ composite-coated Li₅FeO₄ lithium supplement additive according to claim 2, characterized in that, In step S400, the process conditions for the second calcination are: the heating rate is controlled at 2~5℃ / min, the target calcination temperature is 350~550℃, and the holding time at the target calcination temperature is 2~6h; the target calcination temperature is 400~500℃.

10. The method for preparing a carbon and Nb2O5 composite-coated Li5FeO4 lithium supplement additive according to any one of claims 2-9 is applied to lithium supplement additives.

Citation Information

Patent Citations

  • Lithium ferrite lithium supplement agent, positive electrode material, positive electrode plate and secondary battery

    CN119742350A